Method of processing single crystal silicon wafer

By forming peeling layers within single-crystal silicon wafers along specific crystal orientations, the method addresses the challenges of crack propagation and device damage, achieving efficient and timely separation with reduced grinding needs.

KR103046623B1Active Publication Date: 2026-11-10DISCO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020220089523
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-30
Filing Date
2022-07-20
Publication Date
2026-11-10
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

The existing methods for forming peeling layers inside single-crystal silicon wafers to facilitate separation using a laser beam result in cracks that are more likely to propagate perpendicular to the wafer surface, increasing processing time and the risk of device damage.

Method used

A method involving the formation of peeling layers within the single-crystal silicon wafer by irradiating a laser beam along specific crystal orientations, specifically parallel to the crystal plane {100}, reducing the perpendicular component of crack propagation and increasing the parallel component, thereby minimizing processing time and device damage.

Benefits of technology

The method shortens processing time and reduces the likelihood of device damage by aligning crack propagation parallel to the wafer surface, allowing for efficient separation with reduced grinding requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022075745028-PAT00011_ABST
    Figure 112022075745028-PAT00011_ABST
Patent Text Reader

Abstract

(Problem) A method for processing a single-crystal silicon wafer is provided that reduces processing time and the probability of device damage when separating the wafer using the peeling layer formed inside the wafer as a separation point after forming the peeling layer. (Solution) For a single-crystal silicon wafer manufactured such that a specific crystal plane (e.g., crystal plane (100)) included in crystal plane {100} is exposed on each of the surface and back sides, a laser beam is irradiated along a first direction that is parallel to the specific crystal plane and also has an angle of 5° or less with respect to a specific crystal orientation (e.g., crystal orientation [010]) included in crystal orientation <100>, thereby forming a peeling layer that serves as a separation point between the surface side and the back side of the single-crystal silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for processing a single-crystal silicon wafer, wherein a peeling layer is formed inside the single-crystal silicon wafer, and the single-crystal silicon wafer is separated using the peeling layer as a separation point. Background Technology

[0002] A chip of a semiconductor device (hereinafter simply referred to as "device") is generally manufactured using a disc-shaped single-crystal silicon wafer (hereinafter simply referred to as "wafer"). Specifically, this wafer is divided into multiple regions by a grid-shaped line of planned division, and a device is formed on the surface side of each region. Then, a chip is manufactured by dividing this wafer along the line of planned division.

[0003] In addition, through-silicon vias (TSVs) may be formed on the wafer for the purpose of high integration of a package containing multiple chips. In this package, electrodes included in different chips can be electrically connected, for example, through the TSVs.

[0004] TSVs are formed on a wafer in the following sequence, for example. First, a groove is formed on the surface side of the wafer. Next, a TSV is formed in this groove. Next, the surface side of the wafer is bonded to a support wafer. Next, the back side of the wafer is ground until the TSV is exposed on the back side of the wafer.

[0005] Here, in the case of a wafer, the outer edge is often chamfered for purposes such as preventing cracks. Then, if the back side of the wafer with the chamfered outer edge is ground until the wafer thickness is less than half, the back side of this outer edge takes on a shape similar to a knife edge.

[0006] In this case, stress is concentrated on the back side of the outer periphery area during wafer grinding, making the wafer prone to cracking, which may lead to a decrease in the yield of chips obtained from the wafer. Therefore, it has been proposed to perform partial removal of the surface side of the outer periphery area (so-called edge trimming) prior to grinding the back side of such a wafer (see, for example, Patent Document 1).

[0007] Accordingly, at the point when the remainder on the back side of the outer periphery is removed by grinding, the side of the wafer becomes generally perpendicular to the surface and the back side. Therefore, stress concentration does not occur on the back side of the outer periphery during the grinding of the wafer, and the wafer does not crack easily. As a result, the decrease in chip yield can be suppressed.

[0008] However, if the back side of the wafer is ground after edge trimming until the TSV is exposed on the back side of the wafer, the amount of wafer ground increases, and the amount of wear on the grinding wheel required to grind the wafer increases. In this case, the cost of chips or packages manufactured using this wafer increases, and there is a concern that the processing may be prolonged.

[0009] Taking these points into consideration, a method has been proposed in which a formed focusing point is positioned inside the wafer and a laser beam having a wavelength that transmits the wafer is irradiated onto the wafer to form a peeling layer inside the wafer, and then the wafer is separated using this peeling layer as a separation point (see, for example, Patent Document 2).

[0010] In this method, first, a laser beam is irradiated onto a first annular region of the wafer where diffuse reflection does not occur when the laser beam is irradiated (specifically, an annular region inside the chamfered outer region). Accordingly, a peeling layer (cylindrical peeling layer) is formed, which serves as a separation point between the region where the device is formed on the wafer and the outer region.

[0011] Next, a laser beam is irradiated onto a second region of the wafer where diffuse reflection does not occur when the laser beam is irradiated (specifically, a circular region inside the chamfered outer region). Accordingly, a peeling layer (a disc-shaped peeling layer) is formed, which serves as a separation point between the front side and the back side of the wafer.

[0012] Next, by applying an external force to this wafer, the wafer is separated from the cylindrical peeling layer and the disc-shaped peeling layer. That is, the outer periphery is separated from the region where the device of the wafer is formed, and the back side is separated from the surface side of this wafer.

[0013] When the wafer is separated in this way, the amount of wafer grinding required until the TSV is exposed on the back side of the wafer can be reduced, and the amount of wear on the grinding wheel required to grind the wafer can be reduced. As a result, the increase in cost of chips or packages manufactured using this wafer can be suppressed, and the time required for grinding the wafer can be shortened. Prior art literature

[0014] Japanese Published Patent Application No. 2007-158239 Japanese Published Patent Application No. 2020-136442 The problem to be solved

[0015] The peeling layer described above is composed of a modified region in which the crystal structure of the single-crystal silicon constituting the wafer is disrupted, and cracks extending from this modified region. Specifically, when the laser beam described above is irradiated onto the wafer, a modified region is formed inside the wafer centered on the focusing point of the laser beam. Furthermore, within this modified region, cracks extend along a predetermined crystal plane of the single-crystal silicon constituting the wafer.

[0016] Here, single-crystal silicon is generally most prone to cleavage in a specific crystal plane included in crystal plane {111}. For example, for a wafer manufactured such that a specific crystal plane (e.g., crystal plane (100)) included in crystal plane {100} is exposed on each of the front and back surfaces, if a laser beam is irradiated along a crystal orientation (e.g., crystal orientation

[0011] ) parallel to the specific crystal plane among the specific crystal orientations included in crystal orientation <110>, many cracks extending from the modified region along the specific crystal plane (e.g., crystal plane (111)) included in crystal plane {111} occur.

[0017] And, the acute angle formed by a specific crystal plane (e.g., crystal plane (100)) included in the crystal plane {100} of single-crystal silicon and a specific crystal plane (e.g., crystal plane (111)) included in the crystal plane {111} is approximately 54.7°. Therefore, when a laser beam is irradiated onto a wafer as described above, many cracks extending from the modification region occur in a direction tilted approximately 54.7° with respect to the surface or back surface of the wafer.

[0018] That is, if the direction in which such cracks extend is decomposed into a component parallel to the surface and back side of the wafer (parallel component) and a component perpendicular to it (vertical component), the vertical component becomes larger than the parallel component. Therefore, when a peeling layer (disk-shaped peeling layer) that serves as a separation point between the surface side and the back side of the wafer is formed by irradiating the wafer with a laser beam as described above, there is a risk that the following problems may occur.

[0019] First, in this case, since the parallel component in the direction of crack extension is relatively small, it is necessary to narrow the gap between adjacent modified regions in order to connect adjacent modified regions through the crack. And, when narrowing the gap between adjacent modified regions, it is necessary to increase the processing time (laser beam irradiation time) required to form a disc-shaped peeling layer.

[0020] Furthermore, in this case, since the perpendicular component of the crack's propagation direction is relatively large, there is a risk that the crack will propagate from the disc-shaped release layer toward the wafer surface, potentially causing device damage. Additionally, while forming the disc-shaped release layer at a position sufficiently spaced from the wafer surface can reduce the probability of device damage, this results in an increased amount of grinding required when the wafer is subsequently ground.

[0021] Taking the above points into consideration, the objective of the present invention is to provide a processing method for a single-crystal silicon wafer that can reduce the processing time and the probability of device damage when separating the wafer using the peeling layer as a separation point after forming a peeling layer inside the wafer. means of solving the problem

[0022] According to the present invention, for a single-crystal silicon wafer manufactured such that a specific crystal plane included in a crystal plane {100} is exposed on each of the surface and back surfaces, and furthermore, a plurality of devices are formed on the surface side and the outer periphery region is chamfered, a focusing point formed is positioned inside the single-crystal silicon wafer, and a laser beam having a wavelength that transmits single-crystal silicon is irradiated to form a peeling layer inside the single-crystal silicon wafer, and then the single-crystal silicon wafer is separated using the peeling layer as a separation point, the method comprises: a bonding step of bonding the surface side of the single-crystal silicon wafer to the surface side of a support wafer; a first peeling layer forming step of forming a first peeling layer that serves as a separation point between the region where the plurality of devices are formed and the outer periphery region of the single-crystal silicon wafer by irradiating the laser beam from the back side of the single-crystal silicon wafer onto an annular first region inside the outer periphery region of the single-crystal silicon wafer, and the single-crystal silicon A second peeling layer forming step for forming a second peeling layer that serves as a separation point between the surface side and the back side of the single-crystal silicon wafer by irradiating a laser beam from the back side of the single-crystal silicon wafer with respect to a second region inward from the outer periphery region of the wafer, and a separation step for separating the single-crystal silicon wafer with the first peeling layer and the second peeling layer as separation points by applying an external force to the single-crystal silicon wafer after performing the bonding step, the first peeling layer forming step, and the second peeling layer forming step, wherein in the second peeling layer forming step, the single-crystal silicon wafer and the light collection point are moved relatively along a first direction that is parallel to the specific crystal plane and has an angle of 5° or less with respect to a specific crystal orientation included in the crystal orientation <100>,A method for processing a single-crystal silicon wafer in which a second peeling layer is formed is provided by repeatedly performing a laser beam irradiation step of irradiating the laser beam onto a straight line area along the first direction included in the second region, and a output transfer step of moving the internal position of the single-crystal silicon wafer, where the focusing point is formed by the irradiation of the laser beam, along a second direction that is parallel to the specific crystal plane and also orthogonal to the first direction.

[0023] In addition, it is preferable that the first peeling layer forming step be performed before the second peeling layer forming step.

[0024] In addition, it is preferable that the second region be located further inward than the first region.

[0025] In addition, in the step of forming the first peeling layer, it is preferable that the first peeling layer be formed so as not to reach the back side of the single-crystal silicon wafer.

[0026] In addition, in the step of forming the first peeling layer, it is preferable to form the first peeling layer by irradiating the laser beam such that the focusing point to be formed approaches the surface of the single-crystal silicon wafer as it approaches the outer periphery, so that the first bottom surface is located on the surface side of the single-crystal silicon wafer and the second bottom surface, which has a shorter diameter than the first bottom surface, follows the side of the frustum located inside the single-crystal silicon wafer. Effects of the invention

[0027] In the present invention, for a single-crystal silicon wafer manufactured such that a specific crystal plane (e.g., crystal plane (100)) included in crystal plane {100} is exposed on each of the surface and back sides, a laser beam is irradiated along a first direction that is parallel to the specific crystal plane and has an angle of 5° or less with respect to a specific crystal orientation (e.g., crystal orientation

[0010] ) included in crystal orientation <100>, thereby forming a peeling layer (second peeling layer) that serves as a separation point between the surface side and the back side of the single-crystal silicon wafer.

[0028] In this case, cracks extending from the modified region are more likely to follow a specific crystal plane (e.g., crystal plane (101)) included in crystal plane {n10} (n is a natural number less than or equal to 10) than to follow a specific crystal plane (e.g., crystal plane (111)) included in crystal plane {111}. Also, the acute angle formed by a specific crystal plane included in crystal plane {100} and a specific crystal plane included in crystal plane {n10} is 45° or less.

[0029] Accordingly, in the present invention, for a single-crystal silicon wafer manufactured such that a specific crystal plane included in the crystal plane {100} is exposed on each of the surface and back surfaces, a second peeling layer is formed by irradiating a laser beam along a specific crystal orientation (e.g., crystal orientation

[0011] ) that is parallel to the said specific crystal plane and also included in the crystal orientation <110>, and the component parallel to the surface and back surface of the wafer in the direction in which the crack is propagating (parallel component) is increased, and the component perpendicular (perpendicular component) is decreased.

[0030] Accordingly, in the present invention, since the parallel component in the direction of crack extension increases, the spacing between adjacent modified regions can be extended. As a result, the travel distance (index) in the output transfer step can be extended, and the processing time (laser beam irradiation time) required to form a peeling layer serving as a separation point between the surface side and the back side of the wafer can be shortened.

[0031] In addition, in the present invention, since the vertical component of the direction in which the crack extends is reduced, it becomes difficult for the crack to extend from this peeling layer toward the surface side of the wafer. As a result, the probability of the device being damaged can be reduced when separating the surface side and the back side of the wafer. Brief explanation of the drawing

[0032] FIG. 1(A) is a top view schematically showing an example of a wafer, and FIG. 1(B) is a cross-sectional view schematically showing an example of a wafer. Figure 2 is a flowchart schematically illustrating an example of a wafer processing method. FIG. 3 is a cross-sectional view schematically showing the surface side of a wafer being bonded to the surface side of a supporting wafer. FIG. 4 is a perspective view schematically showing an example of a laser processing device. Figure 5 is a schematic diagram showing the progression of a laser beam in a laser beam irradiation unit. Figure 6 is a partial cross-sectional side view schematically showing a laser beam being irradiated onto a rotating wafer. Figure 7 is a flowchart schematically illustrating an example of a second peeling layer formation step. FIG. 8 is a partial cross-sectional side view schematically showing a laser beam being irradiated onto a wafer moving along the X-axis direction. FIG. 9 is a cross-sectional view schematically showing adjacent peeling layers formed inside an ingot. Figures 10(A) and 10(B) are each schematic cross-sectional side views illustrating the separation of wafers. FIG. 11 is a partial cross-sectional side view schematically showing a laser beam being irradiated onto a rotating wafer. Figure 12 is a graph showing the width of the peeling layer formed inside the wafer when a laser beam is irradiated onto a straight line region following different crystal orientations. FIG. 13 is a top view schematically showing an example of a wafer deformation. Figures 14(A) and 14(B) are each schematic cross-sectional side views showing the separation of a region where a plurality of devices are formed on a wafer and an outer region. Figures 15(A) and 15(B) are each schematic cross-sectional side views showing the separation of the front side and the back side of the wafer. Specific details for implementing the invention

[0033] An embodiment of the present invention will be described with reference to the attached drawings. FIG. 1(A) is a top view schematically showing an example of a wafer (single-crystal silicon wafer), and FIG. 1(B) is a cross-sectional view schematically showing an example of a wafer (single-crystal silicon wafer). In addition, FIG. 1(A) also shows the crystal orientation of the single-crystal silicon constituting the wafer.

[0034] The wafer (11) shown in FIG. 1(A) and FIG. 1(B) is made of cylindrical single-crystal silicon in which a specific crystal plane (here, for convenience, referred to as crystal plane (100)) included in the crystal plane {100} is exposed on the surface (11a) and the back surface (11b), respectively. That is, the wafer (11) is made of cylindrical single-crystal silicon in which the vertical line (crystal axis) of the surface (11a) and the back surface (11b), respectively, follows the crystal orientation

[0100] .

[0035] Additionally, although the wafer (11) is manufactured such that the crystal plane (100) is exposed on each of the surface (11a) and the back surface (11b), the surface (11a) and the back surface (11b) may each be a surface that is slightly inclined from the crystal plane (100) due to processing errors during manufacturing, etc. Specifically, the surface (11a) and the back surface (11b) of the wafer (11) may each be a surface in which the acute angle formed between the surface (11a) and the crystal plane (100) is 1° or less.

[0036] That is, the crystal axis of the wafer (11) may follow a direction in which the acute angle formed between it and the crystal orientation

[0100] is 1° or less. Also, a notch (13) is formed on the side (11c) of the wafer (11), and the center of the wafer (11) is located on a specific crystal plane (here, for convenience, referred to as crystal orientation

[0011] ) that is included in the crystal orientation <110> when viewed from the notch (13).

[0037] Additionally, the wafer (11) is divided into multiple regions by multiple intersecting lines of division, and on the surface (11a) side of each region, a device (15) such as an IC (Integrated Circuit) and LSI (Large Scale Integration), a semiconductor memory or a CMOS (Complementary Metal Oxide Semiconductor) image sensor is formed.

[0038] Additionally, a groove for installing a TSV may be formed on the surface (11a) side of the wafer (11). Also, the outer periphery of the wafer (11) is chamfered. That is, the side (11c) of the wafer (11) is curved so as to be convex outward. Also, no device (15) is formed on the outer periphery of the wafer (11). That is, the area where a plurality of devices (15) of the wafer (11) are formed is surrounded by the outer periphery.

[0039] FIG. 2 is a flowchart schematically illustrating an example of a wafer processing method. Specifically, in this method, a concentrated point formed is positioned inside the wafer (11), and a laser beam having a wavelength that passes through the wafer (11) is irradiated onto the wafer (11) to form a peeling layer inside the wafer (11), and then the wafer (11) is separated using this peeling layer as a separation point.

[0040] Specifically, in this method, first, the surface (11a) side of the wafer (11) is bonded to the surface side of the support wafer (bonding step: S1). FIG. 3 is a cross-sectional view schematically showing the bonding of the surface (11a) side of the wafer (11) to the surface side of the support wafer. In addition, the support wafer (17) bonded to the wafer (11) has, for example, the same shape as the wafer (11).

[0041] This support wafer (17), like the wafer (11), may be made of single-crystal silicon, and may also have a plurality of devices formed on its surface (17a). Additionally, an adhesive (19), such as an acrylic adhesive or an epoxy adhesive, is formed on the surface (17a) of the support wafer (17).

[0042] Then, in the bonding step (S1), while supporting the back side (17b) of the support wafer (17), the surface (11a) of the wafer (11) is pressed firmly against the surface (17a) of the support wafer (17) through an adhesive (19). Accordingly, a bonded wafer is formed in which the surface (11a) side of the wafer (11) is bonded to the surface (17a) side of the support wafer (17).

[0043] Next, a peeling layer is formed inside the wafer (11) using a laser processing device. FIG. 4 is a schematic perspective view showing an example of a laser processing device used to form a peeling layer inside the wafer (11). In addition, the X-axis direction (left-right direction) and the Y-axis direction (front-back direction) shown in FIG. 4 are directions that are orthogonal to each other on a horizontal plane, and the Z-axis direction (up-down direction) is a direction orthogonal to each of the X-axis direction and the Y-axis direction (vertical direction).

[0044] The laser processing device (2) shown in FIG. 4 has a support (4) that supports each component. A horizontal movement mechanism (6) is disposed on the upper surface of the support (4). The horizontal movement mechanism (6) has a pair of Y-axis guide rails (8) that are fixed to the upper surface of the support (4) and extend along the Y-axis direction.

[0045] On the upper side of a pair of Y-axis guide rails (8), a Y-axis moving plate (10) is connected in a manner that allows it to slide along the pair of Y-axis guide rails (8). Additionally, a screw shaft (12) extending along the Y-axis direction is arranged between the pair of Y-axis guide rails (8). A motor (14) for rotating the screw shaft (12) is connected to the front end (one end) of the screw shaft (12).

[0046] Additionally, on the surface of the screw shaft (12) where a spiral groove is formed, a nut portion (not shown) is formed to accommodate a plurality of balls rolling on the surface of the rotating screw shaft (12), and a ball screw is configured. That is, when the screw shaft (12) rotates, a plurality of balls circulate within the nut portion, and the nut portion moves along the Y-axis direction.

[0047] In addition, this nut part is fixed to the lower side of the Y-axis moving plate (10). Therefore, when the screw shaft (12) is rotated by the motor (14), the Y-axis moving plate (10) moves along the Y-axis direction together with the nut part. Also, a pair of X-axis guide rails (16) extending along the X-axis direction are fixed to the upper surface of the Y-axis moving plate (10).

[0048] On the upper side of a pair of X-axis guide rails (16), an X-axis moving plate (18) is connected in a manner that allows it to slide along the pair of X-axis guide rails (16). Additionally, a screw shaft (20) extending along the X-axis direction is disposed between the pair of X-axis guide rails (16). A motor (22) for rotating the screw shaft (20) is connected to one end of the screw shaft (20).

[0049] Additionally, on the surface of the screw shaft (20) where a spiral groove is formed, a nut portion (not shown) is formed to accommodate a plurality of balls rolling on the surface of the rotating screw shaft (20), and a ball screw is configured. That is, when the screw shaft (20) rotates, a plurality of balls circulate within the nut portion, and the nut portion moves along the X-axis direction.

[0050] In addition, this nut part is fixed to the lower side of the X-axis moving plate (18). Therefore, when the screw shaft (20) is rotated by the motor (22), the X-axis moving plate (18) moves along the X-axis direction together with the nut part.

[0051] A cylindrical table support (24) is disposed on the upper side of the X-axis moving plate (18). A holding table (26) for holding the bonded wafer described above is disposed on the upper side of this table support (24). This holding table (26) has, for example, a circular upper surface (holding surface) parallel to the X-axis direction and the Y-axis direction, and a porous plate (26a) is exposed on this holding surface.

[0052] Additionally, a rotational driving source (not shown), such as a motor, is connected to the lower part of the table support (24). When this rotational driving source operates, the holding table (26) passes through the center of the holding surface and rotates with a straight line parallel to the Z-axis direction as the axis of rotation. Also, when the horizontal movement mechanism (6) described above operates, the holding table (26) moves along the X-axis direction and / or the Y-axis direction.

[0053] Additionally, the porous plate (26a) is connected to a suction source (not shown), such as a vacuum pump, through a channel formed inside the holding table (26). When this suction source operates, negative pressure is generated in the space near the holding surface of the holding table (26).

[0054] Additionally, a support structure (30) having sides that are generally parallel to the Y-axis and Z-axis directions is installed on the rear area of ​​the support structure (4). A vertical movement mechanism (32) is disposed on the sides of this support structure (30). The vertical movement mechanism (32) has a pair of Z-axis guide rails (34) that are fixed to the sides of the support structure (30) and extend along the Z-axis direction.

[0055] A Z-axis moving plate (36) is connected to the surface side of a pair of Z-axis guide rails (34) in a manner that allows it to slide along the pair of Z-axis guide rails (34). Additionally, a screw shaft (not shown) extending along the Z-axis direction is arranged between the pair of Z-axis guide rails (34). A motor (38) for rotating the screw shaft is connected to the upper end (one end) of this screw shaft.

[0056] Additionally, on the surface of the screw shaft where a helical groove is formed, a nut portion (not shown) is formed to accommodate a plurality of balls that roll on the surface of the rotating screw shaft, and a ball screw is configured. That is, when this screw shaft rotates, a plurality of balls circulate within the nut portion, causing the nut portion to move along the Z-axis direction.

[0057] In addition, this nut part is fixed to the back side of the Z-axis moving plate (36). Therefore, when the screw shaft placed between the pair of Z-axis guide rails (34) is rotated by the motor (38), the Z-axis moving plate (36) moves along the Z-axis direction together with the nut part.

[0058] A support member (40) is fixed to the surface side of the Z-axis moving plate (36). This support member (40) supports a part of the laser beam irradiation unit (42). FIG. 5 is a schematic diagram showing the appearance of a laser beam (LB) traveling in the laser beam irradiation unit (42). In FIG. 5, a part of the components of the laser beam irradiation unit (42) is shown as a functional block.

[0059] The laser beam irradiation unit (42) has a laser oscillator (44) fixed to the support (4). This laser oscillator (44) has, for example, Nd:YAG as a laser medium and emits a laser beam (LB) of a wavelength (e.g., 1342 nm) that passes through the wafer (11). This laser beam (LB) is, for example, a pulsed laser beam with a frequency of 60 kHz.

[0060] Then, the laser beam (LB) is supplied to the spatial light modulator (48) after its output is adjusted in the attenuator (46). In this spatial light modulator (48), the laser beam (LB) is branched. For example, the spatial light modulator (48) branches the laser beam (LB) adjusted in the attenuator (46) so that the laser beam (LB) emitted from the irradiation head (52) described later forms a plurality of concentrated points that have different positions (coordinates) in a plane (XY coordinate plane) parallel to the X-axis and Y-axis directions and / or positions (heights) in the Z-axis direction.

[0061] Also, the laser beam (LB) branched from the spatial light modulator (48) is reflected by the mirror (50) and guided to the irradiation head (52). The irradiation head (52) is equipped with a focusing lens (not shown) for focusing the laser beam (LB). Then, the laser beam (LB) focused by this focusing lens is emitted toward the holding surface of the holding table (26).

[0062] Additionally, as shown in FIG. 4, the investigation head (52) is formed at the front end of the cylindrical housing (54). A support member (40) is fixed to the rear side of the housing (54). Additionally, an imaging unit (56) is fixed to the front side of the housing (54).

[0063] This imaging unit (56) has, for example, a light source such as an LED (Light Emitting Diode), an objective lens, and an imaging element such as a CCD (Charge Coupled Device) image sensor or a CMOS image sensor.

[0064] And, when the vertical movement mechanism (32) described above operates, the laser beam irradiation unit (42) and the imaging unit (56) move along the Z-axis direction. In addition, a cover (not shown) covering the components described above is installed on the base (4). A touch panel (58) is placed on the front of this cover.

[0065] This touch panel (58) is composed of an input device, such as a capacitive or resistive touch sensor, and a display device, such as a liquid crystal display or an organic EL (Electro Luminescence) display, and functions as a user interface.

[0066] When forming a peeling layer inside a wafer (11) using a laser processing device (2), first, a bonded wafer is placed on a holding table (26) so that the center of the holding surface of the holding table (26) aligns with the center of the back surface (17b) of the support wafer (17). Then, a suction source communicating with the holding table (26) is operated so that the bonded wafer is held by the holding table (26).

[0067] Next, the imaging unit (56) captures the back side (11b) of the wafer (11) of the bonded wafer to form an image. Then, referring to this image, the horizontal movement mechanism (6) is operated so that the irradiation head (52) of the laser beam irradiation unit (42) is positioned just above an area slightly inside the outer periphery of the wafer (11).

[0068] Also, by referring to this image, the holding table (26) may be rotated so that the crystal orientation

[0010] of the single-crystal silicon constituting the wafer (11) becomes parallel to the X-axis direction, and the crystal orientation

[0001] becomes parallel to the Y-axis direction, and the rotation driving source connected to the lower part of the table support (24) may be operated.

[0069] Next, by irradiating a laser beam (LB) onto a first annular region that is inner to the outer region of the wafer (11), a first peeling layer is formed that serves as a separation point between the region where a plurality of devices (15) of the wafer (11) are formed and the outer region (first peeling layer formation step: S2).

[0070] In this first peeling layer forming step (S2), a laser beam (LB) is irradiated onto a first annular region inside the outer circumference of the wafer (11), and a holding table (26) that holds the wafer (11) is rotated with the support wafer (17) interposed therebetween. FIG. 6 is a partial cross-sectional side view schematically showing the laser beam (LB) being irradiated onto the rotating wafer (11).

[0071] Specifically, in this first peeling layer forming step (S2), a laser beam (LB) branched to form a plurality (e.g., 2 to 10) of different positions (heights) in the Z-axis direction is irradiated onto the wafer (11).

[0072] These multiple light-gathering points are, for example, positioned such that the lowest light-gathering point is positioned slightly higher than the surface (11a) of the wafer (11), and the highest light-gathering point is positioned at an intermediate height between the surface (11a) and the back surface (11b) of the wafer (11). Additionally, the multiple light-gathering points are arranged such that their positions (heights) in the Z-axis direction are spaced at equal intervals (for example, every 5 μm to 15 μm).

[0073] In this case, a modified region (21) with a disordered crystal structure is formed inside the wafer (11) centered around each of the multiple light-gathering points. Additionally, in each of the multiple modified regions (21), a crack (23) extends to connect an adjacent pair of modified regions (21).

[0074] Accordingly, a peeling layer comprising a plurality of modified regions (21) and a crack (23) advancing from each of the plurality of modified regions (21) is formed inside the wafer (11). Subsequently, while irradiating the wafer (11) with a laser beam (LB), a rotation drive source connected to the lower part of the table support (24) is operated to rotate the holding table (26) holding the bonded wafer by one rotation.

[0075] As a result, a peeling layer (first peeling layer) is formed between the region where a plurality of devices (15) of the wafer (11) are formed and the outer region. This first peeling layer has a cylindrical shape that follows the side of a cylinder, for example, with the lower bottom surface located on the surface (11a) side of the wafer (11) and the upper bottom surface located inside the wafer (11).

[0076] Next, by irradiating a second region inside the outer region of the wafer (11) with a laser beam (LB), a second peeling layer is formed that serves as a separation point between the surface (11a) side and the back side (11b) side of the wafer (11) (second peeling layer formation step: S3). FIG. 7 is a flowchart schematically showing an example of the second peeling layer formation step (S3).

[0077] In this second peeling layer formation step (S3), first, a laser beam (LB) is irradiated onto a straight line area along the crystal orientation

[0010] of the single-crystal silicon constituting the wafer (11) (laser beam irradiation step: S31). For example, when the bonded wafer is held on a holding table (26) while the crystal orientation

[0010] is parallel to the X-axis direction, the laser beam (LB) is irradiated onto the wafer (11) while moving the holding table (26) along the X-axis direction.

[0078] FIG. 8 is a partial cross-sectional side view schematically showing a laser beam (LB) being irradiated onto a wafer (11) moving along the X-axis direction. In this laser beam irradiation step (S31), a laser beam (LB) branched to form a plurality (e.g., 2 to 10) of different positions (coordinates) in the Y-axis direction is irradiated onto the wafer (11).

[0079] These multiple light-gathering points are positioned at the same height as the uppermost modified region (21) among the multiple modified regions (21) included in the first peeling layer described above. Also, the multiple light-gathering points are arranged such that their positions (coordinates) in the Y-axis direction are spaced equally (e.g., every 5 μm to 15 μm).

[0080] In this case, similar to the first peeling layer forming step (S2), a plurality of modified regions (21) and a crack (23) advancing from each of the plurality of modified regions (21) are formed inside the wafer (11). Then, while irradiating the wafer (11) with a laser beam (LB), a horizontal movement mechanism (6) is operated to move a holding table (26) holding the bonded wafer along the X-axis direction.

[0081] As a result, a peeling layer (25) is formed in a straight line along the X-axis direction that is included in a second region that is inner to the outer region of the wafer (11). Here, most of the cracks (23) included in this peeling layer (25) extend along the crystal plane (k01) (where k is an integer whose absolute value is 10 or less, excluding 0). That is, when a laser beam (LB) is irradiated onto the wafer (11) in this way, the cracks (23) are more likely to extend along the following crystal planes.

[0082]

[0083]

[0084] And, the acute angle formed by the crystal plane (100) and the crystal plane (k01) exposed on the surface (11a) and back surface (11b) of the wafer (11) is 45° or less. Therefore, if the direction in which this crack (23) extends is decomposed into a component parallel to the surface (11a) and back surface (11b) of the wafer (11) (parallel component) and a component perpendicular to it (perpendicular component), the parallel component becomes larger than the perpendicular component.

[0085] Next, the holding table (26) is moved along the crystal orientation

[0001] of the single-crystal silicon constituting the wafer (11) (output transfer step (S32)). For example, if the bonded wafer is held on the holding table (26) while the crystal orientation

[0001] of the single-crystal silicon constituting the wafer (11) is parallel to the Y-axis direction, the holding table (26) is moved along the Y-axis direction.

[0086] Next, the laser beam irradiation unit (42) and the horizontal movement mechanism (6) are operated so that a peeling layer (25) is formed in a straight line area parallel to a straight line area where a peeling layer (25) has already been formed. That is, the laser beam irradiation step (S31) is performed again. FIG. 9 is a cross-sectional view schematically showing adjacent peeling layers (25) formed inside the wafer (11) by performing the laser beam irradiation step (S31) twice.

[0087] In this case, a peeling layer (25) (peeling layer (25-1)) formed in the first laser beam irradiation step (S31) is formed in the interior of the wafer (11) and is also spaced apart from the peeling layer (25-1) in the Y-axis direction. Additionally, the output transfer step (S32) and the laser beam irradiation step (S31) are repeated so that the peeling layer (25) is formed over the entire area of ​​the second region that is inner to the outer periphery region of the wafer (11) (from the region on one end side to the region on the other end side in the Y-axis direction).

[0088] Then, when a peeling layer (25) is formed over the entire second region that is inner to the outer region of the wafer (11) (step (S33): e.g.), the second peeling layer formation step (S3) is completed. As a result, a peeling layer (second peeling layer) is formed between the surface (11a) side and the back side (11b) side of the wafer (11). This second peeling layer has a disc-shaped form that follows the upper bottom surface of a cylinder having a side that follows the first peeling layer described above, for example.

[0089] In the method shown in FIG. 2, after performing the first peeling layer forming step (S2) and the second peeling layer forming step (S3), the wafer (11) is separated by applying an external force to the wafer (11) with the first peeling layer and the second peeling layer as separation points (separation step: S4).

[0090] FIGS. 10(A) and FIGS. 10(B) are each partial cross-sectional side views schematically illustrating the separation of a wafer (11). This separation step (S4) is performed, for example, in a separation device (60) shown in FIGS. 10(A) and FIGS. 10(B). This separation device (60) has a holding table (62) that holds a bonded wafer comprising a wafer (11) having a first peeling layer and a second peeling layer formed thereon.

[0091] This holding table (62) has a circular upper surface (holding surface), and a porous plate (not shown) is exposed on this holding surface. In addition, this porous plate is in communication with a suction source (not shown), such as a vacuum pump, through a flow path formed inside the holding table (62). And when this suction source operates, negative pressure is generated in the space near the holding surface of the holding table (62).

[0092] Additionally, a separation unit (64) is formed above the maintenance table (62). This separation unit (64) has a cylindrical support member (66). For example, a ball screw type lifting mechanism (not shown) is connected to the upper part of this support member (66), and the separation unit (64) is raised by operating this lifting mechanism.

[0093] Additionally, the lower end of the support member (66) is fixed to the center of the upper part of the disc-shaped gripping claw support (68). On the lower side of the outer circumference area of ​​this gripping claw support (68), a plurality of gripping claws (70) are formed at generally equal intervals along the circumference direction of the gripping claw support (68). This gripping claw (70) has a plate-shaped erected part (70a) that extends downward.

[0094] The upper part of this erection section (70a) is connected to an actuator, such as an air cylinder, built into the gripping claw support (68), and by operating this actuator, the gripping claw (70) moves along the diameter direction of the gripping claw support (68). Also, on the inner surface of the lower part of this erection section (70a), a plate-shaped claw section (70b) is formed that extends toward the center of the gripping claw support (68) and becomes thinner as it approaches the center of the gripping claw support (68).

[0095] In the separation device (60), for example, the separation step (S4) is performed in the following order. Specifically, first, the bonded wafer is placed on the holding table (62) so that the center of the back surface (17b) of the supporting wafer (17) of the bonded wafer including the wafer (11) on which the first peeling layer and the second peeling layer are formed aligns with the center of the holding surface of the holding table (62).

[0096] Next, a suction source communicating with a porous plate exposed on the holding surface is actuated so that the bonded wafer is held by the holding table (62). Next, an actuator is actuated to position each of the plurality of gripping claws (70) radially outward of the gripping claw support (68).

[0097] Next, a lifting mechanism is operated to position the tip of each claw portion (70b) of a plurality of gripping claws (70) at a height corresponding to the adhesive (19) of the bonded wafer. Next, an actuator is operated to bring the claw portion (70b) into contact with the bonded wafer. Next, a lifting mechanism is operated to raise the claw portion (70b) (see FIG. 10(A)).

[0098] Accordingly, an upward external force, that is, an external force along the thickness direction of the wafer (11), is applied to the outer periphery of the wafer (11). As a result, the crack (23) included in the first peeling layer and the second peeling layer is further extended, so that the outer periphery of the wafer (11) is separated from the area where the plurality of devices (15) are formed, and also the surface (11a) side and the back side (11b) side are separated (see FIG. 10(B)).

[0099] In the above-described wafer processing method, a laser beam (LB) is irradiated along the crystal orientation

[0010] on a wafer (11) manufactured such that a crystal plane (100) is exposed on each of the surface (11a) and the back side (11b), thereby forming a peeling layer (second peeling layer) that serves as a separation point between the surface (11a) side and the back side (11b) side of the wafer (11).

[0100] In this case, the crack (23) extending from the modification region (21) tends to follow the crystal plane (k01) (where k is an integer with an absolute value of 10 or less, excluding 0). Also, the acute angle formed by the crystal plane (100) of the single-crystal silicon and the crystal plane (k01) is 45° or less. Therefore, in the processing method of this wafer, the component (parallel component) parallel to the surface (11a) and back surface (11b) of the wafer (11) in the direction in which the crack (23) extends is larger than the component (vertical component).

[0101] Accordingly, in the processing method of this wafer, the distance between adjacent modification regions (21) can be extended. As a result, the travel distance (index) in the output transfer step (S32) can be extended, and the processing time (irradiation time of the laser beam (LB)) required to form the peeling layer (25) which serves as the separation point between the surface (11a) side and the back side (11b) side of the wafer (11) can be shortened.

[0102] In addition, in the processing method of this wafer, it is difficult for the crack (23) to extend from the peeling layer (25) toward the surface (11a) side of the wafer (11). As a result, when separating the surface (11a) side and the back side (11b) side of the wafer (11), the probability of the device (15) being damaged can be reduced.

[0103] In addition, the wafer processing method described above is an embodiment of the present invention, and the present invention is not limited to the method described above. For example, in the present invention, after the first peeling layer and the second peeling layer are formed on the wafer (11), the surface (11a) side of the wafer (11) may be bonded to the surface (17a) side of the support wafer (17). That is, in the present invention, the bonding step (S1) may be performed after the first peeling layer formation step (S2) and the second peeling layer formation step (S3) are performed.

[0104] In addition, the structure of the laser processing device used in the present invention is not limited to the structure of the laser processing device (2) described above. For example, the present invention may be implemented using a laser processing device having a horizontal movement mechanism formed to move the irradiation head (52) of the laser beam irradiation unit (42) along the X-axis direction and / or the Y-axis direction, respectively.

[0105] That is, in the present invention, the holding table (26) that holds the bonded wafer including the wafer (11) and the irradiation head (52) of the laser beam irradiation unit (42) that emits the laser beam (LB) can move relatively along the X-axis direction and the Y-axis direction, respectively, and there is no limitation on the structure for that.

[0106] In addition, in the present invention, the order of the first peeling layer forming step (S2) and the second peeling layer forming step (S3) is not limited. That is, in the present invention, the first peeling layer forming step (S2) may be performed after the second peeling layer forming step (S3).

[0107] However, in the second peeling layer formation step (S3), if the disc-shaped second peeling layer is formed inside the wafer (11), there is a concern that it may become impossible or difficult to form a new peeling layer on the surface (11a) side of the wafer (11) rather than the second peeling layer.

[0108] Therefore, in the present invention, it is preferable to perform the second peeling layer formation step (S3) after performing the first peeling layer formation step (S2). Accordingly, a peeling layer (first peeling layer) that serves as a separation point between the region where a plurality of devices (15) of the wafer (11) are formed and the outer region can be reliably formed.

[0109] Alternatively, in the present invention, it is preferable that the second region where the second peeling layer of the wafer (11) is formed is located further inward than the first region where the first peeling layer is formed. Accordingly, even if the first peeling layer forming step (S2) is performed after the second peeling layer forming step (S3), the first peeling layer can be reliably formed.

[0110] In addition, in the first peeling layer forming step (S2) of the present invention, it is sufficient to form a first peeling layer that can function as a separation point between the region where a plurality of devices (15) of the wafer (11) are formed and the outer region, and the shape of the first peeling layer is not limited. For example, the first peeling layer may have a shape that follows the side of a cylinder, with the lower bottom surface located on the surface (11a) side of the wafer (11) and the upper bottom surface located on the back side (11b) side of the wafer (11).

[0111] That is, the first peeling layer may be formed to penetrate the surface (11a) and back surface (11b) of the wafer (11). However, if the first peeling layer has such a shape, there is a risk that the outer periphery of the wafer (11) may scatter as a cut material during the separation step (S4). Therefore, in the first peeling layer formation step (S2) of the present invention, it is preferable that the first peeling layer be formed so as not to reach the back surface (11b) of the wafer (11).

[0112] Additionally, the first peeling layer may have a shape that follows the side of a frustum, in which the lower bottom surface (first bottom surface) is located on the surface (11a) side of the wafer (11), and the upper bottom surface (second bottom surface), which has a diameter shorter than the lower bottom surface, is located inside the wafer (11). Such a first peeling layer is formed, for example, by irradiating a laser beam (LB) onto the wafer (11) such that the light-gathering point formed approaches the surface (11a) of the wafer (11) as it approaches the outer periphery region.

[0113] FIG. 11 is a partial cross-sectional side view schematically showing a laser beam (LB) being irradiated onto a rotating wafer (11) to form a first peeling layer having such a shape. Specifically, when forming such a first peeling layer, a laser beam (LB) is first irradiated onto the wafer (11) to form a plurality (e.g., 8) of condensing points, in each of the diameter direction (direction perpendicular to the Z-axis direction) and thickness direction (Z-axis direction) of the wafer (11), such that the positions of adjacent condensing points are offset by 10 μm inside the wafer (11).

[0114] In this case, a modified region (21) is formed inside the wafer (11) with the crystal structure of the material constituting the wafer (11) disturbed, centered on each of the multiple light-gathering points. That is, when viewed from a plane, multiple modified regions (21) are formed that are arranged in a straight line along the diameter direction of the wafer (11), and the acute angle formed between this straight line and the surface (11a) of the wafer (11) is 45°.

[0115] Additionally, the acute angle formed by the surface (11a) of the wafer (11) and the multiple modified regions (21) arranged in a straight line is not limited to 45°. That is, a laser beam (LB) may be irradiated onto the wafer (11) so that multiple points of light are formed such that the spacing in the diameter direction of adjacent points of light on the wafer (11) is different from the spacing in the thickness direction.

[0116] Additionally, from each of the plurality of modified regions (21), a crack (23) extends to connect an adjacent pair of modified regions (21). Accordingly, a peeling layer comprising the plurality of modified regions (21) and the crack (23) extending from each of the plurality of modified regions (21) is formed inside the wafer (11).

[0117] Next, while operating the laser beam irradiation unit (42), a rotation drive source connected to the lower part of the table support (24) is operated to rotate the holding table (26) that holds the bonded wafer by one rotation.

[0118] As a result, a peeling layer (first peeling layer) is formed along the side of a cone, with the lower bottom surface located on the surface (11a) of the wafer (11) and the upper bottom surface located inside the wafer (11), in a first annular region that is inner than the outer circumference region of the wafer (11).

[0119] When such a first peeling layer is formed, when separating the wafer (11) in the separation device (60) described above, the probability of the side of the region where a plurality of newly exposed devices (15) are formed and the inner side of the outer periphery region coming into contact with each other is reduced. Also, in this case, the crack (23) is more likely to extend from the first peeling layer in the direction along the side of the cone.

[0120] Therefore, in this case, the probability of the crack (23) extending toward the device (15) is reduced, and damage to the device (15) can be suppressed. In addition, when such a first peeling layer is formed, it becomes easier to manufacture a chip using an area close to the outer edge of the surface (11a) of the wafer (11). Therefore, in this case, the number of chips that can be manufactured from the wafer (11) can be increased.

[0121] In addition, in the first peeling layer forming step (S2) of the present invention, a laser beam (LB) may be irradiated onto the wafer (11) while operating a horizontal movement mechanism (6) and a vertical movement mechanism (32) in addition to or instead of a rotational driving source connected to the lower part of the table support (24). That is, not only the wafer (11) may be rotated, but a laser beam (LB) may also be irradiated onto the wafer (11) while changing the coordinates and height in the XY coordinate plane of the focusing point.

[0122] Additionally, in the first peeling layer formation step (S2) of the present invention, irradiation of multiple laser beams (LB) may be performed such that the positions of the focusing points are the same or close to each other. In this case, the size of the modified region (21) included in the peeling layer increases, and the crack (23) included in the peeling layer is further extended. Therefore, in this case, the separation of the wafer (11) in the separation step (S4) becomes easier.

[0123] In addition, in the first peeling layer forming step (S2) of the present invention, a laser beam (LB) may be irradiated onto the wafer (11) so that adjacent modified regions (21) are connected directly to each other rather than being connected via cracks (23). In this case, since the shape of the peeling layer can be determined without relying on the shape of the cracks (23) advancing from the modified regions (21), stable processing of the wafer (11) becomes possible.

[0124] In addition, in the laser beam irradiation step (S31) of the second peeling layer forming step (S3) of the present invention, the area where the laser beam (LB) is irradiated is not limited to a straight line area following the crystal orientation

[0010] of the single-crystal silicon constituting the wafer (11). For example, in this laser beam irradiation step (S31), the laser beam (LB) may be irradiated to a straight line area following the crystal orientation

[0001] .

[0125] In addition, when a laser beam (LB) is irradiated onto a wafer (11) in this manner, cracks (23) are more likely to spread on the crystal plane below.

[0126]

[0127]

[0128] In addition, in the present invention, a laser beam (LB) may be irradiated onto a straight line region that follows a direction slightly inclined from the crystal orientation

[0010] or crystal orientation

[0001] when viewed in a plane. This point will be explained with reference to FIG. 12.

[0129] FIG. 12 is a graph showing the width of the peeling layer formed inside the wafer (11) when a laser beam (LB) is irradiated onto a straight line area following different crystal orientations. In addition, the horizontal axis of this graph represents the angle formed between the direction in which a straight line area (reference area) orthogonal to the crystal orientation

[0011] extends and the direction in which a straight line area (measurement area) to be measured extends, when viewed from a plane.

[0130] That is, when the value of the horizontal axis of this graph is 45°, the area along the straight line following the crystal orientation

[0001] becomes the measurement target. Likewise, when the value of the horizontal axis of this graph is 135°, the area along the straight line following the crystal orientation

[0010] becomes the measurement target. Also, the vertical axis of this graph represents the value when the width of the peeling layer formed in the measurement area by irradiating the measurement area with a laser beam (LB) is divided by the width of the peeling layer formed in the reference area by irradiating the reference area with a laser beam (LB).

[0131] As shown in FIG. 12, the width of the peeling layer widens when the angle formed by the direction in which the reference region extends and the direction in which the measurement region extends is 40° to 50° or 130° to 140°. That is, the width of the peeling layer widens when a laser beam (LB) is irradiated on a straight line area along a direction in which the angle formed with the crystal orientation

[0001] or crystal orientation

[0010] is 5° or less.

[0132] For this reason, in the laser beam irradiation step (S31) of the second peeling layer forming step (S3) of the present invention, a laser beam (LB) may be irradiated in a straight line area along a direction tilted at 5° or less from the crystal orientation

[0001] or crystal orientation

[0010] when viewed from a plane.

[0133] That is, in this laser beam irradiation step (S31), a laser beam (LB) may be irradiated in a straight line along a direction (first direction) that is parallel to the crystal plane (here, crystal plane (100)) exposed to each of the surface (11a) and back surface (11b) of the wafer (11) among the specific crystal planes included in the crystal plane {100}, and also has an angle of 5° or less with respect to a specific crystal orientation (here, crystal orientation

[0001] or crystal orientation

[0010] ) included in the crystal orientation <100>.

[0134] Also, when the laser beam irradiation step (S31) is performed in this manner, the output transfer step (S32) is performed by moving the internal position of the wafer (11) where a point of concentration is formed by irradiation of the laser beam (LB) along a direction (second direction) that is parallel to the crystal plane (100) that is exposed to each of the surface (11a) and back surface (11b) of the wafer (11) among the specific crystal planes included in the crystal plane {100}.

[0135] In addition, in the second peeling layer formation step (S3) of the present invention, after the peeling layer (25) is formed over the entire second region that is inner to the outer region of the wafer (11) (from the region on one side in the Y-axis direction to the region on the other side) (step S33: yes), the laser beam irradiation step (S31) and the output transfer step (S32) may be repeated.

[0136] That is, regarding the second region where the peeling layer (25) has already been formed, irradiation with the laser beam (LB) that forms the peeling layer (25) may be performed again. In this case, the density of each of the modified region (21) and crack (23) included in the peeling layer (25) increases. Accordingly, the separation of the wafer (11) in the separation step (S4) becomes easier.

[0137] In addition, in the second peeling layer formation step (S3) of the present invention, the laser beam irradiation step (S31) may be performed again after the laser beam irradiation step (S31) and before the output transfer step (S32). That is, the laser beam (LB) forming the peeling layer (25) may be irradiated again on a straight area where the peeling layer (25) has already been formed. In this case, as with the above, the separation of the wafer in the separation step (S4) becomes easier.

[0138] Additionally, in the separation step (S4) of the present invention, ultrasonic waves may be applied to the wafer (11) before separation of the wafer (11) having the first peeling layer and the second peeling layer formed thereon. In this case, the cracks (23) included in the first peeling layer and the second peeling layer are extended, so separation of the wafer (11) becomes easier.

[0139] Additionally, in the separation step (S4) of the present invention, the wafer (11) may be separated using a device other than the separation device (60) described above. For example, in the separation step (S4) of the present invention, after separating the area where a plurality of devices (15) of the wafer (11) are formed and the outer periphery area, the surface (11a) side and the back side (11b) side of the wafer (11) may be separated.

[0140] Hereinafter, an example of such a separation step (S4) will be described with reference to FIGS. 13 to 15. FIG. 13 is a top view schematically showing a wafer (11) provided for such a separation step (S4). In the outer periphery of this wafer (11), prior to the bonding step (S1) described above, a plurality of cuts (11d) are formed, each extending along the diameter direction of the wafer (11).

[0141] These multiple cuts (11d) are formed at generally equal intervals along the circumferential direction of the wafer (11), except for the portion where the notch (13) is formed. And each of the multiple cuts (11d) is formed such that the portion of the wafer (11) in the diameter direction inner reaches the first peeling layer formed in the first peeling layer forming step (S2) described above.

[0142] Additionally, the first peeling layer formed inside the wafer (11) has a shape that follows the side of a cylinder, with the lower bottom surface located on the surface (11a) side of the wafer (11) and the upper bottom surface located on the back side (11b) side of the wafer (11). That is, in this wafer (11), a first peeling layer is formed that penetrates the surface (11a) and the back side (11b) of the wafer (11).

[0143] Additionally, a plurality of cuts (11d) are formed by cutting the wafer (11) in a known cutting device, for example. Alternatively, a plurality of cuts (11d) may be formed by irradiating the wafer (11) with a laser beam that causes laser ablation in a known laser processing device.

[0144] Additionally, instead of a plurality of cuts (11d) in the outer region of the wafer (11), a plurality of peeling layers, each extending along the diameter direction of the wafer (11), may be formed in the outer region of the wafer (11). Additionally, these peeling layers are formed, for example, by the same method as the method for forming the first peeling layer and the second peeling layer described above.

[0145] FIGS. 14(A) and FIGS. 14(B) are each schematic cross-sectional side views showing the separation of the region where a plurality of devices (15) are formed and the outer region of the wafer (11) shown in FIGS. 13. The separation of the wafer (11) is carried out using the expansion device (72) shown in FIGS. 14(A) and FIGS. 14(B).

[0146] This expansion device (72) has a fixed cylindrical drum (74). A support unit (76) is formed around this drum (74). This support unit (76) has an annular support (78) formed to surround the upper part of the drum (74). On this support (78), a plurality of clamps (80) are installed at generally equal intervals along the circumferential direction of the support (78).

[0147] Additionally, a plurality of air cylinders are installed at roughly equal intervals along the circumferential direction of the support (78) below the support (78), and the upper end of the piston rod (82) of each air cylinder is fixed to the lower part of the support (78). Therefore, in the expansion device (72), by operating the plurality of air cylinders, the support (78) and the plurality of clamps (80) can be raised and lowered together with the piston rod (82).

[0148] When separating the area where a plurality of devices (15) of the wafer (11) shown in FIG. 13 are formed from the outer area, first, an annular frame (29) is attached to the peripheral area of ​​one side of the disc-shaped expanded tape (27), and then the back side (11b) of the wafer (11) is attached to the central area. Accordingly, a frame unit is formed in which the annular frame (29) is integrated with the bonded wafer, in which the wafer (11) and the support wafer (17) are bonded.

[0149] Next, a plurality of air cylinders are operated so that the upper surface of the support (78) is positioned on the same plane as the top of the drum (74). Next, an annular frame (29) is placed on the support (78) through an expanded tape (27). That is, the frame unit is placed on the support (78) so that the support wafer (17) faces upward.

[0150] Next, the annular frame (29) is secured by a plurality of clamps (80) (see FIG. 14(A)). Next, a plurality of air cylinders are operated to lower the annular frame (29) secured by the plurality of clamps (80). Accordingly, the central area of ​​the expanded tape (27) is expanded along the diameter direction of the wafer (11) by the amount that the annular frame (29) has lowered.

[0151] At this time, a force directed outward in the diameter direction of the wafer (11) is applied to the wafer (11) attached to the expanded tape (27). As a result, the first peeling layer becomes the separation point, and the region where the plurality of devices (15) of the wafer (11) are formed and the outer region are separated (see FIG. 14(B)).

[0152] FIGS. 15(A) and FIGS. 15(B) are each schematic cross-sectional side views illustrating the separation of the surface (11a) side and the back side (11b) side of the wafer (11) shown in FIGS. 14(B). The separation of the wafer (11) is carried out using a separation device (84) shown in FIGS. 15(A) and FIGS. 15(B). The separation device (84) has a holding table (86) that holds a bonded wafer including the wafer (11) shown in FIGS. 14(B).

[0153] This holding table (86) has a circular upper surface (holding surface), and a porous plate (not shown) is exposed on this holding surface. In addition, this porous plate is in communication with a suction source (not shown), such as a vacuum pump, through a flow path formed inside the holding table (86). Therefore, when this suction source operates, negative pressure is generated in the space near the holding surface of the holding table (86).

[0154] Additionally, a separation unit (88) is formed above the maintenance table (86). This separation unit (88) has a cylindrical support member (90). For example, a ball screw type lifting mechanism (not shown) is connected to the upper part of this support member (90), and the separation unit (88) is raised by operating this lifting mechanism.

[0155] Additionally, the lower part of the support member (90) is fixed to the center of the upper part of the disc-shaped suction plate (92). A plurality of suction holes are formed on the lower surface of the suction plate (92), and each of the plurality of suction holes is connected to a suction source (not shown), such as a vacuum pump, through a flow path formed inside the suction plate (92). Therefore, when this suction source operates, negative pressure is generated in the space near the lower surface of the suction plate (92).

[0156] When separating the front side (11a) and the back side (11b) of the wafer (11) shown in FIG. 14(B), first, the bonded wafer containing the wafer (11) is removed from the expanded tape (27). Then, the bonded wafer is placed on the holding table (86) so that the center of the back side (17b) of the supporting wafer (17) of the bonded wafer aligns with the center of the holding surface of the holding table (86).

[0157] Next, a suction source communicating with a porous plate exposed on the holding surface is operated so that the bonded wafer is held by the holding table (86). Next, a lifting mechanism is operated to lower the separation unit (88) so that the lower surface of the suction plate (92) comes into contact with the back surface (11b) of the wafer (11).

[0158] Next, a suction source communicating with a plurality of suction ports is operated so that the back side (11b) of the wafer (11) is sucked through a plurality of suction ports formed in the suction plate (92). Next, a lifting mechanism is operated to raise the separation unit (88) so that the suction plate (92) is separated from the holding table (86) (see FIG. 15(A)).

[0159] At this time, a force acting in the upward direction of the thickness of the wafer (11) is applied to the wafer (11) which is being sucked in through a plurality of suction holes formed in the suction plate (92) on the back side (11b). As a result, the second peeling layer becomes the separation point, and the surface (11a) side and the back side (11b) side of the wafer (11) are separated (see FIG. 15(B)).

[0160] Furthermore, the structures and methods related to the embodiments described above may be appropriately modified and implemented as long as they do not deviate from the scope of the purpose of the present invention. Explanation of the symbols

[0161] 11 : Wafer (11a : Surface, 11b : Back side, 11c : Side, 11d : Cutout) 13 : Notch 15 : Device 17: Support wafer (17a: Surface, 17b: Back side) 19: Glue 21: Modification Zone 23: Crack 25 (25-1, 25-2): Delamination layer 27 : Expand Tape 29 : Fantasy Frame 2 : Laser processing device 4 : Expectation 6: Horizontal movement mechanism 8: Y-axis guide rail 10: Y-axis movement plate 12: Screw shaft 14 : Motor 16: X-axis guide rail 18: X-axis movement plate 20 : Screw shaft 22 : Motor 24: Table Expectation 26 : Retention table (26a : Porous plate) 30: Support structure 32: Vertical movement mechanism 34: Z-axis guide rail 36 : Z-axis moving plate 38 : Motor 40 : Jijigu 42: Laser beam irradiation unit 44 : Laser oscillator 46 : Damper 48 : Spatial optical modulator 50 : Mirror 52: Investigation Head 54 : Housing 56 : Imaging unit 58 : Touch panel 60: Separator 62 : Maintenance Table 64: Separation unit 66: Support member 68: Expectation of Phage Claw 70 : Phage Claw (70a : Orthotic part, 70b : Claw part) 72 : Expansion device 74 : Drums 76 : Support Unit 78 : Support 80 : Clamp 82 : Piston rod 84: Separator 86 : Maintenance Table 88 : Separation unit 90 : Support member 92 : Suction plate

Claims

Claim 1 A processing method for a single-crystal silicon wafer, wherein a specific crystal plane included in a crystal plane {100} is exposed on each of the surface and back surfaces, and the outer periphery region is chamfered, wherein a focused point formed thereon is positioned inside the single-crystal silicon wafer, and wherein a laser beam having a wavelength that transmits single-crystal silicon is irradiated to form a peeling layer inside the single-crystal silicon wafer, and wherein the single-crystal silicon wafer is separated using the peeling layer as a separation point, the method comprises: a first peeling layer forming step in which a first peeling layer serving as a separation point when separating the outer periphery region from the single-crystal silicon wafer is formed by irradiating the laser beam from the back surface of the single-crystal silicon wafer onto a first annular region inside the outer periphery region of the single-crystal silicon wafer; and a second region inside the outer periphery region of the single-crystal silicon wafer, wherein the laser beam is irradiated from the back surface of the single-crystal silicon wafer. The method comprises a second peeling layer forming step for forming a second peeling layer that serves as a separation point between the surface side and the back side, and a separation step for separating the single-crystal silicon wafer with the first peeling layer and the second peeling layer as separation points by applying an external force to the single-crystal silicon wafer after performing the first peeling layer forming step and the second peeling layer forming step, wherein in the second peeling layer forming step, the method comprises a laser beam irradiation step for irradiating the laser beam onto a linear region along the first direction included in the second region while moving the single-crystal silicon wafer and the focusing point relatively along a first direction parallel to the specific crystal plane, and along a second direction parallel to the specific crystal plane and also orthogonal to the first direction.A method for processing a single-crystal silicon wafer, wherein a second peeling layer is formed by repeatedly performing a calculation transfer step that moves the internal position of the single-crystal silicon wafer in which the focusing point is formed by irradiation of the laser beam, and the first direction has an angle of 5° or less with respect to a specific crystal orientation included in crystal orientation <100>. Claim 2 delete Claim 3 A method for processing a single-crystal silicon wafer according to claim 1, wherein a plurality of devices are formed on the surface side of the single-crystal silicon wafer. Claim 4 A method for processing a single-crystal silicon wafer according to claim 1, further comprising a bonding step of bonding the surface side of the single-crystal silicon wafer to the surface side of a support wafer before performing the first peeling layer forming step and the second peeling layer forming step. Claim 5 A method for processing a single-crystal silicon wafer according to claim 4, wherein a plurality of devices are formed on the surface side of the support wafer. Claim 6 A method for processing a single-crystal silicon wafer according to claim 1, wherein the first peeling layer is each located between the surface of the single-crystal silicon wafer and the second peeling layer in the thickness direction of the single-crystal silicon wafer, and further comprises a plurality of modified regions having different positions relative to each other in the thickness direction. Claim 7 In claim 1, the first peeling layer forming step is a method for processing a single-crystal silicon wafer performed before performing the second peeling layer forming step. Claim 8 A method for processing a single-crystal silicon wafer, wherein the second region is located inside the first region. Claim 9 A method for processing a single-crystal silicon wafer according to claim 1, wherein in the first peeling layer forming step, the first peeling layer is formed such that it does not reach the back surface of the single-crystal silicon wafer. Claim 10 A method for processing a single-crystal silicon wafer according to any one of claims 1 and 3 to 9, wherein in the step of forming the first peeling layer, the laser beam is irradiated such that the focusing point formed approaches the surface of the single-crystal silicon wafer as it approaches the outer periphery region, thereby forming the first peeling layer along the side of a truncated cone in which the first bottom surface is located on the surface side of the single-crystal silicon wafer and the second bottom surface, having a diameter shorter than the first bottom surface, is located inside the single-crystal silicon wafer.

Citation Information

Patent Citations

  • Laser processing device setting method, laser processing method, laser processing device, thinning system, and substrate processing method

    JP2020136442A

  • Laser processing device, thinning system, laser processing method and thining method

    JP2020163447A

  • Method for producing wafer and apparatus for producing wafer

    KR1020190089730A

  • Substrate treatment system and substrate treatment method

    WO2020017599A1