Transparent conductive layer and transparent conductive film

A transparent conductive layer with a specific crystallite size ratio and krypton/argon-containing indium tin complex oxide layers addresses the need for lower resistivity, achieving a resistivity of 2.3×10⁻⁴ Ω·cm for improved conductivity in optical applications.

KR103046627B1Active Publication Date: 2026-11-10NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020227030816
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-02
Filing Date
2021-03-18
Publication Date
2026-11-10
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Transparent conductive films require lower resistivity for improved performance in optical applications such as touch panels.

Method used

A transparent conductive layer with a specific crystallite size ratio and the inclusion of krypton atoms in a krypton-containing indium tin complex oxide layer, combined with a krypton-free argon-containing indium tin complex oxide layer, to achieve low resistivity.

Benefits of technology

The resulting transparent conductive layer and film exhibit resistivity as low as 2.3×10⁻⁴ Ω·cm, enhancing conductivity and reducing resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022093415099-PCT00002_ABST
    Figure 112022093415099-PCT00002_ABST
Patent Text Reader

Abstract

The transparent conductive layer (1) has a ratio of the size of the crystallites in the (440) plane to the size of the crystallites in the (400) plane of 0.80 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a transparent conductive layer and a transparent conductive film. More specifically, it relates to a transparent conductive layer and a transparent conductive film having the transparent conductive layer. Background Technology

[0002] Optical films, such as transparent conductive films, are known to be used for optical applications such as touch panels.

[0003] As such, a transparent conductive film is proposed that comprises an organic polymer film substrate and a transparent conductive film in sequence (see, for example, Patent Document 1).

[0004] In addition, such a transparent conductive film is obtained by forming a transparent conductive film on the surface of an organic polymer film substrate by sputtering in the presence of argon gas. Prior art literature

[0005] Japanese Published Patent Application No. 2014-157814 The problem to be solved

[0006] Meanwhile, transparent conductive films are required to have even lower resistivity.

[0007] The present invention provides a transparent conductive layer having low resistivity and a transparent conductive film having the transparent conductive layer. means of solving the problem

[0008] The present invention [1] is a transparent conductive layer in which the ratio of the size of the crystallizer in the (440) plane to the size of the crystallizer in the (400) plane is 0.80 or more.

[0009] The present invention [2] includes a transparent conductive layer described in [1] containing krypton atoms.

[0010] The present invention [3] comprises a transparent conductive layer described in [1] or [2] containing an indium tin complex oxide.

[0011] The present invention [4] has a resistivity of 2.3×10 -4 It includes a transparent conductive layer described in any one of [1] to [3] above, with a thickness of less than Ω·cm.

[0012] The present invention [5] includes a transparent conductive layer described in any one of claims [1] to [4] having a pattern shape.

[0013] The present invention [6] comprises a transparent conductive film having a substrate layer and a transparent conductive layer described in any one of claims [1] to [5] arranged in order toward one side in the thickness direction. Effects of the invention

[0014] The transparent conductive layer of the present invention has a ratio of the size of the crystallites in the (440) plane to the size of the crystallites in the (400) plane of 0.80 or more. Therefore, the resistivity can be lowered.

[0015] The transparent conductive film of the present invention comprises a transparent conductive layer of the present invention. Accordingly, the resistivity can be lowered. Brief explanation of the drawing

[0016] FIG. 1 is a schematic diagram showing a first embodiment of a transparent conductive layer of the present invention. FIG. 2 is a schematic diagram showing a first embodiment of a transparent conductive film of the present invention. FIG. 3 is a schematic diagram illustrating a first embodiment of a method for manufacturing a transparent conductive layer and a transparent conductive film according to the present invention. FIG. 3A illustrates a process of preparing a transparent substrate in a first process. FIG. 3B illustrates a process of placing a hard coat layer on one side in the thickness direction of the transparent substrate in a first process. FIG. 3C illustrates a fourth process of placing a krypton-containing transparent conductive layer on one side in the thickness direction of the substrate layer in a second process. FIG. 3D illustrates a fifth process of placing an argon-containing transparent conductive layer on one side in the thickness direction of the krypton-containing transparent conductive layer in a second process. FIG. 3E illustrates a third process of heating the transparent conductive layer. Figure 4 is a graph showing the relationship between the resistivity of an amorphous transparent conductive layer and the amount of oxygen introduced. FIG. 5 is a schematic diagram showing a second embodiment of the transparent conductive layer of the present invention. FIG. 6 is a schematic diagram showing a second embodiment of the transparent conductive film of the present invention. FIG. 7 is a schematic diagram illustrating a second embodiment of a method for manufacturing a transparent conductive layer and a transparent conductive film according to the present invention. FIG. 7A illustrates a first process of preparing a substrate layer. FIG. 7B illustrates a second process of placing a transparent conductive layer on one side in the thickness direction of the substrate layer. FIG. 7C illustrates a third process of heating the transparent conductive layer. FIG. 8 is a schematic diagram showing one embodiment of an article with a transparent conductive layer film attached. FIG. 9 is a schematic diagram showing one embodiment of an article with a transparent conductive layer attached. Specific details for implementing the invention

[0017] Transparent Challenge Layer

[0018] The transparent conductive layer (1) has a film shape (including a sheet shape) having a predetermined thickness. The transparent conductive layer (1) extends in a plane direction orthogonal to the thickness direction. The transparent conductive layer (1) has a flat upper surface and a flat lower surface.

[0019] The transparent conductive layer (1) is a transparent layer that exhibits excellent conductivity. The transparent conductive layer (1) includes a crystalline material and is preferably made of a crystalline material.

[0020] The transparent conductive layer (1) preferably contains krypton atoms. In other words, the transparent conductive layer (1) preferably has a krypton-containing transparent conductive layer (10) (sometimes called KrITO) containing krypton atoms.

[0021] In addition, the transparent conductive layer (1) may also include a krypton-containing transparent conductive layer (10) and a krypton-free transparent conductive layer (11) that does not contain krypton atoms.

[0022] In the following description, the case in which the transparent conductive layer (1) contains krypton atoms is described in detail. Specifically, a first embodiment in which the transparent conductive layer (1) comprises a krypton-containing transparent conductive layer (10) and a krypton-free transparent conductive layer (11) in sequence, and a second embodiment comprising the krypton-containing transparent conductive layer (10) in sequence are described in sequence.

[0023] 1. First embodiment

[0024] As shown in FIG. 1, the transparent conductive layer (1) comprises, in order, a krypton-containing transparent conductive layer (10) and a krypton-free transparent conductive layer (11). More specifically, the transparent conductive layer (1) comprises a krypton-containing transparent conductive layer (10) and a krypton-free transparent conductive layer (11) disposed on the upper surface (one side in the thickness direction) of the krypton-containing transparent conductive layer (10). Preferably, the transparent conductive layer (1) comprises only the krypton-containing transparent conductive layer (10) and the krypton-free transparent conductive layer (11).

[0025] The krypton-containing transparent conductive layer (10) contains a metal oxide and a trace amount of krypton atoms. The krypton-containing transparent conductive layer (10) is preferably composed of a metal oxide and a trace amount of krypton atoms. Specifically, in the krypton-containing transparent conductive layer (10), a trace amount of krypton atoms is present in the metal oxide matrix.

[0026] As a metal oxide, it is an oxide of at least one metal and / or metalloid selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W. As a metal oxide, specifically, indium-containing oxides and antimony-containing oxides may be used. Examples of indium-containing oxides include indium-tin complex oxide (ITO), indium-gallium complex oxide (IGO), indium-zinc complex oxide (IZO), and indium-gallium-zinc complex oxide (IGZO). Examples of antimony-containing oxides include antimony-tin complex oxide (ATO).

[0027] As a metal oxide, preferably an indium-containing oxide, more preferably an indium-tin composite oxide (ITO). In short, preferably, the krypton-containing transparent conductive layer (10) (transparent conductive layer (1)) contains indium-tin composite oxide (ITO). If the krypton-containing transparent conductive layer (10) (transparent conductive layer (1)) contains indium-tin composite oxide (ITO), the resistivity of the transparent conductive layer (1) can be lowered.

[0028] When the metal oxide is an indium tin composite oxide (ITO), the tin oxide content is, for example, 0.5 mass% or more, preferably 3 mass% or more, more preferably 5 mass% or more, even more preferably 8 mass% or more, particularly preferably 9 mass% or more, with respect to the total amount of tin oxide and indium oxide, and also, for example, 20 mass% or less, preferably 15 mass% or less, more preferably 12 mass% or less.

[0029] If the tin oxide content ratio is above the lower limit mentioned above, low resistance is promoted. If the tin oxide content ratio is below the upper limit mentioned above, the krypton-containing transparent conductive layer (10) has excellent heat stability.

[0030] Also, the krypton-containing transparent conductive layer (10) contains krypton atoms.

[0031] Krypton atoms originate from krypton gas as a sputtering gas, which will be described later. In other words, although details will be described later, in the sputtering method, krypton gas as a sputtering gas is introduced into a krypton-containing transparent conductive layer (10).

[0032] The content of krypton atoms in the krypton-containing transparent conductive layer (10) is, for example, 1.0 atomic% or less, more preferably 0.7 atomic% or less, even more preferably 0.5 atomic% or less, particularly preferably 0.3 atomic% or less, most preferably 0.2 atomic% or less, furthermore less than 0.1 atomic%, and for example 0.0001 atomic% or more.

[0033] The content of krypton atoms can be measured, for example, by Rutherford backscattering spectroscopy. Additionally, the presence of krypton atoms can be confirmed, for example, by fluorescence X-ray analysis. In the case where the content of krypton atoms in the krypton-containing transparent conductive layer (10) is excessively low (specifically, when the content of krypton atoms is not above the detection limit value (lower limit) of Rutherford backscattering analysis), the content of krypton atoms may not be quantified by Rutherford backscattering analysis. However, in the present invention, even in such cases, if the presence of krypton atoms is identified by fluorescence X-ray analysis, the content of krypton atoms is determined to be at least 0.0001 atomic% or more.

[0034] In addition, the krypton-containing transparent conductive layer (10) contains a crystalline material, and preferably is made of a crystalline material.

[0035] If the krypton-containing transparent conductive layer (10) is crystalline, the resistivity can be reduced.

[0036] The crystallinity of the krypton-containing transparent conductive layer (10) can be determined, for example, by observing a cross-section of the krypton-containing transparent conductive layer (10) with FE-TEM and confirming the presence of crystal grains. The magnification of the observation in FE-TEM is not limited as long as it is a magnification at which the presence of crystal grains can be confirmed, but for example, 200,000 times. Also, if the presence of lattice stripes is confirmed in the krypton-containing transparent conductive layer (10) during observation at a higher magnification (for example, 2 million times or more), the corresponding part can be determined to be crystalline.

[0037] The krypton-containing transparent conductive layer (10) is preferably a post-crystalline layer (post-crystalline film). Post-crystalline means that the film is amorphous during and immediately after film formation (e.g., within 10 hours after film formation), and then converted into a crystalline film through a process such as heating. If the krypton-containing transparent conductive layer (10) is a post-crystalline layer, it is easy to obtain a transparent conductive layer (1) with low resistivity and excellent appearance quality, and a transparent conductive film (20) described later.

[0038] The krypton-free transparent conductive layer (11) does not contain krypton atoms. As will be described in detail later, the krypton-free transparent conductive layer (11) contains atoms derived from a sputtering gas (e.g., argon gas, xenon gas) containing a noble gas other than krypton gas in the sputtering method.

[0039] As for a krypton-free transparent conductive layer (11), for example, an argon-containing transparent conductive layer (sometimes called ArITO) can be used.

[0040] The argon-containing transparent conductive layer contains the aforementioned metal oxide and a trace amount of argon atoms.

[0041] Examples of metal oxides include, preferably, indium-containing oxides, and more preferably, indium-tin composite oxides (ITO).

[0042] When the metal oxide is an indium tin composite oxide (ITO), the tin oxide content is, for example, 0.5 mass% or more, preferably 3 mass% or more, more preferably 5 mass% or more, even more preferably 8 mass% or more, particularly preferably 9 mass% or more, with respect to the total amount of tin oxide and indium oxide, and also, for example, 20 mass% or less, preferably 15 mass% or less, more preferably 12 mass% or less.

[0043] In addition, the argon-containing transparent conductive layer contains argon atoms.

[0044] Argon atoms originate from argon gas as a sputtering gas, which will be described later. In other words, as will be described in detail later, in the sputtering method, argon gas as a sputtering gas is introduced into an argon-containing transparent conductive layer.

[0045] The content of argon atoms in the argon-containing transparent conductive layer is, for example, 0.8 atomic% or less, preferably 0.5 atomic% or less, more preferably 0.2 atomic% or less, even more preferably 0.1 atomic% or less, and, for example, 0.0001 atomic% or more.

[0046] The argon atom content can be measured, for example, by Rutherford backscattering spectroscopy.

[0047] In addition, the argon-containing transparent conductive layer contains crystals and is preferably composed of crystals.

[0048] If the argon-containing transparent conductive layer is crystalline, the resistivity can be reduced.

[0049] The crystallinity of the argon-containing transparent conductive layer can be verified in the same way as the crystallinity of the krypton-containing transparent conductive layer (10).

[0050] The transparent conductive layer (1) has transparency. Specifically, the total light transmittance (JIS K 7375-2008) of the transparent conductive layer (1) is, for example, 60% or more, preferably 80% or more, more preferably 85% or more.

[0051] The thickness of the transparent conductive layer (1) is, for example, 10 nm or more, preferably 40 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, and for example, 1000 nm or less, preferably 500 nm or less, more preferably less than 300 nm, even more preferably 280 nm or less, particularly more preferably 200 nm or less, particularly preferably 170 nm or less, even more preferably 150 nm or less, most preferably 148 nm or less.

[0052] Also, in the transparent conductive layer (1), the thickness of the krypton-containing transparent conductive layer (10) is, for example, 1 nm or more, preferably 10 nm or more, more preferably 40 nm or more, even more preferably 60 nm or more, and also, for example, 800 nm or less, preferably less than 300 nm, more preferably 200 nm or less, even more preferably less than 150 nm, particularly preferably 100 nm or less, particularly more preferably less than 100 nm, and most preferably 90 nm or less. In addition, the thickness of the krypton-free transparent conductive layer (11) is, for example, 1 nm or more, preferably 10 nm or more, more preferably 40 nm or more, and also, for example, 500 nm or less, preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 60 nm or less.

[0053] The thickness of the krypton-containing transparent conductive layer (10) relative to the thickness of the transparent conductive layer (1) is, for example, 1% or more, preferably 20% or more, more preferably 30% or more, even more preferably 50% or more, particularly preferably 60% or more, and for example 99% or less, preferably 80% or less, more preferably 70% or less.

[0054] If the thickness of the krypton-containing transparent conductive layer (10) is greater than or equal to the lower limit and less than or equal to the upper limit, the resistivity can be lowered.

[0055] Additionally, the thickness of the transparent conductive layer (1) can be measured by observing the cross-section of the transparent conductive film (20) using, for example, a transmission electron microscope. Also, in FIG. 1, the boundary between the krypton-containing transparent conductive layer (10) and the krypton-free transparent conductive layer (11) is depicted by a solid line, but there are cases where the boundary between the krypton-containing transparent conductive layer (10) and the krypton-free transparent conductive layer (11) cannot be clearly distinguished.

[0056] The resistivity of the transparent conductive layer (1) is, for example, 2.3×10 -4 Less than Ω·cm, preferably 2.2×10⁻⁶ -4 Less than Ω·cm, more preferably 2.0×10⁻⁶ -4 Ω·cm or less, more preferably 1.7×10⁻⁶ -4 Ω·cm or less, particularly preferably 1.5×10⁻⁶ -4 Ω·cm or less, also, for example, 0.01×10⁻⁶ -4 Ω·cm or more, preferably 0.05×10⁻⁶ -4 Ω·cm or more, more preferably 0.1×10⁻⁶ -4 Ω·cm or more, more preferably 0.5×10⁻⁶ -4 Ω·cm or more, even more preferably 1.0×10 -4 Ω·cm or more, particularly preferably 1.01×10⁻⁶ -4 It is greater than Ω·cm.

[0057] In addition, the resistivity can be obtained by multiplying the surface resistance value measured by the 4-terminal method in accordance with JIS K 7194 by the thickness of the transparent conductive layer (1).

[0058] The surface resistance of the transparent conductive layer (1) is, for example, 200 Ω / □ or less, preferably 80 Ω / □ or less, more preferably 60 Ω / □ or less, even more preferably 50 Ω / □ or less, particularly preferably 30 Ω / □ or less, most preferably 20 Ω / □ or less, and typically greater than 0 Ω / □, and greater than 1 Ω / □.

[0059] In addition, the surface resistance value can be measured by the four-terminal method in accordance with JIS K 7194.

[0060] And, in the transparent conductive layer (1), the ratio of the size of the crystallite on the (440) plane to the size of the crystallite on the (400) plane (size of the crystallite on the (440) plane / size of the crystallite on the (400) plane) (hereinafter referred to as the crystallite size ratio) is 0.80 or more, preferably 1.00 or more, more preferably 1.05 or more, even more preferably 1.10 or more, and, for example, 2.00 or less, preferably 1.50 or less.

[0061] If the crystallite size ratio is above the above lower limit, mobility tends to increase, making it possible to reduce resistivity.

[0062] On the other hand, if the crystallite size ratio is below the above lower limit, mobility tends to decrease, making it impossible to reduce resistivity.

[0063] In addition, the size of the crystallites in the (440) plane is, for example, 250 Å or more, preferably 330 Å or more, more preferably 380 Å or more, even more preferably 400 Å or more, particularly preferably 420 Å or more, and also, for example, 850 Å or less, preferably 600 Å or less, more preferably 500 Å or less, even more preferably 450 Å or less.

[0064] In addition, the size of the crystallites in the (400) plane is, for example, 200 Å or more, preferably 300 Å or more, more preferably 350 Å or more, even more preferably 370 Å or more, and also, for example, 700 Å or less, preferably 440 Å or less, more preferably 420 Å or less, even more preferably 400 Å or less.

[0065] (440) If the size of the crystallizer on the plane and the size of the crystallizer on the plane (400) are within the above range, the resistivity can be lowered.

[0066] In addition, the size of the crystallite can be determined by X-ray diffraction measurement. The method for measuring X-ray diffraction will be described in detail in the examples that follow.

[0067] Transparent conductive film

[0068] The transparent conductive film (20) has a film shape (including a sheet shape) having a predetermined thickness, as shown in FIG. 2. The transparent conductive film (20) extends in a plane direction orthogonal to the thickness direction. The transparent conductive film (20) has a flat upper surface and a flat lower surface.

[0069] A transparent conductive film (20) comprises a substrate layer (2) and a transparent conductive layer (1) in sequence toward one side in the thickness direction. More specifically, the transparent conductive film (20) comprises a substrate layer (2) and a transparent conductive layer (1) disposed on the upper surface (one side in the thickness direction) of the substrate layer (2). Preferably, the transparent conductive film (20) comprises only the substrate layer (2) and the transparent conductive layer (1).

[0070] More specifically, the transparent conductive film (20) comprises a substrate layer (2), a krypton-containing transparent conductive layer (10), and a krypton-free transparent conductive layer (11) in sequence toward one side in the thickness direction. Even more specifically, the transparent conductive film (20) comprises a substrate layer (2), a krypton-containing transparent conductive layer (10) disposed on the upper surface (one side in the thickness direction) of the substrate layer (2), and a krypton-free transparent conductive layer (11) disposed on the upper surface (one side in the thickness direction) of the krypton-containing transparent conductive layer (10) in sequence toward one side in the thickness direction.

[0071] The transparent conductive film (20) is, for example, a component for a touch panel or an electromagnetic shield provided in an image display device, and is not an image display device. That is, the transparent conductive film (20) is a component for manufacturing an image display device, and is distributed as a component alone without including an image display element such as an OLED module, and is an industrially usable device.

[0072] The thickness of the transparent conductive film (20) is, for example, 1000 μm or less, preferably 500 μm or less, more preferably 250 μm or less, and, for example, 1 μm or more, preferably 20 μm or more, more preferably 50 μm or more.

[0073] <Source Class>

[0074] The substrate layer (2) is a transparent substrate for securing the mechanical strength of the transparent conductive film (20).

[0075] The substrate layer (2) has a film shape. The substrate layer (2) is placed on the entire lower surface of the transparent conductive layer (1) so as to be in contact with the lower surface of the transparent conductive layer (1).

[0076] The substrate layer (2) is equipped with a transparent substrate (3) and a functional layer (4).

[0077] Specifically, the substrate layer (2) comprises a transparent substrate (3) and a functional layer (4) in sequence toward one side in the thickness direction. Specifically, the substrate layer (2) comprises a transparent substrate (3) and a functional layer (4) disposed on one side in the thickness direction of the transparent substrate (3).

[0078] <Transparent Entry>

[0079] The transparent substrate (3) has a film shape.

[0080] Examples of materials for the transparent substrate (3) include olefin resin, polyester resin, (meth)acrylic resin (acrylic resin and / or methacrylic resin), polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of olefin resins include polyethylene, polypropylene, and cycloolefin polymers. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of (meth)acrylic resins include polymethacrylate. From the perspective of obtaining a transparent conductive layer (1) and a transparent conductive film (20) that have excellent smoothness and low resistivity, even though they have poor heat resistance and cannot withstand a heating process at high temperatures (e.g., 200°C or higher), olefin resin, (meth)acrylic resin, polycarbonate resin, melamine resin, and polyester resin can be used as materials for the transparent substrate (3), and more preferably polyethylene terephthalate (PET).

[0081] The transparent substrate (3) has transparency. Specifically, the total light transmittance (JIS K 7375-2008) of the transparent substrate (3) is, for example, 60% or more, preferably 80% or more, more preferably 85% or more.

[0082] The thickness of the transparent substrate (3) is, for example, 1 μm or more, preferably 10 μm or more, preferably 30 μm or more, and, for example, 1000 μm or less, preferably 500 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, particularly preferably 100 μm or less, most preferably 60 μm or less.

[0083] Functional layer

[0084] The functional layer (4) is placed on one side in the thickness direction of the transparent substrate (3).

[0085] The functional layer (4) has a film shape.

[0086] As for the functional layer (4), for example, a hard coat layer can be used.

[0087] In this case, the substrate layer (2) is provided with a transparent substrate (3) and a hard coat layer in sequence toward one side in the thickness direction.

[0088] In the following description, the case where the functional layer (4) is a hard coat layer is described.

[0089] The hard coat layer is a protective layer to prevent scratches from occurring on the transparent conductive film (20).

[0090] The hard coat layer is formed, for example, from a hard coat composition.

[0091] The hard coat composition contains a resin and, if necessary, particles. In short, the hard coat layer contains a resin and, if necessary, particles.

[0092] Examples of resins include thermoplastic resins and curable resins. Examples of thermoplastic resins include polyolefin resins.

[0093] Examples of curable resins include active energy beam curable resins that are cured by irradiation with active energy beams (e.g., ultraviolet and electron beams), and thermosetting resins that are cured by heating. Preferably, examples of curable resins include active energy beam curable resins.

[0094] Examples of active energy beam curable resins include (meth)acrylic UV-curable resins, urethane resins, melamine resins, alkyd resins, siloxane-based polymers, and organic silane condensates. Preferably, (meth)acrylic UV-curable resins are examples of active energy beam curable resins.

[0095] In addition, the resin may contain a reactive diluent as described in, for example, Japanese Patent Publication No. 2008-88309. Specifically, the resin may contain a polyfunctional (meth)acrylate.

[0096] The resin can be used alone or in combination with two or more types.

[0097] Examples of particles include metal oxide microparticles and organic microparticles. Examples of materials for metal oxide microparticles include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of materials for organic microparticles include polymethyl methacrylate, silicon, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate.

[0098] The particles can be used alone or in combination of two or more types.

[0099] In addition, the hard coat composition may, if necessary, incorporate a thixotropy-importing agent, a photopolymerization initiator, a filler (e.g., organic clay), and a leveling agent in appropriate proportions. In addition, the hard coat composition may be diluted with a known solvent.

[0100] Also, to form a hard coat layer, a diluted solution of the hard coat composition is applied to one side in the thickness direction of a temporary support (2), as described in detail later, and heated as necessary to dry. After drying, the hard coat composition is cured, for example, by irradiation with an active energy beam.

[0101] Thus, a hard coat layer is formed.

[0102] The thickness of the hard coat layer is, for example, 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, and, for example, 20 μm or less, preferably 10 μm or less, more preferably 5 μm or less.

[0103] Method for manufacturing a transparent conductive layer and a transparent conductive film

[0104] A method for manufacturing a transparent conductive layer (1) and a transparent conductive film (20) comprises a first step of preparing a substrate layer (2), a second step of placing a transparent conductive layer (1) on one side in the thickness direction of the substrate layer (2), and a third step of heating the transparent conductive layer (1). In addition, in this manufacturing method, each layer is arranged in sequence, for example, in a roll-to-roll manner.

[0105] <Process 1>

[0106] In the first process, a substrate layer (2) is prepared.

[0107] In order to prepare the substrate layer (2), a transparent substrate (3) is prepared as shown in FIG. 3A.

[0108] Next, as shown in FIG. 3B, a diluted solution of the hard coat composition is applied to one side in the thickness direction of the transparent substrate (3), and after drying, the hard coat composition is cured by ultraviolet irradiation or heating. In this way, a hard coat layer (functional layer (4)) is formed on one side in the thickness direction of the transparent substrate (3). In this way, the substrate layer (2) is prepared.

[0109] <Process 2>

[0110] In the second process, a transparent conductive layer (1) is placed on one side in the thickness direction of the substrate layer (2) (hard coat layer).

[0111] When manufacturing the transparent conductive layer of the first embodiment and the transparent conductive film having the transparent conductive layer, the second process comprises a fourth process of placing a krypton-containing transparent conductive layer (10) on one side in the thickness direction of the substrate layer (2), and a fifth process of placing a krypton-free transparent conductive layer (11).

[0112] In the fourth process, as shown in FIG. 3C, a krypton-containing transparent conductive layer (10) is placed on one side in the thickness direction of the substrate layer (2).

[0113] Specifically, in a sputtering apparatus, sputtering is performed in the presence of krypton gas while facing one side in the thickness direction of the substrate layer (2) against a target made of the material of a krypton-containing transparent conductive layer (10). Also, in the sputtering, the substrate layer (2) is in close contact along the circumferential direction of the film-forming roll. In addition, at this time, in addition to krypton gas, a reactive gas such as oxygen, for example, may be present.

[0114] The partial pressure of krypton gas in the sputtering apparatus is, for example, 0.05 Pa or more, preferably 0.1 Pa or more, and also, for example, 10 Pa or less, preferably 5 Pa or less, more preferably 1 Pa or less.

[0115] As shown in FIG. 4, the amount of reactive gas introduced can be estimated by the surface resistance of the amorphous krypton-containing transparent conductive layer (10). Specifically, since the film quality (surface resistance) of the amorphous krypton-containing transparent conductive layer (10) changes depending on the amount of reactive gas introduced into the amorphous krypton-containing transparent conductive layer (10), the amount of reactive gas introduced can be adjusted according to the desired surface resistance of the amorphous krypton-containing transparent conductive layer (10). In addition, in order to obtain a crystalline krypton-containing transparent conductive layer (10) by heating the amorphous krypton-containing transparent conductive layer (10), it is preferable to obtain the amorphous krypton-containing transparent conductive layer (10) by adjusting the amount of reactive gas introduced within the range of area X in FIG. 4.

[0116] Specifically, the resistivity of the amorphous krypton-containing transparent conductive layer (10) is, for example, 8.0×10 -4 Ω·cm or less, preferably 7.0×10⁻⁶-4 Ω·cm or less, also, for example, 2.0×10⁻⁶ -4 Ω·cm or more, preferably 4.0×10⁻⁶ -4 Ω·cm or more, more preferably 5.0×10⁻⁶ -4 A reactive gas is introduced to make the Ω·cm or higher.

[0117] The pressure within the sputtering apparatus is substantially the sum of the partial pressures of the krypton gas and the reactive gas.

[0118] The power source may be any of, for example, a DC power source, an AC power source, an MF power source, and an RF power source. It may also be a combination of these.

[0119] The value of the discharge output for the long side of the target is, for example, 0.1 W / mm or more, preferably 0.5 W / mm or more, more preferably 1 W / mm or more, even more preferably 5 W / mm or more, and also, for example, 30 W / mm or less, preferably 15 W / mm or less. In addition, the direction of the long side of the target is, for example, a direction orthogonal to the conveying direction (TD direction) in a roll-to-roll sputtering apparatus.

[0120] The horizontal magnetic field strength on the target surface is, for example, 10 mT or more, preferably 60 mT or more, and also, for example, 300 mT or less. By setting the horizontal magnetic field strength on the target surface to the above range, the amount of krypton atoms in the krypton-containing transparent conductive layer (10) can be reduced, thereby enabling the production of a krypton-containing transparent conductive layer (10) with excellent low resistivity.

[0121] Then, the material of the krypton-containing transparent conductive layer (10) ejected from the target by sputtering is deposited on the substrate layer (2). At this time, since thermal energy is generated, when forming the krypton-containing transparent conductive layer (10), the krypton-containing transparent conductive layer (10) is cooled by cooling the substrate layer (2) by a film-forming roll to suppress crystallization of the krypton-containing transparent conductive layer (10).

[0122] In detail, the temperature of the film-forming roll is, for example, -50°C or higher, preferably -30°C, more preferably -20°C or higher, and also, for example, 20°C or lower, preferably 15°C or lower, more preferably 10°C or lower, even more preferably 5°C or lower, and particularly more preferably 0°C or lower. Within the above temperature range, the substrate (2) can be sufficiently cooled, and crystallization of the amorphous krypton-containing transparent conductive layer (10) can be reliably obtained. In addition, out-gas (water or organic solvent) from the substrate (2) is difficult to escape, and impurity components within the krypton-containing transparent conductive layer (10) can be reduced, so the low resistivity of the krypton-containing transparent conductive layer (10) is excellent.

[0123] Thus, an amorphous krypton-containing transparent conductive layer (10) is placed on one side in the thickness direction of the substrate layer (2).

[0124] Also, as mentioned above, since krypton gas is used as the sputtering gas, krypton atoms derived from krypton gas are introduced into the krypton-containing transparent conductive layer (10).

[0125] In the fifth process, as shown in FIG. 3D, a krypton-free transparent conductive layer (11) is placed on one side in the thickness direction of the krypton-containing transparent conductive layer (10).

[0126] In addition, the following description describes in detail the case where the krypton-free transparent conductive layer (11) is an argon-containing transparent conductive layer.

[0127] In the fifth process, in a sputtering apparatus, sputtering is performed in the presence of argon gas while facing one side in the thickness direction of the krypton-containing transparent conductive layer (10) against a target made of the material of the argon-containing transparent conductive layer. Also, in the sputtering, the substrate layer (2) (the substrate layer (2) having the krypton-containing transparent conductive layer (10)) is in close contact along the circumferential direction of the film-forming roll. In addition, at this time, in addition to argon gas, a reactive gas such as oxygen may be present.

[0128] The partial pressure of argon gas in the sputtering apparatus is, for example, 0.1 Pa or more, preferably 0.3 Pa or more, and also, for example, 10 Pa or less, preferably 5 Pa or less, more preferably 1 Pa or less.

[0129] The amount of reactive gas introduced is the same as the amount of reactive gas introduced in the fourth process described above.

[0130] The pressure within the sputtering apparatus is substantially the sum of the partial pressures of the argon gas and the reactive gas. The power source is the same as the power source in the fourth process described above. The discharge output along the long side of the target is the same as the discharge output along the long side of the target in the fourth process described above.

[0131] Then, the material of the argon-containing transparent conductive layer that is ejected from the target by sputtering is deposited on the krypton-containing transparent conductive layer (10). At this time, since thermal energy is generated, when forming the argon-containing transparent conductive layer, the argon-containing transparent conductive layer is cooled by cooling the krypton-containing transparent conductive layer (10) (substrate layer (2)) by means of a film-forming roll, thereby suppressing the crystallization of the argon-containing transparent conductive layer.

[0132] The temperature of the film-forming roll is the same as the temperature of the film-forming roll in the fourth process described above.

[0133] Thus, an amorphous argon-containing transparent conductive layer is placed on one side in the thickness direction of the krypton-containing transparent conductive layer (10).

[0134] In addition, as mentioned above, since argon gas is used as the sputtering gas, argon atoms originating from the argon gas are introduced into the argon-containing transparent conductive layer.

[0135] As described above, by the fourth and fifth processes, an amorphous krypton-containing transparent conductive layer (10) and an amorphous argon-containing transparent conductive layer are arranged in sequence on one side of the thickness direction of the substrate layer (2). By doing so, an amorphous transparent conductive layer (1) (an amorphous krypton-containing transparent conductive layer (10) and an amorphous argon-containing transparent conductive layer) is arranged on one side of the thickness direction of the substrate layer (2).

[0136] <Process 3>

[0137] In the third process, the amorphous transparent conductive layer (1) is heated. For example, the amorphous transparent conductive layer (1) is heated by a heating device (e.g., an infrared heater and a hot air oven).

[0138] The heating temperature is, for example, 80°C or higher, preferably 110°C or higher, and also, for example, less than 200°C, preferably 180°C or lower. In addition, the heating time is, for example, 1 minute or more, preferably 10 minutes or more, more preferably 30 minutes or more, and also, for example, 24 hours or less, preferably 4 hours or less, more preferably 2 hours or less.

[0139] Thus, as shown in FIG. 3E, the amorphous transparent conductive layer (1) is crystallized to form a crystalline transparent conductive layer (1).

[0140] Thus, a transparent conductive layer (1) is obtained, and a transparent conductive film (20) having a substrate layer (2) and a transparent conductive layer (1) in sequence is obtained.

[0141] After that, the transparent conductive layer (1) may be patterned. Patterning is performed, for example, by etching.

[0142] When the transparent conductive layer (1) is patterned, the transparent conductive layer (1) has a pattern shape. If the transparent conductive layer (1) has a pattern shape, the pattern shape can be freely designed.

[0143] 2. Second embodiment

[0144] <Transparent Challenge Layer>

[0145] The transparent conductive layer (1) is made of a krypton-containing transparent conductive layer (10), as shown in FIG. 5.

[0146] The krypton-containing transparent conductive layer (10) is the same as the krypton-containing transparent conductive layer (10) of the first embodiment described above.

[0147] The total light transmittance of the transparent conductive layer (1) is the same as the total light transmittance of the first embodiment described above.

[0148] The thickness of the transparent conductive layer (1) is the same as the thickness of the first embodiment described above.

[0149] The resistivity, surface resistance, and half-width of the X-ray diffraction peak of the transparent conductive layer (1) are the same as the surface resistance and half-width of the X-ray diffraction peak of the first embodiment.

[0150] Transparent conductive film

[0151] As shown in FIG. 6, the transparent conductive film (20) comprises a substrate layer (2) and a transparent conductive layer (1) (a transparent conductive layer containing krypton (10)) in sequence toward one side in the thickness direction. More specifically, the transparent conductive film (20) comprises a substrate layer (2) and a transparent conductive layer (1) (a transparent conductive layer containing krypton (10)) disposed on the upper surface (one side in the thickness direction) of the substrate layer (2). Preferably, the transparent conductive film (20) comprises only the substrate layer (2) and the transparent conductive layer (1) (a transparent conductive layer containing krypton (10)).

[0152] Method for manufacturing a transparent conductive layer and a transparent conductive film

[0153] A method for manufacturing a transparent conductive layer (1) and a transparent conductive film (20) comprises a first process of preparing a substrate layer (2), a second process of placing a transparent conductive layer (1) on one side in the thickness direction of the substrate layer (2), and a third process of heating the transparent conductive layer (1).

[0154] <Process 1>

[0155] In the first process, as shown in FIG. 7A, a substrate layer (2) is prepared in the same way as in the first embodiment described above.

[0156] <Process 2>

[0157] In the second process, a transparent conductive layer (1) is placed on one side in the thickness direction of the substrate layer (2) (hard coat layer).

[0158] When manufacturing the transparent conductive layer of the second embodiment and the transparent conductive film having the transparent conductive layer, the fifth step of placing the krypton-free transparent conductive layer (11) is not performed in the second process. In short, in the second process, only the fourth step of placing the krypton-containing transparent conductive layer (10) is performed.

[0159] In the fourth process, as shown in FIG. 7B, a krypton-containing transparent conductive layer (10) is placed on one side in the thickness direction of the substrate layer (2) in the same manner as in the first embodiment described above. By doing so, a transparent conductive layer (1) is placed on one side in the thickness direction of the substrate layer (2).

[0160] <Process 3>

[0161] In the third process, as shown in FIG. 7C, the amorphous transparent conductive layer (1) is heated in the same manner as in the first embodiment described above. As a result, the amorphous transparent conductive layer (1) is crystallized, and a crystalline transparent conductive layer (1) is formed.

[0162] Thus, a transparent conductive layer (1) is obtained, and a transparent conductive film (20) having a substrate layer (2) and a transparent conductive layer (1) in sequence is obtained.

[0163] 3. Effects of Action

[0164] The transparent conductive layer (1) has a ratio of the size of the crystallites in the (440) plane to the size of the crystallites in the (400) plane of 0.80 or more. Therefore, the resistivity can be lowered.

[0165] Also, the transparent conductive film (20) has a transparent conductive layer (1). Therefore, the resistivity can be lowered.

[0166] In particular, when the transparent substrate (3) is an organic polymer film (e.g., a film made of the material of the transparent substrate (3) above), the transparent conductive layer (1) cannot be crystallized at a high temperature, and the crystallization of the transparent conductive layer (1) may be inhibited by the gas absorbed by the organic polymer film. Therefore, it may be difficult to achieve low resistivity.

[0167] Meanwhile, this transparent conductive layer (1) has a ratio of the size of the crystallites on the (440) plane to the size of the crystallites on the (400) plane of 0.80 or more. Therefore, even if the transparent substrate (3) is an organic polymer film, the resistivity can be lowered.

[0168] Also, in the method for manufacturing a transparent conductive layer (1) and a transparent conductive film (20), in the fourth step of the second step, an amorphous transparent conductive layer (1) (a transparent conductive layer containing krypton (10)) is formed by sputtering in the presence of krypton gas.

[0169] Typically, when an amorphous transparent conductive layer (1) is placed by the sputtering method, a sputtering gas is introduced into the amorphous transparent conductive layer (1).

[0170] However, in this method, krypton gas with a larger atomic weight than argon is used as the sputtering gas instead of the commonly used argon. Because of this, the introduction of krypton atoms into the amorphous transparent conductive layer (1) can be suppressed.

[0171] And, such an amorphous transparent conductive layer (1) becomes a crystalline transparent conductive layer (1) in the third process.

[0172] The crystalline transparent conductive layer (1) (krypton-containing transparent conductive layer (10)) contains krypton atoms, but as described above, the amount of krypton atoms introduced is suppressed. Therefore, when the amorphous transparent conductive layer (1) is heated, the crystal growth properties of the transparent conductive layer (1) are particularly excellent. In this way, the crystallite size ratio of the transparent conductive layer (1) can be set to a predetermined range. As a result, a transparent conductive layer (1) with low resistivity and a transparent conductive film (20) can be manufactured.

[0173] 4. Article with a transparent conductive layer film attached and article with a transparent conductive layer attached

[0174] A transparent conductive film (20) may be placed on one side in the thickness direction of a part (31) to obtain an article (30) with a transparent conductive layer film attached.

[0175] As shown in FIG. 8, the article (30) with the transparent conductive layer film attached comprises a component (31) and a transparent conductive film (20) in sequence toward one side in the thickness direction. In detail, the article (30) with the transparent conductive layer film attached comprises a component (31), a substrate layer (2), and a transparent conductive layer (1) in sequence toward one side in the thickness direction.

[0176] In addition, FIG. 8 shows an article (30) with a transparent conductive layer film attached having a transparent conductive layer (1) of the second embodiment.

[0177] The article (30) is not particularly limited and may include, for example, elements, components, and devices. More specifically, elements may include, for example, dimming elements and photoelectric conversion elements. Dimming elements may include, for example, current-driven dimming elements and electric field-driven dimming elements. Current-driven dimming elements may include, for example, electrochromic (EC) dimming elements. Electric field-driven dimming elements may include, for example, PDLC (polymer dispersed liquid crystal) dimming elements, PNLC (polymer network liquid crystal) dimming elements, and SPD (suspended particle device) dimming elements. Photoelectric conversion elements may include, for example, solar cells. Solar cells may include, for example, organic thin-film solar cells, perovskite solar cells, and dye-sensitized solar cells. Components may include, for example, electromagnetic shielding components, heat wire control components, heater components, lighting, and antenna components. Examples of devices include touch sensor devices and image display devices.

[0178] An article (30) with a transparent conductive layer film attached is obtained, for example, by bonding a component (31) and a substrate layer (2) of a transparent conductive film (20) through a fixing functional layer.

[0179] Examples of fixing functional layers include adhesive layers and adhesive layers.

[0180] As for the fixing functional layer, any material having transparency can be used without any particular material restrictions. The fixing functional layer is preferably formed of a resin. Examples of resins include acrylic resin, silicone resin, polyester resin, polyurethane resin, polyamide resin, polyvinyl ether resin, vinyl acetate / vinyl chloride copolymer, modified polyolefin resin, epoxy resin, fluoropolymer, natural rubber, and synthetic rubber. In particular, acrylic resin is preferably selected as the resin from the view that it has excellent optical transparency, exhibits adhesive properties such as suitable wettability, cohesiveness, and adhesion, and also has excellent weather resistance and heat resistance.

[0181] In the fixing functional layer (resin forming the fixing functional layer), known corrosion inhibitors and migration inhibitors (e.g., materials disclosed in Japanese Patent Publication No. 2015-022397) may be added to suppress corrosion and migration of the transparent conductive layer (1). In addition, in the fixing functional layer (resin forming the fixing functional layer), known ultraviolet absorbers may be added to suppress deterioration of the article (30) with the transparent conductive layer film attached during outdoor use. Examples of ultraviolet absorbers include benzophenone-based compounds, benzotriazole-based compounds, salicylic acid-based compounds, oxalate anilide-based compounds, cyanoacrylate-based compounds, and triazine-based compounds.

[0182] In addition, a cover layer may be placed on the upper surface of the transparent conductive layer (1) in the article (30) to which the transparent conductive layer film is attached.

[0183] The cover layer is a layer that covers the transparent conductive layer (1), and can improve the reliability of the transparent conductive layer (1) and suppress functional deterioration caused by scratches.

[0184] The cover layer is preferably a dielectric. The cover layer is formed from a mixture of a resin and an inorganic material. Examples of resins include the resins exemplified in the fixing functional layer. The inorganic material is composed of a composition containing, for example, inorganic oxides such as silicon oxide, titanium oxide, niobium oxide, aluminum oxide, zirconium dioxide, and calcium oxide, and fluorides such as magnesium fluoride.

[0185] In addition, a corrosion inhibitor, a migration inhibitor, and a UV absorber may be added to the cover layer (a mixture of resin and inorganic materials) in the same way as the adhesive functional layer described above.

[0186] Also, although not shown, by bonding the transparent conductive layer (1) in the transparent conductive film (20) with the part (31) and the transparent conductive film (20) through a fixing functional layer, an article (30) with a transparent conductive layer film attached can be obtained.

[0187] An article (30) with a transparent conductive film attached has a transparent conductive film (20). Therefore, the resistivity can be lowered.

[0188] In addition, a transparent conductive layer (1) may be placed on one side in the thickness direction of the part (31) to obtain an article (40) with a transparent conductive layer attached.

[0189] As shown in FIG. 9, an article (40) with a transparent conductive layer attached comprises a component (31) and a transparent conductive layer (1) in sequence toward one side in the thickness direction. In detail, an article (40) with a transparent conductive layer attached comprises a component (31), a krypton-containing transparent conductive layer (10), and a krypton-free transparent conductive layer (11) in sequence toward one side in the thickness direction.

[0190] In addition, FIG. 9 shows an article (40) with a transparent conductive layer attached, having a transparent conductive layer (1) of the second embodiment.

[0191] An article (40) with a transparent conductive layer attached is obtained by placing a transparent conductive layer (1) on one side in the thickness direction of a part (31) by sputtering, or by transferring a transparent conductive layer (1) from a transparent conductive film (20) on one side in the thickness direction of a part (31).

[0192] In addition, the component (31) and the transparent conductive layer (1) may be bonded together by interposing the adhesive functional layer.

[0193] In addition, a cover layer may be placed on the upper surface of the transparent conductive layer (1) in the article (40) to which the transparent conductive layer is attached.

[0194] An article (40) with a transparent conductive layer attached has a transparent conductive layer (1). Therefore, the resistivity can be lowered.

[0195] 5. Variation Example

[0196] In the modified example, the same reference numerals are assigned to the same components and processes as in the first and second embodiments, and their detailed descriptions are omitted. In addition, the modified example may exhibit the same functional effects as the first and second embodiments, except as not specified. Furthermore, the first embodiment, the second embodiment, and the modified example may be appropriately combined.

[0197] In the above description, the transparent conductive layer (1) contains krypton atoms. In other words, the transparent conductive layer (1) is provided with a krypton-containing transparent conductive layer (10). Meanwhile, the transparent conductive layer (1) does not have to contain krypton atoms. In the case where the transparent conductive layer (1) does not contain krypton atoms, for example, a noble gas with an atomic weight greater than that of a krypton atom is used alone, or a noble gas with an atomic weight smaller than that of a krypton atom is mixed with a noble gas with an atomic weight greater than that of a krypton atom to form an amorphous transparent conductive layer (1) as a sputtering gas, and then, by heating, the crystallite size ratio of the transparent conductive layer (1) can be set to a predetermined range.

[0198] In the above description, the case where the functional layer (4) is a hard coat layer was described, but the functional layer (4) may also be an optical adjustment layer.

[0199] The optical adjustment layer is a layer that adjusts the optical properties (e.g., refractive index) of the conductive film (10) in order to suppress pattern visibility of the transparent conductive layer (1) or suppress reflection at the interface within the transparent conductive film (20) while ensuring excellent transparency of the transparent conductive film (20).

[0200] The optical adjustment layer is formed, for example, from an optical adjustment composition.

[0201] The optical adjustment composition contains, for example, a resin and particles. Examples of resins include the resins exemplified in the hard coat composition. Examples of particles include the particles exemplified in the hard coat composition. The optical adjustment composition may be a resin alone or an inorganic alone. Examples of resins exemplified in the hard coat composition. In addition, examples of inorganic materials include metalloid oxides and / or metal oxides such as silicon oxide, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. It is not necessary to specify whether the metalloid oxides and / or metal oxides are stoichiometric in composition.

[0202] The thickness of the optical adjustment layer is, for example, 1 nm or more, preferably 5 nm or more, more preferably 10 nm or more, and also, for example, 200 nm or less, preferably 100 nm or less. The thickness of the optical adjustment layer can be calculated, for example, based on the wavelength of the interference spectrum observed using an instantaneous multiphotometric system. In addition, the thickness may be determined by observing the cross-section of the optical adjustment layer using FE-TEM.

[0203] Also, as a functional layer (4), a hard coat layer and an optical adjustment layer may be used in combination (a multilayer including a hard coat layer and an optical adjustment layer).

[0204] In the above description, in the first embodiment, the transparent conductive film (20) is provided with a substrate layer (2), a krypton-containing transparent conductive layer (10), and a krypton-free transparent conductive layer (11) in order toward one side in the thickness direction. Meanwhile, the order of the krypton-containing transparent conductive layer (10) and the krypton-free transparent conductive layer (11) is not particularly limited. In detail, the transparent conductive film (20) may be provided with a substrate layer (2), a krypton-free transparent conductive layer (11), and a krypton-containing transparent conductive layer (10) in order toward one side in the thickness direction. In order to manufacture such a transparent conductive film (20), the fourth process is performed after the fifth process in the second process.

[0205] In the above description, the krypton-containing transparent conductive layer (10) contains a metal oxide and a trace amount of krypton atoms, but the krypton-containing transparent conductive layer (10) may also contain a trace amount of a noble gas other than krypton atoms (e.g., argon, xenon). In such cases, in the krypton-containing transparent conductive layer (10), trace amounts of krypton atoms and a noble gas other than krypton atoms exist in the metal oxide matrix. Such a krypton-containing transparent conductive layer (10) can be manufactured, for example, by using a combination of krypton gas and a noble gas other than krypton atoms as a sputtering gas.

[0206] In the above description, in the third process, the transparent conductive layer (1) is crystallized by heating the amorphous transparent conductive layer (1), but the amorphous transparent conductive layer (1) may also be crystallized by leaving it undisturbed for a long period (e.g., 5 days or more) at a temperature below room temperature (e.g., 40°C or lower).

[0207] In the above description, the article (30) with the transparent conductive layer film attached comprises the article (31), the substrate layer (2), and the transparent conductive layer (1) in order toward one side in the thickness direction, but the article (30) with the transparent conductive layer film attached may also comprise the substrate layer (2), the transparent conductive layer (1), and the article (31) in order toward one side in the thickness direction.

[0208] In the above description, the article (40) with the transparent conductive layer attached comprises the article (31), the krypton-containing transparent conductive layer (10), and the krypton-free transparent conductive layer (11) in sequence toward one side in the thickness direction, but the article (40) with the transparent conductive layer attached may also comprise the krypton-containing transparent conductive layer (10), the krypton-free transparent conductive layer (11), and the article (31) in sequence toward one side in the thickness direction.

[0209] Examples

[0210] Specific numerical values ​​of mixing ratios (content ratios), physical property values, parameters, etc. used in the following descriptions may be replaced with the upper limit values ​​(numerical values ​​defined as “less than” or “less than”) or lower limit values ​​(numerical values ​​defined as “greater than” or “greater than”) of the corresponding mixing ratios (content ratios), physical property values, parameters, etc. described in the “forms for carrying out the invention” above. Additionally, unless specifically stated otherwise in the following descriptions, “parts” and “%” are based on mass.

[0211] 1. Manufacture of transparent conductive layer and transparent conductive film

[0212] Example 1

[0213] <Process 1>

[0214] A hard coat composition (UV-curable resin containing acrylic resin) was applied to one side in the thickness direction of a long PET film (thickness 50 μm, manufactured by Toray Corporation) used as a transparent substrate to form a coating film. Next, the coating film was cured by UV irradiation. In this way, a hard coat layer (thickness 2 μm) was formed. By this, a substrate layer was prepared.

[0215] <Process 2>

[0216] Next, an amorphous transparent conductive layer (krypton-containing transparent conductive layer) with a thickness of 130 nm was deposited on one side in the thickness direction of the substrate layer (hard coat layer) by reactive sputtering. In the reactive sputtering method, a sputtering device (DC magnetron sputtering device) capable of performing a film deposition process in a roll-to-roll manner was used.

[0217] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used as the target. A DC power source was used to apply voltage to the target. The horizontal magnetic field strength on the target was set to 90 mT. In the sputtering apparatus, the substrate layer was adhered along the circumferential direction of the deposition roll. The temperature of the deposition roll was set to -5 ℃. In addition, the achievable vacuum level in the deposition chamber equipped with the sputtering deposition apparatus was 0.8 × 10⁻⁶ -4 After vacuuming the sputtering apparatus until the pressure reached Pa, krypton as a sputtering gas and oxygen as a reactive gas were introduced into the apparatus, and the atmospheric pressure inside the apparatus was set to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of krypton and oxygen introduced into the sputtering apparatus was approximately 2.5 flow%. As shown in Fig. 4, the amount of oxygen introduced falls within region X of the resistivity-oxygen introduction curve, where the resistivity of the amorphous krypton-containing transparent conductive layer is 6.6 × 10⁻⁶. -4The resistivity-oxygen introduction curve shown in Fig. 4 can be prepared by first investigating the dependence of the resistivity of an amorphous krypton-containing transparent conductive layer on the amount of oxygen introduced, when the amorphous krypton-containing transparent conductive layer is formed by reactive sputtering under conditions other than the amount of oxygen introduced as above.

[0218] <Process 3>

[0219] An amorphous transparent conductive layer was crystallized by heating in a hot air oven. The heating temperature was set to 165°C, and the heating time was set to 1 hour.

[0220] Thus, a transparent conductive film was obtained together with a transparent conductive layer.

[0221] Example 2

[0222] A transparent conductive film was obtained together with a transparent conductive layer in the same manner as in Example 1.

[0223] However, the second process was modified as follows.

[0224] <Process 2>

[0225] In the second process, the fourth and fifth processes were carried out in that order.

[0226] <Process 4>

[0227] In the fourth process, a krypton-containing transparent conductive layer was disposed on one side in the thickness direction of the substrate layer, in the same manner as in the second process of Example 1.

[0228] However, the amount of oxygen introduced is such that the resistivity of the amorphous krypton-containing transparent conductive layer is 6.5×10 -4 It was adjusted to Ω·cm (the ratio of oxygen introduction amount to the total introduction amount of krypton and oxygen was approximately 2.6 flow%). In addition, the thickness of the amorphous krypton-containing transparent conductive layer was changed according to Table 1.

[0229] <Process 5>

[0230] In the fifth process, a krypton-free transparent conductive layer (argon-containing transparent conductive layer) was placed on one side in the thickness direction of the krypton-containing transparent conductive layer in the same manner as the second process.

[0231] However, the sputtering gas was changed to argon gas, and the pressure inside the sputtering film deposition apparatus was changed to 0.4 Pa. In addition, the pressure inside the sputtering film deposition apparatus was changed to 0.4 Pa. Also, the thickness of the amorphous argon-containing transparent conductive layer was changed according to Table 1.

[0232] Example 3

[0233] A transparent conductive film was obtained together with a transparent conductive layer in the same manner as in Example 2.

[0234] However, the krypton-containing transparent conductive layer and the argon-containing transparent conductive layer were changed according to Table 1.

[0235] Example 4

[0236] A transparent conductive film was obtained together with a transparent conductive layer in the same manner as in Example 1.

[0237] However, the sputtering gas was changed to a mixed gas of krypton and argon (98 vol% krypton, 2 vol% argon). In addition, the thickness of the amorphous krypton-containing transparent conductive layer was changed according to Table 1.

[0238] Comparative Example 1

[0239] A transparent conductive film was obtained together with a transparent conductive layer in the same manner as in Example 1.

[0240] However, in the second process, the sputtering gas was changed to argon gas. In addition, the pressure inside the sputter film deposition apparatus was changed to 0.4 Pa.

[0241] 2. Evaluation

[0242] Thickness of the transparent conductive layer

[0243] The thickness of the transparent conductive layer of each example and each comparative example was measured by FE-TEM observation. Specifically, first, samples for cross-sectional observation of the transparent conductive layer of each example and each comparative example were prepared by the FIB microsampling method. For the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the thickness of the transparent conductive layer in the cross-sectional observation samples was measured by FE-TEM observation. For FE-TEM observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0244] In addition, in Examples 2 and 3, the thickness of the krypton-containing transparent conductive layer was measured by preparing a sample for cross-sectional observation from the krypton-containing transparent conductive layer before placing the argon-containing transparent conductive layer on one side in the thickness direction of the krypton-containing transparent conductive layer, and observing the sample using FE-TEM. In addition, the thickness of the argon-containing transparent conductive layer was calculated by subtracting the thickness of the krypton-containing transparent conductive layer from the thickness of the transparent conductive layer.

[0245] <Size of the crystallizer in plane (440), and size of the crystallizer in plane (400)>

[0246] The X-ray diffraction peaks of the transparent conductive layer of each example and each comparative example were obtained by X-ray diffraction measurement using a horizontal X-ray diffraction device (product name “SmartLab”, manufactured by Rigaku Co., Ltd.) based on the following measurement conditions. In addition, the X-ray peak profiles were obtained by subtracting the background originating from the PET film of each example and each comparative example (a PET film heated under the same conditions as the transparent conductive layer of each example and each comparative example). Then, using analysis software (software name “SmartLab Studio II”), an X-ray diffraction peak profile corresponding to the (400) plane was created such that 2θ was in the range of 34.5° to 36.0°. In addition, an X-ray diffraction peak profile corresponding to the (440) plane was created such that 2θ was in the range of 49.8° to 51.8°. The profiles of each generated X-ray diffraction peak were fitted (peak shape: split Pearson VII function, background type: B-spline, fitting condition: automatic) to determine the crystallite size (Å) in the (440) plane and the crystallite size (Å) in the (400) plane. Additionally, the ratio of the crystallite size in the (440) plane to the crystallite size in the (400) plane was determined. The results are shown in Table 1.

[0247] [Measurement Conditions]

[0248] Parallel beam optical arrangement

[0249] Light source: CuKα line (Wavelength: 1.54059 Å)

[0250] Output: 45 kV, 200 mA

[0251] Incident side slit system: Solar slit 5.0°

[0252] Incident slit: 1,000 mm

[0253] Receiving slit: 20,100 mm

[0254] Receiving side slit: Parallel Slit Analyzer (PSA) 0.114 deg.

[0255] Detector: Multidimensional Pixel Detector Hypix-3000

[0256] Sample stage: A sample in which glass is laminated to a transparent substrate of a transparent conductive film with an adhesive layer interposed therebetween is placed on a sample plate (4-inch wafer sample plate).

[0257] Scan Axis: 2θ / θ (Out of Plane measurement)

[0258] Step interval: 0.02°

[0259] Measurement speed: 0.8° / min

[0260] Measurement range: 10°–90°

[0261] Resistivity

[0262] The resistivity was measured for the transparent conductive layer of each example and each comparative example. Specifically, the surface resistance of the transparent conductive layer was measured by the four-terminal method in accordance with JIS K 7194 (1994). Subsequently, the resistivity (Ω·cm) was calculated by multiplying the surface resistance value by the thickness of the transparent conductive layer. The results are shown in Table 1.

[0263] <Confirmation of Kr atoms within the transparent conductive layer>

[0264] It was confirmed as follows that each transparent conductive layer in each example contains Kr atoms. First, using a scanning fluorescence X-ray analyzer (product name "ZSX Primus IV", manufactured by Rigaku Co., Ltd.), fluorescence X-ray analysis measurements were repeated five times under the following measurement conditions, and the average value of each scanning angle was calculated to create an X-ray spectrum. Then, by confirming that a peak appeared near a scanning angle of 28.2° in the created X-ray spectrum, it was confirmed that the transparent conductive layer contains Kr atoms.

[0265] [Measurement Conditions]

[0266] Spectrum ; Kr-KA

[0267] Measured diameter: 30 mm

[0268] Atmosphere: Vacuum

[0269] Target: Rh

[0270] Tube voltage: 50 kV

[0271] Tube current: 60 mA

[0272] Primary filter: Ni40

[0273] Scan angle (deg): 27.0 ~ 29.5

[0274] Step (deg) : 0.020

[0275] Speed ​​(deg / min): 0.75

[0276] Attenuator : 1 / 1

[0277] Slit : S2

[0278] Spectroscopic crystal: LiF (200)

[0279] Detector: SC

[0280] PHA : 100 ∼ 300

[0281]

[0282] Furthermore, although the above invention has been provided as an exemplary embodiment of the present invention, this is merely an example and should not be interpreted restrictively. Variations of the present invention that are obvious to those skilled in the art are included in the claims set forth below.

[0283] Industrial applicability

[0284] The transparent conductive layer and transparent conductive film of the present invention are preferably used, for example, in an electromagnetic shielding member, a heat wire control member, a heater member, a lighting member, an antenna member, a touch sensor device, and an image display device. Explanation of the symbols

[0285] 1 : Transparent conductive layer 2 : Base layer 20: Transparent conductive film

Claims

Claim 1 A transparent conductive layer, wherein the ratio of the size of the crystallites in the (440) plane of the transparent conductive layer to the size of the crystallites in the (400) plane is 0.80 or greater. Claim 2 A transparent conductive layer, wherein the ratio of the size of the crystallites in the (440) plane of the transparent conductive layer to the size of the crystallites in the (400) plane is 0.80 or greater, and the transparent conductive layer is a sputtering layer. Claim 3 A transparent conductive layer containing krypton atoms, according to claim 1 or 2. Claim 4 A transparent conductive layer containing an indium tin complex oxide, in accordance with claim 1 or 2. Claim 5 In claim 1 or 2, the resistivity is 2.3×10 -4 Transparent conductive layer with less than Ω·cm. Claim 6 A transparent conductive layer having a pattern shape according to claim 1 or 2. Claim 7 A transparent conductive film comprising a substrate layer and a transparent conductive layer described in claim 1 or 2 in sequence toward one side in the thickness direction.

Citation Information

Patent Citations

  • Transparent conductive film and method for producing same

    KR1020170008196A

  • Transparent conductive film and manufacturing method therefor

    US20130280554A1

  • Organic light-emitting device

    WO2016088378A1

  • Manufacture of transparent conductive film

    JP1993334924A

  • Fibrous fine metal oxide particles

    JP2004043293A