Composition using functionalized graphene for deck facility
Functionalized graphene mixed with resin addresses the issues of metal joists' weight and corrosion by providing a lightweight, salt-resistant alternative with enhanced strength and safety for deck facilities.
Patent Information
- Application Number
- KR1020230053739
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Existing metal joists used in deck facilities are heavy, prone to corrosion, especially in coastal areas due to salt exposure, leading to reduced strength and safety hazards.
A composition using functionalized graphene mixed with resin, comprising 75-80% waste synthetic resin, 17.5-20.5% calcium carbonate, 2.0-3.0% zinc, and 0.5-1.5% graphene, which is resistant to salt and lightweight, enhancing strength and heat dissipation.
Functionalized graphene provides a lightweight, corrosion-resistant alternative to metal joists, improving strength and safety by combining with resin, offering improved workability and durability.
Smart Images

Figure 112023046212509-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a composition for deck facilities using functionalized graphene, and more specifically, to a composition for deck facilities using functionalized graphene that overcomes the problems of existing metals such as iron, stainless steel, and aluminum, which are made of metal, are heavy, making movement inconvenient and significantly reducing workability, and are susceptible to salt, causing corrosion and making long-term use impossible. It possesses characteristics such as resistance to salt and improved mobility and work efficiency due to lightweighting, and effects such as increased strength, thereby enabling it to be used as a substitute for the main materials of metal lower joists, railings, and fences (hereinafter referred to as deck facilities). Background Technology
[0003] In general, composite wood decking is primarily used as a flooring finish for indoor and outdoor spaces. It has the advantage of being not only eco-friendly compared to other materials but also efficiently absorbing vibrations to create a quiet environment, while also providing a visually soft and comfortable feel.
[0004] These existing synthetic wood decks have excellent durability, are easy to maintain, and have the advantage of reducing fatigue due to their elasticity and shock absorption capabilities when walking. As shown in FIG. 1a, the installation structure of the aforementioned existing synthetic wood deck mainly uses a construction method in which, after leveling the floor surface of the installation site, metal joists (400) are connected to each other in a horizontal or vertical direction to form a certain shape, and then synthetic wood (100) is fitted onto them in an assembly manner, and then the joists (400) and synthetic wood (100) are combined and fixed using fastening means (300) such as nails, screws, and bolts.
[0005] However, the above-mentioned joists (400) are made of metal and are susceptible to moisture rising from the ground, so they have the disadvantage of being susceptible to corrosion and cannot be used for a long time. In particular, in coastal areas close to the sea, corrosion caused by salt accelerates and loses function, so the composite wood (100) cannot be firmly held in place. Consequently, when installing the composite wood (100), the deck facilities used together with it face a problem of serious safety accidents due to this lifting phenomenon and reduced strength. Prior art literature
[0007] Republic of Korea Published Patent Application No. 2011-0039900 Republic of Korea Published Patent Application No. 2012-0072622 The problem to be solved
[0008] The present invention, devised in consideration of these conventional problems, provides a composition for deck facilities using functionalized graphene that can be used as a substitute for metal joists installed at the bottom of a deck and for railings and fences, etc., by mixing functionalized graphene with a resin. This functionalized graphene improves physical properties such as strength by combining graphite or graphene with silicon (Si), boron nitride (BN), nickel (Ni), aluminum (Al), etc., and is resistant to salt, lightweight, and has excellent heat dissipation effects. means of solving the problem
[0010] The objective of the present invention described above is achieved by a composition for deck facilities using functionalized graphene, characterized by being formed by mixing 75-80% by weight of waste synthetic resin, 17.5-20.5% by weight of calcium carbonate, 2.0-3.0% by weight of zinc, and 0.5-1.5% by weight of graphite or graphene.
[0011] This is achieved by a composition for deck facilities using functionalized graphene, characterized in that the zinc is zinc stearate (Zn-St).
[0012] The above graphite or graphene is achieved by a composition for deck facilities using functionalized graphene, characterized in that the graphite or graphene is prepared by adding 2 to 3 parts by weight of a metal oxide with a particle size of 100 mesh or less to 100 parts by weight of graphite or graphene with a particle size of 250 to 300 mesh in a melting furnace, raising the temperature to 200 to 500°C under a gas atmosphere to completely melt the graphene and metal additive for 1 to 3 hours, then lowering the temperature to 200°C or lower, and annealing for 2 to 3 hours to activate ferrosilicon and silicon groups.
[0013] Here, this is achieved by a composition for deck facilities using functionalized graphene, characterized in that the metal oxide is selected from the group consisting of silicon (Si), boron nitride (BN), nickel (Ni), aluminum (Al), or metal oxides thereof.
[0014] Here, this is achieved by a composition for deck facilities using functionalized graphene, characterized in that the metal additive is in the form of a powder with a particle size of 100 to 150 mesh. Effects of the invention
[0016] The present invention has the advantage of being able to be used as a substitute for metal joists installed at the bottom when installing a deck, and for railings and fences, etc., by mixing functionalized graphene with a resin, which improves physical properties such as strength by combining Si, BN, Ni, Al, etc. with graphite or graphene, is resistant to salt, and has excellent lightweight and heat dissipation effects. Brief explanation of the drawing
[0018] FIG. 1 is an SEM image of graphene functionalized using a metal additive according to an embodiment of the present invention and a graph showing the measured binding energy (eV). Specific details for implementing the invention
[0019] Preferred embodiments of the present invention are described in more detail below with reference to the accompanying drawings. However, it should be understood that the present invention may be implemented in a number of different forms and is not limited to the described embodiments.
[0020] Looking at the manufacturing method of the composition for deck facilities using functionalized graphene according to the present invention, calcium carbonate, waste synthetic resin, graphite or graphene, and zinc are mixed, placed in an extruder, and molded into a specific size and shape by applying pressure at a constant temperature and time.
[0021] The composition for a deck facility using functionalized graphene according to the present invention is a mixture formed by mixing 75-80% by weight of waste synthetic resin, 17.5-20.5% by weight of calcium carbonate (CaCO3), 2.0-3.0% by weight of zinc, and 0.5-1.5% by weight of graphene.
[0022] Preferably, calcium carbonate (CaCO3), waste synthetic resin, and graphene are mixed first, followed by the addition of zinc. The reason for mixing the calcium carbonate (CaCO3), waste synthetic resin, and graphene first to form a mixture, and then adding zinc, is that this has the effect of enhancing transparency, preservation, and heat resistance.
[0023] At this time, the waste synthetic resin used as a base to form a lightweight structure and to provide flame retardancy, preventing deformation and discoloration and fading, is used in an amount of 75 to 80 weight percent. This is because if the waste synthetic resin is 75 weight percent or less, there are problems with gloss (prevention of discoloration and fading), vaporization, physical strength (deformation), and durability enhancement, and if the waste synthetic resin is 80 weight percent or more, there are problems with the properties being too strong or the effectiveness being reduced.
[0024] Meanwhile, when using 17.5 to 20.5 weight percent of calcium carbonate (CaCO3) to provide the above-mentioned binder and moldability, if the calcium carbonate (CaCO3) is 17.5 weight percent or less, there is a problem with the function as a binder, such as binder and moldability, being reduced, and if the calcium carbonate (CaCO3) is 20.5 weight percent or more, there is a problem with cracks in the binder and inside or on the surface of the molded body.
[0025] The graphene used is 0.5 to 1.5 weight percent, which prevents discoloration and fading, has excellent durability and flame retardant performance, minimizes the moisture content of the wood powder, and minimizes shrinkage and expansion due to temperature changes. This is because if the graphene is 0.5 weight percent or less, there are problems with tensile strength and elongation, and if the graphene is 1.5 weight percent or more, the tensile strength increases but the elongation decreases.
[0026] Zinc used for preservation purposes is used in an amount of 2.0 to 3.0 weight percent. If the zinc is less than 2.0 weight percent, there is a problem with reduced transparency, preservation, and heat resistance, and if the zinc is more than 3.0 weight percent, there is a problem with surface cracking during the molding of the binder.
[0027] Meanwhile, it is preferable to use zinc stearate for the zinc, and the synthetic resin is to use any one of PP, PE, HLDPE, and LDPE, preferably LDPE, and the reason for using LDPE as the synthetic resin is that it has a linear skeleton effect.
[0028] The method for synthesizing functionalized graphene used in the present invention involves adding 2 to 3 parts by weight of a powdered additive with a particle size of 100 to 150 mesh to 100 parts by weight of graphene with a particle size of 250 to 300 mesh in a melting furnace, raising the temperature to 200 to 500°C under a gas atmosphere, and completely melting it for 1 to 3 hours.
[0029] After completely melting the graphene and additives, the temperature is lowered to 200°C or lower, and then annealed at a temperature range of 400°C to 500°C for 2 to 3 hours to activate the ferrosilicon and silicon groups.
[0030] Here, the graphene structure has various functional groups in addition to ferrosilicon and silicon groups on the top or edges, and as mentioned above, as a method to activate the functional groups, the ferrosilicon and silicon groups of graphene are functionalized with metallic materials to increase the bonding strength with other materials (polymers, etc.) in the future.
[0031] At this time, the graphene used in the melting step is preferably one that satisfies a particle size of 250 to 300 mesh. If graphene outside the above particle size range is used, it may be difficult to control structural performance at the nanoscale, or there may be a problem of reduced flexibility and elasticity due to non-covalent bonding between heterogeneous components.
[0032] Meanwhile, the melting step is carried out under a gas atmosphere, and the process is performed by raising the temperature under an atmosphere of N2, H2, or argon (Ar). Preferably, graphene is introduced into a furnace, then heated for 1 to 2 hours under a nitrogen (N2) gas or argon (Ar) atmosphere at a temperature of 200 to 500°C to activate the functional groups of the graphene, then a functional additive is introduced and hydrogen (H2) is supplied to combine the activated functional groups of the graphene with the functional groups of the functional additive in a hydrogen atmosphere, thereby preparing functionalized graphene.
[0033] Through this process, functionalized graphene combined with functional additives becomes functional graphene that possesses both hydrophilic and hydrophobic properties.
[0034] Here, the method of supplying the N2, H2, and argon (Ar) gases is to use a furnace capable of performing the alloy annealing process in an inert gas and reducing gas environment under high vacuum conditions up to the micro Torr level.
[0035]
[0036] As shown in one example in Table 1 above, by combining desired materials such as BN, Ni, and Al using functionalizing materials present on the top surface and edges of graphene, the properties of BN, Ni, and Al can be exhibited and realized by manufacturing graphene with other powders.
[0037] According to the present invention, the functional additive is a ceramic powder selected from silicon (Si) or boron nitride (BN), or the functional additive is a powdered metal additive selected from the group consisting of nickel (Ni), aluminum (Al), or metal oxides thereof.
[0038] As shown in the attached drawing Fig. 1, when BN, C, and Ni are used as additives to graphene, a is a graph showing SAM images showing the reactivity of graphene with BN added and FT-IR peaks from Raman spectrum analysis of the reaction between graphene and metal BN, b is a graph showing SAM images showing the reaction of graphene with metal BN added and FT-IR peaks from Raman spectrum analysis of the reaction between graphene and metal BN, and c is a graph showing SAM images showing the reactivity of graphene with Ni added and FT-IR peaks from Raman spectrum analysis of the reaction between graphene and metal BN. While general graphene forms energy at 1200 (ev) to form tensile strength among its physical properties, when the additive of the present invention is mixed, the binding energy that forms tensile strength is formed within the range of 180 to 400 (ev), so binding energy can be formed early, thereby shortening the manufacturing time of functionalized graphene.
[0039] At this time, it is preferable to use the ceramic powder or metal oxide in powder form having a fineness within the range of 100 to 150 mesh. If the above particle size threshold is exceeded, it may be difficult for the activated functional groups of graphene and the functional groups of the functional additive to structurally bond, or the reinforcing particles may be easily destroyed during plastic deformation of the composite material using functionalized graphene, resulting in a decrease in tensile strength and ductility.
[0040] According to the present invention, preferably, the activation step involves adding 1 to 3 parts by weight of an oxidizing agent, 0.2 to 0.3 parts by weight of an inoculant, and 0.1 to 0.3 parts by weight of a modifier to 100 parts by weight of graphene. At this time, the oxidizing agent used is magnesium (Mg), the inoculant is iron (Fe), and the modifier is calcium (Ca).
[0041] The above oxidizing agent is a reactive substance that takes electrons from other substances to oxidize them and is itself reduced. If the amount added is less than 1 weight part, it is difficult to expect an effect of enhancing oxidizing power, and if it exceeds 3 weight parts, there is a problem that the effect of enhancing oxidizing power is excessive and a difference in characteristics may occur.
[0042] In addition, the above-mentioned inoculant induces a reaction that promotes nucleation and inhibits growth. If the amount added is less than 0.2 parts by weight, the fine and uniform distribution of the material is not achieved well, resulting in a problem of reduced mechanical properties. If it exceeds 0.3 parts by weight, the bonding strength of the material decreases, and there may be problems with increased workability and residual stress.
[0043]
[0044] As shown in Table 2 above, when paint for steel plates was manufactured by combining functionalized graphene with a polymer and applied, it was confirmed that microcracks appeared within the thin film depending on the type. This is believed to be due to shear stress generated at the interface between the metal thin film and the hard coating caused by shrinkage and expansion during the hard coating curing process, leading to the additional creation and expansion of cracks by these forces.
[0045] In addition, the above modifier induces a reaction that can improve the physical adhesion ability between materials. If the amount added is less than 0.1 parts by weight, there may be a problem with the adhesion ability between materials decreasing, and if it exceeds 0.3 parts by weight, there may be a problem with no significant difference in physical adhesion ability.
[0046] As described above, the mixture is placed in an extruder, and during manufacturing, the temperature of the extruder is maintained at 150 to 180°C, and preferably, the extrusion operation is carried out at 160°C.
[0047] The extrusion method involves supplying the raw material to the extruder and pressurizing the mixture in the pressure pipe to achieve a constant pressure, and then performing a degassing process when the internal temperature of the pressure pipe reaches 120~130℃.
[0048] The reason for performing the above gas evacuation process is to prevent quality degradation caused by cracks inside or on the surface during extrusion molding.
[0049] The present invention has the advantage of being usable as a substitute for metal joists installed underneath decks and as auxiliary materials such as railings and fences by manufacturing synthetic wood by mixing functionalized graphene with resin. This is achieved by combining graphite or graphene with silicon (Si), boron nitride (BN), nickel (Ni), aluminum (Al), etc., to increase physical properties such as tensile strength and elongation, enhance UV blocking effects, provide resistance to salt, and offer excellent lightweight and heat dissipation effects.
Claims
Claim 1 A composition for deck facilities using functionalized graphene, wherein the composition is formed by mixing 75-80% by weight of waste synthetic resin, 17.5-20.5% by weight of calcium carbonate, 2.0-3.0% by weight of zinc, and 0.5-1.5% by weight of graphite or graphene, and wherein the graphite or graphene is prepared by adding 2-3 parts by weight of a metal oxide with a particle size of 100 mesh or less to 100 parts by weight of graphite or graphene with a particle size of 250-300 mesh in a melting furnace, raising the temperature to 200-500°C under a gas atmosphere to completely melt the graphene and the metal additive for 1-3 hours, lowering the temperature to 200°C or lower, and then annealing for 2-3 hours to activate ferrosilicon and silicon groups. Claim 2 A composition for a deck facility using functionalized graphene, characterized in that, in claim 1, the zinc is zinc stearate (Zn-St). Claim 3 delete Claim 4 A composition for a deck facility using functionalized graphene, characterized in that, in claim 1, the metal oxide is selected from the group consisting of silicon (Si), boron nitride (BN), nickel (Ni), aluminum (Al), or metal oxides thereof. Claim 5 A composition for deck facilities using functionalized graphene, characterized in that, in claim 4, the metal oxide is in the form of a powder with a particle size of 100 to 150 mesh.
Citation Information
Patent Citations
Deck plate waterproof method
JP2016053254A
Resin composition with enhanced heat-releasing properties, heat-releasing film, insulating film, and prepreg
KR1020140086581A
A decorative piping and Manufacturing method thereof
KR1020230034485A
Construction, works, cleaning, treatment, material, products, equipment, facility, drone, 3D printer, mobility
KR1020230036637A
Olefin block copolymers, production processes of thesame and use thereof
KR1020020063300A