Complex cement walls for environmental protection of landfills in soft soil areas and construction methods

LAP733AUndetermined Publication Date: 2025-07-25BEIJING GEOENVIRON ENGINEERING & TECHNOLOGY INC (CN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP733
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Filing Date
2018-10-12
Publication Date
2025-07-25

AI Technical Summary

Technical Problem

In landfills in soft soil areas, the anti-seepage performance and strength of the existing anti-seepage walls are reduced when faced with seawater erosion, making it difficult to control the migration and diffusion of pollutants. Moreover, continuous vertical grooves during the construction process will affect the stability of the soil. properties, causing the ground to crack.

Method used

Adopt a composite anti-seepage wall structure, including a flexible core wall (HDPE geomembrane), a plastic wall (optimized plastic concrete pouring) and a supporting wall (high-pressure jet grouting pile), combined with groundwater pumping wells to form a vertical composite anti-seepage wall The main structure controls the migration of pollutants and groundwater levels, and improves environmental safety performance and structural stability.

Benefits of technology

It can effectively prevent the migration and spread of pollutants, improve the stability of the landfill embankment and soil, enhance the resistance to seawater erosion, and ensure the safety of environmental protection and construction safety of the landfill.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The disclosure is a complex concrete wall for environmental protection of a landfill in a soft soil area and a method of constructing the same. The complex concrete wall includes a flexible main wall arranged around the landfill area, the depth of the flexible main wall being sufficient for the flexible main wall to protrude from the ground to be buried in a weak layer, the plastic walls are arranged sequentially on the inner and outer sides of the flexible main wall; the supporting walls are arranged sequentially on the inner side of the inner plastic wall and the outer side of the outer plastic wall; a transition zone is arranged between the inner supporting wall and the landfill, and a drainage pipe is arranged underground in the transition zone.The current disclosure, based on specific procedures, includes: construction of retaining walls, vertical trenching, installation of flexible vertical retaining walls, preparation of plastic concrete according to specific proportions, and construction of plastic structures in a submerged manner. With technical methods, there is a solution that can effectively separate landfills, including hazardous wastes caused by accidental liquid spills, to protect the soil and groundwater on the basis of supporting the stability of the surrounding soil and the foundation of the landfill.
Need to check novelty before this filing date? Find Prior Art

Description

Composite cutoff wall for environmental protection of landfills in soft soil areas and its construction method Technical Field

[0001] This invention relates to a composite impermeable wall for environmental protection of landfill sites in soft soil areas and its construction method. Background Technology

[0002] In existing technologies, with rapid socio-economic development and accelerated urbanization and industrialization, urban waste and industrial waste are increasing dramatically, and the environmental pressure from petrochemical and mining processes is growing. In coastal soft soil areas, due to geological defects and high groundwater levels, hazardous waste landfills pose a significant risk to soil and groundwater if leaks occur during operation, necessitating the construction of HDPE membrane vertical impermeable walls to enhance environmental protection. Continuous vertical trenching in soft soil areas can affect the trench edges and soil, causing displacement and leading to ground cracking.

[0003] In addition, in the prior art, patent application CN102617073A discloses a plastic concrete for seepage prevention walls, including cementitious materials, aggregates, water-reducing agents, and water. High utilization of fly ash in the plastic concrete is achieved by adjusting the aggregate particle size, sand ratio, and water-cement ratio. CN105236901A discloses a plastic concrete for seepage prevention and its preparation method, including cement, bentonite, fly ash, gypsum, clay, fine aggregates, coarse aggregates, redispersible latex powder, sodium carbonate, calcium acrylate, sodium dodecylbenzene sulfonate, sodium silicate, and water. By using a combination of ordinary silicate cement and slag silicate cement, the early strength and impermeability of the plastic concrete are improved; the addition of redispersible latex powder improves the workability and strength of the plastic concrete; and the addition of calcium acrylate further improves the impermeability of the concrete.

[0004] However, the plastic concrete in the above technologies is corroded by seawater, especially by inorganic salts in seawater, which will affect the bentonite effect and reduce the strength and impermeability of the plastic concrete.

[0005] Summary of the Invention

[0006] In view of this, the main objective of the present invention is to provide a composite anti-seepage wall for landfill environmental protection in soft soil areas. Through the technical solution of the present invention, displacement is effectively controlled and ground cracking is avoided while ensuring the safety of the landfill embankment, soil and anti-seepage structure. A continuous underground composite anti-seepage wall is constructed to control the migration and diffusion of pollutants in contaminated soil or groundwater. The groundwater level is effectively controlled through groundwater pumping wells, and the intercepted seepage liquid is promptly pumped out and treated.

[0007] To achieve the above objectives, the technical solution of the present invention is implemented as follows:

[0008] A composite impermeable wall for environmental protection of landfills in soft soil areas includes a waterproof layer buried underground in the landfill, a flexible core wall arranged around the landfill, the depth of the flexible core wall being sufficient to extend from the ground surface and embed into the waterproof layer, plastic walls being arranged on the inner and outer sides of the flexible core wall, support walls being arranged on the inner side of the inner plastic wall and the outer side of the outer plastic wall, a transition zone being arranged between the inner support wall and the landfill, and a groundwater pumping well being arranged in the transition zone.

[0009] More preferably, the flexible core wall is composed of an HDPE geomembrane with a thickness of at least 3.0 mm and an overall permeability coefficient ≤ 10. -8 cm / s; the impermeability coefficient of the plastic wall is ≤5×10 -8 cm / s, thickness ≥600mm, the supporting wall is constructed of multiple high-pressure jet grouting piles arranged around the perimeter, single pile diameter ≥800mm, pile interlocking 200mm, and the horizontal distance between the pile centerline and the edge of the plastic wall ≥ single pile radius + 300mm.

[0010] More preferably, the depth of the supporting wall and the plastic wall is the same as the depth of the flexible core wall, and the groundwater level in the control well of the groundwater pumping well is always 3m lower than the bottom impermeable layer of the landfill, and at least 1m lower than the groundwater level outside the composite impermeable wall.

[0011] More preferably, the plastic wall is constructed by underwater pouring of plastic concrete symmetrically on both sides of the flexible core wall. The plastic concrete is composed of cement, bentonite, clay, coarse sand, rice sand, corn kernels, polyoxyethylene-modified ionic surfactants, fluorocarbon surfactants, polyether-type nonionic surfactants, nonionic polyacrylamide, and water, in the following specific weight proportions:

[0012] Cement: 150-210 parts;

[0013] Bentonite: 40-80 parts;

[0014] Clay: 75-105 parts;

[0015] Medium sand: 398-513 portions;

[0016] Rice sand: 398-513 parts;

[0017] Sunflower seed chips: 398-513 servings;

[0018] Polyoxyethylene-modified ionic surfactant: 0.6-1 part;

[0019] Fluorocarbon surfactant: 0.1-2 parts;

[0020] Polyether-type nonionic surfactant: 0.5-1.5 parts;

[0021] Nonionic polyacrylamide: 0.0002-0.02 parts;

[0022] Water: 300-380 servings.

[0023] More preferably, the cement is silicate cement;

[0024] The bentonite used is sodium-based bentonite, and its particle size meets the requirement that the residue on a 400-mesh sieve is no more than 10%.

[0025] The clay used is silty clay with a moisture content of no more than 8% and a particle size that meets the requirement of a 100-mesh sieve residue of no more than 10%.

[0026] The coarse sand is selected from river sand with a particle size of 0.5-3mm;

[0027] The rice sand is made from crushed mountain pebbles with a particle size of 3-5mm;

[0028] The sunflower seed chips are made from crushed pebbles with a particle size of 5-10mm.

[0029] The weight ratio of coarse sand: rice sand: melon seed chips is 1:1:1;

[0030] The polyoxyethylene-modified ionic surfactant is an alcohol ether sulfate;

[0031] The fluorocarbon surfactant is selected from polyethylene glycol hydrophilic nonionic fluorocarbon surfactants.

[0032] The polyether-type nonionic surfactant is an adduct of polypropylene glycol and ethylene oxide, wherein the number of ethylene oxides is 40-50.

[0033] More preferably, the plastic concrete is prepared by the following steps:

[0034] Step A: Mix the polyoxyethylene-modified ionic surfactant with a certain proportion of water and a certain proportion of bentonite, then let it stand to expand and make bentonite slurry.

[0035] Step B: Mix nonionic polyacrylamide with the remaining water, fluorocarbon surfactant, and polyether nonionic surfactant to prepare a conditioning solution;

[0036] Step C: Mix the sunflower seed chips, rice sand, coarse sand, clay, cement, and the remaining bentonite in descending order of particle size to form a mixed dry material. Then mix it with the bentonite slurry and the conditioning liquid to obtain the final product.

[0037] More preferably, the amount of water used in step A is 90% of the total water volume, and the mass ratio of the water volume to the bentonite used is 100:10-15.

[0038] A construction method for a composite impermeable wall used for environmental protection of landfills in soft soil areas includes the following steps:

[0039] Step 1: Construct two layers of spaced support walls around the perimeter of the landfill, extending underground to a depth sufficient to extend from the surface and embed into the waterproof layer.

[0040] Step 2: Set up a flexible core wall between the two supporting walls, the depth of which is sufficient to extend from the ground surface and be embedded into the waterproof layer;

[0041] Step 3: Install a plastic wall between the inner and outer perimeter of the flexible core wall and the inner and outer supporting walls;

[0042] Step 4: Install groundwater pumping wells in the transition zone between the inner supporting wall and the landfill.

[0043] More preferably, in step two, the flexible core wall is made of 3.0mm thick HDPE geomembrane with a single width of 4.1m. Multiple HDPE geomembranes are set around the perimeter of the landfill. The two sides of adjacent HDPE geomembranes are welded together with E-type interlocking. The installation of HDPE geomembrane is completed by using a film spreading roller and a gravity film laying machine.

[0044] More preferably, in step three, the plastic wall is made of plastic concrete, and the mixed plastic concrete is poured from bottom to top underwater using a steel conduit. A steel conduit is set at certain intervals around the circumference. Initially, the steel conduit is a certain distance from the bottom of the tank on the waterproof layer in the depth direction. The conduit is raised once every time a specified depth is poured, until it is level with the ground. The plastic concrete is composed of cement, bentonite, clay, coarse sand, rice sand, sunflower seed chips, polyoxyethylene ionic surfactant, fluorocarbon surfactant, polyether nonionic surfactant, nonionic polyacrylamide, and water.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] This invention provides a composite seepage barrier wall for environmental protection of landfills in soft soil areas. It utilizes a flexible core wall (HDPE geomembrane) and a plastic wall body (preferably cast plastic concrete) to form the main structure of a vertical composite seepage barrier wall. This controls the migration and diffusion of pollutants in contaminated soil or groundwater, improving environmental safety performance and structural stability. The supporting wall strengthens the strength and stability of the soft soil surrounding the landfill, enhancing construction safety.

[0047] This invention provides a construction method for a composite seepage barrier wall for environmental protection of hazardous waste landfills in soft soil areas. The plastic wall is formed by pouring plastic concrete. During the preparation of the plastic concrete, dry materials are pre-mixed according to particle size from large to small, improving material uniformity and enhancing the early strength of the plastic concrete. A conditioning liquid is prepared by mixing nonionic polyacrylamide, fluorocarbon surfactants, and the ethylene oxide adduct of polypropylene glycol, which is then mixed with the stirred dry materials, improving the internal cohesion and resistance to inorganic salts of the plastic concrete. A portion of bentonite is pre-expanded into a slurry, and alcohol ether sulfates are added to form a water-resistant, inorganic salt-resistant mud skin on the surface of the plastic concrete, further enhancing its early strength and resistance to inorganic salts, thus providing a safe, stable, and highly effective seepage barrier layer for the flexible core wall (HDPE geomembrane).

[0048] This invention provides a construction method for a composite seepage barrier wall for environmental protection of hazardous waste landfills in soft soil areas. It uses a membrane-spreading roller and a gravity-operated membrane-laying machine to install HDPE geomembrane. The HDPE geomembrane has high installation accuracy, high verticality, high construction efficiency, low energy consumption, small footprint, and the installation speed of HDPE geomembrane can be freely adjusted.

[0049] This invention provides a construction method for a composite anti-seepage wall for environmental protection of hazardous waste landfills in soft soil areas. The method can effectively control the groundwater level through groundwater pumping wells and promptly pump out and treat the intercepted seepage. Attached Figure Description

[0050] Figure 1 is a schematic cross-sectional view of the composite seepage barrier wall of the present invention;

[0051] Figure 2 is a schematic cross-sectional view of the composite seepage barrier wall of the present invention;

[0052] Figure 3 is a schematic diagram of the vertical installation of the HDPE geomembrane of the present invention.

[0053] In the diagram, 1 is the flexible core wall, 2 is the plastic wall, 3 is the supporting wall, 4 is the waterproof layer, 5 is the landfill, 6 is the dike, 7 is the soil, and 8 is the groundwater pumping well. Detailed Implementation

[0054] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0055] The specific embodiments of the present invention will now be described in further detail with reference to the accompanying drawings.

[0056] As shown in Figures 1 and 2, the composite impermeable wall for environmental protection of hazardous waste landfills in soft soil areas involved in this invention includes a water-proof layer 4, a flexible core wall 1, a plastic wall 2, a supporting wall 3, and a groundwater pumping well 8.

[0057] The waterproof layer 4 is typically provided and used as the bottom impermeable layer of the landfill 5. It is buried underground, above the groundwater layer, and extends at least to the corresponding underground area of ​​the entire landfill 5. It serves to block water, preventing water above it (such as leachate from the landfill) from seeping downwards and contaminating the groundwater, while also preventing clean groundwater below it from flowing up into the landfill area of ​​the landfill 5.

[0058] The flexible core wall 1 extends from the ground surface and is embedded in the waterproof layer 4, and is set around the landfill 5. Its depth extends from the ground surface and is embedded in the underground waterproof layer 4. It mainly plays the role of preventing seepage and preventing pollutants accidentally leaked during operation from spreading horizontally underground.

[0059] The plastic wall 2 comprises inner and outer layers, located on the inner and outer sides of the flexible core wall 1 respectively. Its depth is also embedded in the waterproof layer 4, protecting the flexible core wall 1 from external damage (such as corrosion, puncture, etc.). It possesses considerable strength, capable of withstanding the static pressure of the soil 7 without significant deformation or damage (such as cracks, holes, etc.). Simultaneously, the plastic wall 2 also provides a certain degree of seepage prevention. The thickness of the plastic wall 2 on each side is generally 300mm. The flexible core wall 1 and plastic wall 2 are arranged in a core-layer, wrapping-layer structure, with the core layer (flexible core wall 1) completely enclosed by the wrapping layer (plastic wall 2). This combined wall encloses the landfill area of ​​the landfill 5 internally, forming a combined wall with independent functions. It is the main horizontal seepage prevention structure of the composite seepage-proof wall of this invention, exhibiting good seepage prevention performance.

[0060] In a roughly vertical direction, the flexible core wall 1 and the plastic wall 2 extend from the ground surface and are embedded into the waterproof layer 4, respectively, forming a firmly bonded and stable composite structure. This bonding can be achieved through a structure where the waterproof layer 4 has grooves or holes, and the ends of the flexible core wall 1 and the plastic wall 2 extending underground into the waterproof layer 4 can be embedded into these grooves or holes. Obviously, to ensure the airtightness of the bond between the flexible core wall 1, the plastic wall 2, and the waterproof layer 4, the joints between the waterproof layer 4 and the flexible core wall 1 and the plastic wall 2 can be filled or sealed with various sealing materials.

[0061] The supporting wall 3 comprises two layers, an inner supporting wall and an outer supporting wall, located inside the inner plastic wall 2 and outside the outer plastic wall 2, respectively. It is constructed using high-pressure jet grouting piles, thereby supporting both sides of the composite wall formed by the inner and outer flexible core walls 1 and plastic walls 2, and reinforcing the surrounding soil 7 of the landfill 5, reducing displacement, and improving the construction safety of the composite anti-seepage wall. In some improved examples, the inner plastic wall 2 and its inner supporting wall (i.e., the inner supporting wall), as well as the outer plastic wall 2 and its outer plastic wall 2 (i.e., the outer supporting wall), can be separated by soil 7.

[0062] A transition zone exists between the landfill 5 and the innermost impermeable zone 3 formed by this invention. This transition zone is formed by filling the transition zone with soil 7 and includes a groundwater drainage well 8. The groundwater drainage well 8 is used to control the groundwater level and to promptly remove and treat intercepted leachate, effectively isolating accidental leaks from the hazardous waste landfill and protecting the soil and groundwater. Its depth is generally close to, but above, the underground aquitard 4, effectively controlling the groundwater level and allowing for timely removal and treatment of intercepted leachate.

[0063] The composite impermeable wall provided by this invention surrounds the landfill 5, consisting of a support wall 3, a plastic wall 2, a flexible core wall 1, another plastic wall 2, and another support wall 3 arranged sequentially from the inside out. This prevents the spread of pollutants from the landfill 5 in the event of accidental leakage during operation. Furthermore, a groundwater drainage well 8 is installed in the transition zone between the inner support wall 3 and the landfill 5, effectively controlling the groundwater level and allowing for timely extraction and treatment of intercepted leachate. This invention constructs a composite impermeable wall while ensuring the stability of the landfill 5's dike foundation 6, effectively isolating the hazardous waste landfill 5 from accidental leakage and protecting the soil and groundwater.

[0064] Composite impermeable walls are used for environmental protection of hazardous waste landfills in soft soil areas, forming underground structures around the landfill. In other words, the area defined by the composite impermeable wall is larger than the actual landfill area. The composite impermeable wall is mainly used to confine the landfill within its walls, thereby limiting the pollutants carried by the waste to the entire landfill site and preventing leakage (primarily in the horizontal and vertical directions). In the vertical direction, the impermeable layer 4 prevents leachate from seeping deeper into the soil 7.

[0065] As a further embodiment, the flexible core wall 1 is composed of an HDPE geomembrane with a thickness of at least 3.0 mm and an overall permeability coefficient of ≤10-8 cm / s.

[0066] As a further embodiment, the impermeability coefficient of the plastic wall 2 is ≤5×10⁻⁶. -8cm / s, 28-day unconfined compressive strength ≥4.5MPa, thickness ≥600mm.

[0067] As a further embodiment, the plastic wall 2 is formed by casting plastic concrete. The plastic concrete is composed of cement, bentonite, clay, coarse sand, rice sand, corn kernels, polyoxyethylene-modified ionic surfactants, fluorocarbon surfactants, polyether-type nonionic surfactants, nonionic polyacrylamide, and water, mixed in a certain proportion and process, and is formed by underwater casting symmetrically on both sides of the flexible core wall 1.

[0068] As a further embodiment, the supporting wall 3 is constructed from high-pressure jet grouting piles, with a single pile diameter ≥ 800 mm, a pile interlocking length of 200 mm, a pile depth consistent with the height of the plastic wall 2, a horizontal distance between the pile centerline and the edge of the plastic wall ≥ single pile radius + 300 mm, and a single pile with a 28-day unconfined compressive strength ≥ 1.5 MPa. The piles are located on both sides of the plastic wall 2. The specific number of piles is determined based on the trench stability calculation. If the compressive strength of a single row of supporting walls is insufficient, multiple rows of compressive walls can be formed on each side. The installation of the supporting wall reduces the displacement of the surrounding soil and improves the construction safety of the flexible core wall 1 and the plastic wall 2.

[0069] As a further embodiment, the groundwater pumping well 8 is located in the transition zone between the inner support wall 3 and the landfill 5. The deep well pump of the groundwater pumping well 8 is used to control the groundwater level in the well to always be 3m lower than the bottom impermeable layer of the landfill 5, and at least 1m lower than the groundwater level outside the composite impermeable wall.

[0070] As a further embodiment, the inorganic salt-resistant plastic concrete used in the plastic wall 2 contains the following components in parts by weight:

[0071] Cement: 150-210 parts, preferably 160-210 parts, further preferably 160-200 parts, and most preferably 180-200 parts;

[0072] Bentonite: 40-80 parts, preferably 50-80 parts, further preferably 50-70 parts, and most preferably 60-80 parts;

[0073] Clay: 75-105 parts, preferably 80-105 parts, further preferably 80-100 parts, and most preferably 90-105 parts;

[0074] Coarse sand: 398-513 parts, preferably 450-513 parts, further preferably 450-490 parts, and most preferably 450-480 parts;

[0075] Rice sand: 398-513 parts, preferably 450-513 parts, further preferably 450-490 parts, and most preferably 450-480 parts;

[0076] Sunflower seed chips: 398-513 parts, preferably 450-513 parts, further preferably 450-490 parts, and most preferably 450-480 parts;

[0077] Polyoxyethylene-modified ionic surfactant: 0.6 to 1 part, preferably 0.8 to 1 part;

[0078] Fluorocarbon surfactant: 0.1 to 2 parts, preferably 0.5 to 2 parts, more preferably 0.5 to 1.5 parts;

[0079] Polyether-type nonionic surfactant: 0.5 to 1.5 parts, preferably 1 to 1.5 parts;

[0080] Nonionic polyacrylamide: 0.0002 to 0.02 parts, preferably 0.005 to 0.02 parts, more preferably 0.005 to 0.01 parts;

[0081] Water: 300-380 parts.

[0082] This invention improves the resistance of plastic concrete to inorganic salt penetration by changing the composition of aggregates and adding composite surfactants, and improves the overall performance of plastic concrete by utilizing the synergistic effect between aggregates, cementitious materials and surfactants, so as to meet the performance requirements of impermeability applications.

[0083] Among them, the gradient particle size of coarse sand, rice sand, melon seed powder, clay, bentonite, and cement improves the uniformity of plastic concrete and is beneficial to improving the early strength of plastic concrete.

[0084] Polyoxyethylene-based ionic surfactants can effectively improve the resistance of plastic concrete to inorganic salts, ensuring strength and permeability.

[0085] Polyether-type nonionic surfactants improve the resistance of plastic concrete to chemical reagents and enhance its stability.

[0086] This invention incorporates a polyethylene glycol hydrophilic nonionic fluorocarbon surfactant to form a protective layer on the surface of plastic concrete, reducing the adsorption of ions by the plastic concrete and further improving its resistance to inorganic salts.

[0087] The invention incorporates nonionic polyacrylamide, which reduces the impact of groundwater on plastic concrete, strengthens the cohesion between components, and helps improve the early strength of plastic concrete.

[0088] Although the above polymers play their respective dominant roles, research has found that if only one, two, or three of them are added, instead of all of them, or if other ratios are used, the ideal resistance to inorganic salts cannot be obtained.

[0089] The cement used is ordinary Portland cement with a strength grade of 42.5;

[0090] The bentonite used is sodium-based bentonite, and its particle size meets the requirement that the residue on a 400-mesh sieve is no more than 10%.

[0091] The clay used is silty clay with a moisture content of no more than 8% and a particle size that meets the requirement of a 100-mesh sieve residue of no more than 10%.

[0092] The coarse sand is selected from river sand with a particle size of 0.5–3 mm;

[0093] The rice sand is made from crushed mountain pebbles with a particle size of 3-5 mm.

[0094] The sunflower seed chips are made from crushed pebbles with a particle size of 5-10 mm.

[0095] The weight ratio of coarse sand: rice sand: melon seed chips is 1:1:1;

[0096] The polyoxyethylene ionic surfactant is an alcohol ether sulfate, preferably a fatty alcohol polyoxyethylene ether sulfate, and more preferably a C12-C14 fatty alcohol polyoxyethylene ether sulfate.

[0097] The fluorocarbon surfactant is selected from polyethylene glycol hydrophilic nonionic fluorocarbon surfactants. Preferably, the polyethylene glycol in the polyethylene glycol hydrophilic nonionic fluorocarbon surfactant has a molecular weight of 0.4k to 2k. More preferably, the fluorocarbon in the polyethylene glycol hydrophilic nonionic fluorocarbon surfactant is a perfluoro(2-methyl-3-oxahexyl) fluoride or a perfluoro-2,5-dimethyl-3,6-dioxonanoyl fluoride.

[0098] The polyether-type nonionic surfactant is an adduct of polypropylene glycol and ethylene oxide, wherein the number of ethylene oxides is 40-50, such as 42, 44, 45, 47, 49, 50, etc.

[0099] The plastic concrete provided by this invention can be prepared using any conventional method, such as simple mixing. However, research has found that the mixing order, the timing of adding water and surfactants, and the method of adding expanded clay have a significant impact on the performance of the plastic concrete. Therefore, this invention provides the following preferred preparation method:

[0100] Step A: Mix the polyoxyethylene-modified ionic surfactant with some water and some bentonite, then let it stand to expand, and make bentonite slurry.

[0101] Step B: Mix nonionic polyacrylamide with the remaining water, fluorocarbon surfactant, and polyether nonionic surfactant to prepare a conditioning solution;

[0102] Step C: Mix the remaining raw materials (sunflower seed chips, rice sand, coarse sand, clay, cement and remaining bentonite) together to form a mixed dry material, and then mix it with the bentonite slurry and the conditioning liquid.

[0103] The amount of water used in steps A and B can be adjusted according to actual needs. Preferably, the amount of water used in step A is 90% of the total water volume (mass), and the ratio of water volume to bentonite mass is 100:10 to 15, such as 100:11, 100:12, 100:13, 100:14, 100:15, etc. The puffing time is preferably 24 hours or more.

[0104] Preferably, step B further comprises:

[0105] Nonionic polyacrylamide is mixed with residual water under heating conditions, and then fluorocarbon surfactant and polyether nonionic surfactant are added after cooling and mixed thoroughly to prepare a conditioning solution. Dissolving the polyacrylamide in water first can stimulate the formation of network nodes in the gel, which is beneficial to improving the molecular cohesion of plastic concrete. The preferred heating temperature is 60–80℃.

[0106] Step C further comprises: adding and mixing the sunflower seed chips, rice sand, coarse sand, clay, cement, and remaining bentonite one by one in descending order of particle size to form a mixed dry material, and then mixing it with the bentonite slurry and the conditioning liquid; the pre-mixing of the dry material in descending order of particle size improves the uniformity of the material and is beneficial to improving the early strength of plastic concrete.

[0107] In each of the three steps, mixing requires stirring. For example, in step A, the mixture can be stirred at 3000 rpm for 15 minutes. In step B, the mixture can be stirred at 200 rpm for 10 minutes. In step C, the dry materials are mixed first, adding them one at a time from largest to smallest particle size: sunflower seed flakes, rice sand, coarse sand, clay, cement, and bentonite. Each new material is added and stirred for 5-10 minutes to create a mixed dry material.

[0108] In step A, when mixing the polyoxyethylene-modified ionic surfactant with some water and some bentonite, the polyoxyethylene-modified ionic surfactant can be mixed with water first, usually at room temperature (20-40°C), and then bentonite can be added and stirred at high speed.

[0109] This invention provides a construction method for a composite impermeable wall for environmental protection of landfills in soft soil areas, specifically including the following steps:

[0110] Step 1: Two layers of spaced support walls 3 are set up around the perimeter of the landfill and extend underground. The inner support wall is set close to the perimeter of the landfill, and there is a gap between the outer support wall and the inner support wall. The depth of the support wall is sufficient to extend from the ground surface and be embedded into the waterproof layer 4.

[0111] The inner and outer support walls are formed by multiple continuously interlocking high-pressure jet grouting piles around the perimeter. The pile depth is sufficient to extend from the ground surface and embed into the waterproof layer 4. Multiple high-pressure jet grouting piles with two adjacent piles interlocking with each other in a continuous perimeter form a circumferentially arranged support wall 3.

[0112] Step 2: A flexible core wall 1 is set at a certain distance between the two supporting walls 3, and the depth of the flexible core wall 1 is such that it extends from the ground surface and is embedded into the waterproof layer 4.

[0113] The flexible core wall 1 is made of 3.0mm thick HDPE geomembrane. During operation, the single width of HDPE geomembrane 9 is 4.1m. Multiple HDPE geomembranes are set around the circumference of the landfill 5. The two sides of adjacent HDPE geomembranes are welded together. It is preferred to use E-type locking buckles. The buckles are distributed on both sides of the HDPE geomembrane. The protruding part of the buckle faces away from the HDPE geomembrane, and the smooth part faces the HDPE geomembrane for welding. As shown in Figure 3, the HDPE geomembrane 9 is pre-rolled onto the film-laying roller trolley 10 and moved to the vicinity of a pre-cut trench 11 in the waterproof layer 4 (the waterproof layer 4 has been pre-set according to the dimensions of the composite impermeable wall, and the waterproof layer 4 needs to form a trench around the HDPE geomembrane as required for its installation, with the trench recessed in the waterproof layer 4). The bottom end of the HDPE geomembrane 9 is adjusted to hang directly above the trench and be as parallel as possible to the length of the trench. The bottom end of the HDPE geomembrane is temporarily fixed to the gravity module 12-1 of the gravity-laying machine 12. The force on the gravity-laying machine 12 is balanced by the balance block 12-2. The HDPE geomembrane is vertically installed to the specified depth using the gravity module 12-1. The specified depth is required to extend from the ground surface and embed into the underground waterproof layer 4. A ring of HDPE geomembrane is installed around the landfill 5, between the inner and outer supporting walls 3, using the same method. Adjacent HDPE geomembrane sections are connected by E-type interlocking, with a sealing strip inserted into the cavity between adjacent interlocking. The flexible core wall 1 must be installed around the landfill 5 continuously and without interruption, and the bottom of the flexible core wall 1 (i.e., the HDPE geomembrane) must be sealed (e.g., by grouting or filling) with the waterproof layer 4. This invention uses a membrane-laying roller and a gravity-operated membrane-laying machine, resulting in high installation accuracy and verticality of the HDPE geomembrane, high construction efficiency, low energy consumption, small footprint, and adjustable installation speed.

[0114] Step 3: Set up a plastic wall 2 between the inner and outer perimeter of the flexible core wall 1 and the inner and outer supporting walls. The depth of the plastic wall 2 is the same as the depth of the flexible core wall.

[0115] The plastic wall 2 is made of plastic concrete. The plastic concrete is prepared according to the preparation method described above. After preparation, before pouring the plastic concrete, a slag-blocking pipe needs to be placed to prevent accidental splashing to other areas when pouring a certain section along the axial direction. The plastic concrete is poured using a DN250 steel conduit. The mixed plastic concrete is poured underwater from bottom to top, with a DN250 steel conduit spaced 2-3m apart along the circumference. During the initial pour in the depth direction, the DN250 steel conduit is 0.5m from the bottom of the trench (and the water-proof layer 4 needs to be pre-formed to form a trench around the plastic wall). Every 0.5m of pouring depth, the conduit is raised until it is level with the ground, completing the pouring of the flexible core wall 1. The joint between the water-proof layer 4 and the plastic wall 2 can be filled and sealed with various sealing materials.

[0116] Step 4: Install groundwater pumping well 8 in the soil of the transition zone between the inner supporting wall and the landfill. The deep well pump of the groundwater pumping well controls the groundwater level in the well to always be 3m lower than the bottom impermeable layer of the landfill, and at least 1m lower than the groundwater level outside the composite impermeable wall.

[0117] Example 1:

[0118] The composition of the plastic concrete provided in this embodiment is as follows: per cubic meter of plastic concrete, 150 kg of cement (42.5 ordinary Portland cement), 40 kg of sodium bentonite (particle size meets the requirement of less than 10% on a 400-mesh sieve), 75 kg of clay (moisture content less than 8%, particle size meets the requirement of less than 10% residue on a 100-mesh sieve), 513 kg of coarse sand (0.5-3 mm), 513 kg of rice sand (3-5 mm), and 513 kg of sunflower seeds. The following ingredients are used: flakes (5-10 mm), 0.6 kg of alcohol ether sulfate (sodium fatty alcohol polyoxyethylene ether sulfate), 0.1 kg of polyethylene glycol hydrophilic nonionic fluorocarbon surfactant (wherein the polyethylene glycol has a molecular weight of 1.8k and the fluorocarbon is a perfluorinated (2-methyl-3-oxahexyl) fluoride), 0.5 kg of polypropylene glycol ethylene oxide adduct (wherein the number of ethylene oxide alkyl groups is 45), 0.0002 kg of nonionic polyacrylamide, and 300 kg of water. Plastic concrete is prepared according to the method described in this invention.

[0119] Example 2

[0120] The composition of the plastic concrete provided in this embodiment is as follows: per cubic meter of plastic concrete, 160 kg of cement (42.5 ordinary Portland cement), 50 kg of sodium bentonite (same type as in Example 1), 80 kg of clay (same type as in Example 1), 487 kg of coarse sand (same type as in Example 1), 487 kg of rice sand (same type as in Example 1), 487 kg of dried melon seed chips (same type as in Example 1), 0.7 kg of alcohol ether sulfate (same type as in Example 1), 0.4 kg of polyethylene glycol hydrophilic nonionic fluorocarbon surfactant (same type as in Example 1), 0.7 kg of polypropylene glycol ethylene oxide adduct (same type as in Example 1), 0.005 kg of nonionic polyacrylamide, and 320 kg of water. Plastic concrete is prepared according to the preparation method described in this invention.

[0121] Example 3

[0122] The composition of the plastic concrete provided in this embodiment is as follows: per cubic meter of plastic concrete, 180 kg of cement (42.5 ordinary Portland cement), 60 kg of sodium bentonite (same type as in Example 1), 90 kg of clay (same type as in Example 1), 465 kg of coarse sand (same type as in Example 1), 465 kg of rice sand (same type as in Example 1), 465 kg of dried melon seed chips (same type as in Example 1), 0.8 kg of alcohol ether sulfate (same type as in Example 1), 1 kg of polyethylene glycol hydrophilic nonionic fluorocarbon surfactant (same type as in Example 1), 1 kg of polypropylene glycol ethylene oxide adduct (same type as in Example 1), 0.01 kg of nonionic polyacrylamide, and 330 kg of water. Plastic concrete is prepared according to the preparation method described in this invention.

[0123] Example 4

[0124] The composition of the plastic concrete provided in this embodiment is as follows: per cubic meter of plastic concrete, 200 kg of cement (42.5 ordinary Portland cement), 72 kg of sodium bentonite (same type as in Example 1), 100 kg of clay (same type as in Example 1), 424 kg of coarse sand (same type as in Example 1), 424 kg of rice sand (same type as in Example 1), 424 kg of dried melon seed chips (same type as in Example 1), 0.9 kg of alcohol ether sulfate (same type as in Example 1), 1.8 kg of polyethylene glycol hydrophilic nonionic fluorocarbon surfactant (same type as in Example 1), 1.3 kg of ethylene oxide adduct of polypropylene glycol (same type as in Example 1), 0.015 kg of nonionic polyacrylamide, and 360 kg of water. Plastic concrete is prepared according to the preparation method described in this invention.

[0125] Example 5

[0126] The composition of the plastic concrete provided in this embodiment is as follows: per cubic meter of plastic concrete, 210 kg of cement (42.5 ordinary Portland cement), 80 kg of sodium bentonite (same type as in Example 1), 105 kg of clay (same type as in Example 1), 398 kg of coarse sand (same type as in Example 1), 398 kg of rice sand (same type as in Example 1), 398 kg of dried melon seed chips (same type as in Example 1), 1 kg of alcohol ether sulfate (same type as in Example 1), 2 kg of polyethylene glycol hydrophilic nonionic fluorocarbon surfactant (same type as in Example 1), 1.5 kg of polypropylene glycol ethylene oxide adduct (same type as in Example 1), 0.02 kg of nonionic polyacrylamide, and 380 kg of water. Plastic concrete is prepared according to the preparation method described in this invention.

[0127] The preparation methods of the plastic concrete in Examples 1 to 5 above are all as follows:

[0128] (1) Mix alcohol ether sulfate with 90% by weight of water at 20-40℃, then mix with 11% by weight of sodium bentonite at 3000r / min for 15min, and then let it stand to expand for 24h to make bentonite slurry.

[0129] (2) Mix nonionic polyacrylamide with 10% water at 60-80℃, cool to 20-40℃, and then mix with polyethylene glycol hydrophilic nonionic fluorocarbon surfactant and ethylene oxide adduct of polypropylene glycol in sequence. Stir and mix at 200r / min for 10min to prepare conditioning solution.

[0130] (3) Add the sunflower seed flakes, rice sand, coarse sand, clay, cement and bentonite in order of decreasing particle size. Stir for 5 to 10 minutes after each addition to make a mixed dry material.

[0131] (4) Mix the dry mixture with the conditioning liquid first, and then mix it with the bentonite slurry to obtain the inorganic salt resistant plastic concrete for seepage prevention.

[0132] Comparative Example 1

[0133] For each cubic meter of plastic concrete, there are 180 kg of cement (42.5 ordinary Portland cement), 60 kg of sodium bentonite (same type as in Example 1), 90 kg of clay (same type as in Example 1), 465 kg of coarse sand (same type as in Example 1), 465 kg of rice sand (same type as in Example 1), 465 kg of sunflower seed chips, and 330 kg of water.

[0134] The preparation method is as follows: add water to bentonite and let it stand for 24 hours to expand. Mix clay, coarse sand, rice sand, melon seed chips and cement in order of particle size from large to small. Then mix them with the expanded bentonite, water and other raw materials. Stir and mix at 3000 r / min for 15 minutes.

[0135] The properties of the plastic concrete obtained in Examples 1 to 5 and Comparative Example 1 are shown in Table 1 below.

[0136] Table 1

[0137]

[0138] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the invention. The above are only preferred embodiments of the present invention and are not intended to limit the invention. For those skilled in the art, the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A composite impermeable wall for environmental protection of landfills in soft soil areas, comprising a waterproof layer buried underground in the landfill site, characterized in that, The system includes a flexible core wall surrounding the landfill, the depth of which extends from the ground surface and is embedded into the waterproof layer. Plastic walls are provided on both the inner and outer sides of the flexible core wall. Supporting walls are provided on the inner side of the inner plastic wall and the outer side of the outer plastic wall. A transition zone is provided between the inner supporting wall and the landfill, and a groundwater pumping well is provided in the transition zone.

2. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 1, characterized in that, The flexible core wall is composed of an HDPE geomembrane with a thickness of at least 3.0 mm and an overall permeability coefficient ≤10. -8 cm / s; the impermeability coefficient of the plastic wall is ≤5×10 -8 cm / s, thickness ≥600mm, the supporting wall is constructed of multiple high-pressure jet grouting piles arranged around the perimeter, single pile diameter ≥800mm, pile interlocking 200mm, and the horizontal distance between the pile centerline and the edge of the plastic wall ≥ single pile radius + 300mm.

3. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 1, characterized in that, The depth of the supporting wall and the plastic wall is the same as the depth of the flexible core wall. The groundwater level in the deep well pump control well of the groundwater pumping well is always 3m lower than the bottom impermeable layer of the landfill, and at least 1m lower than the groundwater level outside the composite impermeable wall.

4. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 1, characterized in that, The plastic wall is constructed by underwater casting of plastic concrete symmetrically on both sides of the flexible core wall. The plastic concrete is composed of cement, bentonite, clay, coarse sand, rice sand, sunflower seed chips, polyoxyethylene-modified ionic surfactants, fluorocarbon surfactants, polyether-type nonionic surfactants, nonionic polyacrylamide, and water, in the following specific weight proportions: Cement: 150-210 parts; Bentonite: 40-80 parts; Clay: 75-105 parts; Medium sand: 398-513 portions; Rice sand: 398-513 parts; Sunflower seed chips: 398-513 servings; Polyoxyethylene-modified ionic surfactant: 0.6-1 part; Fluorocarbon surfactant: 0.1-2 parts; Polyether-type nonionic surfactant: 0.5-1.5 parts; Nonionic polyacrylamide: 0.0002-0.02 parts; Water: 300-380 servings.

5. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 4, characterized in that, The cement is silicate cement; The bentonite used is sodium-based bentonite, and its particle size meets the requirement that the residue on a 400-mesh sieve is no more than 10%. The clay used is silty clay with a moisture content of no more than 8% and a particle size that meets the requirement of a 100-mesh sieve residue of no more than 10%. The coarse sand is selected from river sand with a particle size of 0.5-3mm; The rice sand is made from crushed mountain pebbles with a particle size of 3-5mm; The sunflower seed chips are made from crushed pebbles with a particle size of 5-10mm. The weight ratio of coarse sand: rice sand: melon seed chips is 1:1:1; The polyoxyethylene-modified ionic surfactant is an alcohol ether sulfate; The fluorocarbon surfactant is selected from polyethylene glycol hydrophilic nonionic fluorocarbon surfactants. The polyether-type nonionic surfactant is an adduct of polypropylene glycol and ethylene oxide, wherein the number of ethylene oxides is 40-50.

6. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 4, characterized in that, The plastic concrete is prepared through the following steps: Step A: Mix the polyoxyethylene-modified ionic surfactant with a certain proportion of water and a certain proportion of bentonite, then let it stand to expand and make bentonite slurry. Step B: Mix nonionic polyacrylamide with the remaining water, fluorocarbon surfactant, and polyether nonionic surfactant to prepare a conditioning solution; Step C: Mix the sunflower seed chips, rice sand, coarse sand, clay, cement, and the remaining bentonite in descending order of particle size to form a mixed dry material. Then mix it with the bentonite slurry and the conditioning liquid to obtain the final product.

7. The composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 6, characterized in that, The amount of water used in step A is 90% of the total water volume, and the ratio of the amount of water used to the mass of bentonite used is 100:10-15.

8. A construction method for a composite impermeable wall used for environmental protection of landfills in soft soil areas, characterized in that, Specifically, it includes the following steps: Step 1: Construct two layers of spaced support walls around the perimeter of the landfill, extending underground to a depth sufficient to extend from the surface and embed into the waterproof layer. Step 2: Set up a flexible core wall between the two supporting walls, the depth of which is sufficient to extend from the ground surface and be embedded into the waterproof layer; Step 3: Install a plastic wall between the inner and outer perimeter of the flexible core wall and the inner and outer supporting walls; Step 4: Install groundwater pumping wells in the transition zone between the inner supporting wall and the landfill.

9. The construction method of the composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 8, characterized in that, In step two, the flexible core wall is made of 3.0mm thick HDPE geomembrane with a single width of 4.1m. Multiple HDPE geomembranes are set around the perimeter of the landfill. The two sides of adjacent HDPE geomembranes are welded together with E-type interlocking. The installation of HDPE geomembrane is completed by using a film spreading roller and a gravity film laying machine.

10. The construction method of the composite seepage barrier wall for environmental protection of landfills in soft soil areas according to claim 8, characterized in that, In step three, the plastic wall is made of plastic concrete. The mixed plastic concrete is poured underwater from bottom to top using a steel conduit. A steel conduit is set at certain intervals around the perimeter. Initially, the steel conduit is a certain distance from the bottom of the tank above the waterproof layer in the depth direction. The conduit is raised once after each specified pouring depth until it is level with the ground. The plastic concrete is composed of cement, bentonite, clay, coarse sand, rice sand, sunflower seed chips, polyoxyethylene ionic surfactant, fluorocarbon surfactant, polyether nonionic surfactant, nonionic polyacrylamide, and water.