Catalytic composition and method for removing nitrogen oxides

TWI945611BActive Publication Date: 2026-11-11IND TECH RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
TW113145444
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-11-26
Publication Date
2026-11-11
Estimated Expiration
2044-11-25

AI Technical Summary

Technical Problem

The ammonia selective catalytic reduction (NH3-SCR) technology for NOx removal faces issues such as heater fouling and catalyst deterioration, necessitating the development of alternative technologies for efficient NOx removal.

Method used

A catalyst composition comprising a carrier coated with manganese oxide as a first active ingredient and a second active ingredient containing platinum or palladium, and optionally potassium or sodium oxides, is used for a hydrogen selective catalytic reduction (H2-SCR) process to convert NOx into N2 and H2O.

Benefits of technology

The catalyst composition achieves high efficiency in NOx removal, with removal rates exceeding 90% and N2 selectivity above 80% across various temperatures, promoting sustainable hydrogen energy use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920356_001
    Figure TWG2TB001920356_001
  • Figure TWG2TB001920356_002
    Figure TWG2TB001920356_002
  • Figure TWG2TB001920356_003
    Figure TWG2TB001920356_003
Patent Text Reader

Abstract

A catalyst composition includes a carrier, a first active ingredient, and a second active ingredient. The first active ingredient is coated on the surface of the carrier and includes a first catalyst, which is manganese oxide. The second active ingredient includes a second catalyst and a third catalyst and is coated on the surface of the first active ingredient and the surface of the carrier where the first active ingredient is not coated. The second catalyst comprises platinum metal, palladium metal, or a combination thereof, and the third catalyst comprises potassium oxide, sodium oxide, or a combination thereof. The molar ratio of the first catalyst to the second catalyst is from 1:0.001 to 1:0.2, and the molar ratio of the first catalyst to the third catalyst is from 1:0.1 to 1:10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a catalyst composition and a method for removing nitrogen oxides. Prior Technology

[0002] Nitrogen in the air reacts with oxygen at high temperatures (>800°C) to produce nitrogen oxides (NOx), which contribute to problems such as acid rain, photochemical smog, ozone layer depletion, and eutrophication. Therefore, reducing NOx emissions is crucial for environmental protection. Currently, the most mature and mainstream method for NOx removal globally is the ammonia selective catalytic reduction (NH3-SCR) process.

[0003] However, the NH3-SCR technology encounters problems such as heater fouling and catalyst deterioration during use. Therefore, there is an urgent need to develop other technologies for NOx removal and improve treatment efficiency. Summary of the Invention

[0004] The catalyst composition of the present invention includes a carrier, a first active ingredient, and a second active ingredient. The first active ingredient is coated on the surface of the carrier, wherein the first active ingredient includes a first catalyst, which is manganese oxide. The second active ingredient includes a second catalyst and a third catalyst, and is coated on the surface of the first active ingredient and the surface of the carrier not coated with the first active ingredient. The second catalyst comprises platinum metal, palladium metal, or a combination thereof, and the third catalyst comprises potassium oxide, sodium oxide, or a combination thereof. The molar ratio of the first catalyst to the second catalyst is from 1:0.001 to 1:0.2, and the molar ratio of the first catalyst to the third catalyst is from 1:0.1 to 1:10.

[0005] The method for removing nitrogen oxides according to the present invention includes using the above-described catalyst composition to perform a selective catalytic reduction with hydrogen (H2-SCR) reaction on nitrogen oxides.

[0006] Based on the above, the catalyst composition of the present invention can be used as a high-efficiency H2-SCR catalyst. This catalyst composition can be used to convert low-concentration H2 into NOx into N2 and H2O, thereby achieving the goal of purifying harmful gases.

[0007] To make the above features of the present invention more apparent and understandable, specific embodiments are described below, and detailed descriptions are provided in conjunction with the accompanying drawings. Simple Explanation of the Diagram

[0008] Figure 1 is a schematic diagram of a catalyst composition according to a first embodiment of the present invention. Figure 2 is a schematic diagram of a catalyst composition according to a second embodiment of the present invention. Figure 3 is a block diagram of the equipment used to remove nitrogen oxides in the experimental example. Implementation

[0009] The following description provides detailed examples and accompanying drawings, but these examples are not intended to limit the scope of the invention. Furthermore, the drawings are for illustrative purposes only and are not drawn to scale. For ease of understanding, the same elements will be indicated by the same symbols in the following description.

[0010] Figure 1 is a schematic diagram of a catalyst composition according to a first embodiment of the present invention.

[0011] Referring to Figure 1, the catalyst composition 100 of the first embodiment includes a carrier 102, a first active ingredient 104, and a second active ingredient 106. In some embodiments, the carrier 102 includes aluminum oxide, titanium oxide, zirconium oxide, cerium oxide, magnesium oxide, or a combination thereof. The first active ingredient 102 is coated on the surface 102s of the carrier 102, wherein the first active ingredient 104 includes a first catalyst C1, which is manganese oxide. The first active ingredient 104 may partially or completely coat the surface of the carrier 102. The second active ingredient 106 includes a second catalyst C2 and a third catalyst C3, and is coated on the surface 104s of the first active ingredient 104 and the surface 102s of the carrier 102 where the first active ingredient 104 is not coated. The second catalyst C2 comprises platinum metal, palladium metal, or a combination thereof, and the third catalyst C3 comprises potassium oxide, sodium oxide, or a combination thereof.

[0012] The molar ratio of the first catalyst C1 to the second catalyst C2 is 1:0.001 to 1:0.2, for example, 1:0.001 to 1:0.1 or 1:0.001 to 1:0.02. The molar ratio of the first catalyst C1 to the third catalyst C3 is 1:0.1 to 1:10, for example, 1:0.1 to 1:5 or 1:0.1 to 1:2. In some embodiments, the molar ratio of the first catalyst C1 to the carrier 102 is 1:3 to 1:20.

[0013] In some embodiments, the specific surface area (BET) of the catalyst composition 100 may be from 140 m²g⁻¹ to 500 m²g⁻¹, for example, from 160 m²g⁻¹ to 400 m²g⁻¹ or from 170 m²g⁻¹ to 300 m²g⁻¹. In some embodiments, the particle size 100 of the catalyst composition may be from 100 µm to 10 mm, for example, from 500 µm to 10 mm or from 1 mm to 10 mm, but is not limited thereto.

[0014] In Figure 1, the first catalyst C1 in the first active ingredient 104 adsorbs nitrogen oxides (NOx) and uses hydrogen (H2) as a reducing agent. The second catalyst C2 in the second active ingredient 106 adsorbs H2 and dissociates it into hydrogen free radicals (hydrogen atoms). The strongly reducing hydrogen free radicals then break the nitrogen-oxygen bonds of the adsorbed nitrogen oxides (NOx), reacting to generate nitrogen (N2) and water (H2O). The third catalyst C3 can adjust the activity, acidity, alkalinity, and other properties of the catalyst composition 100. Therefore, the catalyst composition 100 of this embodiment can not only reduce pollutant emissions but also promote the application of hydrogen energy in the energy structure and drive sustainable development.

[0015] Figure 2 is a schematic diagram of a catalyst composition according to a second embodiment of the present invention, wherein the same element symbols as in the first embodiment are used to represent the same or similar parts, structures or size definitions, and the description of the same parts, structures or size definitions can be referred to the relevant description of the first embodiment, and will not be repeated here.

[0016] In Figure 2, the difference between the second embodiment and the first embodiment is that the first active ingredient 202 in the catalyst composition 200 also includes a fourth catalyst C4. Therefore, the first active ingredient 202 contains both the first catalyst C1 and the fourth catalyst C4. The fourth catalyst C4 comprises copper oxide, nickel oxide, or a combination thereof, and is formed together with the first catalyst C1 on the surface 102s of the carrier 102. In other words, the first catalyst C1 and the fourth catalyst C4 are coated on the surface 102s of the carrier 102, while the second catalyst C2 and the third catalyst C3 in the second active ingredient 106 can be coated on the surface 202s of the first active ingredient 202 and on the surface 102s of the carrier 102 where the first active ingredient 202 is not coated. The fourth catalyst C4 has the effect of improving the dispersibility of the first active ingredient 202 and suppressing side reactions. In some embodiments, the molar ratio of the first catalyst C1 to the fourth catalyst C4 is 1:0.01 to 1:10, for example, 1:0.01 to 1:5 or 1:0.01 to 1:2.

[0017] The catalyst composition of the present invention can be used to treat process gases or waste gases containing NOx, such as those from electronics factories, power plants, incinerators, glass factories, cement plants, and oil refineries. The catalyst composition can be used alone, for example, by filling a column with the catalyst composition and allowing the gas to be treated to flow through the column to achieve the treatment purpose; or, the catalyst composition can be combined with certain carriers, for example, by placing the catalyst composition on the surface or in the structure of such carriers, placing it in a chamber or container, and allowing the gas to be treated to flow through the chamber or container to achieve the treatment purpose.

[0018] A third embodiment of the present invention provides a method for removing nitrogen oxides, comprising using the catalyst composition 100 or 200 of the above embodiments to perform a hydrogen selective reduction reaction (H2-SCR) on nitrogen oxides (NOx).

[0019] In the third embodiment, the removal rate of nitrogen oxides can reach more than 90%, for example, more than 95% or more than 98%.

[0020] In the third embodiment, the above-described selective reduction reaction of hydrogen can be carried out at a temperature of 100°C to 250°C, but is not limited thereto. In other embodiments, the above-described selective reduction reaction of hydrogen can be carried out at a higher temperature, such as 250°C to 300°C.

[0021] The following experiments are listed to verify the implementation effect of the present invention, but the present invention is not limited to the following content.

[0022] The following preparation examples (including comparative preparation examples) mainly use a hot water granulation process to introduce the active ingredients into the carrier, followed by high-temperature calcination to form a catalyst composition. Compared with conventional catalyst powders that do not undergo a granulation process and are directly calcined at high temperatures after hydrothermal drying, the catalyst compositions prepared in the examples of this invention have more uniform particle sizes and can be made into specific sizes that facilitate stacking and industrial operation. They are also less likely to generate dust and are suitable for dust-free environments, such as semiconductor plants.

[0023] First, the alumina support used in the following preparation examples (including comparative preparation examples) is alumina. Essentially, the support must be able to bind with the metal ions to be introduced, and its specific surface area must be large enough. The alumina in the preparation examples has a specific surface area of ​​373 m² g⁻¹.

[0024] <Preparation Example 1>

[0025] In Preparation Example 1, a colloidal solution was first prepared, in which the weight ratio of carrier, sodium alginate powder, and water was 20:3:200. Then, the colloidal solution was added to a hot aqueous solution (approximately 40 to 90°C) containing divalent manganese ions to form particles containing the first active ingredient, wherein the concentration of divalent manganese ions was 30,000 ppm.

[0026] Then, a 0.4 M K₂C₂O₄ reducing solution, 0.02 M Pd(NO₃)₂, and particles containing the first active ingredient were mixed and stirred in a ratio of 8.5:85:18. After being dried and calcined at 500°C for 6 hours, the catalyst composition of Preparation Example 1 was obtained.

[0027] <Preparation Example 2>

[0028] The same method as in Preparation Example 1 was used, but the components added to the colloidal solution were changed to a hot aqueous solution containing 25,000 ppm manganese ions and 5,000 ppm nickel ions.

[0029] <Preparation Example 3>

[0030] The same method as in Preparation Example 1 was used, but the components added to the colloidal solution were changed to a hot aqueous solution containing 25,000 ppm manganese ions and 5,000 ppm copper ions.

[0031] <Preparation Example 4>

[0032] The same method as in Preparation Example 1 was used, but the components added to the colloidal solution were changed to a hot aqueous solution containing 25,000 ppm manganese ions and 5,000 ppm nickel ions, and the reducing solution was changed to Na3C6H5O7.

[0033] <Preparation Example 5>

[0034] The same method as in Preparation Example 4 was used, but the components added to the colloidal solution were changed to a hot aqueous solution containing 25,000 ppm manganese ions and 5,000 ppm copper ions.

[0035] <Preparation Example 6>

[0036] The same method as in Preparation Example 1 was used, but Pd(NO3)2 was replaced with Pt(NO3)2.

[0037] <Comparative Preparation Example 1>

[0038] After obtaining particles containing the first active ingredient using the same method as in Preparation Example 1, the particles were directly calcined to obtain a catalyst composition containing only manganese oxide.

[0039] <Comparative Preparation Example 2>

[0040] The same method as in Preparation Example 1 was used, but without the addition of K₂C₂O₄ reducing solution.

[0041] <Comparative Preparation Example 3>

[0042] The same method as in Preparation Example 6 was used, but without the addition of K₂C₂O₄ reducing solution.

[0043] <Comparative Preparation Example 4>

[0044] The same method as in Preparation Example 2 was used, but the components added to the colloidal solution were changed to a hot aqueous solution containing 25,000 ppm manganese ions and 5,000 ppm iron ions, and the K 2C 2O 4 reducing solution was replaced with Ca 3(C 6H 5O 7) 2.

[0045] <Comparative Preparation Example 5>

[0046] The same method as in Preparation Example 5 was used, but the manganese ions added to the colloidal solution were replaced with 25,000 ppm of molybdenum ions.

[0047] <Component Analysis>

[0048] 1. The component ratios of the catalyst compositions of Preparation Examples 1-6 and Comparative Preparation Examples 1-5 were determined by energy-scattered X-ray spectroscopy (EDS) and are recorded in Table 1 below.

[0049] 2. The specific surface areas of the catalyst compositions of Preparation Examples 1-6 and Comparative Preparation Examples 1-5 were obtained by nitrogen adsorption-desorption (BET method) and are also recorded in Table 1 below.

[0050] Table 1 C1 C2 C3 C4 carrier Specific surface area manganese oxide Pt Pd potassium oxide Sodium oxide copper oxide Nickel oxide Comparative Preparation Example 1 19.2 80.8 233 m 2g -1 Preparation Example 1 14.5 0.01 5.1 80.4 222 m 2g -1 Preparation Example 2 4.6 0.01 5.2 3.2 87.0 141 m 2g -1 Preparation Example 3 5.4 0.03 6.2 8.8 79.6 163 m 2g -1 Preparation Example 4 4.6 0.06 7.3 5.8 82.2 143 m 2g -1 Preparation Example 5 5.5 0.01 5.4 7.5 81.6 151 m 2g -1 Preparation Example 6 14.8 0.1 4.9 80.2 219 m 2g -1 Comparative Preparation Example 2 17.4 0.01 82.5 225 m 2g -1 Comparative Preparation Example 3 21.3 0.05 78.6 237 m 2g -1 Comparative preparation example 4 6.9 0.01 (Calcium oxide) 2.9 (Iron oxide) 10.4 79.8 142 m 2g -1 Comparative Preparation Example 5 (Molybdenum oxide) 6.7 0.01 4.6 4.4 84.3 151 m 2g -1 The component values ​​in Table 1 are all in atomic percentage (at%), and the oxides in parentheses represent other catalyst components used in the comparative preparation examples.

[0051] Table 2 below shows the calculated molar ratios of each catalyst in the catalyst compositions of Preparation Examples 1-6 and Comparative Preparation Examples 2-5.

[0052] Table 2 Mole ratio C1:C2 C1:C3 C1:C4 C1: Carrier Preparation Example 1 1:0.001 1:0.35 - 1:5.54 Preparation Example 2 1:0.002 1:1.13 1:0.7 1:18.91 Preparation Example 3 1:0.006 1:1.15 1:1.63 1:14.74 Preparation Example 4 1:0.013 1:1.59 1:1.26 1:17.87 Preparation Example 5 1:0.002 1:0.98 1:1.36 1:14.84 Preparation Example 6 1:0.007 1:0.33 - 1:5.42 Comparative Preparation Example 2 1:0.001 - - 1:4.74 Comparative Preparation Example 3 1:0.002 - - 1:3.69 Comparative preparation example 4 1:0.001 1:0.42 1:1.51 1:11.57 Comparative Preparation Example 5 1:0.001 1:0.69 1:0.66 1:12.58

[0053] To verify the treatment efficiency of the above catalyst composition, a device for removing nitrogen oxides was constructed, the block diagram of which is shown in Figure 3. In Figure 3, the reactor (i.e., the heating furnace) contains the catalyst composition, and the gas to be tested is fed into the heating furnace via path 2 through a three-way valve. A Fourier transform infrared spectroscopy (FTIR) instrument can be used to determine the NOx concentration.

[0054] <Experimental Example 1>

[0055] Take 20 ml of the catalyst composition of Preparation Example 1 and place it in the heating furnace shown in Figure 3. The temperature is controlled between 100°C and 350°C. 1% NO X, 3% H 2 (reducing agent) and compressed dry air (CDA) are delivered to the three-way valve through the mass flow controller (MFC) to mix into a test gas with a total gas flow rate of 600 sccm, wherein the gas hourly space velocity (GHSV) is about 1800 h -1, the NO gas flow rate is about 360 ppm, and the NO 2 gas flow rate is about 240 ppm.

[0056] The NOx concentration of the test gas entering the FTIR via path 1 and the NOx concentration of the test gas entering the FTIR via path 2 were tested respectively. The treatment efficiency and selectivity were calculated based on the NOx concentrations measured before and after treatment and recorded in Table 3 below.

[0057] Table 3 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C > 99.6% > 98.1% 84.8% 150°C 97.5% > 98.1% 82.2% 200°C 91.3% > 98.1% 81.0% 250°C 87.5% > 98.1% 93.6% 300°C 67.8% 92.3% 97.8% The destruction and removal efficiency (DRE) in the table is calculated as follows: [1 - (NOx concentration entering FTIR via path 2 ÷ NOx concentration entering FTIR via path 1)] × 100%. In the table, N2 selectivity = [NO2 X reacted - (byproducts generated × byproduct N equivalent)] ÷ NO2 X reacted.

[0058] As shown in Table 3, the catalyst composition of Preparation Example 1 achieved a NO2 removal rate of over 98.1% at temperatures ranging from 100°C to 250°C, and a NO2 removal rate of over 87.5% at the same temperatures. The N2 selectivity was greater than 80% in both cases.

[0059] <Experimental Example 2>

[0060] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Preparation Example 2 for testing. The results are shown in Table 4 below.

[0061] Table 4 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C 96.5% > 97.7% 83.5% 150°C 95.6% > 97.7% 82.3% 200°C 84.0% > 97.7% 92.6% 250°C 89.2% > 97.7% 95.9% 300°C 74.2% 89.9% 96.6%

[0062] As shown in Table 4, the catalyst composition of Preparation Example 2 achieved a NO2 removal rate of over 97.7% at temperatures ranging from 100°C to 250°C, and a NO2 removal rate of over 80% at the same temperature range. The N2 selectivity was greater than 80% in both cases.

[0063] <Experimental Example 3>

[0064] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Preparation Example 3 for testing. The results are shown in Table 5 below.

[0065] Table 5 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C 99.1% > 98.7% 98.9% 150°C > 99.4% > 98.7% 92.6% 200°C 82.7% > 98.7% 97.3%

[0066] As shown in Table 5, the catalyst composition of Preparation Example 3 achieved a NO2 removal rate of over 98.7% and an NO removal rate of over 80% at temperatures ranging from 100°C to 200°C. The N2 selectivity was greater than 90% in both cases.

[0067] <Experimental Example 4>

[0068] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Preparation Example 4 for testing. The results are shown in Table 6 below.

[0069] Table 6 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C > 99.5% > 98.2% 81.1% 150°C > 99.5% > 98.2% 81.5% 200°C > 99.5% > 98.2% 82.9% 250°C > 99.5% > 98.2% 94.3% 300°C 88.2% > 98.2% 99.9% 350°C 55.6% 80.6% 99.5%

[0070] As shown in Table 6, the catalyst composition of Preparation Example 4 achieved a NO2 removal rate of over 98.2% at temperatures ranging from 100°C to 300°C, and a NO2 removal rate of over 88.2% at the same temperatures. The N2 selectivity was greater than 80% in both cases.

[0071] <Experimental Example 5>

[0072] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Preparation Example 5 for testing. The results are shown in Table 7 below.

[0073] Table 7 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C > 99.6% > 98.3% 98.8% 150°C > 99.6% > 98.3% 90.4% 200°C > 99.6% > 98.3% 92.5%

[0074] As shown in Table 7, the catalyst composition of Preparation Example 5 achieved a NO2 removal rate and a NO removal rate of over 98.3% at temperatures ranging from 100°C to 200°C. The N2 selectivity was also greater than 90%.

[0075] <Experimental Example 6>

[0076] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Preparation Example 6 for testing. The results are shown in Table 8 below.

[0077] Table 8 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C > 99.3% > 98.7% 78.2% 150°C > 99.3% > 98.7% 93.1% 200°C > 99.3% > 98.7% 94.2% 250°C > 99.3% > 98.7% 96.5% 300°C > 99.3% > 98.7% 98.2% 350°C 97.6% 95.7% 98.7%

[0078] As shown in Table 8, the catalyst composition of Preparation Example 6 achieved NO2 removal rates and NO removal rates of over 95% at temperatures ranging from 100°C to 350°C. The N2 selectivity was greater than 90% at temperatures ranging from 150°C to 350°C.

[0079] <Comparative Example 1>

[0080] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Comparative Preparation Example 2 for testing. The results are shown in Table 9 below.

[0081] Table 9 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C 18.2% 61.2% 85.3% 150°C 9.2% 52.3% 72.1% 200°C 9.1% 49.4% 57.6% 250°C 14.8% 55.9% 44.6% 300°C 45.9% 85.8% 47.0%

[0082] As shown in Table 9, the catalyst composition of Preparation Example 2 exhibits poor nitrogen oxide treatment efficiency and unsatisfactory N2 selectivity. Therefore, the lack of a second active ingredient in the catalyst composition is detrimental to nitrogen oxide treatment.

[0083] <Comparative Example 2>

[0084] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Comparative Preparation Example 3 for testing. The results are shown in Table 10 below.

[0085] Table 10 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C 13.2% 6.4% 98.5% 150°C 15.9% 7.6% 98.7% 200°C 5.3% < 5% NA 250°C < 5% < 5% NA 300°C 31.4% < 5% NA 350°C 37.1% < 5% NA

[0086] As shown in Table 10, the catalyst composition of Comparative Preparation Example 3 exhibits very poor nitrogen oxide treatment efficiency, and shows no N2 selectivity above 200°C. Therefore, the lack of a second active ingredient in the catalyst composition is detrimental to nitrogen oxide treatment.

[0087] <Comparative Example 3>

[0088] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Comparative Preparation Example 4 for testing. The results are shown in Table 11 below.

[0089] Table 11 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C 25.1% 67.8% 46.3% 150°C 32.9% 78.3% 12.5% 200°C 34.2% 83.8% 11.8% 250°C 40.2% 85.5% 11.5% 300°C 36.1% 80.3% 46.3%

[0090] Table 11 shows that the catalyst composition of Preparation Example 4 has poor nitrogen oxide treatment efficiency and very poor N2 selectivity. Therefore, if the second active ingredient in the catalyst composition is replaced with another metal oxide, it will also be detrimental to nitrogen oxide treatment.

[0091] <Comparative Example 4>

[0092] The same equipment and parameters as in Experimental Example 1 were used, but the catalyst composition of Preparation Example 1 was replaced with the catalyst composition of Comparative Preparation Example 5 for testing. The results are shown in Table 12 below.

[0093] Table 12 reaction temperature NO processing efficiency NO 2 Processing efficiency N 2 selectivity 100°C < 5% 26.6% 87.9% 150°C 5.2% 30.9% 35.6% 200°C 44.8% 83.1% 72.9% 250°C 80.8% > 96.4% 72.3% 300°C 60.1% 94.0% 32.4% 350°C 38.1% 83.6% 26.2%

[0094] Table 12 shows that the nitrogen oxide treatment efficiency of the catalyst composition in Comparative Preparation Example 5 is poor, especially at low reaction temperatures. The N2 selectivity is also poor. Therefore, if the first active ingredient in the catalyst composition does not include manganese oxide, it will be detrimental to nitrogen oxide treatment.

[0095] Although the present invention has been disclosed above by way of embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make some modifications and refinements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.

[0096] 100, 200: Catalyst Composition 102: Carrier 102s, 104s, 202s: surface 104, 202: First active ingredient 106: Second active ingredient C1: First Catalyst C2: Second Catalyst C3: Third Catalyst C4: Fourth Catalyst FTIR: Fourier Transform Infrared Spectrometer H2: Hydrogen H₂O: water MFC: Mass Flow Controller N2: Nitrogen gas NOx: Nitrogen oxides

Claims

1. A catalyst composition comprising: A carrier; a first active ingredient coated on the surface of the carrier, wherein the first active ingredient includes a first catalyst, the first catalyst being manganese oxide; The carrier contains a second active ingredient, including a second catalyst and a third catalyst, coated on the surface of the first active ingredient and the surface of the carrier not coated with the first active ingredient. The second catalyst comprises platinum metal, palladium metal, or a combination thereof, and the third catalyst comprises potassium oxide, sodium oxide, or a combination thereof. The molar ratio of the first catalyst to the second catalyst is from 1:0.001 to 1:0.2, and the molar ratio of the first catalyst to the third catalyst is from 1:0.1 to 1:

10.

2. The catalyst composition of claim 1, wherein the first active ingredient further comprises a fourth catalyst comprising copper oxide, nickel oxide, or a combination thereof.

3. The catalyst composition as claimed in claim 2, wherein the molar ratio of the first catalyst to the fourth catalyst is from 1:0.1 to 1:

10.

4. The catalyst composition as claimed in claim 1, wherein the molar ratio of the first catalyst to the carrier is 1:3 to 1:

20.

5. The catalyst composition as claimed in claim 1, wherein the carrier comprises alumina, titanium oxide, zirconium oxide, cerium oxide, magnesium oxide, or a combination thereof.

6. The catalyst composition as claimed in claim 1, wherein the specific surface area (BET) of the catalyst composition is from 140 m²g⁻¹ to 500 m²g⁻¹.

7. The catalyst composition as claimed in claim 1, wherein the particle size of the catalyst composition is from 100 µm to 10 mm.

8. A method for removing nitrogen oxides, comprising using a catalytic composition as described in any one of claims 1 to 7 to perform a hydrogen-selective reduction reaction of nitrogen oxides.

9. The method for removing nitrogen oxides as described in claim 8, wherein the removal rate of the nitrogen oxides is 90% or more.

10. The method for removing nitrogen oxides as claimed in claim 8, wherein the hydrogen selective reduction reaction is carried out at a temperature of 100°C to 250°C.

Citation Information

Patent Citations

  • Catalyst, device and method for selective NOx reduction by means of hydrogen in NOx-containing exhaust gases

    DE102016107466A1

  • A well-structured catalyst for reducing NOx emissions from flue gas, and its preparation and application methods.