Plasma-resistant glass, chamber interior part for semiconductor manufacturing process, and methods for manufacturing glass and part
Patent Information
- Application Number
- PCT/KR2023/012475
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-15
- Filing Date
- 2023-08-23
- Publication Date
- 2024-11-07
AI Technical Summary
Semiconductor manufacturing processes face challenges with plasma-resistant glass components that are prone to thermal shock damage, have high dielectric constants, and are difficult to mold due to high melting temperatures, leading to defects and reduced production yield.
Development of plasma-resistant glass containing Si-based oxide, Al-based oxide, Mg-based oxide, Mg-based halide, and Ge-based oxide, with specific composition ranges to achieve low melting temperatures, reduced thermal expansion coefficients, and controlled viscosity for improved moldability and durability.
The solution provides components with enhanced plasma resistance, thermal shock resistance, and improved moldability, reducing defects and extending usage time in semiconductor manufacturing processes while maintaining high light transmittance and mechanical properties.
Smart Images

Figure KR2023012475_07112024_PF_FP_ABST
Abstract
Description
Plasma-resistant glass, components for use in chambers for semiconductor manufacturing processes, and methods for manufacturing them
[0001] The present invention claims the benefit of Korean Patent Application No. 10-2022-0135711, filed with the Korean Intellectual Property Office on October 20, 2022, and the benefit of Korean Patent Application No. 10-2023-0076784, filed with the Korean Intellectual Property Office on June 15, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to plasma-resistant glass, components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing the same, and more particularly, to plasma-resistant glass, components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing the same, in which the content of plasma-resistant glass components is controlled to lower the melting temperature, the coefficient of thermal expansion is reduced to prevent damage from thermal shock during high-temperature use, the light transmittance and durability are improved, the dielectric constant is reduced, and the formability is improved by controlling the viscosity of the melt.
[0003] Plasma etching processes are used in semiconductor and / or display manufacturing. With the recent adoption of nanotechnology, the difficulty of etching has increased. Internal components of process chambers exposed to high-density plasma environments are primarily made of corrosion-resistant oxide ceramics, such as alumina (Al2O3) and yttria (Y2O3).
[0004] When polycrystalline materials are exposed to high-density plasma etching environments using fluorine-based gases for extended periods, localized erosion can cause particle loss, increasing the likelihood of contaminating particles. This can lead to defects in semiconductors and displays and negatively impact production yields. Furthermore, oxide-based ceramic materials have a high melting temperature, which limits workability.
[0005] Therefore, there is a need for technology development that can prevent thermal shock damage to existing plasma-resistant glass while having a low melting temperature, reduce the dielectric constant, and control the viscosity to easily form it into a desired shape.
[0006] The technical problem to be achieved by the present invention is to provide plasma-resistant glass having excellent resistance to plasma inside a chamber used in a semiconductor manufacturing process, excellent heat resistance under high temperature conditions to prevent damage to components used inside the chamber, capable of implementing a low melting temperature, and having a dielectric constant in an appropriate range and being easily moldable into a desired shape by controlling viscosity, components for use inside a chamber for a semiconductor manufacturing process, and a method for manufacturing them.
[0007] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0008] One embodiment of the present invention provides a plasma-resistant glass comprising a Si-based oxide, an Al-based oxide, a Mg-based oxide, a Mg-based halide, and a Ge-based oxide.
[0009] According to one embodiment of the present invention, the content of the Si-based oxide may be 20 wt% or more and 70 wt% or less, the content of the Al-based oxide may be 5 wt% or more and 30 wt% or less, the content of the Mg-based oxide may be 5 wt% or more and 50 wt% or less, the content of the Mg-based halide may be 0.01 wt% or more and 10 wt% or less, and the content of the Ge-based oxide may be 0.01 wt% or more and 25 wt% or less.
[0010] According to one embodiment of the present invention, the light transmittance may be 80% or more and 100% or less.
[0011] According to one embodiment of the present invention, the Vickers hardness may be 550 HV or more and 1,000 HV or less.
[0012] According to one embodiment of the present invention, the glass transition temperature may be 600°C or higher and 850°C or lower.
[0013] According to one embodiment of the present invention, the coefficient of thermal expansion is 4.0×10 -6 m / (m℃) or more than 6.0×10 -6 It may be less than m / (m℃).
[0014] According to one embodiment of the present invention, the etching rate by a mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than or equal to 100 nm / min.
[0015] According to one embodiment of the present invention, the melting point may be 1,400°C or higher and 1,700°C or lower.
[0016] One embodiment of the present invention provides a chamber internal component for a semiconductor manufacturing process made of the above plasma-resistant glass.
[0017] According to one embodiment of the present invention, the internal component may be any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electro static chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame.
[0018] One embodiment of the present invention provides a method for manufacturing plasma-resistant glass, comprising the steps of: melting a composition comprising 20 wt% or more and 70 wt% or less of Si-based oxide, 5 wt% or more and 30 wt% or less of Al-based oxide, 5 wt% or more and 50 wt% or less of Mg-based oxide, 0.01 wt% or more and 10 wt% or less of Mg-based halide, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide; and cooling the molten composition.
[0019] According to one embodiment of the present invention, the melting temperature of the step of melting the composition may be 1,400°C or more and 1,700°C or less.
[0020] One embodiment of the present invention provides a method for manufacturing a chamber-internal component for a semiconductor manufacturing process, comprising the steps of: melting the plasma-resistant glass; injecting the molten plasma-resistant glass into a mold; and annealing the injected plasma-resistant glass.
[0021] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,400°C or more and 1,700°C or less.
[0022] According to one embodiment of the present invention, the temperature of the annealing step may be 400°C or more and 900°C or less.
[0023] A plasma-resistant glass according to one embodiment of the present invention can have a dielectric constant within a specific range, can have a low melting temperature to improve processability, and can easily manufacture parts for use inside a chamber for a semiconductor manufacturing process.
[0024] The plasma-resistant glass according to one embodiment of the present invention can improve plasma resistance and increase formability by reducing viscosity due to the addition of F.
[0025] The plasma-resistant glass according to one embodiment of the present invention exhibits a low thermal expansion coefficient characteristic, and thus can prevent damage due to thermal shock in a high-temperature atmosphere.
[0026] The plasma-resistant glass according to one embodiment of the present invention has improved light transmittance and improved hardness, thereby improving mechanical properties, thereby improving durability in a plasma etching environment.
[0027] A component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can improve the usability in a semiconductor manufacturing process by implementing a low etching rate for plasma, and can improve durability by preventing damage to the component due to thermal shock.
[0028] A method for manufacturing plasma-resistant glass according to one embodiment of the present invention can easily manufacture plasma-resistant glass and prevent damage due to thermal shock in a high-temperature atmosphere.
[0029] A method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can manufacture components having various shapes, prevent damage due to thermal shock in a high-temperature atmosphere, and easily manufacture components.
[0030] A method for manufacturing plasma-resistant glass according to one embodiment of the present invention can improve formability by controlling the viscosity of the composition.
[0031] The effects of the present invention are not limited to the effects described above, and effects not mentioned will be clearly understood by those skilled in the art from the present specification and the attached drawings.
[0032] Figure 1 is a flow chart of a method for manufacturing plasma-resistant glass according to one embodiment of the present invention.
[0033] Figure 2 is a flowchart of a method for manufacturing a chamber internal component for a semiconductor manufacturing process according to one embodiment of the present invention.
[0034] Figure 3 is a photograph of plasma-resistant glass of Example 1 according to one embodiment of the present invention.
[0035] Figure 4 is a photograph of plasma-resistant glass of Example 2 according to one embodiment of the present invention.
[0036] Figure 5 is a photograph of plasma-resistant glass of Example 3 according to one embodiment of the present invention.
[0037] Figure 6 is a photograph of plasma-resistant glass of Example 4 according to one embodiment of the present invention.
[0038] Figure 7 is a photograph of plasma-resistant glass of Example 5 according to one embodiment of the present invention.
[0039] Figure 8 is a photograph of the plasma-resistant glass of Comparative Example 1.
[0040] Figure 9 is a photograph of the plasma-resistant glass of Comparative Example 2.
[0041] [Explanation of symbols]
[0042] S 11: Composition melting stage
[0043] S 13: Cooling stage
[0044] S 21: Plasma-resistant glass melting stage
[0045] S 23: Mold injection stage
[0046] S 25: Annealing step
[0047] S 27: Processing stage
[0048] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise stated.
[0049] Throughout this specification, “A and / or B” means “A and B, or A or B.”
[0050] Hereinafter, the present invention will be described in more detail.
[0051] One embodiment of the present invention provides a plasma-resistant glass comprising a Si-based oxide, an Al-based oxide, a Mg-based oxide, a Mg-based halide, and a Ge-based oxide.
[0052] The plasma-resistant glass according to one embodiment of the present invention can have a low dielectric constant, improve processability by implementing a low melting temperature, and can easily manufacture parts for use inside a chamber for a semiconductor manufacturing process, and exhibits a low thermal expansion coefficient characteristic, so as to prevent damage caused by thermal shock in a high-temperature atmosphere, improve light transmittance, and improve hardness to improve mechanical properties, thereby improving durability in a plasma etching environment. Furthermore, the viscosity of the melt of the composition can be adjusted to improve formability.
[0053] According to one embodiment of the present invention, the plasma-resistant glass may be formed by melting a plasma-resistant glass composition including a Si-based oxide, an Al-based oxide, a Mg-based oxide, a Mg-based halide, and a Ge-based oxide.
[0054] According to one embodiment of the present invention, in the plasma-resistant glass, the content of the Si-based oxide may be 20 wt% or more and 70 wt% or less, the content of the Al-based oxide may be 5 wt% or more and 30 wt% or less, the content of the Mg-based oxide may be 5 wt% or more and 50 wt% or less, the content of the Mg-based halide may be 0.01 wt% or more and 10 wt% or less, and the content of the Ge-based oxide may be 0.01 wt% or more and 25 wt% or less. Specifically, the plasma-resistant glass may include 20 wt% or more and 70 wt% or less of a Si-based oxide, 5 wt% or more and 30 wt% or less of an Al-based oxide, 5 wt% or more and 50 wt% or less of a Mg-based oxide, 0.01 wt% or more and 10 wt% or less of a Mg-based halide, 0.01 wt% or more and 50 wt% or less of a Ge-based oxide, and unavoidable impurities. Specifically, the plasma-resistant glass may be formed by melting a composition containing 20 wt% or more and 70 wt% or less of Si-based oxide, 5 wt% or more and 30 wt% or less of Al-based oxide, 5 wt% or more and 50 wt% or less of Mg-based oxide, 0.01 wt% or more and 10 wt% or less of Mg-based halide, 0.01 wt% or more and 25 wt% or less of Ge-based oxide, and unavoidable impurities, and the plasma-resistant glass may be uniformly contained in the above respective component ratios.
[0055] According to one embodiment of the present invention, the plasma-resistant glass may include 20 wt% or more and 70 wt% or less of a Si-based oxide. Specifically, the content of the Si-based oxide may be 25 wt% or more and 69 wt% or less, 30 wt% or more and 68 wt% or less, 35 wt% or more and 67 wt% or less, 40 wt% or more and 66 wt% or less, 45 wt% or more and 65 wt% or less, 50 wt% or more and 65 wt% or less, or 55 wt% or more and 65 wt% or less. As described above, by including the Si-based oxide and controlling the content of the Si-based oxide within the above-described range, the basic properties of the plasma-resistant glass can be secured, durability and reliability can be improved, and processing of the plasma can be facilitated, thereby reducing the production cost of parts.
[0056] According to one embodiment of the present invention, the plasma-resistant glass may include 5 wt% or more and 30 wt% or less of an Al-based oxide. Specifically, the content of the Al-based oxide may be 6 wt% or more and 29 wt% or less, 7 wt% or more and 28 wt% or less, 8 wt% or more and 27 wt% or less, 9 wt% or more and 26 wt% or less, or 10 wt% or more and 25 wt% or less. As described above, by including the Al-based oxide and controlling the content of the Al-based oxide within the above-described range, outgasing can be prevented, the generation of particles can be suppressed, and the wear resistance of components inside a chamber for a semiconductor manufacturing process can be improved.
[0057] According to one embodiment of the present invention, the plasma-resistant glass includes 5 wt% or more and 50 wt% or less of a Mg-based oxide. Specifically, the content of the Mg-based oxide may be 6 wt% or more and 40 wt% or less, 6 wt% or more and 30 wt% or less, 6 wt% or more and 20 wt% or less, or 6 wt% or more and 15 wt% or less. As described above, by including the Mg-based oxide and controlling the content of the Mg-based oxide within the above-described range, the thermal expansion coefficient and glass transition temperature of the glass can be lowered, thermal shock at high temperatures can be minimized, the durability of components inside a chamber for a semiconductor manufacturing process can be improved, and the dielectric constant can be implemented within an appropriate range.
[0058] According to one embodiment of the present invention, the plasma-resistant glass includes 0.01 wt% or more and 10 wt% or less of a Mg-based halide. Specifically, the Mg-based halide may be 1 wt% or more and 9 wt% or less, 2 wt% or more and 7 wt% or less, or 2 wt% or more and 5 wt% or less. As described above, by including the Mg-based halide and controlling the amount of the Mg-based halide within the above-described range, the viscosity of the melt of the plasma-resistant glass can be reduced, thereby improving the formability of the plasma-resistant glass.
[0059] According to one embodiment of the present invention, the plasma-resistant glass includes a Ge-based oxide of 0.01 wt% or more and 25 wt% or less. Specifically, the Ge-based oxide may be 1 wt% or more and 24 wt% or less, 2 wt% or more and 23 wt% or less, 3 wt% or more and 22 wt% or less, 4 wt% or more and 21 wt% or less, or 5 wt% or more and 20 wt% or less. As described above, when the plasma-resistant glass includes the Ge-based oxide, it has the same outermost electrons as the Si atoms, so that the glass after melting has similar properties to the Si and is cooled. In addition, the low melting point of Ge makes the melting process difficult, but the inclusion of the Ge-based oxide can implement a low dielectric constant. In addition, by controlling the content of the Ge-based oxide within the above-described range, the melting temperature of the plasma-resistant glass can be implemented low, enabling melting, and the dielectric constant can be implemented low. Furthermore, as described above, when the composition includes the Ge-based oxide, the fluorine (F2) gas used in the etching process reacts with the Ge-based oxide to generate GeF2 (Boiling point: 130°C, Melting point: 120°C) or GeF4 (Boiling point: -15°C, Melting point: -36.5°C), and since these fluorine compounds have low BP and MP, they are blown away as gas during the etching process, so particles may not be formed.
[0060] According to one embodiment of the present invention, the Si-based oxide may contain an O atom with a Si atom as a central atom. Specifically, the Si-based oxide is SiO2. It is preferable. As described above, by selecting the Si-based oxide containing O atoms with Si atoms as the central atom, the basic properties of the plasma-resistant glass can be secured, durability and reliability can be improved, and the processing of the plasma-resistant glass can be facilitated, thereby reducing the production cost of the parts.
[0061] According to one embodiment of the present invention, the Al-based oxide may contain an O atom with an Al atom as a central atom. Specifically, the Al-based oxide is Al2O3. Preferably, as described above, by selecting the Al-based oxide containing O atoms with Al atoms as the central atom, outgasing can be prevented, particle generation can be suppressed, and the wear resistance of internal parts of a chamber for a semiconductor manufacturing process can be improved.
[0062] According to one embodiment of the present invention, the Mg-based oxide may contain an O atom with a Mg atom as a central atom. Specifically, the Mg-based oxide is MgO. Preferably. As described above, by selecting the Mg-based oxide containing O atoms with Mg atoms as the central atom, the thermal expansion coefficient and glass transition temperature of the glass can be lowered, thermal shock at high temperatures can be minimized, the durability of components inside a chamber for a semiconductor manufacturing process can be improved, and the dielectric constant can be implemented within an appropriate range.
[0063] According to one embodiment of the present invention, the Mg-based halide may contain a halogen atom with a Mg atom as a central atom. Specifically, the Mg-based halide is preferably MgF2. As described above, by selecting the Mg-based halide as containing a halogen atom with a Mg atom as a central atom, the viscosity of the molten material of the composition can be reduced, thereby improving the formability of a plasma-resistant glass using the composition.
[0064] According to one embodiment of the present invention, the Ge-based oxide may be one selected from the group consisting of GeO, GeO2, Ge2O3, and combinations thereof. Preferably, the Ge-based oxide may be GeO2. By selecting the Ge-based oxide from the above, the melting temperature of the plasma-resistant glass can be lowered to enable melting, and the dielectric constant can be lowered.
[0065] According to one embodiment of the present invention, the plasma-resistant glass may be formed by melting a composition containing SiO2, Al2O3, MgO, MgF2, and GeO2. More specifically, the plasma-resistant glass may be formed by melting a composition containing SiO2, Al2O3, MgO, MgF2, and GeO2. As described above, by forming the plasma-resistant glass by melting the composition, each component can be uniformly distributed in the plasma-resistant glass, and an etching rate can be uniformly implemented over the entire area of the plasma-resistant glass.
[0066] According to one embodiment of the present invention, the plasma-resistant glass has a dielectric constant of 6.00 or more and 7.40 or less. Specifically, the plasma-resistant glass may have a dielectric constant of 6.70 or more and 8.05 or less, 6.75 or more and 8.00 or less, 6.80 or more and 7.95 or less, 6.85 or more and 7.90 or less, 6.90 or more and 7.85 or less, 6.95 or more and 7.80 or less, 7.00 or more and 7.75 or less, 7.05 or more and 7.70 or less, 7.10 or more and 7.65 or less, 7.15 or more and 7.60 or less, 7.20 or more and 7.55 or less, 7.25 or more and 7.50 or less, 7.30 or more and 7.45 or less, or 7.35 or more and 7.40 or less. More specifically, the plasma-resistant glass may have a dielectric constant of 6.79 or more and 6.99 or less, 6.79 or more and 7.19 or less, 6.79 or more and 7.39 or less, 6.79 or more and 7.59 or less, 6.99 or more and 7.19 or less, 6.99 or more and 7.39 or less, 6.99 or more and 7.59 or less, 7.19 or more and 7.39 or less, 7.19 or more and 7.59 or less, 7.39 or more and 7.59 or less. Methods for measuring the dielectric constant include a capacitance method using an LCR meter, a reflectance coefficient method using a network analyzer, a resonant frequency method, etc. As an example of a dielectric constant measurement method, the capacitance method using an LCR meter is primarily used to measure low-frequency characteristics (kHz, MHz), and the dielectric constant can be determined from the physical size and capacitance of the capacitor. More specifically, it can refer to measuring the dielectric constant in the frequency range of 20 Hz to 100 Hz using the Keysight E4990A Impedence Analyzer.By implementing the dielectric constant of the plasma-resistant glass within the above-described range, thermal shock at high temperatures can be minimized, durability of components inside a chamber for a semiconductor manufacturing process can be improved, and light transmittance and durability can be improved.
[0067] According to one embodiment of the present invention, the plasma-resistant glass may be composed only of Si-based oxides, Al-based oxides, Mg-based oxides, Mg-based halides, Ge-based oxides, and unavoidable impurities. Specifically, the plasma-resistant glass may be composed only of SiO2, Al2O3, MgO, MgF2, GeO2 oxides, and unavoidable impurities. Specifically, according to one embodiment of the present invention, the plasma-resistant glass may not contain any other components except for SiO2, Al2O3, MgO, MgF2, GeO2 oxides, and unavoidable impurities. By manufacturing the plasma-resistant glass with the above-described components, the melt has an appropriate viscosity, so that a product having a complex shape can be easily formed.
[0068] According to one embodiment of the present invention, the light transmittance of the plasma-resistant glass may be 80% or more and 100% or less. Specifically, the light transmittance of the plasma-resistant glass may be 82% or more and 98% or less, 85% or more and 95% or less, or 87% or more and 92% or less. In the present specification, “light transmittance” may mean a value measured using a haze meter (JCH-300S, Oceanoptics Co.). By implementing the light transmittance of the plasma-resistant glass within the above-described range, the melting degree of the plasma-resistant glass can be improved while simultaneously implementing high vitrification.
[0069] According to one embodiment of the present invention, the Vickers hardness of the plasma-resistant glass may be 550 HV or more and 1,000 HV or less. The Vickers hardness of the above plasma glass may be 560 HV or more and 980 HV or less, 570 HV or more and 950 HV or less, 580 HV or more and 930 HV or less, 600 HV or more and 900 HV or less, 620 HV or more and 880 HV or less, 650 HV or more and 850 HV or less, 680 HV or more and 820 HV or less, 690 HV or more and 810 HV or less, 700 HV or more and 800 HV or less, 710 HV or more and 790 HV or less, 720 HV or more and 780 HV or less, 730 HV or more and 770 HV or less, or 740 HV or more and 760 HV or less. In this specification, “Vickers hardness” may refer to a value measured using a Vickers hardness tester (Helmut Fischer, FISCHERSCOPE HM-2000). By implementing the Vickers hardness of the plasma-resistant glass within the above-described range, the mechanical properties can be increased and durability in a plasma etching environment can be improved.
[0070] According to one embodiment of the present invention, the glass transition temperature of the plasma-resistant glass may be 600°C or more and 850°C or less. Specifically, the glass transition temperature of the plasma-resistant glass may be 620°C or more and 830°C or less, 650°C or more and 800°C or less, 670°C or more and 780°C or less, or 700°C or more and 750°C or less. By controlling the glass transition temperature of the plasma-resistant glass within the above-described range, the thermal shock of components for use inside a chamber for a semiconductor manufacturing process at high temperatures can be minimized, and the durability can be improved.
[0071] According to one embodiment of the present invention, the coefficient of thermal expansion of the plasma-resistant glass is 4.0Х10 -6 m / (m℃) or more 6.0Х10 -6m / (m℃) or less. Specifically, the coefficient of thermal expansion of the plasma-resistant glass is 4.1×10 -6 m / (m℃) or more than 5.9×10 -6 m / (m℃) or less, 4.2×10 -6 m / (m℃) or more than 5.8×10 -6 m / (m℃) or less, 4.3×10 -6 m / (m℃) or more than 5.7×10 -6 m / (m℃) or less, 4.4×10 -6 m / (m℃) or more than 5.6×10 -6 m / (m℃) or less, 4.5×10 -6 m / (m℃) or more than 5.5×10 -6 m / (m℃) or less, 4.6×10 -6 m / (m℃) or more than 5.4×10 -6 m / (m℃) or less, 4.7×10 -6 m / (m℃) or more than 5.3×10 -6 m / (m℃) or less, 4.8×10 -6 m / (m℃) or more than 5.2×10 -6 m / (m℃) or less or 4.9×10 -6 m / (m℃) or more than 5.1×10 -6 It may be m / (m℃) or less. By controlling the coefficient of thermal expansion of the plasma-resistant glass within the above-described range, damage to components due to thermal shock can be prevented, thereby improving durability.
[0072] According to one embodiment of the present invention, the etching rate of the plasma-resistant glass by the mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than 100 nm / min. Specifically, the etching rate of the plasma-resistant glass by the mixed plasma of fluorine and argon (Ar) may be greater than 0 nm / min and less than 95 nm / min, greater than 10 nm / min and less than 90 nm / min, greater than 20 nm / min and less than 85 nm / min, greater than 30 nm / min and less than 80 nm / min, or greater than 35 nm / min and less than 65 nm / min. By implementing the etching rate by the mixed plasma of fluorine and argon (Ar) in the above-described range, the internal components of the chamber for the semiconductor manufacturing process can implement a low etching rate for plasma, thereby improving the use time in the semiconductor manufacturing process.
[0073] According to one embodiment of the present invention, the melting point of the plasma-resistant glass may be 1,400°C or more and 1,700°C or less. In the present specification, the melting point may mean the melting temperature. Specifically, the above plasma-resistant glass has a melting point of 1,410 ℃ to 1,690 ℃, 1,420 ℃ to 1,680 ℃, 1,430 ℃ to 1,670 ℃, 1,440 ℃ to 1,660 ℃, 1,450 ℃ to 1,650 ℃, 1,460 ℃ to 1,640 ℃, 1,470 ℃ to 1,630 ℃, 1,480 ℃ to 1,620 ℃, 1,490 ℃ to 1,610 ℃, 1,500 ℃ to 1,600 ℃, 1,510 ℃ to 1,590 ℃, 1,520 ℃ to 1,580 ℃, It may be 1,530 ℃ or more and 1,570 ℃ or less, or 1,540 ℃ or more and 1,560 ℃ or less. By controlling the melting point of the plasma-resistant glass within the above-described range, the viscosity of the melt of the plasma-resistant glass can be controlled, and the workability of the process using the plasma-resistant glass can be improved.
[0074] According to one embodiment of the present invention, the viscosity of the molten composition is 1 poise or more and 10 poise or more at 1,400 ℃ or more and 1,700 ℃ or less or 1500 ℃ or more and 1750 ℃ or less. 9 poise or less. Specifically, the viscosity of the molten composition may be 10 poise or more and 10 poise or less at 1,550°C or more and 1,750°C or less. 8 Poise or less, 10 2 Poise 10 or higher 7 Poise or less, 10 3 Poise 10 or higher 6 poise or less or 10 4 Poise 10 or higher 5poise or less. By controlling the viscosity of the molten composition within the above-described range, the formability of the plasma glass can be improved.
[0075] According to one embodiment of the present invention, the plasma-resistant glass may be amorphous. By implementing the structure of the plasma-resistant glass as amorphous as described above, the durability of components using the plasma-resistant glass can be improved, while at the same time reducing the etching rate due to plasma.
[0076] One embodiment of the present invention provides a chamber internal component for a semiconductor manufacturing process made of the above plasma-resistant glass.
[0077] A component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can improve the usability in a semiconductor manufacturing process by implementing a low etching rate for plasma, and can improve durability by preventing damage to the component due to thermal shock.
[0078] According to one embodiment of the present invention, the internal component may be any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By using the internal component described above, the resistance to plasma in the semiconductor manufacturing process can be improved, thereby extending the usage time, and minimizing the cost required for semiconductor manufacturing.
[0079] One embodiment of the present invention provides a method for manufacturing plasma-resistant glass, comprising the steps of: melting a composition including Si-based oxide, Al-based oxide, Mg-based oxide, Mg-based halide, and Ge-based oxide (S11); and cooling the molten composition (S13).
[0080] A method for manufacturing plasma-resistant glass according to an embodiment of the present invention can easily manufacture plasma-resistant glass, prevent damage due to thermal shock in a high-temperature atmosphere, and manufacture glass with higher hardness than existing glass, thereby increasing mechanical properties and improving durability in a plasma etching environment.
[0081] FIG. 1 is a flowchart of a method for manufacturing plasma-resistant glass according to an embodiment of the present invention. Referring to FIG. 1, the method for manufacturing plasma-resistant glass according to an embodiment of the present invention will be described in detail.
[0082] In the method for manufacturing plasma-resistant glass, which is an embodiment of the present invention, description of the overlapping content with the plasma-resistant glass is omitted.
[0083] According to one embodiment of the present invention, a step (S11) of melting a composition comprising a composition including a Si-based oxide, an Al-based oxide, a Mg-based oxide, a Mg-based halide, and a Ge-based oxide is included. From the above, by controlling the components of the plasma-resistant glass, and controlling the content of the components, the dielectric constant of the plasma-resistant glass can be appropriately implemented, damage to the plasma-resistant glass due to thermal shock in a high-temperature atmosphere can be prevented, the melting temperature can be implemented low, light transmittance and durability can be improved, and the viscosity of the melt can be controlled to easily manufacture a product having a complex shape.
[0084] According to one embodiment of the present invention, the melting step may be performed by placing the composition in a platinum crucible and melting it. By melting the composition in a platinum crucible as described above, the components eluted from the crucible can be minimized and the properties of the plasma-resistant glass can be realized.
[0085] According to one embodiment of the present invention, a step (S13) of cooling the molten glass composition is included. By including the step of cooling the molten glass composition as described above, the crystal structure of the plasma-resistant glass can be controlled and breakage due to rapid thermal changes can be prevented.
[0086] According to one embodiment of the present invention, the temperature of the cooling step may be room temperature. By controlling the temperature of the cooling step within the above-described range, the crystallinity of the plasma-resistant glass can be controlled, and melting can be easily performed during the process of manufacturing components for use inside a chamber for the semiconductor manufacturing process.
[0087] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,400°C or more and 1,700°C or less. Specifically, the melting temperature of the step of melting the composition may have a melting point of 1,400°C or more and 1,700°C or less. In the present specification, the melting point may mean the melting temperature. Specifically, the above plasma-resistant glass has a melting point of 1,410 ℃ to 1,690 ℃, 1,420 ℃ to 1,680 ℃, 1,430 ℃ to 1,670 ℃, 1,440 ℃ to 1,660 ℃, 1,450 ℃ to 1,650 ℃, 1,460 ℃ to 1,640 ℃, 1,470 ℃ to 1,630 ℃, 1,480 ℃ to 1,620 ℃, 1,490 ℃ to 1,610 ℃, 1,500 ℃ to 1,600 ℃, 1,510 ℃ to 1,590 ℃, 1,520 ℃ to 1,580 ℃, It may be 1,530 ℃ or more and 1,570 ℃ or less, or 1,540 ℃ or more and 1,560 ℃ or less. By controlling the melting temperature of the step of melting the composition within the above-described range, the viscosity of the molten composition can be controlled, thereby improving the workability of the process of manufacturing the plasma-resistant glass.
[0088] One embodiment of the present invention provides a method for manufacturing a chamber-internal component for a semiconductor manufacturing process, comprising the steps of: melting the plasma-resistant glass; injecting the molten plasma-resistant glass into a mold (S21); and annealing the injected plasma-resistant glass (S23).
[0089] A method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process according to one embodiment of the present invention can manufacture components having various shapes, prevent damage due to thermal shock in a high-temperature atmosphere, and easily manufacture components.
[0090] FIG. 2 is a flowchart illustrating a method for manufacturing internal components for a chamber for a semiconductor manufacturing process according to an embodiment of the present invention. Referring to FIG. 2, a method for manufacturing internal components for a chamber for a semiconductor manufacturing process according to an embodiment of the present invention will be described in detail.
[0091] According to one embodiment of the present invention, the method for manufacturing a chamber-internal component for the semiconductor manufacturing process includes a step of melting the plasma-resistant glass (S21). By including the step of melting the plasma-resistant glass as described above, the workability of the process for manufacturing the chamber-internal component for the semiconductor manufacturing process is improved, and at the same time, by injecting the molten plasma-resistant glass into a mold, the component can be formed into various shapes.
[0092] According to one embodiment of the present invention, the method for manufacturing a component for use inside a chamber for the semiconductor manufacturing process includes a step (S23) of injecting the molten plasma-resistant glass into a mold. As described above, by injecting the molten plasma-resistant glass into a mold, components of various shapes can be manufactured.
[0093] According to one embodiment of the present invention, the mold may have any one shape among a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electrostatic chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame. By implementing the shape of the mold in various ways as described above, the shape of the part can be easily implemented, thereby reducing the manufacturing time.
[0094] According to one embodiment of the present invention, the method for manufacturing a component for use inside a chamber for the semiconductor manufacturing process includes a step (S25) of annealing the injected plasma-resistant glass. By including the step of annealing the injected plasma-resistant glass as described above, the stress caused by heat generated in the component manufactured by injection into the mold is minimized, thereby improving the durability of the component and minimizing thermal shock at high temperatures.
[0095] According to one embodiment of the present invention, the melting temperature of the step of melting the plasma-resistant glass may be 1,400°C or more and 1,700°C or less. Specifically, the melting temperature of the step of melting the plasma-resistant glass may be 1,400°C or more and 1,700°C or less. In the present specification, the melting point may mean the melting temperature. Specifically, the above plasma-resistant glass has a melting point of 1,410 ℃ to 1,690 ℃, 1,420 ℃ to 1,680 ℃, 1,430 ℃ to 1,670 ℃, 1,440 ℃ to 1,660 ℃, 1,450 ℃ to 1,650 ℃, 1,460 ℃ to 1,640 ℃, 1,470 ℃ to 1,630 ℃, 1,480 ℃ to 1,620 ℃, 1,490 ℃ to 1,610 ℃, 1,500 ℃ to 1,600 ℃, 1,510 ℃ to 1,590 ℃, 1,520 ℃ to 1,580 ℃, It may be 1,530 ℃ or more and 1,570 ℃ or less, or 1,540 ℃ or more and 1,560 ℃ or less. By controlling the melting temperature in the step of melting the plasma-resistant glass within the above-described range, the viscosity of the molten plasma-resistant glass can be controlled, thereby improving workability.
[0096] According to one embodiment of the present invention, the temperature of the annealing step may be 400°C or more and 900°C or less. Specifically, the temperature of the annealing step is 430°C or more and 890°C or less, 450°C or more and 880°C or less, 470°C or more and 870°C or less, 500°C or more and 860°C or less, 550°C or more and 850°C or less, 560°C or more and 840°C or less, 570°C or more and 830°C or less, 580°C or more and 820°C or less, 590°C or more and 810°C or less, 600°C or more and 800°C or less, 610°C or more and 790°C or less, 620°C or more and 780°C or less, 630°C or more and 770°C or less, 640°C or more and 760°C or less, 650°C or more and 750°C or less, 660°C or more It may be 740°C or less, 670°C or more and 730°C or less, 680°C or more and 720°C or less, or 690°C or more and 710°C or less. By controlling the temperature of the annealing step within the above-described range, the heat-induced stress formed within the components inside the chamber for the semiconductor manufacturing process can be reduced, and the thermal shock at high temperatures can be minimized, thereby improving the durability of the components.
[0097] According to one embodiment of the present invention, the method may include a step (S27) of processing a precursor for a chamber-internal component for a semiconductor manufacturing process manufactured using the annealed plasma-resistant glass. By processing the precursor for a chamber-internal component for the semiconductor manufacturing process as described above, precise components can be manufactured.
[0098] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0099] <Examples and Comparative Examples>
[0100] A composition was prepared by mixing the ingredients and contents shown in Table 1 below. The composition was then heated to 1,650°C for 4 hours to melt it, and then cooled to room temperature to prepare a plasma-resistant glass.
[0101] <Reference example>
[0102] Quartz was prepared.
[0103] Ingredients Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 SiO2 (unit: weight%) 65656055556555 Al2O3 (unit: weight%) 1015152510155 MgO (unit: weight%) 151012613155 MgF2 (unit: weight%) 5552255 GeO2 (unit: weight%) 5581220-30
[0104] <Experimental Example 1: Dielectric Constant Measurement>
[0105] For the above examples, comparative examples, and reference examples, dielectric constants were measured using an LCR meter (Keysight E4990A Impedence Analyzer) using the capacitance method in the frequency range of 20 Hz to 100 Hz, and the results are summarized in Table 2 below.
[0106] <Experimental Example 2: Etching Rate Measurement>
[0107] For the above examples, the comparative examples and some of the reference examples, etching was performed with a mixed plasma of fluorine and argon (Ar), and the etching step difference, which is the step difference between the etched part and the non-etched part, was measured using a confocal laser microscope (Olympus OLS 5100 equipment, x 400 magnification), and the etching rate was calculated by dividing it by the measured time, which is summarized in Table 2 below.
[0108] Type Reference Example Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Dielectric constant (unit: / 1MHz) 4.377.317.136.526.386.27.49 - Etch rate (unit: nm / m) 251494455356036 -
[0109] FIG. 3 is a photograph of plasma-resistant glass according to Example 1 according to an embodiment of the present invention. FIG. 4 is a photograph of plasma-resistant glass according to Example 2 according to an embodiment of the present invention. FIG. 5 is a photograph of plasma-resistant glass according to Example 3 according to an embodiment of the present invention. FIG. 6 is a photograph of plasma-resistant glass according to Example 4 according to an embodiment of the present invention. FIG. 7 is a photograph of plasma-resistant glass according to Example 5 according to an embodiment of the present invention.
[0110] Referring to Table 2 and Figures 3 to 7 above, it was confirmed that Examples 1 to 5 were all vitrified by including Si-based oxides, Al-based oxides, Mg-based oxides, Mg-based halides, and Ge-based oxides within specific ranges, and that a dielectric constant of 6.0 or more and 7.4 or less could be implemented while an etching rate of 100 nm / m or less could be implemented.
[0111] Fig. 8 is a photograph of the plasma-resistant glass of Comparative Example 1. Fig. 9 is a photograph of the plasma-resistant glass of Comparative Example 2.
[0112] Referring to Table 2 above and Figures 8 and 9, it was confirmed that the reference quartz had a low dielectric constant and a high etching rate. In addition, it was confirmed that Comparative Example 1 was implemented with a low etching rate but a high dielectric constant. Furthermore, Comparative Example 2 was not vitrified, so the etching rate and dielectric constant were not measured.
[0113] Although the present invention has been described above through limited embodiments, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. Plasma-resistant glass containing Si-based oxides, Al-based oxides, Mg-based oxides, Mg-based halides, and Ge-based oxides.
2. In claim 1, The content of the above Si-based oxide is 20 wt% or more and 70 wt% or less, The content of the above Al-based oxide is 5 wt% or more and 30 wt% or less, The content of the above Mg-based oxide is 5 wt% or more and 50 wt% or less, The content of the above Mg-based halide is 0.01 wt% or more and 10 wt% or less, Plasma-resistant glass having a content of the above Ge-based oxide of 0.01 wt% or more and 25 wt% or less.
3. In claim 1, Plasma-resistant glass with a light transmittance of 80% or more and 100% or less.
4. In claim 1, Plasma-resistant glass with a Vickers hardness of 550 HV or more and 1,000 HV or less.
5. In claim 1, Plasma-resistant glass with a glass transition temperature of 600°C or higher and 850°C or lower.
6. In claim 1, The coefficient of thermal expansion is 4.0×10 -6 m / (m℃) or more than 6.0×10 -6 Plasma-resistant glass with a temperature of m / (m℃) or less.
7. In claim 1, Plasma-resistant glass having an etching rate of more than 0 nm / min and less than 100 nm / m by a mixed plasma of fluorine and argon (Ar).
8. In claim 1, Plasma-resistant glass with a melting point of 1,400°C or higher and 1,700°C or lower.
9. A component for use inside a chamber for a semiconductor manufacturing process, the component being made of the plasma-resistant glass of any one of claims 1 to 8.
10. In claim 9, The internal components are any one of a focus ring, an edge ring, a cover ring, a ring shower, an insulator, an EPD window, an electrode, a view port, an inner shutter, an electro static chuck, a heater, a chamber liner, a shower head, a CVD (Chemical Vapor Deposition) boat, a wall liner, a shield, a cold pad, a source head, an outer liner, a deposition shield, an upper liner, an exhaust plate, and a mask frame, and are internal components of a chamber for a semiconductor manufacturing process. A method for manufacturing plasma-resistant glass, comprising: a step of melting a composition comprising 11.20 wt% or more and 70 wt% or less of Si-based oxide, 5 wt% or more and 30 wt% or less of Al-based oxide, 5 wt% or more and 50 wt% or less of Mg-based oxide, 0.01 wt% or more and 10 wt% or less of Mg-based halide, and 0.01 wt% or more and 50 wt% or less of Ge-based oxide; and a step of cooling the molten composition.
12. In claim 11, A method for manufacturing plasma-resistant glass, wherein the melting temperature of the step of melting the above composition is 1,400°C or more and 1,700°C or less.
13. A method for manufacturing a chamber-internal component for a semiconductor manufacturing process, comprising the steps of: melting the plasma-resistant glass of any one of claims 1 to 9; injecting the molten plasma-resistant glass into a mold; and annealing the injected plasma-resistant glass.
14. In claim 13, A method for manufacturing a chamber internal component for a semiconductor manufacturing process, wherein the melting temperature of the step of melting the above plasma-resistant glass is 1,400°C or more and 1,700°C or less.
15. In claim 13, A method for manufacturing a component for use inside a chamber for a semiconductor manufacturing process, wherein the temperature of the above annealing step is 400°C or more and 900°C or less.
Citation Information
Patent Citations
Methods of making alumina-silica glasses orglass-ceramics
KR1020060093326A
Glass composition and paste composition suitable for a plasma display panel, and plasma display panel
US20050242725A1
Glass compositions useful for RIE structuring
US20080179294A1
Methods making alumina-silica glasses and ceramics
WO2004071976A1