Method for reducing cracking during continuous casting of aluminium alloyed steel

WO2024115602A9PCT designated stage expired Publication Date: 2024-10-31TATA STEEL IJMUIDEN BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2023/083608
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-04
Filing Date
2023-11-29
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Continuous casting of aluminum alloyed steels often results in transverse cracking due to the formation of aluminum nitrides at grain boundaries, which increases cracking susceptibility and affects the surface quality and impact toughness of the final product, particularly in peritectic steels with high aluminum content.

Method used

The method involves producing a steel melt with specific composition ranges and adding titanium to bind free nitrogen, preventing the formation of aluminum nitrides while controlling other alloying elements to optimize ferrite grain size and microstructure, thereby reducing transverse cracking during casting.

Benefits of technology

This approach effectively reduces transverse cracking, enhances surface quality, and improves impact toughness by preventing aluminum nitride formation and optimizing grain structure, leading to higher quality aluminum alloyed steel products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

This invention relates to a method for reducing transverse cracking during casting of aluminium alloyed steels and to steels produced in accordance with said method.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR REDUCING CRACKING DURING CONTINUOUS CASTING OF ALUMINIUM

[0002] ALLOYED STEEL

[0003] Field of the invention

[0004] This invention relates to a method for reducing transverse cracking during continuous casting of aluminium alloyed steels and to said steels.

[0005] Background of the invention

[0006] The quality of finished steel products is sometimes impaired by the presence of 'surface' defects such as slivers or cracks, by the presence of 'internal' defects such as cracks, porosity or segregation. Defects in finished steel products may arise from poor steel quality, e.g. high non-metallic inclusion content, at steel making stages or may be caused during subsequent downstream operations such as casting, reheating, hot / cold rolling or drawing. Such defects may remain undetected in intermediate processing stages and ultimately show up in the finished product during final inspection.

[0007] Continuous casting, also called strand casting, is the process where molten metal is solidified into a "semifinished" billet, bloom or slab for subsequent rolling in the finishing mills. Molten metal is tapped into the ladle from furnaces. The ladle is transported to the top of the casting machine. From the ladle, the hot metal is transferred via a pipe to a holding bath called a tundish. The tundish allows a reservoir of metal to feed the casting machine while ladles are switched, thus acting as a buffer of hot steel, as well as smoothing out flow, regulating steel feed. Molten steel is drained from the tundish through another pipe into the top of an open-base copper mould. The mould is water-cooled to solidify the hot metal directly in contact with it; this is the primary cooling process. It also oscillates vertically to prevent the metal sticking to the mould walls.

[0008] The castability of high-quality steel depends on avoiding breakouts, cracks, and surface quality problems. The surface quality of steel products is mainly determined by the early stages of solidification in the meniscus region of the casting mould. Steels which undergo the peritectic transition are the most difficult to cast. This is attributed to the volume contraction (shrinkage) associated with the peritectic phase transformation. This shrinkage leads to the formation of an air gap between the steel shell and the mould during the continuous casting process and decreases the heat flux. This leads to locally thinner and hotter regions of the solidified shell, which causes uneven shell growth that may lead to surface depressions, deep oscillation marks, cracks, and breakouts. Steels within the peritectic composition range include High- Strength Low-Alloy (HSLA) Steels, and recently Advanced High-Strength Steels (AHSS), which are all used extensively in different products due to their excellent mechanical properties, which include high strength and toughness. The automotive industry is increasingly utilizing steels with the peritectic composition range (AHSS, HSLA, etc.) to reduce vehicle weight. Peritectic steels are also widely applied in pipelines, navy vessels, and nuclear power plant components. Therefore, there is a great demand to produce these steels without defects.

[0009] Peritectic steel solidification occurs in two distinct stages involving liquid (L), dendritic delta-ferrite (d), and austenite (c): the peritectic reaction (L + d c) followed by the peritectic transformation (d - c). The peritectic reaction occurs just below the peritectic temperature, when liquid and delta-ferrite are in contact and react to form austenite. This corresponds to the L + d + c three-phase point in the binary phase diagram or to the 3-phase region on sections through a multicomponent phase diagram.

[0010] During the peritectic reaction, an austenite layer grows along the L -i-d interface. After the liquid locally runs out, then the remaining delta-ferrite transforms to austenite by solid-state transformation. The peritectic transformation starts by thickening of the austenite layer immediately behind the tip of this advancing c-platelet where it proceeds on two fronts, growing into both the liquid on one side of the c-platelet and the d interior on the other. Later, toward the centre of the dendrite, the interior d-c interface has moved far away from the liquid, so further austenite growth into the delta-ferrite involves only a single moving interface. Note that spatially, these different steps of peritectic solidification occur at different places, and proceed in different directions relative to the thermal gradient.

[0011] Understanding peritectic solidification in steels is of great practical importance, because peritectic solidification causes many different problems during commercial casting processes such as continuous casting. These problems include the formation of deep oscillation marks, surface depressions, and interfacial gaps in the mould that lead to lower heat flux, thinner, and non-uniform (rippled) solidified shell thickness and accompanying catastrophic breakouts, increased susceptibility to surface crack formation and accompanying oxide slivers, larger austenite grain size leading to lower hot ductility, and consequently more defects in the final product, including internal cracks and accompanying macro-segregation.

[0012] The known production of hot-rolled steel strips starts with the production of liquid steel, e.g. in a BOS-plant or an EAF-plant or the like. The liquid steel is brought to a continuous caster in a ladle. In the caster, the still liquid steel passes through a mould and then through a sequence of 'segments', during which its vertical path out of the ladle and the mould gradually becomes horizontal, as it cools. It then emerges as a continuous and solid slab of steel. The continuous slab is then cut to length into semifinished products known as slabs. The thickness of these slabs may be 'thick' (between 150 and 350 mm) or 'thin' (between 50 and 150 mm). These slabs are further processed in a hot strip mill and processed into hot rolled strip. These hot strips can be used as such or be further processed into cold rolled strip in a cold strip mill.

[0013] Slivers have been found incidentally in some hot rolled slabs being cast with reduced casting speed, particularly at the end of a casting sequence. From the slivers analysis it does not seem to have any entrapped slag, oxide or mould powder and the cause of these slivers is unknown. A constant casting speed appears to reduce or eliminate the occurrence of said slivers. From a process point of view the reduction of the casting speed leads to a reduction in the water sprayed at the secondary cooling; however below a certain casting speed the amount of water will not be reduced any further and will remain constant, where relatively the cooling will be more intense at the lowest casting speed range.

[0014] For particular types of AHSS the addition of aluminium is one of the important measures taken to achieve the favourable mechanical properties. However, the addition of aluminium also tends to increase the occurrence of aluminium-based slivers which is potentially detrimental to the mechanical properties in general and to the impact toughness values in particular, but also may lead to poor surface quality.

[0015] Objects of the invention

[0016] It is an object of the invention to provide a method of producing an aluminium based AHSS product with a reduced amount of aluminium based slivers.

[0017] It is also an object to provide an aluminium based AHSS product with improved surface quality.

[0018] It is also an object of the invention to provide a method of producing an aluminium based AHSS product with improved impact toughness values.

[0019] It is also an object of the invention to provide an aluminium based AHSS product with a reduced amount of aluminium based slivers.

[0020] It is also an object of the invention to provide an aluminium based AHSS product with improved impact toughness values.

[0021] Description of the invention

[0022] One or more of the objects is reached with a method for reducing transverse cracking during casting of aluminium alloyed steels by a) producing a steel melt comprising (in wt.%): o C: 0.050-0.140; o Mn: 1.00-3.50 ; o Si: 0.010-1.80; o Al: 0.150-1.00; o Ti: 0.001 - 0.100; o P: at most 0.050; o S: at most 0.020; o N: at most 0.010; o Nb: at most 0.010; o V: at most 0.010; o Mo: at most 0.015; o Cr: at most 1.000; o Cu: at most 0.060; o Ni: at most 0.060; o Ca: at most 0.0050; o Sn: at most 0.050; o Rare earth elements (REM): at most 0.0030; o the balance being Fe and inevitable impurities resulting from the ironmaking and steelmaking process; b) adding Ti (=Ti_added) in relation to the N_free content wherein o Ti_excess = (([Ti_added] / 3.4176) - N_free), and o wherein Ti_excess > 0, and o wherein Ti_excess / Ti_added is at most 0.20 and wherein Ti_added: 0.001 - 0.100 wt.%. c) continuously casting the thusly produced melt in a continuous caster to produce a thick slab, a thin slab or a strip.

[0023] The AHSS steel grade in the context of this invention is a grade where aluminium is added as an alloying element, thus the aluminium content in the steel alloy is significantly higher than usual for, e.g. HSLA grades or structural steels, where the aluminium content is usually less than about 0.05 wt.%. Further, other micro-alloy elements such as Nb and V may be included in the compositional recipe but these are optional. Consequently, since nitrogen is inevitably present in the alloy, aluminium nitrides (AIN) will be formed because AIN forms in preference to most of the other nitrides (except forTiN and BN). Apart from the effect of Al as a nitride forming element, Al in solid solution affects the ferrite grain size and ferrite grain size distribution in the as-rolled structure. Higher Al content leads to an enlarged grain size because Al is a ferrite former and thus promotes the formation of ferrite and delays the formation of austenite, giving the time (and thus kinetics) to the ferrite grains to form and grow. Some precipitates may refine the structure as these appear on grain boundaries and thus stops / reduces the grain growth, but the AIN precipitation as it occurs at the boundaries of the already enlarged grains, it has the opposite effect, being more detrimental by increasing cracking susceptibility during casting, rather than refining the structure. On the other hand the challenge posed by the presence of the Al during the casting stage is two-fold. Firstly it is believed that the Al addition significantly accelerates the growth of ferrite grains. The larger the ferrite grain, the higher the transverse cracking susceptibility. Excessive grain growth, especially at the roots of oscillation marks, has been implicated as a possible cause of reduced ductility during unbending of continuously cast slabs. The detrimental effect of the large ferrite grain size is most severe in alloys of near-peritectic composition that are already more sensitive to uneven shrinkage. Secondly the remaining Al will segregate and precipitate as AIN at the large grain boundaries. These precipitates form long trails of precipitates and contribute to the cracking susceptibility by means of the cracking mechanism that resembles the ripping off a post stamp through the perforated line.

[0024] Moreover, Al is known to cause cracking problems, particularly in peritectic steels due to AIN precipitation at the grain boundaries. The above-referenced oscillation mark act as a stress concentrator (notch effect) and also result in different local cooling conditions due to the deepness and gap formation (between steel and the mould). It will not only concentrate stresses but also locally causes thermal shrinkages.

[0025] The invention is based on a study by the inventor(s) that the stoichiometric addition of titanium to nitrogen to a steel melt results in the binding of all free nitrogen (N_free) to titanium and thereby in the formation of precipitates of Ti and N. This means that ideally no nitrogen should be available for the formation of aluminium-nitride (AIN) in the steel during solidification. The standard enthalpy of formation (Enthalpy of formation, AHf (kJ / mol), at 298 K) for TiN is -337 and for AIN is -318.0 kJ / mol. The nitrogen binds preferentially to Ti leaving no nitrogen available to bind to Al. On the other hand, it is also important to limit the amount of Ti to prevent the formation of TiC. The Enthalpy of formation for TiC is significantly higher (- 184 kJ / mol) than for TiN, but the excess Ti will inevitably bind to C. TiC adversely affects the impact toughness values of the final product. B is an element that, when in solid solution, significantly increases the hardness of the steel. Depending on the type of steel and carbon content, the amount of boron can be as little as 3 ppm to make a difference. It is therefore essential that the amount of free nitrogen is determined as accurately as possible to ensure sufficient addition of Ti while preventing overdosing with Ti.

[0026] The invention is also embodied in certain preferred ranges. These preferred ranges can be selected independent of each other as the inventors found that their effects on the mechanical properties are additive and not particularly synergistic.

[0027] Carbon (C) is a necessary and inexpensive element in the steel according to the invention for strength and hardenability and enables the formation of martensite and ferritic bainite or bainite. The strength of the steel, the amount of the martensite increase as the carbon content is increased. For the steels according to the invention the carbon content is from 0.050 to 0.140 wt.%. Carbon content lower than 0.050 wt.% makes it difficult to ensure the required strength. Preferably carbon is at least 0.060 wt.%. Carbon content exceeding 0.140 wt.% will impair the formability and the toughness of the steel. C is preferably between 0.065 wt.% and 0.115 wt.%.

[0028] Silicon (Si) and Aluminium (Al) are compulsory alloying elements in the steel. Si has the main function to prevent carbon from precipitating in the form of iron carbides, most commonly cementite and to suppress decomposition of retained austenite. Si is a ferrite stabilizer and is known to be quite effective for the retention of austenite during cooling after hot rolling. Silicon may be added between 0.010 and 1.80 wt.%. If silicon is added to suppress the carbide formation then a minimal amount of 0.80 wt.% Si is needed to effectively suppress the carbide formation. Addition of Si in excess of 1.80 wt.% is undesirable, as it deteriorates the formability. However, if the carbide formation does not need to be suppressed but if the intended application is for surface critical applications, such as visible parts of an outer-part of an automobile, then the preferred maximum value of Si is at most 0.20 wt.%, more preferably at most 0.15 wt.% or at most 0.10 wt.% to prevent the formation of a difficult to remove scale during hot-rolling. A suitable minimum Si value is 0.020 wt.%.

[0029] Al is controlled to a value between 0.150 to 1.00 wt.%. A primary function of Al is to deoxidise the liquid steel before casting. The lower amount of Al is ample for this function. In addition, Al has a similar function as Si to prevent the formation of carbides and to stabilize the retained austenite, although Al is not as effective as Si and has no significant effect on strengthening. Too high levels of Al increase the ferrite to austenite transformation temperature Ar3 and therefore facilitate the formation of pro-eutectoid ferrite during cooling after hot rolling. In addition, the risk of cracking during casting increases as the Al content is increased. Therefore, the upper limit is set to 1.00 wt.%. Preferably Al is between 0.200 and 0.500 wt.%, and more preferably between 0.250 to 0.400 wt.%.

[0030] Manganese (Mn) is an austenite former and an important strengthening element. It is required to obtain hardenability of the steel. Mn is also added to balance the elevated phase transformation point as a result of high amounts of Si and Al. In order to obtain sufficient hardenability, Mn should be 1.00 wt.% or more. A Mn content in excess of 3.50 wt.% will result in a decrease in the Ms point of the steel, resulting in difficulties during continuous annealing of the rolled steel product. In addition, a large amount of Mn promotes macro-segregation during casting, which results in unfavourable band structure formation, which is detrimental to ductility and formability. Therefore, the Mn content is limited to 3.50 wt.%, preferably to 3.00 wt.%. A suitable Mn range was found to be from 1.50 to 2.50 wt.%, preferably from 1.70 to 2.50 wt.% and more preferably from 1.70 to 2.25 wt.%. Chromium (Cr) can be added as alloying element in the steel, which promotes the strength of the steel by increasing the hardenability and retards the formation of carbides. Chromium is also quite expensive, and when Cr is added excessively, the effect is saturated. The upper limit is therefore 1.00 wt.%. To benefit from the contribution of Cr a suitable minimum addition is 0.100 wt.% and preferably between 0.200 and 0.800 wt.%, more preferably between 0.450 and 0.700 wt.%.

[0031] The amount of Niobium (Nb) and / or Vanadium (V), when added, is preferably limited to 0.010 wt.%. Their addition may result in too much carbo-nitrides precipitation which results in a deterioration of the formability of the steel. Preferably Nb and / or V are not added and only present, if any, as residual elements.

[0032] The composition optionally contains one or two elements selected from Ca and a rare earth metal (REM), in an amount consistent with a treatment for MnS inclusion control. Examples of the rare earth element include scandium, yttrium, and lanthanide. It is recommended that for these elements to be useful they have to be present in amounts of 0.0003 wt.% or higher. However, when added excessively, the effect is saturated and the economic efficiency is reduced. Therefore, a suitable maximum amount is 0.0050 and 0.0030 wt.% respectively.

[0033] The amount of titanium added to the melt (Ti_added) is at most 0.100 wt.%. Titanium is expensive, and therefore its addition is limited for economic reasons, and also, if the titanium content is too high TiC may be formed which is not desirable from a fracture toughness point of view. A suitable upper boundary is 0.080 wt.%, preferably at most 0.060 wt.%. The minimum amount of Ti that needs to be added is mainly governed by the requirements that Ti_excess = (([Ti_added] / 3.4176) - N_free) > 0, and Ti_excess / Ti_added is at most 0.20 and is therefore dependent on N_free. N_free in the melt is identical to the total amount of nitrogen. Ti_excess is therefore the amount of titanium added over the amount that is needed to bind all the free nitrogen, i.e. ([Ti_added] / 3.4176) - N_free. If T_excess > 0, then there is no free nitrogen in the steel after solidification. If T_excess < 0, then there is still free nitrogen around that can bind to aluminium, which in this case is undesired. So the allowable amount of Ti_added is between 0.001 and 0.100 wt%, but the amount of titanium that is to be added is chosen in relation to the total nitrogen (=N_free in the melt) content in accordance with the requirements as outlined above.

[0034] It is preferable to limit (Ti_excess / Ti_added) to at most 0.17, preferably to at most 0.15 and more preferably to at most 0.12 or even 0.10 or even to at most 0.05 to reduce the risk of TiC formation and to reduce the adverse impact thereof on the impact toughness values of the final product.

[0035] Prior to casting all elements are mixed in the liquid steel, including nitrogen. .The free nitrogen (N_free) content is, prior to casting, the same as the total nitrogen (N) content in the melt. After solidification and cooling of the slab the amount of free nitrogen is normally smaller than the total nitrogen content because some or all of the nitrogen is present as a metal-nitride. Prior to casting and alloying, all nitrogen is free nitrogen. By adding titanium to the melt prior to casting TiN will be the first compound to be formed due to the thermodynamic stability of TiN. The amount of titanium to be added is determined on the basis of the total nitrogen content in the melt. By adding excess titanium all nitrogen (N) will be bound to TiN, and in that case the free nitrogen content of the solidified steel slab is then 0.

[0036] The measurement of N_free can be done at-line, on-line or in-line (see figure 3). With an in-line measurement of N_free, measurements are taken directly in the manufacturing process of the steel slab. In-line process analytics usually takes place continuously, i.e. as long as the production process is running, automatic measurements are made repeatedly or continuously. The advantage of in-line measurement is that it measures what is momentarily taking place in the process.

[0037] An on-line measurement is usually also performed repeatedly or continuously. Here, however, measurements are not made directly in the process, but rather in a built-in branch (or "bypass") into which samples of the steel to be measured are automatically fed. This is done, for example, when the measuring device cannot withstand the harsh conditions that are encountered directly near the process. Such online measurements no longer measure exactly what takes place in the process at that moment. There is a (limited) time lag and the material to be measured may behave a little differently than under the time pressures existing directly in the process. On-line measurements also enable measurement methods that would not be possible as an inline variant, for example if the molten metal needs to be solidified before performing the measurement.

[0038] Sometimes an on-line measurement is difficult to implement economically or simply is not technically possible. Then a sample has to be taken and measured elsewhere. If this measuring location is still close to production, for example if the lab is in the adjoining room, this is called an at-line measurement. At-line measurements enable the implementation of more complex measurement processes: Samples can be prepared in practically any way, and there is sufficient time for the measurement process to take place. This precision is bought at the price of an increased time lag between the sampling and the availability of the measurement result.

[0039] Lastly, if the production site does not have the capacity for the necessary measurements, the sample must be sent to an external laboratory: an offline measurement takes place. This measurement variant is thus largely decoupled from the production process and useless for direct process control. Preferably the measurement of free nitrogen is performed in-line. Preferably the Ti_excess is as small as possible, preferably therefore at most 0.004 wt.%, more preferably at most 0.003 wt.%, even more preferably at most 0.002 wt.% and most preferably at most 0.001 wt.%. By limiting the Ti_excess the adverse effects of the Ti_excess are minimized.

[0040] Phosphorus (P) is an impurity element in steels. P segregates the grain boundaries and therefore decreases the workability and deteriorate impact resistance. Therefore, the amount of P should be suppressed to 0.050 wt.% or less. For the properties of the steel, the content of P is preferably minimized as far as possible. In an embodiment P is at most 0.020 wt.% , preferably at most 0.010 wt.%. For production cost, the lower limit of the P content in steel is preferably around 0.005 wt.% because decreasing P below 0.005 significantly increases production costs.

[0041] Sulphur (S) is a harmful impurity in the steel which forms sulphide-based inclusions such as MnS, which may serve as a crack initiator, thereby deteriorating processability, impact resistance and formability of the steel. Therefore, it is desirable to reduce the amount of S as much as possible. Accordingly, S is 0.020 or less. In an embodiment S is at most 0.010 wt.%, preferably at most 0.005 wt.%.

[0042] In an embodiment Ni and / or Cu is not present as an alloying element, but only as inevitable impurity and more preferably completely absent.

[0043] Residual elements (aka inevitable impurities, such as Cu, Ni, As, Pb, Sn, Mo, etc.) are defined as elements which are not added on purpose to steel and which cannot be removed by simple metallurgical processes. Residual elements enter steel from impurities in ore, coke, flux and scrap; from these, scrap is considered to be the main source of residuals. Consequently, the level of residual elements in an Electric Arc Furnace process route (100% scrap based) is significantly higher than in the Basic Oxygen Steelmaking (BOS) process route. The most commonly found residuals are Cu, Ni, Cr, Mo, and Sn. The acceptance limits of these residuals depend mainly on product requirements. Preferably the steel according to the invention is produced in a BOS- process route, in which case the allowable levels of residual elements for Cu, Ni, Mo and Sn are 0.060, 0.060, 0.020 and 0.025 wt.%, respectively.

[0044] In an embodiment the slab or strip is hot-rolled to produce a hot-rolled strip. The hot-rolled strip typically has a thickness between 1.5 and 8 mm, preferably between 2 and 5 mm.

[0045] Preferably the hot-rolled strip is subsequently pickled, cold-rolled, recrystallisation annealed, preferably continuously annealed, and, optionally, provided with a metallic coating e.g. by hot dip galvanising. The cold-rolling reduction is typically between 40% and 80%, preferably between 45% and 75%, even more preferably at most 70%. A careful balance between rolling forces during cold rolling and the development of the optimal combination of crystallographic texture, surface texture and microstructure must be struck to obtain the desired properties after annealing and the optional metallic coating step.

[0046] The metallic coating layer deposited onto the strip in the hot-dip galvanising is preferably a zinc coating layer or a zinc alloy coating layer. Preferably the zinc alloy coating layer contains one or more alloying elements selected from the group consisting of Mg, Al, and each with a content of at least 0.3 wt.% and at most 10 wt.%, and optionally one or more additional elements selected from the group consisting of Ni, Si, Sb, Pb, Ti, Ca, Mn, Sn, La, Ce, Cr, or Bi, wherein the content by weight of each additional element in the zinc alloy coating is less than 0.3 weight %, inevitable impurities, the remainder being zinc. Preferably the zinc alloy coating layer comprises 0.2 - 5 wt.% Al and 0.3 - 5 wt.% Mg. More preferably the zinc alloy coating layer comprises 0.2 to 1.4 wt.% of Al. More preferably the Al content of the zinc-alloy layer is at 0.5 - 1.1 wt.%, more preferably 0.55 - 1.0, even more preferably 0.60-0.90 wt.%.

[0047] According to a second aspect the invention is also embodied in a hot-rolled steel strip, optionally cold-rolled and recrystallisation annealed, and optionally hot-dip galvanised strip having a composition comprising (in wt.%): o C: 0.050-0.140; o Mn: 1.00-3.50 ; o Si: 0.010-1.80; o Al: 0.150-1.00; o Ti: 0.001-0.100; o P: at most 0.050; o S: at most 0.020; o N: at most 0.010; o Nb: at most 0.010; o V: at most 0.010; o Mo: at most 0.020; o Cr: at most 1.000; o Cu: at most 0.060; o Ni: at most 0.060; o Sn: at most 0.050; o Ca: at most 0.0050; o Rare earth elements (REM): at most 0.0030; o the balance being Fe and inevitable impurities resulting from the ironmaking and steelmaking process; b) adding Ti (=Ti_added) wherein o Ti_excess = (([Ti_added] / 3.4176) - N_free), and o wherein Ti_excess > 0, and

[0048] 0 wherein Ti_excess / Ti_added is at most 0.20, and

[0049] 0 wherein Ti_added: 0.001 - 0.100 wt.%.

[0050] Examples

[0051] As substrates the materials according to table 1 were used.

[0052] Table 1. Alloy compositions considered in this study (in 1 / 1000 wt.% unless otherwise indicated).

[0053] From thermodynamic calculations (Thermo-Calc version 2017a), the precipitates appearing during solidification and further cooling until 500°C are listed in table 2. The free nitrogen content is, prior to casting, the same as the total nitrogen content. The total nitrogen content is determined using an Eltra type ON-900 and ONH-2000. A steel sample is introduced into a graphite crucible and melted. The nitrogen subsequently escapes from the melt and the amount of nitrogen is measured. On the basis of this measurement the amount of titanium needed to bind the nitrogen to TiN is determined and added to the steel melt prior to casting.

[0054] Table 2. Phases appearing in the calculations (amounts of TiN and AIN are in mol volume fractions) This table 2 shows the start temperature of precipitation of TiN and AIN, indicating that TiN forms at higher temperatures than AIN as expected. It also shows the amount of both TiN and AIN formed at 750°C.

[0055] The comparison between alloys 1 and 3, where at the same low level of N, and same Al content, shows that when there is more Ti present in the alloy, there will be a preference to form TiN and not AIN. Even at 750°C AIN has not formed yet in the alloy 3 as it starts to precipitate only at 711°C. Moreover, the temperature at where TiN starts to form is 90 °C higher in alloy 3 than in alloy 1. The same effect can be seen in the comparison between alloys 1 and 4; however here the amount of AIN at 750°C is low and the temperature of AIN precipitation is higher than that in alloy 3.

[0056] When comparing alloys 2 and 5, where the maximum level of N in both cases is slightly different by 10 ppm, the temperature of AIN formation is 200 °C higher and the amount of AIN phase at 750°C is about 40% higher in alloy 2. Nevertheless, the difference in temperature of TiN transformation and the amount of TiN-phase present at 750°C are both similar in both cases. The results of steels 3,4 and 6 are comparable.

[0057] The amount of alloying elements does have an effect in these all cases on the precipitate formation at a temperature range that is expected in the secondary cooling region of the caster. Adding more Ti in the alloy does have a significant effect in the TiN and AIN formation, not only the amount of phase formed at 750°C, but also the temperature at which it starts to precipitate are considerably different. The amount of Al present in the alloy does influence the AIN formation but it does not influence the TiN formation Considering that the N does also have an effect in the TiN and AIN precipitation, it is preferable to keep the N levels as low as possible to avoid cracking in case the steel has to be cast at lower casting speed.

[0058] An additional advantage of the aluminium alloyed steels according to the invention is that the impact toughness is higher than with the steels in the art. The impact toughness is strongly related to the grainsize of the steel. According to the Mintz equation ("Effect of TiN Particles and Grain Size on the Charpy Impact Transition Temperature in Steels", Du et al, J. Mater. Sci. Technol., 2012, 28(10), 878-888), reliable predictions of the ductile-brittle transition temperature (DBTT) of a steel can be made successfully for ferrite-pearlite steels using the following equation:

[0059] DBTT = 112-t0 5- 13.7-d0-5+ 15-pearlite%0 33+0.43-AY + 20 (1) which can be read as DBBT as a function of d, where t is the grain boundary carbide thickness (in pm), d is the average grain size of ferrite (in pm), % pearlite is the amount of pearlite (area percent) in the steel, AY is the precipitation-hardening component, which is calculated from the differences between the measured yield strength at room temperature (CTYS) and the non-precipitation-hardened yield strength (nnp-Ys) according to:

[0060] AY = SYS - Snp-Ys (2) and Snp-Ys can be determined from the following relationship:

[0061] Snp-Ys = 43.1-%Mn + 83-° / oSi + 15.4-d - 0.5 + 1540-%N_free + 105 (3) where N_free is the free-nitrogen content (in wt.%).

[0062] The relationship between the chemical composition and the grainsize is provided by the temperature at which the steel no longer recrystallises during hot rolling. During hot-rolling the microstructure is austenitic, and at room temperature the microstructure is predominantly ferritic with a second phase. The austenite stops recrystallising at the aptly named "non-recrystallisation temperature" (Tnr) and this value is largely determined by the chemical composition. Tnr can be calculated on the basis of the Boratto equation (Boratto, F. et al. In: THERMEC '88. Proceedings. Iron and Steel Institute of Japan, Tokyo, 1988, p. 383-390):

[0063] Tnr = 887 + 464-C + (6445. Nb - 644VNb) + (732 V - 230VV ) + 890 Ti_added + 363 AI - 357 Si (4)

[0064] The higher the value for Tnr, the less the austenitic structure recrystallises during the hot-rolling, and the more stored energy is present in the deformed nonrecrystallised austenite before the phase transformation from austenite to ferrite starts. More stored energy means a higher driving force for transformation, and thus abundant nucleation of new ferrite grains, resulting in a small grainsize. A smaller grainsize is immediately effective in reducing the DBTT. The microstructure of the hot-rolled steels according to the invention mainly consist of polygonal ferrite, pearlite and some acicular or bainitic ferrite.

[0065] Table 3: Transformation temperatures and non-recrystallisation temperatures.

[0066] The cold rolled and annealed steels comprise a mix of polygonal ferrite and a finely dispersed second phase of martensite / retained austenite, giving the steel its dual phase characteristics. Brief description of the drawings

[0067] The invention will now be further explained by means of the following, non-limiting figures.

[0068] Figure 1 shows the temperature of start precipitation from table 2.

[0069] Figure 2 shows the equilibrium phase fractions at 750 °C.

[0070] Figure 3 shows the difference between off-line, in-line, on-line and at-line measurements of N_free.

[0071] Figure 4 indicates the mechanism of the formation of the precipitates on the grain boundary, which the inventors believe to be the cause for the post-stamp- 1 ike fracture over the grain boundaries. This happens predominantly during unbending of the strands in the brittle temperature range of (depending on the steel's composition) about 700 to 900°C. The brittleness in this temperature range has been confirmed to be due to (a) hardening by the precipitation of fine AIN and / or (b) precipitation of a ferrite film along the austenite grain boundaries during y^o transformation, so that the AIN precipitates end up (in a 2D-image) as a string of particles in the ferrite film surrounding the remaining austenite (B.G. Thomas, J.K. Brimacombe and I.V. Samarasekera, "The Formation of Panel Cracks in Steel Ingots: A State-of-the-Art Review," ISS Trans., 7 (1986): 7-20.).

[0072] Figure 5 shows the occurrence of surface defects in a continuous cast slab in alloys not according to the invention. These surface defects have been detected by means of an automatic surface inspection system. Using the system typical defects such as scratches, scale and slivers can be detected automatically and stored per strip with their respective location on the strip. This enables to construct the images as in figure 5 and 6, and it allows to study the physical strips afterwards, for instance to study the causes of the occurrence of the defects.

[0073] Figure 6 shows the occurrence of surface defects in a continuous cast slab in alloys according to the invention.

[0074] Figure 7 shows the solubility products for some carbides and nitrides in austenite (B. Hutchinson, J. of Iron and Steel Res. Int., May 2011) as a function of temperature. Titanium forms an extremely stable nitride that persists as particles in the steel even close to the melting point.

Claims

CLAIMS1. Method for reducing transverse cracking during casting of aluminium alloyed steels by a) producing a steel melt comprising (in wt.%): o C: 0.050-0.140; o Mn: 1.00-3.50; o Si: 0.010-1.80; o Al: 0.150-1.00; o Ti: 0.001 - 0.100 o P: at most 0.050; o S: at most 0.020; o N: at most 0.010; o Nb: at most 0.010; o V: at most 0.010; o Mo: at most 0.020; o Cr: at most 1.000; o Cu: at most 0.060; o Ni: at most 0.060; o Sn: at most 0.050; o Ca: at most 0.0050; o Rare earth elements (REM): at most 0.0030; o the balance being Fe and inevitable impurities resulting from the ironmaking and steelmaking process; b) adding Ti (Ti_added) in relation to the N_free content and wherein o Ti_excess = (([Ti_added] / 3.4176) - N_free), and o wherein Ti_excess > 0, and o wherein Ti_excess / Ti_added is at most 0.20, and o wherein Ti_added: 0.001 - 0.100 wt.% c) continuously casting the thusly produced melt in a continuous caster to produce a thick slab, a thin slab or a strip.

2. Method according to claim 1, wherein the slab or strip is hot-rolled to produce a hot-rolled strip.

3. Method according to claim 2, wherein the hot-rolled strip is cold-rolled, continuously recrystallisation annealed and hot dip galvanised.

4. Method according to any one of claims 1 to 3, wherein Ti_excess / Ti_added is at most 0.10.

5. Method according to any one of claims 1 to 4, wherein C is between 0.065 and 0.115 wt.%6. Method according to any one of the preceding claims wherein Mn is between 1.70 and 2.50 wt.%.

7. Method according to any one of the preceding claims wherein Si is between 0.020 and 0.10 wt.%.

8. Method according to any one of the preceding claims wherein Al is between 0.200 to 1.000, and preferably between 0.200 and 0.500 wt.%.

9. Method according to any one of the preceding claims wherein Nb is not present as an alloying element, but only as inevitable impurity and preferably completely absent.

10. Method according to any one of the preceding claims wherein Ti_added is at most 0.080 wt.%.

11. Method according to any one of the preceding claims wherein Cr is between 0.100 and 1.000 wt.%, and preferably between 0.200 and 0.800 wt.%.

12. Method according to any one of the preceding claims wherein Cr is between 0.450 and 0.700 wt.%.

13. Method according to any one of the preceding claims wherein P is at most 0.020 wt.%.

14. Method according to any one of the preceding claims wherein S is at most 0.010 wt.%.

15. Hot-rolled steel strip, optionally cold-rolled and recrystallisation annealed and optionally provided with a metallic coating, the strip having a composition comprising (in wt.%): o C: 0.050-0.140; o Mn: 1.00-3.50; o Si: 0.010-1.80; o Al: 0.150-1.00; o P: at most 0.050;o Ti: 0.001 - 0.100 wt.%. o S: at most 0.020; o N: at most 0.010; o Nb: at most 0.010; o V: at most 0.010; o Mo: at most 0.020; o Cr: at most 1.000; o Cu: at most 0.060; o Ni: at most 0.060; o Sn: at most 0.050; o Ca: at most 0.0050; o Rare earth elements (REM): at most 0.0030; o the balance being Fe and inevitable impurities; wherein Ti = Ti_added and wherein (([Ti_added] / 3.4176) - N_free) > 0, and wherein Ti_excess / Ti_added is at most 0.20, and wherein Ti_added: 0.001 - 0.100 wt.%