Methods of forming colloidal copper nanoparticle-based, air-stable, conductive, multiscale features
Patent Information
- Application Number
- PCT/US2024/019181
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-08
- Filing Date
- 2024-03-08
- Publication Date
- 2024-11-07
AI Technical Summary
Current methods for forming conductive films using copper nanoparticles require high-temperature processing, which is incompatible with flexible and biodegradable substrates, and result in oxidation that reduces electrical conductivity, limiting their application in flexible electronics and IoT devices.
A method involving the exchange of labile ligands associated with copper nanoparticles for compact ligands like thiocyanate or chloride, allowing for the formation of air-stable, conductive films without high-temperature processing, using room-temperature chemical treatments to achieve closely-packed copper nanoparticle films with reduced resistivity.
The approach results in copper nanoparticle films with resistivity as low as 1.24 times that of bulk copper, maintaining air stability and enabling the use of these films in flexible and biodegradable substrates for electronic devices, particularly in RF and optical applications.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
103241.007033 / 22-9924 METHODS OF FORMING COLLOIDAL COPPER NANOPARTICLE-BASED, AIR-STABLE, CONDUCTIVE, MULTISCALE FEATURES CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] The present application claims priority to and the benefit of United States patent application no.63 / 489,012, “Methods Of Forming Colloidal Copper Nanoparticle- Based, Air-Stable, Conductive, Multiscale Features” (filed March 8, 2023). All foregoing applications are incorporated herein by reference in their entireties for any and all purposes. GOVERNMENT RIGHTS
[0002] This invention was made with government support under 1941529 awarded by the National Science Foundation. The government has certain rights in the invention. TECHNICAL FIELD
[0003] The present disclosure relates to the field of metallic nanoparticles and to the field of ligand-stabilized nanoparticles. BACKGROUND
[0004] The growing demand for flexible electronic, radio frequency (RF), and optical technologies motivates low-cost and large-area fabrication of devices and integrated components on bendable and lightweight substrates.1,2In contrast to multi- staged and high-cost traditional manufacturing, printing technologies deposit inks of functional materials to form patterned structures on various surfaces, including flexible substrates.3,4The solution-based process does not require high vacuum or high temperatures, reducing the instrumentation and operational costs.
[0005] One target at the heart of printed devices is to develop conductive inks and their corresponding printing methods. Metal nanoparticle (NP) inks are one type of conductive ink that consists of metal NPs ranging from 1-100 nm in diameter, a liquid vehicle, and additives that serve as surfactants, stabilizers, or binders.5The batch chemical103241.007033 / 22-9924 synthesis of NPs and the high metal loading of NP inks result in high conductivity and large-scale production of metal NP traces or structures, enabling their applications as electrodes, interconnects, and antennas in flexible lighting and displays, photovoltaics, electronics, electromechanical, and electrochemical sensing.6
[0006] Metal NPs, which are known for their localized surface plasmon effects, have more recently been used as building blocks to construct optical metastructures.7The precise synthetic control of NP size, shape, and composition and their post-synthesis assembly and patterning allow the design of plasmonic structures with tunable resonance frequencies.8–10
[0007] Conductive structures can be achieved by tailoring the metal NP ink materials as well as the post-deposition processing. Ag and Au NP inks have been the most well-established and commercialized systems. However, the relatively high cost of Au and additionally the lack of biocompatibility of Ag NPs restrict their usage in food and health related devices, such as biodegradable and biocompatible conductors, antennas, and sensors for emerging Internet of Things (IoT) technologies being developed to monitor health, agriculture, and the environment. On the other hand, Cu NP inks have lower material costs and are non-toxic and their films maintain high conductivity and possess similar optical properties (i.e., dielectric function) to noble metal Au and Ag NPs.11Nevertheless, post-processing either through thermal annealing (i.e., at temperatures >120 ˚C) or high intensity light irradiation is still necessary to decompose the organic additives introduced during synthesis for stabilizing the NPs in solvents and to sinter the NPs and form conductive films.11
[0008] Consequently, substrates with low thermal resistance, such as some polymers and paper, are incompatible due to the potential damage caused by these high- temperature processes. The propensity for oxidation of Cu NPs reduces their electrical conductivity and poses another challenge in exploring them as active metamaterials in optical devices. Accordingly, there is a long-felt need in the art for improved methods of processing metallic NPs, in particular copper NPs. SUMMARY
[0009] In meeting the described challenges, the present disclosure provides a method, comprising: with a population of metallic nanoparticles comprising a material and103241.007033 / 22-9924 (a) having a labile ligand associated thereon and (b) being disposed on a substrate, and (i) exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles, (ii) removing the labile ligand so as to leave the metallic nanoparticles essentially free of ligand, or both (i) and (ii), the metallic nanoparticles then associating so as to form a conductive film.
[0010] Also provided is a conductive film, comprising a plurality of metallic nanoparticles having a compact ligand associated therewith, the film having a resistivity of less than about 50 times (e.g., from 1.1 to 25 times) the resistivity of the bulk material of the metallic nanoparticles.
[0011] Further provided is a composition, comprising: a population of metallic nanoparticles (i) having a labile ligand associated thereon and (ii) being disposed on a substrate; and a compact ligand that, relative to the labile ligand, preferentially associates with the population of metallic nanoparticles. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The patent or application file contains at least one drawing executed in color. Copies of this patent or patent application publication with color drawing(s) will be provided by the Office upon request and payment of the necessary fee.
[0013] In the drawings, which are not necessarily drawn to scale, like numerals may describe similar components in different views. Like numerals having different letter suffixes may represent different instances of similar components. The drawings illustrate generally, by way of example, but not by way of limitation, various aspects discussed in the present document. In the drawings:
[0014] FIG.1. (a) Schematics of the Cu NP films before (left) and after (right) the ligand exchange process. Black and purple structures represent oleylamine (OLAM) and compact molecules, respectively. (b) UV-vis transmission and (c) FTIR absorption spectra of Cu NP films capped by OLAM (black), SCN- (red), Cl- (green), S2-(blue), and N3- (cyan). TEM images of Cu NPs (d) before and (e) after the SCN ligand exchange.
[0015] FIG.2. (a) Powder XRD patterns of Cu NP films capped by OLAM (black), SCN (red), Cl (green), S (blue), and N3 (cyan). (b) Resistivity of the Cu NP films after different ligand exchange treatments and after 80 °C annealing for 10 min.103241.007033 / 22-9924
[0016] FIG.3. (a) Resistivity of Cu NP films after the SCN (black), 5% AA- SCN (orange), 10% AA-SCN (blue), and 20% AA-SCN (green) treatments as a function of air exposure time. (b) XRD patterns of Cu NP films as-deposited (black) and after the SCN (red) and 10% AA-SCN (green) treatments. High resolution XPS spectra of (c) Cu 2p and (d) O 1s regions from Cu NP films as deposited (the top row) and after the SCN (the middle row) and 10% AA-SCN (the bottom row) treatments.
[0017] FIG.4. Resistivity of AA-SCN treated 4-nm Cu NP films that are (a) 32.4 (black), 61.9 (red), and 94.4 (blue) nm thickness and (b) that are ~100 nm thick and composed of 4 (black), 10 (red), and 20 (blue) nm diameter NPs as a function of air exposure time. (c) AFM images of the corresponding Cu NP films in (b).
[0018] FIG.5. (a) Photograph of an interdigitated capacitor fabricated by photolithographic patterning and spin coating of Cu NP inks and SCN and AA treatments. Inset: surface topology of the Cu NP trace measured by AFM. Frequency-dependent capacitance and loss tangent of the capacitor made of (b) Cu NPs and (c) sputtered Cu.
[0019] FIG.6. The simulated (a) real and (b) imaginary part of the permittivity of Cu NP films with OLAM ligands (black) and after SCN (red) and AA-SCN (green) treatments. (c) SEM image and (d) IR scattering spectrum of a Cu NP based plasmonic metasurface.
[0020] FIG.7. Structural and optical characterization of 4.5 nm diameter Cu NCs deposited as thin films before and after various chemical treatments. TEM images of (a) as-synthesized and OLAM-capped, (b) SCN--treated, and (c) Cl--treated Cu NC films. The ligand exchange time is 240 s. Scale bar: 10 nm. (d) A photograph of a Cl--treated Cu NC film on a glass substrate showing the reflection of the IoT4Ag NSF Engineering Research Center logo printed on an adjacent piece of paper. (e) XRD patterns, (f) FTIR absorbance spectra, and (g) optical transmittance spectra at normal incidence of Cu NC thin films before (black), and after SCN- (red) and Cl- (blue) treatments. Optical transmittance spectrum of an evaporated Cu film (grey) shown in (g). All Cu NC films in (e), (f), and (g) are fabricated by four sequences of Cu NC spin coating and SCN-- or Cl-- treatment for 240 s.
[0021] FIG.8. DC resistivity of Cu NC thin films. (a) The sheet resistance ( ^^^^) of SCN--exchanged (red) and Cl--exchanged (blue), 4.5 nm diameter Cu NC thin films and thermally evaporated Cu films (grey) as a function of (bottom axis) inverse thickness103241.007033 / 22-9924 (1⁄^^), and (top axis) thickness ( ^^), measured using the four-point probe (4pp) method. The ligand exchange time is 240 s. (b) ^^^^of 4.5 nm (blue) and 15.0 nm (orange) diameter Cu NC films fabricated by varying Cl- ligand treatment time (t) and fit (black), as described in the text. (c) SEM images of 4.5 nm diameter Cu NC films fabricated by Cl- treatment with t of 60 s (left), 120 s (middle), and 240 s (right). (d) XRD patterns of 60 s (light blue) and 240 s (blue) Cl--treated 4.5 nm diameter Cu NC films, and 60 s (light orange) and 240 s (orange) Cl--treated 15.0 nm diameter Cu NC films. All Cu NC films in (b), (c) and (d) are fabricated by four sequences of Cu NC spin-coating and Cl- treatment. (e) The stability of ^^^^as a function of air exposure time for SCN--exchanged (red) and Cl- -exchanged (blue) 4.5 nm diameter Cu NC thin films. (f) The resistivity ( ^^) relative to that of bulk Cu(^^^^ ^^ ^^ ^^ ^^ ^^)of 4.5 nm diameter and 15.0 nm diameter Cl--exchanged Cu NC films in comparison to those for films prepared from high-temperature sintering of Cu nanoparticle inks reported in the literature, color-coded by the diameter of the nanoparticles.24,47–51
[0022] FIG.9. Characterization of RF capacitive devices based on Cu NCs. Photographs of Cu NC-based, 14-finger interdigitated capacitors fabricated by five sequences of spin coating of a Cu NC dispersion followed by Cl- treatment for 240 s on (a) glass (sample A) and (b) Kapton®(sample C) substrates. Scale bar: 3 mm (c) Measured (solid lines) and equivalent circuit model fit (dashed lines) of admittance and (d) calculated Q-factor for an evaporated Cu film (grey) and samples A (red), B (blue), and C (magenta). Sample B is fabricated by two sequences of doctor-blade coating of a Cu NC dispersion followed by Cl- treatment for 240 s. Inset of (c): equivalent circuit model used for fitting.
[0023] FIG.10. Characterization of nanoimprinted Cu NC optical metasurfaces. (a) The imaginary and (b) real part of the dielectric function of evaporated Cu (grey), SCN--treated Cu NC films (red), and Cl--treated Cu NC films (blue). (c) Low- and high- resolution (inset) SEM images of Cl--treated Cu NC metasurfaces composed of a square nanopillar array. (d) Measured (solid line) and simulated (dashed line) transmittance spectra of the metasurfaces fabricated with SCN--treated (red), and Cl--treated (blue) Cu NC films.103241.007033 / 22-9924
[0024] FIG.11. Transmission electron microscopy (TEM) images of (a) as- synthesized and oleylamine (OLAM)-capped, (b) SCN--treated, and (c) Cl--treated 15.0 nm diameter Cu NC films. The ligand exchange time is 240 s. Scale bar: 20 nm.
[0025] FIG.12. (a) UV-vis transmittance spectra, (b) Fourier transform infrared (FTIR) absorbance spectra, and (c) X-Ray diffraction (XRD) patterns of OLAM-capped (black), NH4SCN-treated (red), NH4Cl-treated (blue), Na2S-treated (green), and NaN3- treated (magenta) Cu NC films.
[0026] FIG.13. Cu 2p X-ray photoelectron spectroscopy (XPS) of Cu NC films with OLAM (top), SCN- (middle), and Cl- (bottom) capping ligands.
[0027] FIG.14. Diffuse reflectance spectra of evaporated Cu (grey) and Cu NC films with OLAM (black), SCN- (red), and Cl- (blue) ligands.
[0028] FIG.15. (a) Atomic form microscopy (AFM) image of one layer of 4.5 nm diameter, Cu NC films with Cl- ligand treatment for 240 s. (b) FTIR absorbance spectra of films prepared by depositing four layers of 4.5 nm diameter Cu NC films and treating the films after each layer is deposited with Cl- for 60 s. (c) Histogram of particle size distribution from Cu NC films treated with Cl- ligand for 240 s, analyzing the SEM image in FIG.8c (240 s) of the main text using image J.
[0029] FIG.16. (a) The sheet resistance of 15.0 nm diameter Cu NC films at various film thicknesses treated by SCN- (orange) and Cl- (gold) ligand solutions for 240 s. (b) Scanning electron microscopy (SEM) images of films prepared by depositing four layers of 15.0 nm diameter Cu NCs and treating the films after each layer is deposited with Cl- for 60 s (left) and 240 s (right).
[0030] FIG.17. (a) XRD patterns of films prepared by depositing four layers of 4.5 nm diameter Cu NCs and treating the films after each layer is deposited with SCN- for 60 s (green) and 240 s (dark green). Corresponding SEM images of these NC films with SCN- treatment times of (b) 60 s and (c) 240 s.
[0031] FIG.18. Resistivity change of SCN--treated Cu NC films with different thicknesses measured over time that the films are stored in air.
[0032] FIG.19. Optical microscopy images of (a) sample A fabricated by spin coating Cu NCs on a glass substrate, (b) sample B fabricated by doctor blading Cu NCs on a glass substrate, and (c) sample C fabricated by spin coating Cu NCs on a Kapton substrate. Scale bar: 1 mm. (d) Measured geometrical parameters for these three samples.103241.007033 / 22-9924
[0033] FIG.20. Calculated capacitances for RF devices fabricated by evaporating Cu (grey), spin coating Cu NCs (sample A, red), and doctor blading Cu NCs on glass substrates (sample B, blue), and by spin coating Cu NCs on a Kapton substrate (sample C, magenta).
[0034] FIG.21. The measured (dotted) and fitted (solid) (a) real ( ^^1) and (b) imaginary ( ^^2) parts of the dielectric constants of evaporated Cu (grey) and SCN--treated (red) and Cl--treated (blue) 4.5 nm diameter Cu NC films with four sequences of Cu NC spin-coating and 240 s ligand treatment. The ratio between (c) −and ^^2and (d) ^^1and ^^2for evaporated Cu (grey) and SCN--treated (red), and Cl--treated (blue) 4.5 nm diameter Cu NC films.
[0035] FIG.22. AFM image of 4.5 nm diameter Cu NC optical metasurfaces with the Cl- treatment.
[0036] FIG.23. Example, non-limiting illustration of a process according to the present disclosure. DETAILED DESCRIPTION OF ILLUSTRATIVE EMBODIMENTS
[0037] The present disclosure may be understood more readily by reference to the following detailed description of desired embodiments and the examples included therein.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. In case of conflict, the present document, including definitions, will control. Preferred methods and materials are described below, although methods and materials similar or equivalent to those described herein can be used in practice or testing. All publications, patent applications, patents and other references mentioned herein are incorporated by reference in their entirety. The materials, methods, and examples disclosed herein are illustrative only and not intended to be limiting.
[0039] The singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise.
[0040] As used in the specification and in the claims, the term "comprising" may include the embodiments "consisting of" and "consisting essentially of.” The terms “comprise(s),” “include(s),” “having,” “has,” “can,” “contain(s),” and variants thereof, as103241.007033 / 22-9924 used herein, are intended to be open-ended transitional phrases, terms, or words that require the presence of the named ingredients / steps and permit the presence of other ingredients / steps. However, such description should be construed as also describing compositions or processes as "consisting of" and "consisting essentially of" the enumerated ingredients / steps, which allows the presence of only the named ingredients / steps, along with any impurities that might result therefrom, and excludes other ingredients / steps.
[0041] As used herein, the terms “about” and “at or about” mean that the amount or value in question can be the value designated some other value approximately or about the same. It is generally understood, as used herein, that it is the nominal value indicated ±10% variation unless otherwise indicated or inferred. The term is intended to convey that similar values promote equivalent results or effects recited in the claims. That is, it is understood that amounts, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but can be approximate and / or larger or smaller, as desired, reflecting tolerances, conversion factors, rounding off, measurement error and the like, and other factors known to those of skill in the art. In general, an amount, size, formulation, parameter or other quantity or characteristic is “about” or “approximate” whether or not expressly stated to be such. It is understood that where “about” is used before a quantitative value, the parameter also includes the specific quantitative value itself, unless specifically stated otherwise.
[0042] Unless indicated to the contrary, the numerical values should be understood to include numerical values which are the same when reduced to the same number of significant figures and numerical values which differ from the stated value by less than the experimental error of conventional measurement technique of the type described in the present application to determine the value.
[0043] All ranges disclosed herein are inclusive of the recited endpoint and independently of the endpoints (e.g., "between 2 grams and 10 grams, and all the intermediate values includes 2 grams, 10 grams, and all intermediate values"). The endpoints of the ranges and any values disclosed herein are not limited to the precise range or value; they are sufficiently imprecise to include values approximating these ranges and / or values. All ranges are combinable.103241.007033 / 22-9924
[0044] As used herein, approximating language may be applied to modify any quantitative representation that may vary without resulting in a change in the basic function to which it is related. Accordingly, a value modified by a term or terms, such as “about” and “substantially,” may not be limited to the precise value specified, in some cases. In at least some instances, the approximating language may correspond to the precision of an instrument for measuring the value. The modifier “about” should also be considered as disclosing the range defined by the absolute values of the two endpoints. For example, the expression “from about 2 to about 4” also discloses the range “from 2 to 4.” The term “about” may refer to plus or minus 10% of the indicated number. For example, “about 10%” may indicate a range of 9% to 11%, and “about 1” may mean from 0.9-1.1. Other meanings of “about” may be apparent from the context, such as rounding off, so, for example “about 1” may also mean from 0.5 to 1.4. Further, the term “comprising” should be understood as having its open-ended meaning of “including,” but the term also includes the closed meaning of the term “consisting.” For example, a composition that comprises components A and B may be a composition that includes A, B, and other components, but may also be a composition made of A and B only. Any documents cited herein are incorporated by reference in their entireties for any and all purposes.
[0045] Herein, we develop a colloidal Cu NP ink and room-temperature chemical treatments with, for example, thiocyanate, acetic acid, and chloride to achieve highly conductive and air-stable thin films. We also demonstrate the integration of such Cu NP ink and chemical treatments with solution-based fabrication processes to construct structures at multi-scales for device applications at DC, RF, and optical frequencies. The thiocyanate ligand exchange and acid treatment induce fusion of Cu NPs in the absence of high-temperature processing, achieving closely-packed Cu NP films with air-stable DC resistivity as low as 1.24 times that of bulk Cu. The chemical treatment is compatible with spin coating and doctor blade coating to fabricate sub-micron to micron-thick Cu NP films. Patterning of the films using standard photolithography is applied to create RF circuit elements with critical dimensions of tens of micrometers, showing low loss under AC bias. Arrays of subwavelength nanoresonators, with individual sizes of tens to hundreds of nanometers, have also been fabricated by nanoimprinting Cu NP inks and show size-tunable localized surface plasmonic resonance (LSPR) in the near infrared103241.007033 / 22-9924 (NIR) region. This colloidal NP material and room-temperature process open opportunities for applications of such conductive inks on substrates with low thermal budgets, such as flexible and biocompatible and / or biodegradable polymers and paper.
[0046] As-synthesized Cu NPs are 4 nm in diameter and capped by oleylamine (OLAM) ligands. The long-chain OLAM ligands maintain the NP colloidal stability for solution-based coating and printing of their assemblies. However, these ligands need to be removed or replaced by compact ligands during film fabrication to reduce the interparticle distance and achieve conductivity, as illustrated by FIG.1a. A series of common ligand reagents have been investigated, including ammonium thiocyanate (NH4SCN), ammonium chloride (NH4Cl), sodium sulfide (Na2S), and sodium azide (NaN3). The methanolic solutions containing these ligands are applied to and cover deposited Cu NP films for 1 min. The film is then flushed with pristine methanol three times to remove any excess ligands. The above steps can be repeated by sequential spin coating or doctor blading coating and ligand exchange to achieve tens to hundreds of nanometer or micron thick films, respectively. The fabrication and ligand exchange steps are conducted in nitrogen- filled gloveboxes unless otherwise noted.
[0047] These ligand-exchanged Cu NP films are characterized by UV-vis and FTIR absorption spectroscopies and compared with the original Cu NP film (FIG.1b and c). A distinctive feature is observed at around 610 nm in the UV-Vis absorption spectrum that arises from the LSPR of individual Cu NP cores in the films.12However, this feature disappears after the SCN- or Cl- ligand treatment, where the overall transmittance is lower for all wavelengths of light, indicating a strong coupling among the Cu NPs (i.e., the loss of the individual character of the NPs) and higher reflectance of the metallic film. Consistently, the C-H stretch between 3000-2800 cm-1in the FTIR spectra is reduced after the removal of long-chain organic ligands upon the SCN- and Cl- treatments. The absorption peak at 2128 cm-1suggests the formation of Cu-SCN bonds. The sintering of NPs induced by the SCN- ligand exchange can be further observed by transmission electron microscopes (TEM) imaging shown in FIG.1d and e. The S2-treatment is consistent with the transformation of Cu to CuxS films, as evidenced by the decreasing transmittance below 573 nm, which corresponds to a bandgap energy of 2.16 eV for CuxS.13Lastly, the N3- treatment does not alter the UV-vis spectrum nor remove the C-H103241.007033 / 22-9924 signature significantly. Therefore, the Cu NPs are still distanced and behave as individual NPs.
[0048] The ligand exchange treatments also cause structural evolution of the Cu NP films as characterized by x-ray diffraction (XRD) (FIG.2a). The diffraction peaks at 43.4˚ and 50.6˚ of the Cu NP-OLAM film are consistent with the (111) and (200) crystal planes of the bulk Cu, respectively. These peak positions remain unchanged after the SCN- and Cl- treatment, while the S2-and N3- treated samples show distinctive diffraction patterns. The XRD results indicate that the lattice structure of Cu NPs is preserved by both the SCN- and Cl- ligands. Fitting the width of the (111) peak and using the Scherrer equation to calculate the crystallite size, we obtain 2.4, 7.0 and 21.7 nm for Cu NP films capped by OLAM, SCN-, and Cl-, respectively. This calculated particle size of Cu NP- OLAM is consistent with the 4-nm diameter observed in the TEM images. The growth of the grain size induced by the SCN- and Cl- ligand exchange is consistent with the optical characteristics in FIG.1b and c.
[0049] The DC conductivity of the Cu NP films with different ligand exchange treatments is measured using a two-terminal geometry. FIG.2b provides example, non- limiting resistivity data for thin, single-layer compositions formed at room temperature using the disclosed technology and then also annealed at 80 ºC. It is worth noting that performing the SCN- treatment at room temperature can render the resistivity of Cu NP films as low as 1.26 times that of evaporated Cu thin films of the same thickness. The higher resistance after the Cl- treatment, in comparison to SCN treatment, has similarly been reported in Ag NP films and attributed to the discontinuity of the conductive path caused by uncontrollable grain growth.9Further annealing these films at 80 ˚C, the SCN decomposition temperature, for 10 min does not significantly change the conductivity of the Cu-SCN film, indicating that the Cu NPs are well fused after the SCN- ligand exchange, and the remaining SCN- ligands on the surface do not impede charge transport. In comparison, the resistance decreases after gentle thermal annealing at 80 ˚C for 10 min of Cu-Cl and Cu-N3 samples, probably due to fusion and densification of the Cu NPs.
[0050] To prevent Cu NP films from oxidation, an additional post-deposition chemical treatment is introduced. An increase of resistivity from 2.4 × 10−8to 4.9 × 10−8Ω ∙ ^^ is observed on the Cu NP-SCN films after 72 hours of air exposure, due to the formation of less conductive copper oxide (FIG.3a). To remove the oxide and103241.007033 / 22-9924 passivate the NP surface, a diluted acetic acid (AA) solution in methanol is applied prior to the last SCN ligand exchange step on the top layer of the Cu NP films. We observe a lower resistivity of 1.44 × 10−8Ω ∙ ^^ after the treatment by a 10 vol% AA solution with only a 12.7% increase after prolonged air exposure. However, either higher or lower AA concentrations of 20% or 5% yield more resistive and less air-stable films (FIG.3a). Compared to the evaporated Cu film of the same thickness, the 10% AA treated Cu NP films reach resistivities of 1.10 times that of films as fabricated in an inert environment and stabilizes at 1.24 times after air exposure.
[0051] The improved conductivity originates from the removal of surface oxides and further fusion of Cu NPs by the extra AA treatment. The AA-treated films show XRD peaks at identical positions in 2-theta but narrowed widths in comparison to those of the Cu-OLAM and Cu-SCN films, suggesting the preservation of the Cu lattice and grain growth (FIG.3b). The larger grain size is calculated to be 9.7 nm. Furthermore, high resolution x-ray photoelectron spectroscopy (XPS) spectra show reduced widths of the Cu 2p peak and lower intensities of the O 1s peak after the SCN- and AA-SCN- treatments, indicating effective removal of surface oxides (FIG.3c). The Cu:O ratio has increased from 10.4:89.6 of the as-synthesized Cu NPs to 96.8:3.2 and 97.3:2.7 after the SCN and AA-SCN treatments, respectively. The mechanism of AA treatment is likely akin to previous studies, where AA is reported to etch copper oxide by forming cupric acetate but not to react with Cu.14The more oxide-free surface can facilitate Cu NP fusion during subsequent SCN treatment, corroborating the observation of further grain growth. This densification of Cu NP films leads to improved charge transport and air-stability.
[0052] We also investigate the effect of film thickness and NP size on the DC resistivity. As the film thickness increases from 32 nm to 61 nm and to 94 nm, the resistivity decreases and air-stability increase (FIG.4a). The thickness-dependent air stability suggests that oxidation occurs from the film surface and gradually diffuses into bulk of the film, therefore thicker films still maintain conductive channels even with surface layers oxidized. With the same AA-SCN treatment, a decreasing trend of conductivity is observed when the Cu NP size increases from 4 nm to 10 and 20 nm (FIG. 4b). This trend can be attributed to the change in film morphologies as shown by the AFM images in FIG.4c, where the larger particles tend to form more isolated islands instead of continuous films after the AA and SCN treatment.103241.007033 / 22-9924
[0053] Structures of interdigitated capacitors are fabricated by patterning the Cu NP films using photolithography. Standard bilayer photoresists of LOR3A and S1818 are exposed by a 355 nm laser writer system. The developed pattern is then filled by Cu NPs through multi-layer spin coating or doctor blade coating steps with the SCN- and AA treatments. In contrast to the typical film thickness of 10-100 nm for DC resistivity measurements, micron-thick films that exceed the penetration skin depth of RF waves are required to reduce AC resistance and thus loss. To reach the film thickness above 1 μm, Cu NP concentrations as high as 300 mg / mL are used during film deposition with the same chemical treatment conditions described above. The Cu NP based capacitors fabricated on Kapton (FIG.5a) show a capacitance of ~1.4 pF in the frequency range of 10 kHz to 3 MHz (FIG.5b), close to that of a sample made of sputtered Cu (FIG.5c), and consistent with the capacitance calculated from that of bulk Cu and the geometric parameters of the capacitors. The slightly increased loss tangent in the Cu NP structures could be due to insufficient film thickness and higher surface roughness as shown in the inset of FIG.5a.
[0054] The colloidal Cu NPs can also be used as the building blocks of subwavelength, nanoresonator arrays that are patterned by nanoimprint lithography and that serve as optical metasurfaces. We firstly investigate the dielectric properties of the Cu NP films before and after the SCN- and AA-SCN treatments. By fitting the ellipsometry spectroscopy with the effective medium approximation (EMA) and Drude-Lorentz function, we derive the real ( ^^′) and imaginary ( ^^′′) parts of permittivity as a function of wavelength shown in FIG.6a and b. OLAM-capped Cu NP films show a positive ^^′ at optical wavelengths, consistent with a dielectric material. However, after the SCN- ligand exchange, ^^′ becomes negative at wavelengths longer than 787 nm. The negative ^^′ indicates that SCN-treated Cu NC films are metallic. The additional AA treatment further lowers the zero-crossing wavelength to 645 nm and ^^′ has a steeper slope at infrared wavelengths, yielding a more negative ^^′ over a wider spectral range. The absence of a peak feature around 610 nm in the ^^′′ dispersion after the SCN- and AA-SCN treatment also supports that the LSPR of individual Cu NPs is lost due to delocalization of electrons across the electronically-coupled NP film. Therefore, the metallic behavior of AA-SCN treated Cu NP films enable the construction of subwavelength plasmonic structures, through large-area and solution-based fabrication processes, such as nanoimprint103241.007033 / 22-9924 lithography. FIG.6c shows an example array of square nanopillars fabricated by nanoimprinting. Specifically, Cu NPs are spin-coated atop a patterned resist layer, followed by the AA-SCN treatment and a lift-off process. This plasmonic pattern with a 350-nm edge length of each nanoresonator and an 800-nm pitch shows a resonance at 1242 nm (FIG.6d).
[0055] Additional Disclosure
[0056] Emerging applications of Internet of Things (IoT) technologies in smart health, home, and city, in agriculture and environmental monitoring, and in transportation and manufacturing, require materials and devices with engineered physical properties and that can be manufactured by low-cost and scalable methods, support flexible forms, and are biocompatible and biodegradable. Here, we report the fabrication and device integration of low-cost and biocompatible / biodegradable colloidal Cu nanocrystal (NC) films through room-temperature, solution-based deposition and sintering, achieved via chemical exchange of NC surface ligands. Treatment of organic-ligand capped Cu NC films with solutions of shorter, environmentally-benign and non-corrosive inorganic reagents, namely SCN- and Cl-, effectively removes the organic ligands, drives NC grain growth, and limits film oxidation. We investigate the mechanism of this chemically-driven sintering by systemically varying the Cu NC size, ligand reagent, and ligand treatment time and follow the evolution of their structure and electrical and optical properties. Cl-- treated, 4.5 nm diameter Cu NC films yield the lowest DC resistivity, only 3.2 times that of bulk Cu, and metal-like dielectric functions at optical frequencies. We exploit the high conductivity of these chemically-sintered, Cu NC films, and in combination with photo- and nanoimprint-lithography, pattern multiscale structures to achieve high-Q radio frequency (RF) capacitive sensors and near-infrared (NIR) resonant optical metasurfaces.
[0057] The rapid advancement of the Internet of Things (IoT) has ushered in an era of unprecedented connectivity and data exchange among devices and users, revolutionizing the way we interact with our environment. IoT technologies enable smart health, home, and city, and promise to enhance existing agriculture and environmental monitoring, transportation, and manufacturing.1,2The physical device layer, including electrical, optical, and chemical sensors, detect and transduce signals to communicate data of interest.3Devices must be constructed to meet application-specific needs that often require them to be low cost and scalable in number, flexible in their form, and103241.007033 / 22-9924 biodegradable and / or biocompatible.4,5These requirements, in turn, drive the need to create device fabrication processes that are cost effective, high throughput, and low temperature and to advance compatible materials with engineered physical properties. In particular, IoT technologies motivate the development of solution-based manufacturing techniques and functional nanoscale materials that form inks.6–8
[0058] One target at the heart of solution-processable devices is the development of conductive inks. The inks are composed of metal nanoparticles or nanocrystals (NCs), typically 1 – 100 nm in diameter, a liquid vehicle, and organic / inorganic additives that serve as surfactants, stabilizers, or binders.9–11Batch chemical synthesis and solution- based coating and printing processes lower manufacturing costs,12,13and the high metal loading of NC inks results in high conductivity traces or structures, enabling their applications as electrodes, interconnects, and antennas in flexible electronic devices and circuits,14optical metasurfaces,11and chemical and biological sensors.13Au and Ag NC inks are well-studied and commercialized,11,15–21but Au NC inks are relatively expensive and Ag NC inks raise toxicity concerns,22limiting their use in IoT applications. Cu NC inks stand out as cost-effective and biocompatible / biodegradable alternatives.10,13,23–25Like Ag and Au NCs, Cu NCs can be used to form electrically conductive films and optical materials with similar plasmonic properties.
[0059] However, to achieve high conductivity films, sintering of metal NCs of all compositions is typically required, necessitating the use of post-deposition processing either through thermal annealing (i.e., typically at temperatures >120 ˚C) or high-intensity laser irradiation to decompose the organic additives introduced to stabilize the NCs in solvents as inks and drive grain growth.23,26Consequently, these high-temperature processes preclude substrates with low-thermal resistance, in particular some flexible and biodegradable polymers and papers.27–30Another challenge to developing Cu NC inks is the propensity for surface oxidation that introduces barriers to charge transport and thus lowers DC and AC conductivities, degrading their performance in radio frequency (RF) electronics.9,13,23,31The smaller number of free electrons in oxidized Cu also alters the strength and frequency of plasmonic resonances in optical metasurfaces.32–35Recently, room-temperature sintering of Cu NCs has been reported through consecutive chemical treatments with ligands and reducing reagents; however, these reagents are corrosive and the resistivity of resulting films is still ~20 times that of the bulk Cu.10103241.007033 / 22-9924
[0060] We report room-temperature, chemical treatments that drive sintering of solution-deposited Cu NC films and their integration in electrical and optical devices. By treating the NC films with solutions of compact ligand reagents, such as environmentally- benign and non-corrosive thiocyanate (SCN-) and chloride (Cl-), we exchange the long- chain organic ligands introduced to control NC size during synthesis and to stabilize NC inks with these short inorganic anions, triggering NC fusion and grain growth to form conductive pathways.11,15Cl- ligand exchange of the smallest-studied, 4.5 nm diameter Cu NC films drives the largest grain growth and is used to achieve films with DC resistivities as low as 3.2 times that of bulk Cu and that remain air stable for months. Their dielectric properties at optical frequencies also resemble that of evaporated Cu films. We demonstrate the integration of such Cu NC inks and chemical treatments with lithographic processes to achieve structures at multiple length scales to create devices operating at RF and optical frequencies. Photolithography is applied to pattern the films into micron-scale interdigitated capacitors, that show high Q-factors comparable to those of thermally- evaporated Cu-based devices at RF frequencies. Nanoimprint lithography is used to pattern optical metasurfaces composed of arrays of nanoscale, subwavelength NC superstructures, that show plasmon resonances in the near-infrared (NIR) region of the electromagnetic spectrum.
[0061] Cu NCs are synthesized following methods previously reported in the literature (see Methods).36To avoid oxidation, all of the synthesis, handling, and processing steps of the Cu NCs are conducted under an inert atmosphere unless otherwise noted. In the synthesis, oleylamine (OLAM) is introduced to reduce Cu(II) precursors to form Cu(0) monomers. Controlling the OLAM concentration in the reaction pot regulates NC nucleation and growth and, thus, allows the NC size to be tailored.37To study the size- dependent Cu NC film properties, we synthesize and use two different-size spherical Cu NCs with average diameters of 4.5±0.6 nm and 15.0±1.1 nm, as characterized by transmission electron microscopy (TEM) images shown in FIG.7a and FIG.11, respectively. OLAM also serves to ligate the NC surface and sterically stabilize the NCs in toluene to form inks.
[0062] OLAM-capped Cu NC inks are deposited using spin coating or doctor- blade coating methods on Si wafers, glass, and flexible, polymer Kapton®substrates (Scheme 1; FIG.23). The OLAM ligands in deposited films isolate individual NCs and103241.007033 / 22-9924 prevent electronic coupling between neighboring NCs (FIG.7a). Instead of removing ligands through thermal annealing or laser irradiation, the Cu NC thin films are immersed in room temperature, methanolic salt solutions of Na2S, NaN3, NH4SCN, and NH4Cl for 2- 5 min and then rinsed with pure methanol (MeOH), a process known as solid-state ligand exchange (Scheme 1; FIG.23).15,38,39The salt solutions allow one to examine a series of compact anions often explored as ligands for colloidal NCs. However, S2-anions convert the Cu NCs into CuxS NCs, losing their metallic character, similar to the reaction of S2-with Ag NCs to form Ag2S NCs,11and N3- anions do not substantially remove the organic ligands (FIG.12). SCN- and Cl- are effective ligand-exchange agents for Cu NCs, akin to their utility in increasing the metallicity of Ag and Au NC thin films.11,15Therefore, in the following sections, we focus on SCN- and Cl- ligand treatments to map their effects on the structural, optical, and electrical properties of Cu NC films.
[0063] 4.5 nm diameter Cu NCs are used in depositing films and characterizing their structure and composition before and after ligand exchange. Upon ligand exchange with SCN-, the interparticle distance is substantially reduced or completely lost, and the NCs are seen to fuse (FIG.7b). Treatment with the ligand-exchange agent Cl- drives greater NC fusion and grain growth (FIG.7c), forming highly-reflective NC films (FIG. 7d). Further structural characterization of ligand-treated Cu NC films is extracted from X- ray diffraction (XRD) patterns shown in FIG.7e. For OLAM-capped Cu NC films, XRD patterns have peaks near 43° and 51° in 2θ, corresponding to the (111) and (200) planes of metallic Cu, respectively. A peak at 38° is assigned to the (111) plane of cuprous(I) oxide.25,40The characteristics are consistent with previous reports of Cu NCs and their modest oxidation.9,10After SCN- and Cl- treatments of the NC films, the two Cu peaks narrow, consistent with NC sintering. The Cu NC grain size, calculated from the (111) peak using the Scherrer equation, increases from 3.7 ± 0.24 nm for the OLAM-capped NC films to 7.0 ± 0.24 nm and 21.7 ± 0.39 nm for the SCN-- and Cl--treated films, respectively, consistent with TEM images showing the more effective grain growth with Cl- ligand treatment. The Scherrer analysis may underestimate the particle size but provides a consistent measure to compare the grain growth across Cu NC films measured by the same instrument. Interestingly, the Cu2O reflection is not observed for the SCN-- and Cl--treated films, indicating that the surface chemical treatments remove and suppress surface oxidation.11X-ray photoelectron spectroscopy (XPS) measurements of OLAM-,103241.007033 / 22-9924 SCN--, and Cl--ligated Cu NC films show the Cu 2p peak position shifts from 932.3 eV to 932.8 eV after the SCN- or Cl- treatment (FIG.13), consistent with the suppression of Cu2O bond formation.41Characteristic CuO satellite peaks above 940 eV are absent and also consistent with XRD remeasurements where CuO is not seen in the Cu NC films before or after the ligand exchange.42
[0064] The successful removal of OLAM ligands upon ligand exchange is also confirmed by Fourier transform infrared spectroscopy (FTIR) measurements (FIG.7f), as the C-H fingerprint, ranging from 2800 to 3200 cm-1, present in the OLAM-capped Cu NC films, decreases to <1% in integrated intensity after the SCN- treatment and is undetectable after the Cl- ligand treatment. For the SCN--treated NC films, a new peak appears near 2130 cm-1. The peak is shifted from the vibrational fingerprint of free NH4SCN near ~2050 cm-1, consistent with the formation of surface Cu-SCN chemical bonds.43The presence of surface Cu-SCN bonds and the residual OLAM ligands detected for SCN- ligand treatment may hinder more aggressive diffusion of Cu atoms, leading to the smaller grain size than that seen for Cl--treated Cu NC films.
[0065] In optical transmittance spectra, as-synthesized OLAM-capped Cu NC thin films show a dip near 640 nm (FIG.7g, black), matched with the localized surface plasmon resonance (LSPR) of metallic Cu NCs.44,45Upon SCN- or Cl- ligand exchange, the resonance broadens and decreases in amplitude (FIG.7g, red and blue) as the NCs fuse, and becomes similar to the spectrum of evaporated Cu thin films (FIG.7g, grey). We also measure diffuse reflectance spectra of the same samples, as shown in FIG.14. As the capping ligand is changed from OLAM to SCN-, and Cl-, the overall reflectivity of the Cu NC films increases, and the highest reflectance of Cl--treated films approaches that of evaporated Cu films (FIG.7d and FIG.14). We observe peak features in the reflectance spectra positioned around 605 nm for all samples, which is attributed to the intrinsic interband absorption of metallic copper.46The transmittance and reflectance spectra are consistent with an increase in the density of Cu atoms and, therefore, the metallicity of the NC thin films upon compact ligand exchange.
[0066] The DC resistivity of the Cu NC thin films after SCN-- and Cl- ligand treatments is measured using the four-point probe (4pp) method, which allows for characterization of the thin-film sheet resistance without the interference of contact resistance. We evaporate 3 / 60 nm Cr / Au electrodes on degenerately-doped Si wafers with103241.007033 / 22-9924 250 nm thermally-grown oxide layers and then deposit Cu NC films by spin coating 30 mg / mL Cu NC inks on top to form bottom contacts with the electrodes. The fabrication of Cu NC thin films follows the process described in Scheme 1 and is carried out sequentially to deposit and ligand exchange multiple NC layers to increase the film thickness. For various NC film thicknesses(^^), measured by AFM (Table 2), and 240 s of SCN- and Cl- ligand exchange time, we plot ^^^^−as shown in FIG.8a, where resistivity ( ^^) can be calculated from the slope. For SCN--exchanged Cu NC films, with one deposited NC layer and a 50.5 ± 3.2 nm thickness (Table 2), ^^^^is 19.0 ± 0.6 ^ / □. Sequentially depositing and exchanging seven NC layers yields a 347.9 ± 10.8 nm film thickness (Table 2) and films with a lower ^^^^of 6.7±0.3 ^ / □ (FIG.8a, red). For thicknesses >150 nm, ^^ becomes 136.4 × 10−8Ω ^^, which is 10 orders of magnitude lower than that of the OLAM-capped Cu NC films. The high conductivity is achieved as a result of conductive pathways formed by chemically-sintering Cu NCs, as suggested by the structural characterization above. In comparison to the SCN--ligand treatment, the Cl- ligand treatment yields strong thickness-dependent characteristics of the Cu NC films (FIG.8a, blue). The relatively high ^^^^quickly drops when the film thickness increases beyond 100 nm and reaches 0.45±0.03 ^ / □ at 165 nm and ^^^^ ^^− ^^ ^^of 5.45 × 10−8Ω ^^. Cl--treated Cu NC films are 26 times more conductive than the SCN--treated films and approach the ^^^^of 0.27 ^ / □ measured for thermally-evaporated Cu films of similar thickness (FIG.8a, grey).
[0067] AFM measurements show the thickness of SCN--treated Cu NC films grows linearly with the number of cycles of NC deposition and ligand exchange (Table 2). However, the thickness of Cl--treated Cu NC films does not grow linearly, as the thickness appears to grow more slowly, particularly after three spin coating and exchange cycles (Table 2), giving rise to a smaller thickness than that of the SCN--treated films after multilayer NC deposition with identical conditions. This phenomenon agrees with more substantial NC sintering caused by the Cl- treatment, leading to a larger volume shrinkage after Cl- in comparison to SCN- ligand treatment. For Cl--treated NC films with thickness <100 nm, nanoscale voids are seen which are not entirely compensated for by the infilling of NCs from within the thickness of the films, forming fewer percolation paths to yield porous and less conductive films (FIG.15a). As multiple layers of Cu NCs are deposited and Cl- treated, the additional layers fill voids and densify, and to a smaller degree thicken103241.007033 / 22-9924 the film, increasing pathways for charge transport and thus, dramatically decreasing resistivity. This thickness-dependent resistivity is consistent with that previously reported for ligand-exchanged Ag and Au NC thin films.11,15
[0068] To investigate the energetics and kinetics of the chemically-driven sintering process, we conduct two groups of control experiments by varying the ligand treatment time and Cu NC size, respectively. The ^^^^of 4.5 nm diameter, multilayer Cu NC films, prepared by four sequences of Cu NC spin coating and Cl- treatment, is traced as a function of Cl- treatment time (t) (FIG.8b, blue).60 s of Cl- treatment is sufficient to remove organic ligands following each Cu NC layer deposition (FIG.15b), resulting in continuous films as shown in FIG.8c. However, the ^^^^is still ~3 times higher than the lowest ^^^^found in FIG.8a. As the treatment time is lengthened, ^^^^decreases and reaches its minimum for times longer than 240 s (FIG.8b, blue). We find the measured Rs is well fit by the equation ^^^^( ^^) = ^^^^0+ ^^ / ^^, where ^^^^0= 0.09 ^ / □ is calculated from the bulk Cu resistivity ( ^^^^ ^^ ^^ ^^ ^^ ^^, note: literature values for ^^^^ ^^ ^^ ^^ ^^ ^^= 1.70 × 10−8Ω ^^ is smaller than ^^^^ ^^ ^^ ^^ ^^ ^^= 4.05 × 10−8Ω ^^ measured for a thermally-evaporated Cu film) and A is a constant representing the resistance of grain boundaries52(FIG.8b, dashed line). Therelation is consistent with models relating the resistance of bare metal NC arrays to their NC contact areas.53Therefore, we correlate t to the contact area and thus interfacial resistance between Cu NCs. Corresponding Scanning electron microscopy (SEM) images of Cu NC films show NC coalescence and coarsening with longer Cl- treatment times, leading to a bimodal particle size distribution (FIG.8c) with more, smaller 25.2 ± 3.1 nm and fewer, larger 55.3 ± 3.2 nm grains (FIG.15c). Consistently, powder XRD measurements and Scherrer analysis indicate that the Cu NC grain size increases from 9.4 ± 0.27 nm ( ^^ = 60 ^^) to 21.7 ± 0.33 nm ( ^^ = 240 ^^) (FIG.8d, blue).
[0069] In contrast, thin films of 15.0 nm diameter Cu NCs with the same SCN- and Cl- ligand exchange agents generally exhibit higher ^^^^than those of 4.5 nm diameter Cu NC films at the same thickness (FIG.16a). For Cl--treated, 15.0 nm diameter Cu NC thin films, ^^^^shows a small decrease, significantly less than that for 4.5 nm diameter Cu NCs, even with multi-layer film deposition or extended ligand exchange times. The same ^^^^(^^)equation above fails to describe the small variation in RS (FIG.8b, orange). The Scherrer grain size only slightly increases from 11.3 ± 0.2 nm to 12.1 ± 0.3 nm as the Cl- treatment time is extended from 60 s to 240 s (FIG.8d, orange). Also, the emergence of103241.007033 / 22-9924 large particle aggregation in these 15.0 nm diameter Cu NC films is not as apparent as that in the 4.5 nm diameter NC samples even after 240 s of treatment (FIG.16b). These characterizations corroborate the limited chemically-driven sintering and, hence, higher ^^ of 34.5 × 10−8Ω ^^ for Cl--treated 15.0 nm Cu NC films.
[0070] We incorporate these observations with our earlier Au and Ag NC studies to generalize the mechanism of chemically-driven sintering of metal NCs in closely- packed NC thin-film assemblies.11,15Both the low-resistivity, 4.5 nm diameter, Cl--treated Cu NC films and previous Cl--treated Ag NC films fabricated by multilayer NC deposition and elongated treatment times accompany wider particle size distributions within the NC films (FIG.8c), in comparison to SCN--treated NC films, consistent with grain growth via NC coalescence and Ostwald ripening. Strong NC-ligand bonds, such as Cu-SCN and residual Cu-OLAM, stabilize the surface and limit NC sintering even after treating the 4.5 nm diameter Cu NCs extensively (FIG.17). In contrast, weak NC-ligand bonds facilitate NC sintering. Since the Ag-Cl binding energy is even smaller than Cu-Cl,54,55Cl--treated Ag NCs tend to form isolated micrometer-sized grains, while the sintered Cu particles are still <100 nm. The particle growth rate is proportional to the particle surface energy that decreases with increasing particle size. As the Cu NC diameter increases from 4.5 nm to 15.0 nm, the surface-to-volume ratio as well as the chemical potential decreases, providing a smaller thermodynamic driving force for NC sintering.56Moreover, the fitted and measured RShave a more considerable discrepancy at long chemical treatment times (FIG. 8b), consistent with a slowed sintering rate when the surface energy is released.
[0071] Although the Cu NC dispersions are easily oxidized, their thin films become more air-stable after the ligand exchange treatment.57,58As shown in FIG.8e, the SCN-- and Cl--treated films show less than a 10% increase from their initial ^^^^after being stored in the open air for 60 h. We confirm that the ^^^^increases no more than 2.7 times its original value after eight months of sitting in the air. It's noteworthy that the top surface of the Cu NC films gradually darkens upon transfer from the N2-filled atmosphere of the glovebox to air, while their bottom sides in contact with the substrate maintain highly- reflective, metal-like appearances. This observation is consistent with oxidation starting from the top surface of the films and the thickness-dependent DC resistivity measurements, where the air stability of ^^ is improved for films thicker than 90 nm with103241.007033 / 22-9924 bottom contacts (FIG.18). The oxidized surface layers prevent oxygen from penetrating deeper into the dense ligand-exchanged NC films, maintaining their low resistivity.
[0072] We benchmark the resistivity of our 4.5 nm and 15.0 nm Cu NC films with other Cu nanoparticle-based conductive inks reported in the literature. To keep the ink material consistent, we exclude works on nanoparticles composed of alloys of Cu with other metals. In FIG.8f, we plot the ratio between the ^^ of Cu NC and nanoparticle films to that of ^^^^ ^^ ^^ ^^ ^^ ^^as a function of the sintering temperature and particle diameter. The lowest ^^ of Cl--treated 4.5 nm and 15.0 nm diameter Cu NC films are 3.2 and 20.3 times of ^^^^ ^^ ^^ ^^ ^^ ^^, respectively. The 15.0 nm diameter Cu NC films have resistivities larger than many Cu nanoparticle films sintered at high temperatures, but the 4.5 nm diameter Cu NC films achieve resistivities smaller than many and comparable to the lowest resistivities reported for Cu nanoparticle films involving high-temperature sintering conditions. This comparison suggests that smaller particle sizes advantageously achieve ligand treated films with lower resistivities.
[0073] Table 1. Calculated resistance, capacitance, and Q-factor at a 900 MHz working frequency from equivalent circuit model fitting Q-f Error in Coating Resistance Cap actor Substra acitance admittance method te (Ω) (pF)MHz magnitude (dB) Evap Thermal Cu evaporation21.5 0.62 13.2 0.2 Sample Spin A coating57.2 0.61 5.1 0.1 Sample B Doctor blading glass 63.0 0.61 4.5 0.5 Sample Spin C coating Kapton®74.7 0.31 7.7 0.1
[0074] We exploit the Cu NC inks and the chemically-driven, room temperature sintering of their films to construct, using low-cost and low-temperature processes, low resistivity and biocompatible / biodegradable metal structures for RF devices in IoT103241.007033 / 22-9924 applications. Using a finite element-based electromagnetic solver, we optimize a design for an RF interdigitated capacitive sensor, like those explored in IoT wireless sensing systems for precision agriculture and environmental monitoring.14,59,60The sensors are composed of a single series of interdigitated capacitors with two adjacent ground plane lines, facilitating RF device probing.61All the devices in this section are based on standard photolithographic patterning and spin or doctor-blade coating of 4.5 nm diameter Cu NCs followed by NH4Cl ligand exchange to achieve micron-scale metal structures with the lowest DC resistivity. Three types of samples are created by varying deposition techniques and substrates, respectively. Sample A and B are fabricated on glass, employing spin coating and doctor blading of the NCs, respectively, while sample C is deposited by spin coating on a flexible Kapton®substrate.
[0075] As suggested by the thickness-dependent DC conductivity characteristics above, we compare the effectiveness of spin coating versus doctor-blade coating in forming thick and large-area Cu NC capacitor patterns. For samples A and C, we increase the concentration of the NC ink to 75 mg / mL and spin coat the NC ink at a slower spin speed, to achieve ~100 nm Cu NC layers per deposition and Cl- exchange cycle. For sample B, we use the same NC ink concentration but deposit the NC film by doctor-blade coating, to yield a ~250 nm Cu NC layer thickness per deposition and Cl- exchange cycle. Five consecutive spin coating layers are stacked to reach a film thickness of 490 ± 33 nm for samples A and C, while the doctor-blade coating of sample B is only repeated twice to obtain a 530 ± 28 nm thick film. These sample thicknesses are limited by the thickness of the photoresist layer. FIG.9a illustrates the capacitive structure design composed of 14 fingers, each with lengths and widths of 2500 μm and 100 μm, respectively, spaced by 500 μm. The fabricated capacitor geometries match closely with their designs (FIG.19).
[0076] The admittance parameter (Y12) of the capacitive sensors is measured while varying the AC frequency. The frequency-dependent admittance is fit by an equivalent circuit model (FIG.9c, inset). Three essential elements are included: the equivalent series resistance ( ^^) that reflects electrical losses within the fingers, the self- inductance of the Cu NC lines(^^), and the capacitance of the sensor(^^)that depends on the spacing and dielectric medium between fingers.60,61The fit results for the sensor parameters are detailed in Table 1, with fitting errors below one percent ranging from 0.1103241.007033 / 22-9924 to 0.5 dB, indicating that these devices follow the equivalent circuit model description (FIG.9c). We calculate the self-resonant frequency ^^0of the sensor, defined as:62,63For all devices studied here, the calculated ^^0values exceed 2 GHz. Therefore, in the frequency range of 400 MHz to 1.6 GHz shown in FIG.9c, d, the Cu NC devices are dominated by capacitive and resistive behavior, suitable for sensor operation. At frequencies beyond ^^0, inductance dominates the sensor impedance, causing it to deviate from its capacitive behavior (FIG.20).
[0077] As listed in Table 1, samples A and B show capacitances of ~0.6 pF, close to that of evaporated Cu devices (FIG.9c). These results confirm the compatibility of solution-deposited Cu NC inks and the utility of doctor-blade coating to achieve thick metallic traces for RF device fabrication. We also observe a higher equivalent resistance of ~60 Ω from the Cu NC samples compared to ~20 Ω of an evaporated Cu device. The ratio of their equivalent resistances is consistent with the ratio of their thin film ^^ found in DC measurements (FIG.2f). Altering the substrate material from glass (sample A) to a 0.125 mm thick Kapton®film (sample C) decreases the substrate dielectric constant from 7.1 to 3.4. Sample C has a more negative admittance amplitude at all frequencies and a two-fold smaller capacitance, consistent with the factor of two smaller dielectric function compared to that for sample A fabricated on a glass substrate (FIG.9c, Table 2).
[0078] The Q-factor is a measure of how efficiently energy is stored without loss in a resonant circuit at working frequencies and is defined as:
[0079] FIG.3d shows the frequency-dependent Q-factor calculated including the 902-928 MHz industrial, scientific, and medical (ISM) band, using the equivalent circuit model fitting of the admittance measurements.64The Cu NC-based samples A, B, and C have Q-factors of 5.1, 4.5, and 7.7, respectively. Although still lower than that of the evaporated Cu sample (Q=13.2), these performances are comparable to previous reports of capacitive sensors fabricated using commercial Ag conductive inks.59,64Notably, the capacitor fabricated on Kapton®substrates exhibits the highest Q-factor, suggesting the potential advantage of employing low dielectric constant substrates that can also provide flexible form factors.103241.007033 / 22-9924
[0080] We also integrate the Cu NC inks and ligand-exchange treatments of their thin films to create NC materials with designer dielectric permittivity at optical frequencies, with which we fabricate optical metasurfaces of interest as low-cost optical components and biodegradable / biocompatible optical sensors. We use 4.5 nm diameter Cu NC dispersions (25 mg / mL) and deposit NC films by two sequences of spin coating followed by 90 s of NH4SCN or NH4Cl ligand exchange. We carry out spectroscopic ellipsometry measurements (see Methods) to characterize the dielectric permittivity of Cu NC films after the SCN- and Cl- chemical treatments at optical wavelengths (FIG.10a and b). The real part of the permittivity (ε1) of both SCN-- and Cl--treated Cu NC films decreases as the wavelength λ increases, like that of evaporated Cu. Unlike evaporated Cu, ε1is less negative for the SCN-- and Cl--treated Cu NC films, as there are fewer atoms to contribute electrons to the films and the NC films are better described as diluted metals.65,66The imaginary part of the permittivity (ε2) for the Cl-- and SCN--treated Cu NC films is lower in magnitude than that for evaporated Cu through the visible to NIR spectral region studied, consistent with lower absorption loss.23,67The spectral feature around 600 nm matches with the dip in transmittance spectra (FIG.7g) and is attributed to interband absorption in Cu. We estimate the carrier concentration (n) and scattering time (τ) of these samples using the Drude model description of dielectric function as:
[0081] where m0is the effective mass of the electron, ^^0is the vacuumpermittivity, ^^ is frequency, and where 68– ^^0^^0= ^^^^is known as the plasmon frequency.71At wavelengths longer than that of the interband transition of Cu and for materials with ^^ ^^ ≫ 1, ^^1and ^^2can be simplified and approximated as functions ^^ with slopes related to ^^^^and τ.70,71By simultaneously fitting the simplified ^^1and ^^2, we estimate ^^^^ ^^ ^^ ^^ ^^ ^^= 7.94 ± 2.01 × 1022cm-3and ^^^^ ^^− ^^ ^^= 2.31 ± 1.05 × 1022cm-3and ^^^^ ^^ ^^ ^^ ^^ ^^= 1.57 ± 0.362.01 ± 0.42 × 10−14^^ (FIG.21 and Table 3). For evaporated Cu and Cl--treated NC thin films, ^^ ^^ satisfies the assumption required to make the approximation. The electron mobility(^^)can be calculated from τ and together with ^^, we calculate ^^ using Ohm’s law, to find ^^^^ ^^ ^^ ^^ ^^ ^^and ^^^^ ^^− ^^ ^^at 2.84 ± 0.73 × 10−8103241.007033 / 22-9924 Ω ^^ and 7.64 ± 1.94 × 10−8Ω m, respectively. The relative ^^^^ ^^ ^^ ^^ ^^ ^^and ^^^^ ^^− ^^ ^^to ^^^^ ^^ ^^ ^^ ^^ ^^is similar to that found in DC measurements (FIG.2f). However, ^^ extracted for the SCN--treated Cu NC films is too short and thus does not satisfy the ^^ ^^ ≫ 1 requirement for the approximation in our wavelength range of measurement, and thus is unsuitable to be used for calculating ^^^^ ^^− ^^ ^^ ^^. The ε1of SCN--treated Cu NC films decreases gently and becomes negative at wavelengths longer than the crossover wavelength of 1030 nm, consistent with a dielectric to metal transition at longer wavelengths. We plot − ^^1 / ^^2and ^^1 / ^^2(FIG.21c, d), figures of merit often used to characterize materials for localized surface plasmon- and hyperbolic-based metasurfaces, respectively.
[0082] We integrate the Cu NC inks and the ligand-exchange treatments of their thin films with nanoimprint lithography (see Methods) to pattern 1.5 mm by 1.5 mm arrays of subwavelength, nanoscale NC superstructures and demonstrate optical metasurfaces, as reported previously to fabricate Au and Ag NC-based optical metasurfaces. The metasurface is designed to resonate in the NIR, beyond the crossover wavelength of SCN--treated Cu NC films and is composed of square nanostructures with a side length of 350 nm arrayed at a pitch of 800 nm. SEM images of an example Cl--treated Cu NC metasurface show that the fabricated arrays are square shaped with 381.3 ± 17.5 nm side lengths on a 744.2 ± 22.9 nm pitch (FIG.10c). AFM height profiles show the Cl-- treated Cu NC superstructures have a thickness of 238.1 ± 9.1 nm at the edges and 191.1 ± 4.0 nm in the center, consistent with a “rabbit ear” effect (FIG.22), previously seen in Au NC optical metasurfaces.72
[0083] The SCN--treated Cu NC metasurface resonates near 1360 nm, whereas the Cl--treated Cu NC metasurface with the same structure resonates at around 1330 nm (FIG.10d, left). The resonance peak of the Cl--treated sample is normalized to between 1 and 0 intensity, and the resonance of SCN--treated sample is normalized to that of the Cl- sample to make a direct comparison. The Cl--treated Cu NC metasurface show a sharper and stronger resonance. The difference in the optical properties of the NC metasurfaces arises from the greater metallicity of the Cl--treated NC films, i.e., their higher electron density and thus more negative ε1. Simulations carried out using the dielectric permittivity of the differently-treated Cu NC films reproduce our experimental measurements (FIG. 10d, right), showing the metasurface resonance blue shifts, sharpens, and strengthens for103241.007033 / 22-9924 the Cl- in comparison to the SCN- ligand treatment. Differences in the resonance wavelength between the experimental and simulated spectra are consistent with variations in the size, shape, roughness, and pitch of the fabricated and idealized NC-based structures.73
[0084] In conclusion, we report highly conductive Cu NC films based on the deposition of colloidal Cu NC inks and room-temperature chemical sintering. We achieve DC and optical resistivities as low as ~3 times that of bulk Cu by using small 4.5 nm diameter Cu NCs and Cl- ligand exchange reagent. We showcase the successful integration of these high conductivity Cu NC films in devices. We fabricate micron-scale RF devices operating in the 902-928 MHz ISM band with capacitances similar to those of thermally- evaporated Cu devices and with Q-factors comparable to those reported using Ag NC inks. We also fabricate optical metasurfaces with plasmon resonances in the NIR. The solution- based deposition of Cu NC inks and the room-temperature, environmentally benign, and non-corrosive chemically-driven sintering of their films promises to enable further research to create devices that meet application specific needs, including the scalable and low-cost manufacturing of IoT sensors and the integration of conductors on flexible, low- thermal resistance, and biocompatible / biodegradable substrates, including a wider range of polymers and papers.
[0085] Methods
[0086] Synthesis of Colloidal Cu NCs: 4.5 nm (15.0 nm) diameter colloidal Cu NCs are synthesized following previous reports.1In a three-neck flask, 0.9 g of copper (II) formate tetrahydrate (98%, Thermo Scientific Chemicals) is dissolved in a mixture of 10 mL (6 mL) oleylamine (technical grade, 70%, Sigma Aldrich) and 10 mL (14 mL) anhydrous dodecane (≥99%, Sigma Aldrich). Prior to initiating the reaction, the flask is pre-heated to 60 °C and degassed for 1 h. The temperature is then increased to 140 °C for 10 min under N2 flow, and at approximately 115 °C the reaction rapidly changes color from light blue to dark brown. The reaction product is transferred to a N2-filled glovebox where it is divided equally into three centrifuge tubes.3.5 mL of hexane (≥99%, Sigma Aldrich) is added to each tube. The samples are firstly centrifuged at 6000 RPM for 5 min to remove unreacted precursors from the precipitant.30 mL of acetone (99.8%, Thermo Scientific Chemicals) and 0.5 mL of nitrosyl tetrafluoroborate in acetonitrile is added to the supernatant of each tube to drive flocculation. The samples are centrifuged at 6000103241.007033 / 22-9924 RPM for 20 min to accumulate precipitated Cu NCs at the tube bottom. The supernatant is decanted and the NCs are dispersed in 10 mL hexane. This purification process is repeated three times.
[0087] Preparation and Structural, Optical, and DC Electrical Characterization of Cu NC Thin Films: Test-grade single-side-polished (SSP) Si wafers (4” P-type, <100>, 1- 25 ^-cm; 475-575 µm thick, NOVA,Inc), device-grade SSP thermally-oxidized Si wafers (4” N-type, <100>, ≤0.005 ^-cm; 500±25 µm / 250±25 µm Si / SiO2thickness Virginia Semiconductor, Inc.), prime-grade double-side-polished (DSP) Si wafers (4” N-type, <100>, 50-70 ^-cm; 500±25 µm thick , NOVA, Inc.), and boroaluminosilicate glass pieces (1.1 mm thick, Delta Technologies) are used as substrates for structural, optical, and DC resistivity measurements. Each substrate is cleaved or cut into 1” by 1” Si wafer pieces or glass pieces, cleaned by UV-ozone treatment for 30 min, and immersed overnight in a 5% solution of 3-mercaptopropyltrimethoxysilane (MPTS) in toluene. Cu NC dispersions in hexane with concentrations ranging from 25 mg / mL to 50 mg / mL, selected for different measurements, are deposited by spin coating at 1500 RPM for 60 s. 50 mM solutions of the SCN- ligand are prepared by mixing 78 mg recrystallized NH4SCN (>99%, ACROS) and 20 mL of methanol (>99.9%, Sigma Aldrich).50 mM Cl- ligand solutions are prepared by mixing 54 mg of NH4Cl (>99%, Sigma Aldrich) with 20 mL of methanol. Similarly, methanolic solutions of Na2S and NaN3 are both prepared at 50 mM concentration. The selected ligand solution is dispensed onto the samples, and after 240 s, removed by spinning at 4000 RPM for 10 s. Methanol is then dispensed on the sample and spin dried on the spin coater to remove residual ligand reagents. The NC spin coating and ligand exchange processes are repeated sequentially to stack multiple layers of Cu NCs until the desired film thickness is achieved.
[0088] A JEOL JEM-1400 transmission electron microscope (TEM) operating at 120 keV and a JEOL 7500F high-resolution scanning electron microscope (HRSEM) are used to image the Cu NC films. Colloidal NC thin-film assemblies for TEM imaging are prepared from 25 mg / mL Cu NC dispersions on carbon-coated copper grids using one repetition of spin coating and ligand exchange. SEM imaging is performed on SSP test- grade wafers using varying numbers of repetitions of spin coating for different thicknesses and varying lengths of ligand exchange time.103241.007033 / 22-9924
[0089] A Rigaku Smartlab high-resolution diffractometer with Cu Kα radiation (λ = 0.15416 nm, 45 mA, 40 kV) operating with a resolution of 0.05° / 2θ and a scan speed of 5.0° / min is used to collect x-ray diffraction (XRD) patterns. Cu NC thin films are prepared by spin coating 50 mg / mL dispersions on SSP test-grade Si wafers. Films are formed by three repetitions of spin coating and ligand exchange.
[0090] AFM measurements of film thickness are measured using an MFP-3D- BIO microscope (Asylum Research Corp.) with an AC240TS silicon cantilever (Olympus). Film thicknesses reported are an average of three identically prepared samples. The samples are prepared on SSP test-grade Si wafers with varying numbers of repetitions of deposition and ligand exchange to characterize films of different thicknesses. The concentration of the Cu NC dispersion is 25 mg / mL.
[0091] Optical transmittance data of the Cu NC thin films are collected using a Cary UV-Vis-NIR spectrophotometer from Agilent Technologies. Samples are prepared on glass substrates using three repetitions of Cu NC spin coating and ligand exchange. Fourier Transform Infrared Spectroscopy (FTIR) absorption data are collected using a NICOLET iS50 FT-IR from Thermo Scientific. Samples are prepared on prime grade DSP Si wafers using three repetitions of spin coating and ligand exchange with a 25mg / mL Cu NC dispersion.
[0092] The wavelength-dependent dielectric constants of Cu NC and evaporated Cu films are measured by using a J. A. Woollam V-Vase Spectroscopic Ellipsometer, across a wavelength range from 300 nm to 1100 nm. Data from each sample is collected at three angles (55°, 65°, and 75°) and fitted by the three-parameter Cauchy model on the J. A. Woollam CompleteEASE software. In all fitting, mean square error values are lower than 10.
[0093] Four-point probe DC resistivity measurements are carried out for samples prepared on device grade SSP Si wafers. Four-point probe (4pp) electrodes composed of a bilayer of 3 nm Cr and 60 nm Au are thermally evaporated through a shadow mask with 3 mm spacing. Varying numbers of repetitions of Cu NC spin coating and solid-state ligand exchange are carried out using 30 mg / mL NC dispersions to prepare different thickness films. A cotton swab dipped in acetone is used to gently wipe off Cu NCs from the electrode areas. Four PH110 micromanipulators from Formfactor with 7B Tungsten probe103241.007033 / 22-9924 tips from Micromanipulator are used to make contact to each electrode for 4pp sheet resistance measurements.
[0094] Fabrication and Characterization of RF Devices: Glass substrates are cut into 4” by 4” pieces, cleaned by sonicating in IPA for 5 min and acetone for 5 min, UV- ozone treatment for 30 min, and modified by 3-MPTS. Kapton substrates (125 μm thickness, DuPont) are similarly cut to 4” by 4”, and the same procedure is used except for the 3-MPTS treatment. The photolithography resist LOR 20C (Microchem) is deposited by spin coating at 500 RPM for 5 s and then at 2000 RPM for 45 s. The sample is baked at 180 °C for 5 min. Resist S1818 (Microchem) is then deposited by spin-coating at 500 RPM for 5 s and then at 4000 RPM for 45 s. The sample is baked again at 115 °C for 1 min. A Heidelberg DWL 66+ Laser Writer with exposure wavelength 405 nm is used to pattern the resist according to the RF capacitor design (185 mW, 50% optical filter, 70% intensity, 2 repetitions). The sample is immersed in MF-26A for 90 s and then hard-baked at 140 °C for 5 min. A 0.5 by 0.5 mm bilayer of 5 nm Cr and 12 nm Au contact pads are thermally evaporated through a shadow mask to connect to the capacitor structure and ensure a stable contact between probes and the device.75 mg / mL Cu NC inks are deposited by either spin coating (spin speed 500 RPM, 5 repetitions) or doctor-blading coating (blading speed ~10 cm / s, 2 repetitions) followed by 240 s of Cl- ligand exchange. For the doctor-blade coating, a Micrometer Adjustable Film Applicator (50 mm width, MTI) is used. The sample is immersed in PG remover (Kayaku) for 15 min to lift-off the resist and then methanol is dispensed on the sample followed by spin drying on the spin coater for three times. RF devices are characterized in air using a probe station with ground-signal-ground (GSG) RF probes (Formfactor) at a 550 µm pitch. A Keysight P9374A vector network analyzer (VNA), calibrated to the probe tips using the well- established short-open-load-through (SOLT) method and employing a dedicated calibration set, is used to measure the frequency-dependent device admittance.
[0095] Fabrication, Characterization, and Simulation of Optical Metasurfaces: 1.5” by 1.5” pieces of glass are cleaned by sonicating in IPA for 5 min and acetone for 5 min, UV-ozone treatment for 30 min, and modified using 3-MPTS. PMGI SF5 (Microchem) is deposited by spin coating on the wafers at 2000 RPM for 60 s and then baked on a hotplate at 180 °C for 3 min. Nanonex-1025, 7% is deposited by spin coating at 2000 RPM for 60 s and then baked at 155 °C for 1 min. Nanoimprinting is performed at103241.007033 / 22-9924 155 °C and 350 psi for 330 s using a Nanonex NX2600 Nanoimprint / Mask Aligner with a template previously patterned by electron-beam lithography. After imprinting, a 15s O2 plasma descum process (1 Torr, 25 W) is performed using an Oxford Instruments Plasma Lab 80+ RIE to expose the PMGI layer. The samples are developed by immersion in MF- 26A developer solution (Microchem) for 7 s. Two repetitions of Cu NC deposition from 25 mg / mL NC dispersions and ligand exchange are used to achieve approximately 200 nm thick NC-based superstructures after 90 s of SCN- and Cl- ligand exchange. The confinement effect of the photoresist layer results in a thicker film for the Cu NC metasurface compared to large area Cu NC thin films. Samples are sonicated in acetone for 10 s and then immersed in 1-Methyl-2-pyrrolidone (NMP, Sigma Aldrich) for 1 min to lift-off the resist. The samples are then rinsed with IPA. Optical transmittance data are collected in the FTIR and the patterned metasurfaces are structurally characterized by AFM and HRSEM, using the procedures described above.
[0096] FDTD simulations are carried out using Lumerical simulation software to design the Cu NC metasurfaces such that they resonate in the NIR. Simulations are conducted using periodic boundary conditions, a mesh size of 5 nm, and the measured dielectric function of the SCN- and Cl--treated Cu NC films.
[0097] Table 2 Thickness measured by atomic force microscopy (AFM)
[0098] of 4.5 nm diameter Cu NC films prepared by spin coating 30 mg / mL NC dispersions with Cl- and SCN- ligand treatment for 240 s Number of spin coating Film thickness Film thickness layers with SCN- ligand with Cl- ligand treatment treatment (nm) (nm) 1 50.5 ± 3.2 57.7 ± 4.6 3 149.3 ± 4.9 120.2 ± 3.2 5 255.2 ± 7.5 160.1 ± 5.5 7 347.9 ± 10.8 178.7 ± 8.2 Description of the fitting procedure. 12 To estimate n from the dispersion, we plotagainst ^^ (FIG.21a). Knowing ^^ =2π ^^ = as the speed of light, we can approximate the slope of the −− ^^ ^^ ^^ curve a The ^^ value is extracted by plotting the slope of ^^^^− ^^ as^^^^^^^^^^ ∝ ^^. (FIG.103241.007033 / 22-9924 Table 3 The calculated material properties from fitting dielectric function sample Electron Scattering time Resistivity concentration τ (s) ρ ( ^^ ^^) -3 n (cm ) Evaporated Cu7.96 × ^^ ^^^^ ^^1.57 × ^^ ^^− ^^ ^^2.84 × ^^ ^^− ^^- SCN -treated Cu 2.91 × ^^ ^^^^ ^^8.20 × ^^ ^^− ^^ ^^1.49 × ^^ ^^− ^^NCs* - Cl -treated Cu 2.31 × ^^ ^^^^ ^^2.01 × ^^ ^^− ^^ ^^7.64 × ^^ ^^− ^^NCs * For the SCN--treated Cu NC film, it does not satisfy ^^ ^^ ≫ 1, and therefore, unsuitable for the approximation.
[0099] References
[0100] (1) Asghari, P.; Rahmani, A. M.; Javadi, H. H. S. Internet of Things Applications: A Systematic Review. Computer Networks 2019, 148, 241–261. https: / / doi.org / https: / / doi.org / 10.1016 / j.comnet.2018.12.008.
[0101] (2) Xu, L. D.; He, W.; Li, S. Internet of Things in Industries: A Survey. IEEE Trans Industr Inform 2014, 10 (4), 2233–2243. https: / / doi.org / 10.1109 / TII.2014.2300753.
[0102] (3) Din, I. U.; Guizani, M.; Hassan, S.; Kim, B.-S.; Khan, M. K.; Atiquzzaman, M.; Ahmed, S. H. The Internet of Things: A Review of Enabled Technologies and Future Challenges. IEEE Access 2019, 7, 7606–7640. https: / / doi.org / 10.1109 / ACCESS.2018.2886601.
[0103] (4) Kagan, C. R.; Arnold, D. P.; Allen, M. G.; Olsson, R. H. IoT4Ag: MEMS-Enabled Distributed Sensing, Communications, And Information Systems for The Internet Of Things For Precision Agriculture. In 2021 IEEE 34th International Conference on Micro Electro Mechanical Systems (MEMS); 2021; pp 350–353. https: / / doi.org / 10.1109 / MEMS51782.2021.9375346.
[0104] (5) Portilla, L.; Loganathan, K.; Faber, H.; Eid, A.; Hester, J. G. D.; Tentzeris, M. M.; Fattori, M.; Cantatore, E.; Jiang, C.; Nathan, A.; Fiori, G.; Ibn- Mohammed, T.; Anthopoulos, T. D.; Pecunia, V. Wirelessly Powered Large-Area103241.007033 / 22-9924 Electronics for the Internet of Things. Nat Electron 2023, 6 (1), 10–17. https: / / doi.org / 10.1038 / s41928-022-00898-5.
[0105] (6) Abdolmaleki, H.; Kidmose, P.; Agarwala, S. Droplet-Based Techniques for Printing of Functional Inks for Flexible Physical Sensors. Advanced Materials 2021, 33 (20), 2006792. https: / / doi.org / https: / / doi.org / 10.1002 / adma.202006792.
[0106] (7) Kagan, C. R. At the Nexus of Food Security and Safety: Opportunities for Nanoscience and Nanotechnology. ACS Nano. American Chemical Society March 22, 2016, pp 2985–2986. https: / / doi.org / 10.1021 / acsnano.6b01483.
[0107] (8) Shi, Q.; Yang, Y.; Sun, Z.; Lee, C. Progress of Advanced Devices and Internet of Things Systems as Enabling Technologies for Smart Homes and Health Care. ACS Materials Au. American Chemical Society July 13, 2022, pp 394–435. https: / / doi.org / 10.1021 / acsmaterialsau.2c00001.
[0108] (9) Dai, X.; Xu, W.; Zhang, T.; Shi, H.; Wang, T. Room Temperature Sintering of Cu-Ag Core-Shell Nanoparticles Conductive Inks for Printed Electronics. Chemical Engineering Journal 2019, 364, 310–319. https: / / doi.org / 10.1016 / j.cej.2019.01.186.
[0109] (10) Dai, X.; Zhang, T.; Shi, H.; Zhang, Y.; Wang, T. Reactive Sintering of Cu Nanoparticles at Ambient Conditions for Printed Electronics. ACS Omega 2020, 5 (22), 13416–13423. https: / / doi.org / 10.1021 / acsomega.0c01678.
[0110] (11) Fafarman, A. T.; Hong, S. H.; Oh, S. J.; Caglayan, H.; Ye, X.; Diroll, B. T.; Engheta, N.; Murray, C. B.; Kagan, C. R. Air-Stable, Nanostructured Electronic and Plasmonic Materials from Solution-Processable, Silver Nanocrystal Building Blocks. ACS Nano 2014, 8 (3), 2746–2754. https: / / doi.org / 10.1021 / nn406461p.
[0111] (12) Pardo, D. A.; Jabbour, G. E.; Peyghambarian, N. Application of Screen Printing in the Fabrication of Organic Light-Emitting Devices. Advanced Materials 2000, 12 (17), 1249–1252. https: / / doi.org / 10.1002 / 1521-4095(200009)12:17<1249::AID- ADMA1249>3.0.CO;2-Y.
[0112] (13) Li, Z.; Chang, S.; Khuje, S.; Ren, S. Recent Advancement of Emerging Nano Copper-Based Printable Flexible Hybrid Electronics. ACS Nano. American Chemical Society April 27, 2021, pp 6211–6232. https: / / doi.org / 10.1021 / acsnano.1c02209.103241.007033 / 22-9924
[0113] (14) Oh, H.; Lee, S. W.; Kim, M.; Lee, W. S.; Seong, M.; Joh, H.; Allen, M. G.; May, G. S.; Bakir, M. S.; Oh, S. J. Designing Surface Chemistry of Silver Nanocrystals for Radio Frequency Circuit Applications. ACS Appl Mater Interfaces 2018, 10 (43), 37643–37650. https: / / doi.org / 10.1021 / acsami.8b12005.
[0114] (15) Fafarman, A. T.; Hong, S. H.; Caglayan, H.; Ye, X.; Diroll, B. T.; Paik, T.; Engheta, N.; Murray, C. B.; Kagan, C. R. Chemically Tailored Dielectric-to- Metal Transition for the Design of Metamaterials from Nanoimprinted Colloidal Nanocrystals. Nano Lett 2013, 13 (2), 350–357. https: / / doi.org / 10.1021 / nl303161d.
[0115] (16) Mo, L.; Guo, Z.; Yang, L.; Zhang, Q.; Fang, Y.; Xin, Z.; Chen, Z.; Hu, K.; Han, L.; Li, L. Silver Nanoparticles Based Ink with Moderate Sintering in Flexible and Printed Electronics. Int J Mol Sci 2019, 20 (9). https: / / doi.org / 10.3390 / ijms20092124.
[0116] (17) Zhang, Z.; Zhang, X.; Xin, Z.; Deng, M.; Wen, Y.; Song, Y. Synthesis of Monodisperse Silver Nanoparticles for Ink-Jet Printed Flexible Electronics. Nanotechnology 2011, 22 (42). https: / / doi.org / 10.1088 / 0957-4484 / 22 / 42 / 425601.
[0117] (18) Link, S.; El-Sayed, M. A. Shape and Size Dependence of Radiative, Non-Radiative and Photothermal Properties of Gold Nanocrystals. International Reviews in Physical Chemistry.2000, pp 409–453. https: / / doi.org / 10.1080 / 01442350050034180.
[0118] (19) Magdassi, S.; Bassa, A.; Vinetsky, Y.; Kamyshny, A. Silver Nanoparticles as Pigments for Water-Based Ink-Jet Inks. Chemistry of Materials 2003, 15 (11), 2208–2217. https: / / doi.org / 10.1021 / cm021804b.
[0119] (20) Cui, W.; Lu, W.; Zhang, Y.; Lin, G.; Wei, T.; Jiang, L. Gold Nanoparticle Ink Suitable for Electric-Conductive Pattern Fabrication Using in Ink-Jet Printing Technology. Colloids Surf A Physicochem Eng Asp 2010, 358 (1–3), 35–41. https: / / doi.org / 10.1016 / j.colsurfa.2010.01.023.
[0120] (21) Redinger, D.; Molesa, S.; Yin, S.; Farschi, R.; Subramanian, V. An Ink-Jet-Deposited Passive Component Process for RFID. IEEE Trans Electron Devices 2004, 51 (12), 1978–1983. https: / / doi.org / 10.1109 / TED.2004.838451.
[0121] (22) Levard, C.; Hotze, E. M.; Lowry, G. V.; Brown, G. E. Environmental Transformations of Silver Nanoparticles: Impact on Stability and Toxicity. Environmental Science and Technology. July 3, 2012, pp 6900–6914. https: / / doi.org / 10.1021 / es2037405.103241.007033 / 22-9924
[0122] (23) Abhinav K, V.; Rao R, V. K.; Karthik, P. S.; Singh, S. P. Copper Conductive Inks: Synthesis and Utilization in Flexible Electronics. RSC Advances. Royal Society of Chemistry 2015, pp 63985–64030. https: / / doi.org / 10.1039 / c5ra08205f.
[0123] (24) Tsai, C. Y.; Chang, W. C.; Chen, G. L.; Chung, C. H.; Liang, J. X.; Ma, W. Y.; Yang, T. N. A Study of the Preparation and Properties of Antioxidative Copper Inks with High Electrical Conductivity. Nanoscale Res Lett 2015, 10 (1). https: / / doi.org / 10.1186 / s11671-015-1069-y.
[0124] (25) Kanzaki, M.; Kawaguchi, Y.; Kawasaki, H. Fabrication of Conductive Copper Films on Flexible Polymer Substrates by Low-Temperature Sintering of Composite Cu Ink in Air. ACS Appl Mater Interfaces 2017, 9 (24), 20852–20858. https: / / doi.org / 10.1021 / acsami.7b04641.
[0125] (26) Zhang, Y.; Zhu, P.; Li, G.; Zhao, T.; Fu, X.; Sun, R.; Zhou, F.; Wong, C. P. Facile Preparation of Monodisperse, Impurity-Free, and Antioxidation Copper Nanoparticles on a Large Scale for Application in Conductive Ink. ACS Appl Mater Interfaces 2014, 6 (1), 560–567. https: / / doi.org / 10.1021 / am404620y.
[0126] (27) Hoeng, F.; Denneulin, A.; Bras, J. Use of Nanocellulose in Printed Electronics: A Review. Nanoscale. Royal Society of Chemistry July 21, 2016, pp 13131– 13154. https: / / doi.org / 10.1039 / c6nr03054h.
[0127] (28) Macdonald, W. A. Latest Advances in Substrates for Flexible Electronics. In Large Area and Flexible Electronics; wiley, 2015; pp 291–314. https: / / doi.org / 10.1002 / 9783527679973.ch10.
[0128] (29) Sun, Y.; Rogers, J. A. Inorganic Semiconductors for Flexible Electronics. Advanced Materials. August 3, 2007, pp 1897–1916. https: / / doi.org / 10.1002 / adma.200602223.
[0129] (30) Tewary, A.; Kekatpure, R. D.; Brongersma, M. L. Controlling Defect and Si Nanoparticle Luminescence from Silicon Oxynitride Films with CO 2 Laser Annealing. Appl Phys Lett 2006, 88 (9). https: / / doi.org / 10.1063 / 1.2178769.
[0130] (31) Dhas, N. A.; Raj, C. P.; Gedanken, A. Synthesis, Characterization, and Properties of Metallic Copper Nanoparticles; 1998. https: / / pubs.acs.org / sharingguidelines.
[0131] (32) Loh, J. Y. Y.; Safari, M.; Mao, C.; Viasus, C. J.; Eleftheriades, G. V.; Ozin, G. A.; Kherani, N. P. Near-Perfect Absorbing Copper Metamaterial for Solar103241.007033 / 22-9924 Fuel Generation. Nano Lett 2021, 21 (21), 9124–9130. https: / / doi.org / 10.1021 / acs.nanolett.1c02886.
[0132] (33) Xiong, K.; Tordera, D.; Emilsson, G.; Olsson, O.; Linderhed, U.; Jonsson, M. P.; Dahlin, A. B. Switchable Plasmonic Metasurfaces with High Chromaticity Containing Only Abundant Metals. Nano Lett 2017, 17 (11), 7033–7039. https: / / doi.org / 10.1021 / acs.nanolett.7b03665.
[0133] (34) Falade, O. P.; Jilani, S. F.; Ahmed, A. Y.; Wildsmith, T.; Reip, P.; Rajab, K. Z.; Alomainy, A. Design and Characterisation of a Screen-Printed Millimetre- Wave Flexible Metasurface Using Copper Ink for Communication Applications. Flexible and Printed Electronics 2018, 3 (4). https: / / doi.org / 10.1088 / 2058-8585 / aaf0eb.
[0134] (35) Falade, O. P.; Jilani, S. F.; Ahmed, A. Y.; Wildsmith, T.; Reip, P.; Rajab, K. Z.; Alomainy, A. Design and Characterisation of a Screen-Printed Millimetre- Wave Flexible Metasurface Using Copper Ink for Communication Applications. Flexible and Printed Electronics 2018, 3 (4). https: / / doi.org / 10.1088 / 2058-8585 / aaf0eb.
[0135] (36) Oliva-Puigdomènech, A.; De Roo, J.; Kuhs, J.; Detavernier, C.; Martins, J. C.; Hens, Z. Ligand Binding to Copper Nanocrystals: Amines and Carboxylic Acids and the Role of Surface Oxides. Chemistry of Materials 2019, 31 (6), 2058–2067. https: / / doi.org / 10.1021 / acs.chemmater.8b05107.
[0136] (37) Oliva-Puigdomènech, A.; De Roo, J.; Van Avermaet, H.; De Buysser, K.; Hens, Z. Scalable Approaches to Copper Nanocrystal Synthesis under Ambient Conditions for Printed Electronics. ACS Appl Nano Mater 2020, 3 (4), 3523– 3531. https: / / doi.org / 10.1021 / acsanm.0c00242.
[0137] (38) Andres, R. P.; Bielefeld, J. D.; Henderson, J. I.; Janes, D. B.; Kolagunta, V. R.; Kubiak, C. P. Self-Assembly of a Two-Dimensional Superlattice of Molecularly Linked Metal Clusters; 1996. http: / / www.sciencemag.org.proxy.library.upenn.edu / .
[0138] (39) Choi, Y. C.; Lee, J.; Ng, J. J.; Kagan, C. R. Surface Engineering of Metal and Semiconductor Nanocrystal Assemblies and Their Optical and Electronic Devices. Acc Chem Res 2023, 56 (13), 1791–1802. https: / / doi.org / 10.1021 / acs.accounts.3c00147.103241.007033 / 22-9924
[0139] (40) Dai, X.; Xu, W.; Zhang, T.; Wang, T. Self-Reducible Cu Nanoparticles for Conductive Inks. Ind Eng Chem Res 2018, 57 (7), 2508–2516. https: / / doi.org / 10.1021 / acs.iecr.7b04248.
[0140] (41) Biesinger, M. C.; Lau, L. W. M.; Gerson, A. R.; Smart, R. S. C. Resolving Surface Chemical States in XPS Analysis of First Row Transition Metals, Oxides and Hydroxides: Sc, Ti, V, Cu and Zn. Appl Surf Sci 2010, 257 (3), 887–898. https: / / doi.org / 10.1016 / j.apsusc.2010.07.086.
[0141] (42) Chung, K.; Bang, J.; Thacharon, A.; Song, H. Y.; Kang, S. H.; Jang, W. S.; Dhull, N.; Thapa, D.; Ajmal, C. M.; Song, B.; Lee, S. G.; Wang, Z.; Jetybayeva, A.; Hong, S.; Lee, K. H.; Cho, E. J.; Baik, S.; Oh, S. H.; Kim, Y. M.; Lee, Y. H.; Kim, S. G.; Kim, S. W. Non-Oxidized Bare Copper Nanoparticles with Surface Excess Electrons in Air. Nat Nanotechnol 2022, 17 (3), 285–291. https: / / doi.org / 10.1038 / s41565-021- 01070-4.
[0142] (43) Fafarman, A. T.; Koh, W. K.; Diroll, B. T.; Kim, D. K.; Ko, D. K.; Oh, S. J.; Ye, X.; Doan-Nguyen, V.; Crump, M. R.; Reifsnyder, D. C.; Murray, C. B.; Kagan, C. R. Thiocyanate-Capped Nanocrystal Colloids: Vibrational Reporter of Surface Chemistry and Solution-Based Route to Enhanced Coupling in Nanocrystal Solids. J Am Chem Soc 2011, 133 (39), 15753–15761. https: / / doi.org / 10.1021 / ja206303g.
[0143] (44) Chan, G. H.; Zhao, J.; Hicks, E. M.; Schatz, G. C.; Van Duyne, R. P. Plasmonic Properties of Copper Nanoparticles Fabricated by Nanosphere Lithography. Nano Lett 2007, 7 (7), 1947–1952. https: / / doi.org / 10.1021 / nl070648a.
[0144] (45) Khanna, P. K.; Gaikwad, S.; Adhyapak, P. V.; Singh, N.; Marimuthu, R. Synthesis and Characterization of Copper Nanoparticles. Mater Lett 2007, 61 (25), 4711–4714. https: / / doi.org / 10.1016 / j.matlet.2007.03.014.
[0145] (46) Johnson, P. B.; Christy, R. W. Optical Constants of the Noble Metals. Phys Rev B 1972, 6 (12), 4370–4379. https: / / doi.org / 10.1103 / PhysRevB.6.4370.
[0146] (47) Li, W.; Li, W.; Wei, J.; Tan, J.; Chen, M. Preparation of Conductive Cu Patterns by Directly Writing Using Nano-Cu Ink. Mater Chem Phys 2014, 146 (1–2), 82–87. https: / / doi.org / 10.1016 / j.matchemphys.2014.02.045.
[0147] (48) Jeong, S.; Song, H. C.; Lee, W. W.; Lee, S. S.; Choi, Y.; Son, W.; Kim, E. D.; Paik, C. H.; Oh, S. H.; Ryu, B. H. Stable Aqueous Based Cu Nanoparticle Ink103241.007033 / 22-9924 for Printing Well-Defined Highly Conductive Features on a Plastic Substrate. Langmuir 2011, 27 (6), 3144–3149. https: / / doi.org / 10.1021 / la104136w.
[0148] (49) Kanzaki, M.; Kawaguchi, Y.; Kawasaki, H. Fabrication of Conductive Copper Films on Flexible Polymer Substrates by Low-Temperature Sintering of Composite Cu Ink in Air. ACS Appl Mater Interfaces 2017, 9 (24), 20852–20858. https: / / doi.org / 10.1021 / acsami.7b04641.
[0149] (50) Zhang, Y.; Zhu, P.; Li, G.; Zhao, T.; Fu, X.; Sun, R.; Zhou, F.; Wong, C. P. Facile Preparation of Monodisperse, Impurity-Free, and Antioxidation Copper Nanoparticles on a Large Scale for Application in Conductive Ink. ACS Appl Mater Interfaces 2014, 6 (1), 560–567. https: / / doi.org / 10.1021 / am404620y.
[0150] (51) Li, W.; Chen, M. Synthesis of Stable Ultra-Small Cu Nanoparticles for Direct Writing Flexible Electronics. Appl Surf Sci 2014, 290, 240–245. https: / / doi.org / 10.1016 / j.apsusc.2013.11.057.
[0151] (52) Bakonyi, I. Accounting for the Resistivity Contribution of Grain Boundaries in Metals: Critical Analysis of Reported Experimental and Theoretical Data for Ni and Cu. European Physical Journal Plus. Springer Science and Business Media Deutschland GmbH April 1, 2021. https: / / doi.org / 10.1140 / epjp / s13360-021-01303-4.
[0152] (53) Chen, T.; Reich, K. V.; Kramer, N. J.; Fu, H.; Kortshagen, U. R.; Shklovskii, B. I. Metal-Insulator Transition in Films of Doped Semiconductor Nanocrystals. Nat Mater 2016, 15 (3), 299–303. https: / / doi.org / 10.1038 / nmat4486.
[0153] (54) Wang, J.; An, C.; Zhang, M.; Qin, C.; Ming, X.; Zhang, Q. Photochemical Conversion of AgCl Nanocubes to Hybrid AgCl-Ag Nanoparticles with High Activity and Long-Term Stability towards Photocatalytic Degradation of Organic Dyes. Can J Chem 2012, 90 (10), 858–864. https: / / doi.org / 10.1139 / v2012-079.
[0154] (55) Nair, S. V.; Usukura, J.; Tokunaga, E. Accurate Modeling of Electron-Hole Binding in CuCl. I. Exciton States. Phys Rev B 2020, 102 (7). https: / / doi.org / 10.1103 / PhysRevB.102.075202.
[0155] (56) Molleman, B.; Hiemstra, T. Size and Shape Dependency of the Surface Energy of Metallic Nanoparticles: Unifying the Atomic and Thermodynamic Approaches. Physical Chemistry Chemical Physics 2018, 20 (31), 20575–20587. https: / / doi.org / 10.1039 / c8cp02346h.103241.007033 / 22-9924
[0156] (57) Kanninen, P.; Johans, C.; Merta, J.; Kontturi, K. Influence of Ligand Structure on the Stability and Oxidation of Copper Nanoparticles. J Colloid Interface Sci 2008, 318 (1), 88–95. https: / / doi.org / 10.1016 / j.jcis.2007.09.069.
[0157] (58) Gu, Y.; Wu, A.; Federici, J. F.; Zhang, X. Inkjet Printable Constantan Ink for the Fabrication of Flexible and Conductive Film. Chemical Engineering Journal 2017, 313, 27–36. https: / / doi.org / 10.1016 / j.cej.2016.12.071.
[0158] (59) Zaccarin, A. M.; Iyer, G. M.; Olsson, R. H.; Turner, K. T. Fabrication and Characterization of Soil Moisture Sensors on a Biodegradable, Cellulose- Based Substrate. IEEE Sens J 2023. https: / / doi.org / 10.1109 / JSEN.2023.3299430.
[0159] (60) Den Otter, M. W. Approximate Expressions for the Capacitance and Electrostatic Potential of Interdigitated Electrodes. Sens Actuators A Phys 2002, 96 (2–3), 140–144. https: / / doi.org / 10.1016 / S0924-4247(01)00783-X.
[0160] (61) Esfandiari, R.; Maki, D. W.; Siracusa, M. Design of Interdigitated Capacitors and Their Application to Gallium Arsenide Monolithic Filters. IEEE Trans Microw Theory Tech 1983, 31 (1), 57–64. https: / / doi.org / 10.1109 / TMTT.1983.1131429.
[0161] (62) Dimitrov, K. C.; Song, S.; Chang, H.; Lim, T.; Lee, Y.; Kwak, B. J. Interdigital Capacitor-Based Passive Lc Resonant Sensor for Improved Moisture Sensing. Sensors (Switzerland). MDPI AG November 1, 2020, pp 1–13. https: / / doi.org / 10.3390 / s20216306.
[0162] (63) Zhu, L.; Wu, K. Accurate Circuit Model of Interdigital Capacitor and Its Application to Design of New Quasi-Lumped Miniaturized Filters with Suppression of Harmonic Resonance. IEEE Trans Microw Theory Tech 2000, 48 (3), 347– 356. https: / / doi.org / 10.1109 / 22.826833.
[0163] (64) Iyer, G. M.; Zaccarin, A. M.; Olsson, R. H.; Turner, K. T. Fabrication and Characterization of Cellulose-Based Materials for Biodegradable Soil Moisture Sensors. In Proceedings of IEEE Sensors; Institute of Electrical and Electronics Engineers Inc., 2022; Vol.2022-October. https: / / doi.org / 10.1109 / SENSORS52175.2022.9967089.
[0164] (65) Cai, Y. Y.; Choi, Y. C.; Kagan, C. R. Chemical and Physical Properties of Photonic Noble-Metal Nanomaterials. Advanced Materials. John Wiley and Sons Inc August 24, 2023. https: / / doi.org / 10.1002 / adma.202108104.103241.007033 / 22-9924
[0165] (66) Chen, W.; Guo, J.; Zhao, Q.; Gopalan, P.; Fafarman, A. T.; Keller, A.; Zhang, M.; Wu, Y.; Murray, C. B.; Kagan, C. R. Designing Strong Optical Absorbers via Continuous Tuning of Interparticle Interaction in Colloidal Gold Nanocrystal Assemblies. ACS Nano 2019, 13 (7), 7493–7501. https: / / doi.org / 10.1021 / acsnano.9b02818.
[0166] (67) Seku, K.; Bhagavanth.; Ganapuram, R.; Pejjai, B.; Girija, K.; Golla N.; Hydrothermal Synthesis of Copper Nanoparticles, Characterization and Their Biological Applications. Int. J. Nano Dimens 2018, 9 (1), 7–14.
[0167] (68) Ghosh, S. K.; Pal, T. Interparticle Coupling Effect on the Surface Plasmon Resonance of Gold Nanoparticles: From Theory to Applications. Chemical Reviews. November 2007, pp 4797–4862. https: / / doi.org / 10.1021 / cr0680282.
[0168] (69) Willets, K. A.; Van Duyne, R. P. Localized Surface Plasmon Resonance Spectroscopy and Sensing. Annu Rev Phys Chem 2007, 58, 267–297. https: / / doi.org / 10.1146 / annurev.physchem.58.032806.104607.
[0169] (70) Yang, H. U.; D’Archangel, J.; Sundheimer, M. L.; Tucker, E.; Boreman, G. D.; Raschke, M. B. Optical Dielectric Function of Silver. Phys Rev B Condens Matter Mater Phys 2015, 91 (23). https: / / doi.org / 10.1103 / PhysRevB.91.235137.
[0170] (71) Olmon, R. L.; Slovick, B.; Johnson, T. W.; Shelton, D.; Oh, S. H.; Boreman, G. D.; Raschke, M. B. Optical Dielectric Function of Gold. Phys Rev B Condens Matter Mater Phys 2012, 86 (23). https: / / doi.org / 10.1103 / PhysRevB.86.235147.
[0171] (72) Chen, W.; Tymchenko, M.; Gopalan, P.; Ye, X.; Wu, Y.; Zhang, M.; Murray, C. B.; Alu, A.; Kagan, C. R. Large-Area Nanoimprinted Colloidal Au Nanocrystal-Based Nanoantennas for Ultrathin Polarizing Plasmonic Metasurfaces. Nano Lett 2015, 15 (8), 5254–5260. https: / / doi.org / 10.1021 / acs.nanolett.5b02647.
[0172] (73) Verre, R.; Baranov, D. G.; Munkhbat, B.; Cuadra, J.; Käll, M.; Shegai, T. Transition Metal Dichalcogenide Nanodisks as High-Index Dielectric Mie Nanoresonators. Nat Nanotechnol 2019, 14 (7), 679–683. https: / / doi.org / 10.1038 / s41565- 019-0442-x.
[0173] Aspects
[0174] The following Aspects are illustrative only and do not limit the scope of the present disclosure or the appended claims. Any part or parts of any one or more Aspects can be combined with any part or parts of any one or more other Aspects.103241.007033 / 22-9924
[0175] Aspect 1. A method, comprising: with a population of metallic nanoparticles comprising a material and (a) having a labile ligand associated thereon and (b) being disposed on a substrate, and (i) exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles, (ii) removing the labile ligand so as to leave the metallic nanoparticles essentially free of ligand, or both (i) and (ii), the metallic nanoparticles then associating so as to form a conductive film. The compact ligand can, for example, be smaller in size than the labile ligand.
[0176] Metallic nanoparticles can include a single metal, e.g., Cu nanoparticles. Metallic nanoparticles can also, however, include two or more metals and can thus comprise a metal alloy.
[0177] Suitable labile ligands and compact ligands are described elsewhere herein. As explained, the disclosed methods can include either or both (i) exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles, (ii) removing the labile ligand so as to leave the metallic nanoparticles essentially free of ligand. Without being bound to any particular theory, after the labile ligand is removed, the particles can then be capable of associating to form the conductive film.
[0178] Aspect 2. The method of Aspect 1, further comprising disposing the population of metallic nanoparticles onto the substrate.
[0179] Aspect 3. The method of any one of Aspects 1-2, further comprising contacting the population of metallic nanoparticles with an oxide etchant.
[0180] Aspect 4. The method of Aspect 3, wherein the oxide etchant comprises acetic acid, hydrochloric acid, hydrofluoric acid, sulfuric acid, hydrocyanic acid, or any combination thereof. An etchant can be selected on the basis of the etchant removing the metal oxide but not the metal itself. By reference to acetic acid, acetic acid reacts with copper oxide but is inert to copper. By further reference to copper, diluted HCl, HF and H2SO4may also be used here.
[0181] Aspect 5. The method of Aspect 4, wherein the acetic acid is present at from about 1 vol% to about 50 vol%
[0182] Aspect 6. The method of Aspect 1, the method comprising exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles.103241.007033 / 22-9924
[0183] Aspect 7. The method of Aspect 1, wherein the labile ligand comprises oleylamine. A labile ligand can comprise (or even consist) of hydrocarbon tails and head groups that are attached to the nanoparticle surface. A typical range of the length of the hydrocarbon is C8-C18,and the head group can be, e.g., amine, phosphine oxide, carboxylate, or others. Thus, different ligand molecules can be formed by choosing the head group and length of hydrocarbon chain, e.g., amine and C18for oleylamine. As an example, ligands used during Cu nanoparticle synthesis include oleic acid, trioctylphosphine oxide, and hexadecyltrimethylammonium bromide.
[0184] Aspect 8. The method of any one of Aspects 1-7, wherein the compact ligand comprises thiocyanate, chloride, sulfide, azide, or any combination thereof. A compact ligand can include, e.g., a halide ion, a chalcogenide ion, and / or a pseudohalide ion. As explained elsewhere herein, however, a nanoparticle can, following removal of the labile ligand, have a bare surface.
[0185] Aspect 9. The method of Aspect 8, wherein the compact ligand comprises ammonium thiocyanate (NH4SCN), ammonium chloride (NH4Cl), sodium sulfide (Na2S), sodium azide (NaN3), or any combination thereof. Without being bound to any particular theory or embodiment, the compact ligand can be shorter than the labile ligand, which can more easily allow one to achieve room-temperature sintering during the ligand exchange process. Again without being bound to any particular theory or embodiment, one can use a ligand that through mass action / reactivity, can replace and / or strip the ligand from the nanoparticle surface. Halides, such as Br- and I- can be useful. One can also, for example, select a compact ligand on the basis of the compact ligand being competitive for the NP surface so as to replace or strip the parent ligand, for example, to replace / strip OLAM. One can further select a compact ligand based on that ligand’s size, as a smaller size can favor close approach to nanoparticles. Further, one can select a compact ligand on the basis of the ligand being one that does not react to change the composition of the nanoparticle core.
[0186] Aspect 10. The method of any one of Aspects 1-9, wherein the metallic nanoparticles comprise one or more of Cu nanoparticles, Ni nanoparticles, In nanoparticles, Fe nanoparticles, and Co nanoparticles. As explained elsewhere herein, Cu nanoparticles are considered especially suitable. Without being bound to any particular theory or embodiment, Cu can have a size tailored during synthesis; Cu nanoparticles can103241.007033 / 22-9924 have a diameter in the range of from about 4.5 to about 200 nm. One can make nanoparticles across a wide range. Without being bound to any particular theory or embodiment, in some instances one may elect to use relatively small nanoparticles, as there is a larger energetic driving force for their fusion. As shown elsewhere herein, example 4.5 nm nanoparticles formed more conductive films than 15 nm nanoparticles.
[0187] Aspect 11. The method of Aspect 10, wherein the metallic nanoparticles comprise Cu nanoparticles.
[0188] Aspect 12. The method of any one of Aspects 1-11, further comprising removing excess compact ligand.
[0189] Aspect 13. The method of any one of Aspects 1-12, wherein the exchanging is performed at less than about 120 ºC.
[0190] Aspect 14. The method of Aspect 13, wherein the exchanging is performed at less than about 100 ºC. The exchanging can be performed at, for example, less than 100 ºC, less than 90 ºC, less than 80 ºC, less than 70 ºC, less than 60 ºC, or even at less than 50 ºC.
[0191] Aspect 15. The method of Aspect 14, wherein the exchanging is performed at ambient conditions.
[0192] Aspect 16. The method of any one of Aspects 1-15, wherein the substrate degrades above about 50 ºC. As explained herein, the disclosed technology is suitable for use with substrates that cannot tolerate comparatively high temperatures. For example, flexible and biodegradable polymers and papers have low thermal resistance which makes them unsuitable for high-temperature processes, but the disclosed technology can be applied to such substrates.
[0193] Aspect 17. The method of any one of Aspects 1-16, wherein the substrate degrades above about 75 ºC.
[0194] Aspect 18. The method of any one of Aspects 1-17, wherein the substrate degrades above about 100 ºC.
[0195] Aspect 19. The method of any one of Aspects 1-18, wherein the conductive film has a resistivity of less than about 50 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form. As an example, a conductive film of Cu nanoparticles according to the present disclosure can have a resistance of less than about 50 times the resistance of bulk Cu. As another example, a conductive film of103241.007033 / 22-9924 CuZn (alloy) nanoparticles according to the present disclosure can have a resistance of less than about 50 times the resistance of bulk CuZn alloy.
[0196] Aspect 20. The method of Aspect 19, wherein the conductive film has a resistivity of less than about 25 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form.
[0197] Aspect 21. The method of Aspect 20, wherein the conductive film has a resistivity of less than about 10 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form.
[0198] Aspect 22. The method of Aspect 21, wherein the conductive film has a resistivity of from about 1.1 to about 10 times the resistivity of the bulk metal of the metallic nanoparticles.
[0199] Aspect 23. The method of Aspect 22, wherein the conductive film has a resistivity of from about 1.1 to about 2 times the resistivity of the bulk metal of the metallic nanoparticles.
[0200] Aspect 24. The method of any one of Aspects 1-23, wherein the conductive film exhibits an increase in resistivity of less than about 15% following exposure to ambient air for 72 hours.
[0201] Aspect 25. The method of any one of Aspects 1-23, wherein the conductive film exhibits an increase in resistivity of from about 1 to about 15% following exposure to ambient air for 72 hours.
[0202] Aspect 26. A conductive film, comprising a plurality of metallic nanoparticles, the nanoparticles optionally having a compact ligand associated therewith, the film having a resistivity of less than about 50 times (e.g., from 1.1 to 25 times) the resistivity of the bulk material of the metallic nanoparticles. The metallic nanoparticles can be fused, when in film form.
[0203] Aspect 27. The film of Aspect 26, wherein the metallic nanoparticles comprise copper nanoparticles.
[0204] Aspect 28. The film of any one of Aspects 26-27, wherein the compact ligand comprises thiocyanate, chloride, sulfide, azide, or any combination thereof.
[0205] Aspect 29. The method of Aspect 28, wherein the compact ligand comprises ammonium thiocyanate (NH4SCN), ammonium chloride (NH4Cl), sodium sulfide (Na2S), sodium azide (NaN3), or any combination thereof.103241.007033 / 22-9924
[0206] Aspect 30. A composition, comprising: a population of metallic nanoparticles (i) having a labile ligand associated thereon and (ii) being disposed on a substrate; and a compact ligand that, relative to the labile ligand, preferentially associates with the population of metallic nanoparticles.
[0207] Aspect 31. The composition of Aspect 30, wherein the metallic nanoparticles comprise Cu nanoparticles.
[0208] Aspect 32. The composition of any one of Aspects 30-31, wherein the labile ligand comprises oleylamine.
[0209] References
[0210] (1) Gao, W.; Ota, H.; Kiriya, D.; Takei, K.; Javey, A. Flexible Electronics toward Wearable Sensing. Acc. Chem. Res.2019, 52 (3), 523–533.
[0211] (2) Ray, T. R.; Choi, J.; Bandodkar, A. J.; Krishnan, S.; Gutruf, P.; Tian, L.; Ghaffari, R.; Rogers, J. A. Bio-Integrated Wearable Systems: A Comprehensive Review. Chem. Rev.2019, 119 (8), 5461–5533.
[0212] (3) Kim, J.; Kumar, R.; Bandodkar, A. J.; Wang, J. Advanced Materials for Printed Wearable Electrochemical Devices: A Review. Adv. Electron. Mater.2017, 3 (1), 1600260.
[0213] (4) Garlapati, S. K.; Divya, M.; Breitung, B.; Kruk, R.; Hahn, H.; Dasgupta, S. Printed Electronics Based on Inorganic Semiconductors: From Processes and Materials to Devices. Adv. Mater.2018, 30 (40), 1707600.
[0214] (5) Nayak, L.; Mohanty, S.; Nayak, S. K.; Ramadoss, A. A Review on Inkjet Printing of Nanoparticle Inks for Flexible Electronics. J. Mater. Chem. C 2019, 7 (29), 8771–8795.
[0215] (6) Zeng, M.; Zhang, Y. Colloidal Nanoparticle Inks for Printing Functional Devices: Emerging Trends and Future Prospects. J. Mater. Chem. A 2019, 7 (41), 23301–23336.
[0216] (7) Gwo, S.; Chen, H.-Y.; Lin, M.-H.; Sun, L.; Li, X. Nanomanipulation and Controlled Self-Assembly of Metal Nanoparticles and Nanocrystals for Plasmonics. Chem. Soc. Rev.2016, 45 (20), 5672–5716.
[0217] (8) Fafarman, A. T.; Hong, S.-H.; Caglayan, H.; Ye, X.; Diroll, B. T.; Paik, T.; Engheta, N.; Murray, C. B.; Kagan, C. R. Chemically Tailored Dielectric-to-103241.007033 / 22-9924 Metal Transition for the Design of Metamaterials from Nanoimprinted Colloidal Nanocrystals. Nano Lett.2012, 13 (2), 350–357.
[0218] (9) Fafarman, A. T.; Hong, S.-H.; Oh, S. J.; Caglayan, H.; Ye, X.; Diroll, B. T.; Engheta, N.; Murray, C. B.; Kagan, C. R. Air-Stable, Nanostructured Electronic and Plasmonic Materials from Solution-Processable, Silver Nanocrystal Building Blocks. ACS Nano 2014, 8 (3), 2746–2754.
[0219] (10) Guo, J.; Kim, J.-Y.; Zhang, M.; Wang, H.; Stein, A.; Murray, C. B.; Kotov, N. A.; Kagan, C. R. Chemo- and Thermomechanically Configurable 3D Optical Metamaterials Constructed from Colloidal Nanocrystal Assemblies. ACS Nano 2019, 14 (2), 1427–1435.
[0220] (11) Xin, Y.; Yu, K.; Zhang, L.; Yang, Y.; Yuan, H.; Li, H.; Wang, L.; Zeng, J. Copper-Based Plasmonic Catalysis: Recent Advances and Future Perspectives. Adv. Mater.2021, 33 (32), 2008145.
[0221] (12) Oliva-Puigdomènech, A.; De Roo, J.; Kuhs, J.; Detavernier, C.; Martins, J. C.; Hens, Z. Ligand Binding to Copper Nanocrystals: Amines and Carboxylic Acids and the Role of Surface Oxides. Chem. Mater.2019, 31 (6), 2058–2067.
[0222] (13) Podder, J.; Kobayashi, R.; Ichimura, M. Photochemical Deposition of CuxS Thin Films from Aqueous Solutions. Thin Solid Films 2005, 472 (1), 71–75.
[0223] (14) Chavez, K. L.; Hess, D. W. A Novel Method of Etching Copper Oxide Using Acetic Acid. J. Electrochem. Soc.2001, 148 (11), G640.
Claims
103241.007033 / 22-9924 What is Claimed:
1. A method, comprising: with a population of metallic nanoparticles comprising a material and (a) having a labile ligand associated thereon and (b) being disposed on a substrate, and (i) exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles, (ii) removing the labile ligand so as to leave the metallic nanoparticles essentially free of ligand, or both (i) and (ii) the metallic nanoparticles then associating so as to form a conductive film.
2. The method of claim 1, further comprising disposing the population of metallic nanoparticles onto the substrate.
3. The method of any one of claims 1-2, further comprising contacting the population of metallic nanoparticles with an oxide etchant.
4. The method of claim 3, wherein the oxide etchant comprises acetic acid, hydrochloric acid, hydrofluoric acid, sulfuric acid, hydrocyanic acid, or any combination thereof.
5. The method of claim 4, wherein the acetic acid is present at from about 1 vol% to about 50 vol%.
6. The method of claim 1, the method comprising exchanging the labile ligand for a compact ligand that associates with the population of metallic nanoparticles.
7. The method of claim 1, wherein the labile ligand comprises oleylamine.
8. The method of any one of claims 1-2, wherein the compact ligand comprises thiocyanate, chloride, sulfide, azide, or any combination thereof.
9. The method of claim 8, wherein the compact ligand comprises ammonium thiocyanate (NH4SCN), ammonium chloride (NH4Cl), sodium sulfide (Na2S), sodium azide (NaN3), or any combination thereof.103241.007033 / 22-9924 10. The method of any one of claims 1-2, wherein the metallic nanoparticles comprise one or more of Cu nanoparticles, Ni nanoparticles, In nanoparticles, Fe nanoparticles, and Co nanoparticles.
11. The method of claim 10, wherein the metallic nanoparticles comprise Cu nanoparticles.
12. The method of any one of claims 1-2, further comprising removing excess compact ligand.
13. The method of any one of claims 1-2, wherein the exchanging is performed at less than about 120 ºC.
14. The method of claim 13, wherein the exchanging is performed at less than about 100 ºC.
15. The method of claim 14, wherein the exchanging is performed at ambient conditions.
16. The method of any one of claims 1-2, wherein the substrate degrades above about 50 ºC.
17. The method of any one of claims 1-2, wherein the substrate degrades above about 75 ºC.
18. The method of any one of claims 1-2, wherein the substrate degrades above about 100 ºC.
19. The method of any one of claims 1-2, wherein the conductive film has a resistivity of less than about 50 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form.
20. The method of claim 19, wherein the conductive film has a resistivity of less than about 25 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form.103241.007033 / 22-9924 21. The method of claim 20, wherein the conductive film has a resistivity of less than about 10 times the resistivity of the material of the metallic nanoparticles in the material’s bulk form.
22. The method of claim 21, wherein the conductive film has a resistivity of from about 1.1 to about 10 times the resistivity of the bulk metal of the metallic nanoparticles.
23. The method of claim 22, wherein the conductive film has a resistivity of from about 1.1 to about 2 times the resistivity of the bulk metal of the metallic nanoparticles.
24. The method of any one of claims 1-2, wherein the conductive film exhibits an increase in resistivity of less than about 15% following exposure to ambient air for 72 hours.
25. The method of any one of claims 1-2, wherein the conductive film exhibits an increase in resistivity of from about 1 to about 15% following exposure to ambient air for 72 hours.
26. A conductive film, comprising: a plurality of metallic nanoparticles, the metallic nanoparticles optionally having a compact ligand associated therewith, the film having a resistivity of less than about 50 times the resistivity of the bulk metal of the metallic nanoparticles.
27. The film of claim 26, wherein the metallic nanoparticles comprise copper nanoparticles.
28. The film of any one of claims 26-27, wherein the compact ligand comprises thiocyanate, chloride, sulfide, azide, or any combination thereof.
29. The method of claim 28, wherein the compact ligand comprises ammonium thiocyanate (NH4SCN), ammonium chloride (NH4Cl), sodium sulfide (Na2S), sodium azide (NaN3), or any combination thereof.103241.007033 / 22-9924 30. A composition, comprising: a population of metallic nanoparticles (i) having a labile ligand associated thereon and (ii) being disposed on a substrate; and a compact ligand that, relative to the labile ligand, preferentially associates with the population of metallic nanoparticles.
31. The composition of claim 30, wherein the metallic nanoparticles comprise Cu nanoparticles.
32. The composition of any one of claims 30-31, wherein the labile ligand comprises oleylamine.
Citation Information
Patent Citations
Semiconductor film and method of producing the same, photoelectric conversion element, solid-state imaging element and electronic apparatus
US20190229279A1
Stabilized ink comprising semiconductor particles and uses thereof
US20220204800A1
Conductive film, dispersion, manufacturing methods for these, and device including conductive film
WO2021075495A1