Positive electrode material, preparation method therefor, and use thereof
By forming the Mn4O(PO4)2 coating layer in the manganese-containing cathode material, the problem of poor cycle performance caused by the easy dissolution of Mn3+ is solved, the stability of the material structure and cycle performance are significantly improved, and the cycle performance retention rate reaches as high as 99 %above.
Patent Information
- Application Number
- PCT/CN2023/083943
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Mn3+ in manganese-containing cathode materials is easy to dissolve, resulting in poor cycle performance. Existing modification methods can only improve surface properties, but cannot solve the problem of easy dissolution of Mn3+ inside the material.
The hydrothermal reaction method is used to form a coating layer of Mn4O(PO4)2 in phosphate solution and manganese salt solution. A stable divalent Mn oxide is formed through calcination treatment to prevent Mn ions from contacting the electrolyte and reduce the average concentration of Mn element. Valence.
The cycle performance of the cathode material is significantly improved. The capacity retention rate after 100 cycles can reach more than 99%, the capacity retention rate after 200 cycles can reach more than 97%, and the capacity retention rate after 500 cycles can reach more than 94%. This avoids the problem of the cathode material and the Direct contact with electrolyte and side reactions.
Smart Images

Figure PCTCN2023083943-FTAPPB-I100001 
Figure PCTCN2023083943-FTAPPB-I100002 
Figure PCTCN2023083943-FTAPPB-I100003
Abstract
Description
A positive electrode material and its preparation method and application Technical Field
[0001] The present application relates to the field of lithium-ion batteries, for example, a positive electrode material and its preparation method and application. Background Art
[0002] Mn is commonly found in manganese-containing positive electrode materials. 3+ The problem of disproportionation reaction seriously affects the service life of manganese-containing positive electrode materials. For example, lithium manganese iron phosphate, because lithium iron phosphate and lithium manganese phosphate positive electrode materials have the same olivine structure, the two can form a co-solvent lithium manganese iron phosphate and can be mutually soluble in any proportion. Therefore, lithium iron manganese phosphate positive electrode materials show excellent electrochemical properties, good safety and cycle life, and combine the advantages of lithium iron phosphate and lithium manganese phosphate. At the same time, lithium manganese iron phosphate also has application challenges, such as low electronic conductivity of the material, low lithium ion diffusion coefficient, two different voltage platforms (4.1V and 3.4V), and Mn 3+ The Jahn-Teller effect is easy to produce, which affects the large-scale application of lithium iron manganese phosphate batteries.
[0003] The methods for modifying lithium iron manganese phosphate positive electrode materials are mostly surface coating and element doping.
[0004] CN112885995B discloses a method for manufacturing a lithium iron manganese phosphate-coated high-voltage lithium nickel manganese oxide positive electrode material. The method comprises adding lithium nickel manganese oxide to the lithium iron manganese phosphate material for ultrasonic dispersion, then heating in a high-pressure reactor, and filtering and drying to obtain a product.
[0005] CN104733708A discloses a method for preparing a nickel-cobalt-manganese oxide composite material having a good cycle life and high safety and coated with lithium iron phosphate. The method comprises growing lithium iron phosphate on the surface of lithium nickel-cobalt-manganese oxide particles using a hydrothermal method to coat the lithium nickel-cobalt-manganese oxide.
[0006] Although the above patents have achieved the purpose of improving its interface characteristics and cycle characteristics, the modification only stays on the surface and cannot improve the Mn content inside the material. 3+ The defect of easy dissolution leading to poor cycle performance.
[0007] Therefore, how to improve the internal Mn of the material 3+ The problem of poor cycling performance due to easy dissolution is an important research direction in this field.
[0008] Summary of the Invention
[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0010] The present application provides a positive electrode material, a preparation method thereof, and an application thereof.
[0011] To achieve this goal, this application adopts the following technical solutions:
[0012] An embodiment of the present application provides a positive electrode material, which includes a core and a coating layer, wherein the core includes a manganese-containing positive electrode material, and the coating layer includes Mn4O(PO4)2.
[0013] The embodiment of the present application provides a surface-coated manganese-containing positive electrode material, which solves the problem of easy dissolution of Mn ions in the manganese-containing positive electrode material, thereby maintaining the structural stability of the material and improving the cycle performance of the material.
[0014] As an optional technical solution of an embodiment of the present application, the manganese-containing positive electrode material includes any one or a combination of at least two of lithium nickel cobalt manganese oxide, lithium-rich manganese base, lithium manganese phosphate or lithium manganese iron phosphate, wherein typical but non-limiting examples of the combination include: a combination of lithium nickel cobalt manganese oxide and a lithium-rich manganese base, a combination of a lithium-rich manganese base and lithium manganese phosphate, or a combination of lithium manganese phosphate and lithium manganese iron phosphate, etc.
[0015] The present invention provides a method for preparing the positive electrode material, which comprises:
[0016] The phosphate solution and the manganese salt solution are first mixed to obtain a mixed solution, the mixed solution is hydrothermally reacted with a manganese-containing positive electrode material to obtain a modified positive electrode material, and the modified positive electrode material is first calcined to obtain a positive electrode material with a surface coated with Mn4O(PO4)2.
[0017] The surface of the modified positive electrode material prepared in the embodiment of the present application is coated with Mn2(OH)PO4. The chemical equation for forming Mn4O(PO4)2 after calcination of the material coated with Mn2(OH)PO4 is: The Mn4O(PO4)2 generated in the embodiment of the present application is a stable divalent Mn oxide. After the surface of the material is coated with Mn4O(PO4)2, the average valence of the Mn ions in the material is reduced. The surface coating of Mn4O(PO4)2 can effectively prevent the material from contacting the electrolyte.
[0018] As an optional technical solution of the embodiment of the present application, the solute in the manganese salt solution is manganese salt, and the solvent is an alcohol-water mixed solution.
[0019] In one embodiment, the manganese salt includes any one or a combination of at least two of manganese chloride, manganese acetate or manganese nitrate, wherein typical but non-limiting examples of the combination include: a combination of manganese chloride and manganese acetate, a combination of manganese acetate and manganese nitrate, or a combination of manganese chloride and manganese nitrate.
[0020] In one embodiment, the volume ratio of ethanol to water in the alcohol-water mixed solution is 1:(18-22), wherein the volume ratio can be 1:18, 1:19, 1:20, 1:21 or 1:22, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] In one embodiment, the concentration of the phosphate solution is 0.1 to 10 mol / L, wherein the concentration can be 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] In one embodiment, the solute in the phosphate solution is phosphate, and the solvent is a mixed solution of alcohol and water.
[0023] In one embodiment, the phosphate salt comprises disodium hydrogen phosphate.
[0024] In one embodiment, the volume ratio of ethanol to water in the alcohol-water mixed solution is 1:(18-22), wherein the volume ratio can be 1:18, 1:19, 1:20, 1:21 or 1:22, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] In one embodiment, the concentration of the phosphate solution is 0.1 to 10 mol / L, wherein the concentration can be 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] As an optional technical solution of the embodiment of the present application, the first mixing includes: adding the phosphate solution dropwise to the manganese salt solution at a uniform speed and then stirring.
[0027] In one embodiment, the molar ratio of the manganese salt to the phosphate during the dropwise addition is 1:(1-3), wherein the molar ratio can be 1:1, 1:2 or 1:3, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] In one embodiment, the stirring speed is 70 to 110 r / min, wherein the speed can be 70 r / min, 75 r / min, 80 r / min, 85 r / min, 90 r / min, 95 r / min, 100 r / min, 105 r / min or 110 r / min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] In one embodiment, the stirring time is 30 to 60 min, wherein the time can be 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] As an optional technical solution in an embodiment of the present application, the liquid-to-solid ratio of the mixed solution and the manganese-containing positive electrode material is (0.0003-0.004):1, wherein the liquid-to-solid ratio can be 0.0003:1, 0.0005:1, 0.001:1, 0.0015:1, 0.002:1, 0.0025:1, 0.003:1, 0.0035:1 or 0.004:1, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0031] In one embodiment, the temperature of the hydrothermal reaction is 160-260°C, wherein the temperature can be 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or 260°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] In one embodiment, the hydrothermal reaction time is 12 to 48 hours, wherein the time can be 12 hours, 15 hours, 20 hours, 25 hours, 30 hours, 35 hours, 40 hours, 45 hours or 48 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] In one embodiment, the hydrothermal reaction is sequentially cooled, filtered, and dried.
[0034] In one embodiment, the drying temperature is 120-200°C, wherein the temperature can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] In one embodiment, the drying time is 12 to 20 hours, wherein the time can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] In one embodiment, the temperature of the first calcination treatment is 400-500°C, wherein the temperature can be 400°C, 420°C, 440°C, 460°C, 480°C or 500°C, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0037] In one embodiment, the time of the first calcination treatment is 0.5 to 2 hours, wherein the time can be 0.5 hours, 0.7 hours, 0.9 hours, 1.1 hours, 1.3 hours, 1.5 hours, 1.7 hours, 1.9 hours or 2 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] As an optional technical solution of the embodiment of the present application, when the manganese-containing positive electrode material is lithium manganese iron phosphate, the preparation method of the lithium manganese iron phosphate includes the following steps:
[0039] (1) performing a second mixing of an iron source, a manganese source, and a phosphorus source to obtain a manganese iron phosphate precursor;
[0040] (2) The manganese iron phosphate precursor, lithium source and carbon source described in step (1) are mixed and subjected to a second calcination treatment to obtain lithium manganese iron phosphate.
[0041] The iron source in step (1) includes ferrous nitrate and / or ferrous sulfate.
[0042] In one embodiment, the manganese source includes manganese nitrate and / or manganese sulfate.
[0043] In one embodiment, the phosphorus source includes disodium hydrogen phosphate.
[0044] In one embodiment, the iron source, manganese source and phosphorus source are in the order of Mn x Fe 1-x The stoichiometric ratios of the elements in PO4 are weighed, where 0.1≤x≤0.9, where x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc., but are not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] As an optional technical solution in an embodiment of the present application, the temperature of the second mixing in step (1) is 40-60°C, wherein the temperature can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] In one embodiment, the time for the second mixing in step (1) is 3 to 5 hours, wherein the time can be 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours, 4 hours, 4.2 hours, 4.4 hours, 4.6 hours, 4.8 hours or 5 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] In one embodiment, in step (1), the second mixing is followed by cooling to obtain the ferromanganese phosphate precursor.
[0048] As an optional technical solution in an embodiment of the present application, the molar ratio of the manganese iron phosphate precursor and the lithium source in step (2) is 1:1.05 to 1.2, wherein the molar ratio can be 1:1.05, 1:1.1 or 1:1.2, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] The molar ratio in the embodiments of the present application corresponds to a coating amount of 5 to 15%.
[0050] In one embodiment, the carbon source accounts for 4 to 6 wt % of the total mass of the ferromanganese phosphate precursor and the lithium source, wherein the mass fraction can be 4 wt %, 5 wt % or 6 wt %, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0051] In one embodiment, the lithium source includes lithium hydroxide and / or lithium carbonate.
[0052] In one embodiment, the carbon source comprises glucose and / or sucrose.
[0053] As an optional technical solution of the embodiment of the present application, the atmosphere of the second calcination treatment in step (3) is high-purity nitrogen.
[0054] In one embodiment, the heating rate of the second calcination treatment is 4 to 6°C / min, wherein the heating rate can be 4°C / min, 5°C / min or 6°C / min, etc., but is not limited to the listed values. Other unlisted values within this numerical range are also applicable.
[0055] In one embodiment, the temperature of the second calcination treatment is 600-700°C, wherein the temperature can be 600°C, 620°C, 640°C, 660°C, 680°C or 700°C, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0056] In one embodiment, the second calcination treatment time is 6 to 10 hours, wherein the time can be 6 hours, 7 hours, 8 hours, 9 hours or 10 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] An embodiment of the present application provides an application of the positive electrode material, and the positive electrode material is applied in the field of lithium-ion batteries.
[0058] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, this application no longer exhaustively lists the specific point values included in the range.
[0059] Compared with the related art, the beneficial effects of this application are:
[0060] (1) The present invention coats basic manganese phosphate and then decomposes basic manganese carbonate into Mn4O(PO4)2 by calcination for application in batteries. First, a stable coating layer of divalent manganese compound is formed by this coating method, while other coating methods can only obtain a coating layer of tetravalent manganese or an unstable divalent manganese coating layer, thereby reducing the average valence state of the Mn element in the manganese-containing positive electrode material and inhibiting the Mn 3+ The disproportionation reaction can maintain the capacity of the battery for 100 cycles at over 99%, for 200 cycles at over 97%, and for 500 cycles at over 94%.
[0061] (2) In this application, Mn4O(PO4)2 can avoid direct contact between the positive electrode material and the electrolyte, thereby avoiding the occurrence of side reactions.
[0062] (3) When using Mn4O(PO4)2 to coat manganese-based oxide materials, because this material also has a similar oxide structure, it can be better composited with the inner layer material and better achieve the effect of reducing the average valence state of the Mn element.
[0063] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0064] The technical solution of this application is further explained below through specific implementation methods.
[0065] Example 1
[0066] This embodiment provides a positive electrode material, which includes a core and a coating layer, the core including lithium manganese iron phosphate, and the coating layer including Mn4O(PO4)2.
[0067] This embodiment also provides a method for preparing the above-mentioned positive electrode material, the preparation method comprising the following steps:
[0068] (1) Ferrous nitrate, manganese nitrate and ammonium dihydrogen phosphate were mixed according to Mn 0.4 Fe 0.6 The stoichiometric ratios of the elements in PO4 were weighed, and the raw materials were heated in deionized water and cooled to obtain the manganese iron phosphate precursor.
[0069] (2) Manganese iron phosphate precursor and lithium hydroxide were weighed in a molar ratio of 1:1.05, and 4 wt% glucose was added. Under the protection of high-purity nitrogen, the mixture was placed in a programmable tube furnace and heated to 650°C at a heating rate of 5°C / min, kept warm for 8 hours, and then cooled to room temperature with the furnace to obtain a manganese iron phosphate lithium positive electrode material.
[0070] (3) Manganese chloride and disodium hydrogen phosphate were weighed and dissolved in a mixed solution of ethanol and water in a volume ratio of 1:20 to prepare 0.1 mol / L manganese chloride solution and disodium hydrogen phosphate solution. The disodium hydrogen phosphate solution was slowly and uniformly added dropwise to the manganese chloride solution at room temperature to control the molar ratio of manganese chloride and disodium hydrogen phosphate in the mixed solution to be 1:1. The mixture was stirred at a stirring speed of 70 r / min for 30 minutes to obtain a mixed solution. The mixed solution and lithium manganese iron phosphate were subjected to a hydrothermal reaction at a mass solid-liquid ratio of 0.004:1 at a temperature of 210°C for 30 hours. After the hydrothermal reaction was completed, it was allowed to cool naturally to room temperature. The cooled product was filtered and then placed in an oven for drying at 160°C for 18 hours. It was calcined at 450°C for 1.5 hours to obtain a manganese iron phosphate precursor coated with Mn4O(PO4)2.
[0071] Example 2
[0072] This embodiment provides a positive electrode material, which includes a core and a coating layer, the core including lithium manganese iron phosphate, and the coating layer including Mn4O(PO4)2.
[0073] This embodiment also provides a method for preparing the above-mentioned positive electrode material, the preparation method comprising:
[0074] (1) Ferrous sulfate, manganese sulfate and ammonium phosphate were mixed according to Mn 0.4 Fe 0.6 The stoichiometric ratios of the elements in PO4 were weighed, and the raw materials were heated in deionized water and cooled to obtain the manganese iron phosphate precursor.
[0075] (2) Manganese iron phosphate precursor and lithium carbonate were weighed according to the stoichiometric ratio of 1:1.1, 4 wt% glucose was added, and the mixture was placed in a programmable tubular furnace and heated to 650 ° C at a heating rate of 5 ° C / min under the protection of high-purity nitrogen. The mixture was kept warm for 8 h and then cooled to room temperature with the furnace to obtain a manganese iron phosphate lithium positive electrode material.
[0076] (3) Weigh soluble manganese nitrate and disodium hydrogen phosphate, respectively dissolve them in a mixed solution of ethanol and water in a volume ratio of 1:20 to prepare 0.5 mol / L manganese nitrate solution and disodium hydrogen phosphate solution, slowly and uniformly add the prepared disodium hydrogen phosphate solution to the manganese nitrate solution at room temperature, control the molar ratio of manganese nitrate and disodium hydrogen phosphate in the mixed solution to be 1:2, and then stir at a stirring speed of 90 r / min for 45 minutes to obtain a mixed solution, and hydrothermally react the mixed solution with lithium manganese iron phosphate at a mass solid-liquid ratio of 0.0007:1 at a temperature of 160°C for 48 hours. After the hydrothermal reaction is completed, let it cool naturally to room temperature, filter the cooled product, and then put it into an oven for drying, dry it at 120°C for 20 hours, and calcine it at 400°C for 2 hours to obtain a manganese iron phosphate precursor coated with Mn4O(PO4)2.
[0077] Example 3
[0078] This embodiment provides a positive electrode material, which includes a core and a coating layer, the core including lithium manganese iron phosphate, and the coating layer including Mn4O(PO4)2.
[0079] This embodiment also provides a method for preparing a positive electrode material, the preparation method comprising the following steps:
[0080] (1) Ferrous nitrate, manganese nitrate and ammonium dihydrogen phosphate were mixed according to Mn x Fe 1-x The stoichiometric ratios of the elements in PO4 were weighed, and the raw materials were heated in deionized water and cooled to obtain the manganese iron phosphate precursor.
[0081] (2) Manganese iron phosphate precursor and lithium hydroxide were weighed according to the stoichiometric ratio of 1:1.2, 4 wt% glucose was added, and the mixture was placed in a programmable tubular furnace and heated to 650 ° C at a heating rate of 5 ° C / min under the protection of high-purity nitrogen. The mixture was kept warm for 8 hours and then cooled to room temperature with the furnace to obtain a manganese iron phosphate lithium positive electrode material.
[0082] (3) Soluble manganese acetate and disodium hydrogen phosphate were weighed and dissolved in a mixed solution of ethanol and water in a volume ratio of 1:20 to prepare 1 mol / L manganese acetate solution and disodium hydrogen phosphate solution. The prepared disodium hydrogen phosphate solution was slowly and uniformly added dropwise to the manganese acetate solution at room temperature to control the molar ratio of manganese acetate and disodium hydrogen phosphate in the mixed solution to be 1:3. The mixture was stirred at a stirring speed of 110 r / min for 45 minutes to obtain a mixed solution. The mixed solution and lithium manganese iron phosphate were hydrothermally reacted at a mass solid-liquid ratio of 0.0003:1 at a temperature of 260°C for 12 hours. After the hydrothermal reaction was completed, it was allowed to cool naturally to room temperature. The cooled product was filtered and then placed in an oven for drying at 200°C for 12 hours. It was calcined at 500°C for 0.5 hours to obtain a manganese iron phosphate precursor coated with Mn4O(PO4)2.
[0083] Example 4
[0084] In this example, except that the concentrations of the manganese chloride solution and the sodium hydrogen phosphate solution in step (3) were replaced with 2 mol / L, other conditions were the same as those in Example 1.
[0085] Example 5
[0086] In this example, except that the mass solid-to-liquid ratio of the mixed solution to the manganese phosphate precursor is changed to 0.0035:1, other conditions are the same as those in Example 1.
[0087] Example 6
[0088] In this example, except that the mass solid-to-liquid ratio of the mixed solution to the manganese phosphate precursor is changed to 0.0002:1, other conditions are the same as those in Example 1.
[0089] Example 7
[0090] In this embodiment, except that the core lithium manganese iron phosphate is replaced by lithium nickel cobalt manganese oxide, other conditions are the same as those in embodiment 1.
[0091] The preparation method of lithium nickel cobalt manganese oxide material is as follows:
[0092] Nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in deionized water in a molar ratio of 5:2:3. Sodium hydroxide was used as a precipitant and ammonia water as a complexing agent. A nickel-cobalt-manganese precursor was prepared by a co-precipitation method by hydrothermal reaction at a temperature of 210°C for 30 hours. After the precursor was evenly mixed with a lithium source, it was calcined at 900°C for 12 hours to obtain the target product. Among them, the lithium source was Li2CO3, and the lithium ratio was 1.08 (i.e., the molar ratio Li / Me=1.08, Me is the sum of the transition metals Ni, Co, and Mn).
[0093] Comparative Example 1
[0094] This comparative example provides a positive electrode material, and the preparation method of the positive electrode material comprises the following steps:
[0095] (1) Ferrous nitrate, manganese nitrate and ammonium dihydrogen phosphate were mixed according to Mn 0.4 Fe 0.6 The stoichiometric ratios of the elements in PO4 are weighed; the raw materials are heated in deionized water and cooled to obtain a manganese iron phosphate precursor.
[0096] (2) Weigh the precursor manganese ferrophosphate Mn according to the stoichiometric ratio 0.4 Fe 0.6 PO4 and lithium hydroxide, add 6wt% glucose, place it in a programmable tube furnace under the protection of high-purity nitrogen, heat it to 650℃ at a heating rate of 5℃ / min, keep it warm for 8h, and then cool it to room temperature with the furnace to obtain an uncoated lithium manganese iron phosphate positive electrode material.
[0097] Comparative Example 2
[0098] This comparative example provides a positive electrode material, which is lithium nickel cobalt manganese oxide.
[0099] Nickel sulfate, cobalt sulfate, and manganese sulfate are dissolved in deionized water in a molar ratio of 5:2:3. Sodium hydroxide is used as a precipitant and ammonia water as a complexing agent to prepare a nickel-cobalt-manganese precursor by coprecipitation. After the precursor is evenly mixed with a lithium source, it is calcined at 900°C for 12 hours to obtain the target product. Among them, Li2CO3 is selected as the lithium source, and the lithium ratio is 1.08 (i.e., the molar ratio Li / Me=1.08, Me is the sum of the transition metals Ni, Co, and Mn). That is, uncoated lithium nickel cobalt manganese oxide is obtained.
[0100] Comparative Example 3
[0101] This comparative example provides a positive electrode material, which is different from Example 1 in that the positive electrode material is a material coated with manganese phosphate.
[0102] (1) Ferrous nitrate, manganese nitrate and ammonium dihydrogen phosphate were mixed according to Mn 0.4 Fe 0.6 The stoichiometric ratios of the elements in PO4 were weighed, and the raw materials were heated in deionized water and cooled to obtain the manganese iron phosphate precursor.
[0103] (2) Manganese iron phosphate precursor and lithium hydroxide were weighed in a molar ratio of 1:1.05, and 4 wt% glucose was added. Under the protection of high-purity nitrogen, the mixture was placed in a programmable tube furnace and heated to 650°C at a heating rate of 5°C / min, kept warm for 8 hours, and then cooled to room temperature with the furnace to obtain a manganese iron phosphate lithium positive electrode material.
[0104] (3) According to the mass liquid-solid ratio of 0.004:1, corresponding amounts of manganese phosphate solution and lithium iron manganese phosphate material were taken and hydrothermally reacted at a temperature of 210°C for 30 hours. After the hydrothermal reaction, it was allowed to cool naturally to room temperature. The cooled product was filtered and then placed in an oven for drying at 160°C for 18 hours. It was calcined at 450°C for 1.5 hours to obtain a lithium iron manganese phosphate positive electrode material with a surface coated with Mn3(PO4)2.
[0105] Comparative Example 4
[0106] This comparative example provides a positive electrode material, which is different from Example 1 in that the positive electrode material is a material coated with manganese hydroxide.
[0107] (1) Ferrous nitrate, manganese nitrate and ammonium dihydrogen phosphate were mixed according to Mn 0.4 Fe 0.6 The stoichiometric ratios of the elements in PO4 were weighed, and the raw materials were heated in deionized water and cooled to obtain the manganese iron phosphate precursor.
[0108] (2) Manganese iron phosphate precursor and lithium hydroxide were weighed in a molar ratio of 1:1.05, and 4 wt% glucose was added. Under the protection of high-purity nitrogen, the mixture was placed in a programmable tube furnace and heated to 650°C at a heating rate of 5°C / min, kept warm for 8 hours, and then cooled to room temperature with the furnace to obtain a manganese iron phosphate lithium positive electrode material.
[0109] (3) According to the mass liquid-solid ratio of 0.004:1, corresponding amounts of manganese hydroxide solution and lithium manganese iron phosphate material were taken and hydrothermally reacted at a temperature of 210°C for 30 hours. After the hydrothermal reaction, it was allowed to cool naturally to room temperature. The cooled product was filtered and then placed in an oven for drying at 160°C for 18 hours. It was calcined at 450°C for 1.5 hours to obtain a lithium manganese iron phosphate positive electrode material with a surface coated with Mn(OH)2.
[0110] The positive electrode materials in Examples 1-7 and Comparative Examples 1-4 are assembled into positive electrode sheets. The specific assembly method includes: adding the positive electrode material powder and conductive agent obtained in Examples 1-7 and Comparative Examples 1-4 to PVDF glue (the mass ratio of positive electrode material powder: conductive agent: PVDF glue is 96.8:1.2:2) to mix to obtain a positive electrode slurry, coating the positive electrode slurry on the surface of the positive electrode current collector, and preparing the positive electrode sheet after roller drying.
[0111] After the positive electrode sheet and the graphite negative electrode sheet were assembled into a full battery, the cycle performance and electrochemical corrosion resistance were tested. The test results are shown in Table 1.
[0112] The test method for the cycle performance of lithium manganese iron phosphate is: testing at 25°C (1C / 1C 2.0~4.3V), and the test method for the cycle performance of lithium nickel cobalt manganese oxide is: testing at 25°C (1C / 1C 2.0~4.35V).
[0113] Table 1
[0114] It can be seen from the above table that: From Examples 1-3, it can be seen that the modified lithium manganese iron phosphate positive electrode material described in this application exhibits excellent cycle performance, indicating that this modified lithium manganese iron phosphate material is particularly suitable as a high energy density lithium ion battery positive electrode material.
[0115] In Example 4, the concentrations of the manganese chloride solution and the disodium hydrogen phosphate solution were too high, and the gram capacity of the battery was reduced.
[0116] At the same time, the amount of coating layer also affects the effect. For example, in Examples 5 and 6, the effect is smaller because the coating amount is smaller. In Comparative Example 1, since the Mn4O(PO4)2 modified coating layer is omitted, its cycle performance is significantly worse than that of the examples due to the dissolution of manganese ions.
[0117] The cycle performance of Example 7 is significantly improved compared to that of Comparative Example 2, indicating that this method is also applicable to manganese-containing positive electrode materials such as lithium nickel cobalt manganese oxide, and can also improve the cycle performance of the positive electrode material.
[0118] Comparative Example 3 is a positive electrode material with a surface coated with manganese phosphate. Compared with Example 1, it is found that the surface coating of manganese phosphate on the material affects the conductivity and gram capacity of the material.
[0119] Comparative Example 4 is a positive electrode material with a surface coated with manganese hydroxide. Compared with Example 1, the manganese ions in the manganese hydroxide are easily oxidized to form trivalent manganese ions, which increases the average valence of the manganese ions and affects the cycle performance of the material.
Claims
1. A positive electrode material, comprising a core and a coating layer, wherein the core comprises a manganese-containing positive electrode material, and the coating layer comprises Mn4O(PO4)2.
2. The positive electrode material according to claim 1, wherein The manganese-containing positive electrode material comprises any one of lithium nickel cobalt manganese oxide, lithium-rich manganese base, lithium manganese phosphate or lithium manganese iron phosphate, or a combination of at least two thereof.
3. A method for preparing the positive electrode material according to claim 1 or 2, the preparation method comprising: The phosphate solution and the manganese salt solution are first mixed to obtain a mixed solution, the mixed solution and the manganese-containing positive electrode material are subjected to a hydrothermal reaction to obtain a modified positive electrode material, and the modified positive electrode material is subjected to a first calcination treatment to obtain a positive electrode material with a surface coated with Mn4O(PO4)2.
4. The preparation method according to claim 3, wherein The solute in the manganese salt solution is manganese salt, and the solvent is a mixed solution of alcohol and water.
5. The preparation method according to claim 3 or 4, wherein The manganese salt includes any one of manganese chloride, manganese acetate or manganese nitrate, or a combination of at least two of them.
6. The preparation method according to claim 4, wherein The volume ratio of ethanol to water in the alcohol-water mixed solution is 1:(18-22).
7. The preparation method according to any one of claims 3 to 6, wherein: The concentration of the phosphate solution is 0.1-1.0 mol / L.
8. The preparation method according to claim 3, wherein: The solute in the phosphate solution is phosphate, and the solvent is a mixed solution of alcohol and water.
9. The preparation method according to any one of claims 3 to 8, wherein: The phosphate includes disodium hydrogen phosphate.
10. The preparation method according to claim 8, wherein: The volume ratio of ethanol to water in the alcohol-water mixed solution is 1:(18-22).
11. The preparation method according to any one of claims 3 to 10, wherein: The first mixing comprises: adding the phosphate solution dropwise to the manganese salt solution at a uniform speed, and then stirring; Optionally, the molar ratio of the manganese salt to the phosphate during the dropwise addition is 1:(1-3); Optionally, the stirring speed is 70 to 110 r / min; Optionally, the stirring time is 30 to 60 minutes.
12. The preparation method according to any one of claims 3 to 11, wherein: The liquid-to-solid ratio of the mixed solution to lithium manganese iron phosphate is (0.0003-0.004):1; Optionally, the temperature of the hydrothermal reaction is 160-260°C; Optionally, the hydrothermal reaction time is 12 to 48 hours; Optionally, the hydrothermal reaction is sequentially cooled, filtered and dried; Optionally, the drying temperature is 120-200°C; Optionally, the drying time is 12 to 20 hours; Optionally, the temperature of the first calcination treatment is 400-500°C; Optionally, the first calcination treatment time is 0.5 to 2 hours.
13. The preparation method according to any one of claims 3 to 12, wherein: When the manganese-containing positive electrode material is lithium iron manganese phosphate, the preparation method of the lithium iron manganese phosphate comprises the following steps: (1) a second mixing of an iron source, a manganese source and a phosphorus source to obtain a manganese iron phosphate precursor; (2) mixing the ferromanganese phosphate precursor, the lithium source and the carbon source described in step (1) and performing a second calcination treatment to obtain lithium ferromanganese phosphate; The iron source in step (1) includes ferrous nitrate and / or ferrous sulfate; Optionally, the manganese source includes manganese nitrate and / or manganese sulfate; Optionally, the phosphorus source includes disodium hydrogen phosphate; Optionally, the iron source, manganese source and phosphorus source are in the order of Mn x Fe 1-x The stoichiometric ratios of the elements in PO4 are weighed, where 0.1≤x≤0.
9.
14. The preparation method according to claim 13, wherein: Step (1) The temperature of the first mixing is 40 to 60° C.; Optionally, the second mixing time in step (1) is 3 to 5 hours; Optionally, in step (1), the second mixing is followed by cooling to obtain the ferromanganese phosphate precursor.
15. The preparation method according to claim 13 or 14, wherein: The molar ratio of the ferromanganese phosphate precursor to the lithium source in step (2) is 1:1.05-1.2; Optionally, the carbon source accounts for 4-6 wt% of the total mass of the ferromanganese phosphate precursor and the lithium source; Optionally, the lithium source includes lithium hydroxide and / or lithium carbonate; Optionally, the carbon source comprises glucose and / or sucrose; Optionally, the atmosphere of the second calcination treatment in step (2) is high-purity nitrogen; Optionally, the heating rate of the second calcination treatment is 4 to 6°C / min; Optionally, the temperature of the second calcination treatment is 600-700°C; Optionally, the second calcination treatment is performed for 6 to 10 hours.
16. Use of the positive electrode material according to claim 1 or 2, wherein: The positive electrode material is applied in the field of lithium ion batteries.
Citation Information
Patent Citations
Process for preparing a core-shell structured lithtated manganese oxide
CN104169221A
Thickness-controllable coating method of phosphate
CN105322158A
Ferric-phosphate-coated lithium ion battery cathode material and preparation method thereof
CN107369816A
Method for multiple modification of high-nickel positive electrode material by metal phosphate and obtained positive electrode material
CN112563507A
A cathode active material coated with manganese phosphate for a lithium secondary battery and a preparation method of the same
US20150349339A1