Sodium ion precursor material, and preparation method therefor and use thereof

By using a combined structure of nickel iron manganese core and nickel copper manganese coating in the sodium ion battery cathode material, the problems of hygroscopicity and structural stability are solved, and the high rate performance and cycle stability of the sodium ion battery material are improved.

WO2024198194A1PCT designated stage expired Publication Date: 2024-10-03JINGMEN GEM NEW MATERIAL CO LTD +1

Patent Information

Application Number
PCT/CN2023/111896
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-08-09
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing layered oxide sodium ion battery cathode materials have problems such as strong hygroscopicity and easy structure collapse, resulting in loss of electrochemical activity. High-entropy metal oxide materials synthesized by high-temperature solid-state methods have uneven element distribution and irregular morphology. , difficult to apply on a large scale.

Method used

Using sodium ion precursor material, the core is nickel iron manganese hydroxide, and the outer cladding layer is nickel copper manganese hydroxide. It is prepared by co-precipitation method to form a sodium ion precursor material with uniform morphology and stable structure, improving the material rate performance and cycle stability.

Benefits of technology

The sodium ion cathode material has a uniform morphology and a stable structure, improving its rate performance and cycle stability. The first discharge specific capacity reaches more than 146.1mAh/g, and the capacity retention rate after 50 cycles can reach more than 95.3%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023111896-FTAPPB-I100001
    Figure PCTCN2023111896-FTAPPB-I100001
  • Figure PCTCN2023111896-FTAPPB-I100002
    Figure PCTCN2023111896-FTAPPB-I100002
Patent Text Reader

Abstract

The present application provides a sodium ion precursor material, and a preparation method therefor and a use thereof. The sodium ion precursor material comprises a core and a coating layer on the surface of the core, wherein the core comprises nickel-iron-manganese hydroxide, and the coating layer comprises nickel-copper-manganese hydroxide. According to the sodium ion precursor material provided by the present application, the inner layer is nickel-iron-manganese having high capacity, and the outer layer is nickel-copper-manganese having high stability, so that the stability of an iron-based sodium ion precursor material and an iron-based sodium ion positive electrode material is improved, and the copper element can be uniformly phased in a nickel-iron-manganese-based precursor material and a nickel-iron-manganese-based positive electrode material, thereby improving the rate capability and the cycle stability of a sodium-ion positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

A sodium ion precursor material and its preparation method and use Technical Field

[0001] The present application belongs to the technical field of sodium ion batteries and relates to a sodium ion precursor material and a preparation method and use thereof. Background Art

[0002] Sodium-ion batteries (SIBs), with their resource and cost advantages, show great potential for large-scale energy storage and low-speed electric vehicles. Layered oxides, with their high theoretical capacity and ease of synthesis, are currently one of the most promising cathode materials for SIBs.

[0003] For example, CN112510196A discloses a method for preparing a manganese-based metal oxide positive electrode, and the production steps include the following: S1, grinding and firing: grinding cobalt tetroxide, nickel oxide, manganese oxide, and sodium carbonate in a stoichiometric ratio in an agate mortar and grinding them thoroughly, then firing them in a muffle furnace at 500°C for 3 hours and then continuously heating them to 850°C for 12 hours; S2, cooling and isolation: after cooling to room temperature, storing the obtained solid powder in an argon-protected glove box to isolate it from air and moisture; S3, positive electrode coating; S4, preparing materials; S5, stirring and mixing; S6, adding the slurry dropwise; S7, vacuum drying.

[0004] Layered oxide cathode materials have the following issues: 1) They are highly hygroscopic, absorbing large amounts of moisture from the air and causing them to fail; 2) After long battery cycles, the cathode material structure easily collapses, leading to a loss of electrochemical activity. To achieve efficient resource utilization of layered oxide cathode materials and further reduce the cost of sodium-ion batteries, it is necessary to electrochemically restore the electrochemical activity of failed or inactive layered oxide cathode materials.

[0005] In order to improve the cycle stability and rate performance of layered oxide sodium materials, it is usually possible to prepare multi-element or high entropy metal oxides to suppress the order of transition metals, charge order and Na + / Vacancy ordering.

[0006] Currently reported high-entropy metal oxide sodium-ion battery materials are all synthesized using high-temperature solid-phase methods. For example, CN112467119A discloses a method for preparing and applying a layered high-entropy oxide sodium-ion battery cathode material. This method belongs to the field of sodium-ion battery cathode materials and uses a high-temperature solid-phase method for its preparation. On the one hand, the above method suffers from uneven element distribution and irregular morphology with poor consistency, which affects performance. On the other hand, impurities and metallic foreign matter are difficult to control, making it unsuitable for large-scale application. If a co-precipitation method is used, many elements, such as copper, are difficult to co-precipitate with nickel and manganese to form a single phase when the doping level is high.

[0007] Therefore, how to obtain a homogeneous multi-element sodium ion positive electrode material and improve its electrochemical performance is a technical problem that needs to be solved urgently.

[0008] Summary of the Invention

[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0010] The purpose of this application is to provide a sodium ion precursor material, its preparation method, and its use. This application provides a sodium ion precursor material with a high-capacity inner layer of nickel-iron-manganese and a high-stability outer layer of nickel-copper-manganese. This improves the stability of the iron-based sodium ion precursor material and the positive electrode material, and also allows the copper element to form a uniform phase in the precursor material and positive electrode material of the nickel-iron-manganese system, thereby improving the rate performance and cycle stability of the sodium ion positive electrode material.

[0011] To achieve this goal, this application adopts the following technical solutions:

[0012] In a first aspect, an embodiment of the present application provides a sodium ion precursor material, which includes a core and a coating layer located on the surface of the core; the core includes nickel-iron-manganese hydroxide, and the coating layer includes nickel-copper-manganese hydroxide.

[0013] The embodiments of the present application provide a sodium ion precursor material with uniform morphology and stable structure. The inner core is nickel-iron-manganese with high capacity, and the outer coating layer is nickel-copper-manganese with high stability. It fully utilizes the high capacity characteristics of the iron-based material while improving its stability. It also allows the copper element to form a uniform phase in the precursor material and positive electrode material of the nickel-iron-manganese system, thereby improving the rate performance and cycle stability of the sodium ion positive electrode material.

[0014] In the embodiment of the present application, if there is no coating layer, the copper element is directly located in the core, which will lead to a decrease in cycle stability; and if the material of the core and the material of the coating layer are exchanged with each other, the purpose of improving capacity and cycle stability cannot be achieved.

[0015] In one embodiment, the coating layer has a thickness of 0.3 to 1.5 μm, for example, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm or 1.5 μm.

[0016] In the embodiment of the present application, if the coating layer is too thick, that is, too much nickel-copper-manganese hydroxide is added, it is not conducive to the capacity; and if the thickness is too thin, the cycle stability will deteriorate.

[0017] In one embodiment, the D50 of the core is 3 to 18 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm or 18 μm.

[0018] In the embodiment of the present application, if the D50 of the core is too small, it will affect the compaction density, while if the D50 is too large, it will lead to low capacity.

[0019] In one embodiment, the nickel-iron-manganese hydroxide and the nickel-copper-manganese hydroxide further include doping elements.

[0020] In the sodium ion precursor provided in the embodiment of the present application, a substance with five or more elements is obtained after adding a doping element, thereby obtaining a high-entropy sodium ion positive electrode material, which is beneficial to improving the cycle stability and rate performance of the battery.

[0021] In one embodiment, the doping element includes any one of Mg, Al, Zn, Ti, Zr or W, or a combination of at least two of them.

[0022] In one embodiment, the doping amount of the doping element in the sodium ion precursor is 500-10000 ppm, for example, 500 ppm, 1000 ppm, 2000 ppm, 3000 ppm, 4000 ppm, 5000 ppm, 6000 ppm, 7000 ppm, 8000 ppm, 9000 ppm or 10000 ppm.

[0023] In the embodiment of the present application, if the doping amount of the doping element is too much, the material capacity will be affected.

[0024] In a second aspect, an embodiment of the present application provides a method for preparing the sodium ion precursor material as described in the first aspect, the preparation method comprising the following steps:

[0025] (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution, and a complexing agent solution to a bottom solution in parallel to perform a coprecipitation reaction to obtain a core;

[0026] (2) After obtaining the core of the target particle size described in step (1), the nickel-iron-manganese mixed salt solution is replaced with a nickel-iron-copper mixed salt solution to continue the coprecipitation reaction to obtain the sodium ion precursor material.

[0027] The preparation method provided in the embodiment of the present application first obtains nickel-iron-manganese into balls and then precipitates nickel-copper-manganese, which overcomes the problem that copper is difficult to precipitate homogeneously with nickel-iron-manganese, can greatly increase the copper content, and obtains a sodium ion precursor material with a stable core-shell structure. The sodium ion material obtained by further sintering has high capacity and good stability, and its rate performance and cycle performance are improved.

[0028] In the embodiments of the present application, the method of first obtaining nickel-iron-manganese hydroxide and then precipitating nickel-copper-manganese hydroxide is adopted to effectively solve the problem that copper and nickel-iron-manganese are difficult to precipitate homogeneously, and the core-shell structure can also stabilize the structure of the inner core, that is, the structure of the precursor material and the method complement each other and influence each other.

[0029] In one embodiment, the nickel-iron-manganese mixed salt solution in step (1) further includes a reducing agent.

[0030] The role of the reducing agent in the embodiment of the present application is to prevent the divalent iron ions in the nickel-iron-manganese mixed salt solution from being oxidized to trivalent iron ions. The type of reducing agent is an acidic reducing agent, such as VC.

[0031] In one embodiment, the molar concentration of the nickel-iron-manganese mixed salt solution in step (1) is 0.5 to 2.5 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or 2.5 mol / L.

[0032] In one embodiment, the pH value of the base solution in step (1) is 9-11, for example, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8 or 11.

[0033] In one embodiment, the base solution in step (1) comprises a precipitant, a complexing agent and water.

[0034] In the examples of the present application, the base solution is prepared by conventional techniques, including but not limited to:

[0035] Add pure water accounting for 1 / 3-3 / 4 of the volume of the reactor into the reactor, introduce N2 protection and start stirring, then add precipitant and complexing agent, adjust the pH value and the concentration of the complexing agent to obtain the required base liquid.

[0036] In one embodiment, the mass concentration of the complexing agent in the base solution of step (1) is 10-20 g / L, for example, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L or 20 g / L.

[0037] In one embodiment, the raw materials added in parallel in step (1) also include a dopant solution.

[0038] In one embodiment, the temperature of the coprecipitation reaction in step (1) is 40-70°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C.

[0039] In one embodiment, the pH value of the coprecipitation reaction in step (1) is 10-11, for example, 10, 10.3, 10.5, 10.8 or 11.

[0040] In one embodiment, the stirring speed of the coprecipitation reaction in step (1) is 200-500 rpm, for example, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm or 500 rpm.

[0041] In one embodiment, the nickel-copper-manganese mixed salt solution in step (2) further includes a reducing agent.

[0042] In one embodiment, the molar concentration of the nickel-copper-manganese mixed salt solution in step (2) is 0.5 to 2.5 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or 2.5 mol / L.

[0043] In one embodiment, the raw materials in the co-precipitation reaction process of step (2) also include a dopant solution.

[0044] As an optional technical solution, the preparation method includes the following steps:

[0045] (1) adding a nickel-iron-manganese mixed salt solution having a molar concentration of 0.5 to 2.5 mol / L, a precipitant solution, a dopant solution, and a complexing agent solution to a base solution in parallel, maintaining a pH value of 10 to 11, and performing a coprecipitation reaction at 40 to 70° C. and 200 to 500 rpm to obtain a core;

[0046] (2) After obtaining the core of step (1), the nickel-iron-manganese mixed salt solution is replaced with a nickel-iron-copper mixed salt solution to continue the coprecipitation reaction to obtain the sodium ion precursor material;

[0047] Wherein, the nickel-iron-manganese mixed salt solution in step (1) also includes a reducing agent; and the nickel-copper-manganese mixed salt solution in step (2) also includes a reducing agent.

[0048] In a third aspect, an embodiment of the present application provides a sodium ion oxide positive electrode material, wherein the sodium ion oxide positive electrode material is obtained by mixing and sintering the sodium ion precursor material as described in the first aspect with a sodium source;

[0049] The sodium ion oxide positive electrode material includes a core and a coating layer located on the surface of the core; the core includes nickel-iron-manganese sodium oxide, and the coating layer includes nickel-copper-manganese sodium oxide.

[0050] In one embodiment, the sintering temperature is 800-1000°C.

[0051] In one embodiment, the sintering time is 10 to 20 hours.

[0052] In one embodiment, the nickel-iron-manganese sodium oxide and the nickel-copper-manganese sodium oxide further include doping elements.

[0053] In a fourth aspect, an embodiment of the present application further provides a sodium ion battery, which includes the sodium ion oxide positive electrode material as described in the third aspect.

[0054] Compared with the prior art, this application has the following beneficial effects:

[0055] The sodium ion precursor material provided in the present application has a uniform morphology and a stable structure. The inner core is nickel-iron-manganese with a higher capacity, and the outer coating is nickel-copper-manganese with a higher stability. It fully utilizes the high capacity characteristics of the iron-based material while also improving its stability. In the preparation process, nickel-iron-manganese is first obtained into balls and then nickel-copper-manganese is precipitated, overcoming the problem that copper is difficult to precipitate homogeneously with nickel-iron-manganese, which can greatly increase the copper content and thereby improve the rate performance and cycle stability of the sodium ion positive electrode material. The positive electrode in the sodium ion battery is prepared from the precursor material provided in this application, and the core D50 of the precursor is 3 to 18 μm, the thickness of the coating layer is in the range of 0.3 to 1.5 μm, and under a discharge voltage of 2.0-4.0 V, the battery's first discharge specific capacity at 0.1C can reach more than 146.1 mAh / g, and the rate performance at 1C / 0.1C can reach more than 96.1%. The first cycle is tested at 0.1C / 0.1C charge and discharge, and the capacity retention rate after 50 cycles at 0.5C / 1C can reach more than 95.3%. DETAILED DESCRIPTION

[0056] The technical solution of the present application is further illustrated below by specific examples. Those skilled in the art should understand that the examples are only for facilitating understanding of the present application and should not be regarded as specific limitations of the present application.

[0057] Example 1

[0058] This embodiment provides a sodium ion precursor material, which includes a core (D50 is 3um) and a coating layer (thickness is 0.3um) coated on the surface of the core, the core is magnesium-doped nickel-iron-manganese hydroxide (the molar ratio of Ni, Fe and Mn is 1:1:1), and the coating layer is magnesium-doped nickel-copper-manganese hydroxide (the molar ratio of Ni, Cu and Mn is 1:1:1), wherein the doping amount of magnesium in the precursor material is 1000ppm.

[0059] The preparation method of the sodium ion precursor material is as follows:

[0060] (1) A nickel-iron-manganese mixed sulfate solution (nickel-iron-manganese molar ratio of 1:1:1) containing a reducing agent with a molar concentration of 2 mol / L, a magnesium sulfate solution with a molar concentration of 0.01 mol / L, a sodium hydroxide solution (mass concentration of 32%), and an ammonia solution with a mass concentration of 15% were added to a base liquid (the pH value of the base liquid was 11, and the concentration of ammonia was 10 g / L), and a reaction environment with a pH value of 10.5 was maintained. A coprecipitation reaction was carried out at 50° C. and a rotation speed of 500 rpm. When D50 reached 3 μm, the feeding was stopped to obtain a kernel;

[0061] (2) After obtaining the core, the nickel-iron-manganese mixed sulfate solution is replaced with a nickel-copper-manganese mixed sulfate solution containing a reducing agent with a molar concentration of 2 mol / L, while other raw materials remain unchanged, and the solution is added to the bottom liquid to continue the coprecipitation reaction until D50 reaches 3.6 μm. The material in the kettle is centrifuged, washed, dried, and sieved to obtain the sodium ion precursor material.

[0062] Example 2

[0063] The present embodiment provides a sodium ion precursor material, which includes a core (D50 is 10um) and a coating layer (thickness is 0.5um) coated on the surface of the core, the core is zirconium-doped nickel-iron-manganese hydroxide (the molar ratio of Ni, Fe and Mn is 4:2:4Ni / Fe / Mn40 / 20 / 40), and the coating layer is zirconium-doped nickel-copper-manganese hydroxide (the molar ratio of Ni, Cu and Mn is 4:2:4), wherein the doping amount of zirconium in the precursor material is 3000ppm.

[0064] The preparation method of the sodium ion precursor material is as follows:

[0065] (1) A nickel-iron-manganese mixed sulfate solution (nickel-iron-manganese molar ratio of 4:2:4) containing a reducing agent with a molar concentration of 0.5 mol / L, a zirconium sulfate solution with a molar concentration of 0.01 mol / L, a sodium hydroxide solution (mass concentration of 32%), and an ammonia solution with a mass concentration of 16% were added to a base liquid (the pH value of the base liquid was 10, and the concentration of ammonia was 15 g / L), the reaction environment was maintained at a pH of 10, and a coprecipitation reaction was carried out at 70° C. and a rotation speed of 300 rpm. When the D50 reached 10 μm, the feeding was stopped to obtain a kernel;

[0066] (2) After obtaining the core, the nickel-iron-manganese mixed sulfate solution is replaced with a nickel-copper-manganese mixed sulfate solution containing a reducing agent with a molar concentration of 0.5 mol / L, while other raw materials remain unchanged, and the solution is added to the bottom liquid to continue the coprecipitation reaction until D50 reaches 11 μm. The material in the kettle is centrifuged, washed, dried, and sieved to obtain the sodium ion precursor material.

[0067] Example 3

[0068] This embodiment provides a sodium ion precursor material, which includes a core (D50 is 18um) and a coating layer (thickness is 1.5um) coated on the surface of the core, the core is aluminum-doped nickel-iron-manganese hydroxide (the molar ratio of Ni, Fe and Mn is 5:2:3), and the coating layer is aluminum-doped nickel-copper-manganese hydroxide (the molar ratio of Ni, Cu and Mn is 5:2:3), wherein the doping amount of aluminum in the precursor material is 5000ppm.

[0069] The preparation method of the sodium ion precursor material is as follows:

[0070] (1) A nickel-iron-manganese mixed sulfate solution (nickel-iron-manganese molar ratio of 5:2:3) containing a reducing agent with a molar concentration of 2.5 mol / L, a sodium metaaluminate solution with a molar concentration of 0.05 mol / L, a sodium hydroxide solution (mass concentration of 32%), and an ammonia solution with a mass concentration of 15% were added to a base liquid (the pH value of the base liquid was 9, and the concentration of ammonia was 10 g / L), the reaction environment was maintained at a pH of 10.5, and a coprecipitation reaction was carried out at 40° C. and a rotation speed of 200 rpm. When the D50 reached 18 μm, the feeding was stopped to obtain a kernel;

[0071] (2) After obtaining the core, the nickel-iron-manganese mixed sulfate solution is replaced with a nickel-copper-manganese mixed sulfate solution containing a reducing agent with a molar concentration of 2.5 mol / L, while other raw materials remain unchanged. The solution is added to the bottom liquid and the coprecipitation reaction is continued until the D50 reaches 21 μm. The material in the kettle is centrifuged, washed, dried, and sieved to obtain the sodium ion precursor material.

[0072] Example 4

[0073] The difference between this embodiment and embodiment 1 is that the sodium ion precursor material provided in this embodiment is not doped with magnesium element, and no magnesium sulfate solution is added in the preparation method.

[0074] The rest of the preparation methods and parameters were the same as those in Example 1.

[0075] Example 5

[0076] The difference between this embodiment and embodiment 1 is that the D50 of the core of the sodium ion precursor material in this embodiment is 2 μm, and the co-precipitation time is adaptively adjusted in the preparation method.

[0077] The rest of the preparation methods and parameters were the same as those in Example 1.

[0078] Example 6

[0079] The difference between this embodiment and embodiment 1 is that the D50 of the core of the sodium ion precursor material in this embodiment is 20 μm, and the co-precipitation time is adaptively adjusted in the preparation method.

[0080] The rest of the preparation methods and parameters were the same as those in Example 1.

[0081] Example 7

[0082] The difference between this embodiment and embodiment 1 is that the thickness of the coating layer of the sodium ion precursor material in this embodiment is 2 μm, and the co-precipitation time is adaptively adjusted in the preparation method.

[0083] The rest of the preparation methods and parameters were the same as those in Example 1.

[0084] Example 8

[0085] The difference between this embodiment and embodiment 1 is that the thickness of the coating layer of the sodium ion precursor material in this embodiment is 0.1 μm, and the co-precipitation time is adaptively adjusted in the preparation method.

[0086] The rest of the preparation methods and parameters were the same as those in Example 1.

[0087] Comparative Example 1

[0088] The difference between this comparative example and Example 1 is that the sodium ion precursor material in this comparative example is magnesium-doped nickel-iron-copper-manganese hydroxide (the molar ratio of Ni, Fe, Cu and Mn is 33.3:25.1:8.2:33.3), that is, a non-core-shell structure; and a nickel-iron-manganese-copper mixed sulfate solution is selected for coprecipitation reaction in the preparation method.

[0089] The rest of the preparation methods and parameters were the same as those in Example 1.

[0090] Comparative Example 2

[0091] The difference between this comparative example and Example 1 is that in this comparative example, the core material and the coating layer material are exchanged with each other, and the materials in the preparation method are also exchanged with each other.

[0092] The rest of the preparation methods and parameters were the same as those in Example 1.

[0093] The sodium ion precursor material sodium carbonate provided by Example 1-8 and Comparative Example 1-2 was mixed, sintered at 1000° C. for 12 h, and the obtained material was pulverized to obtain a sodium ion oxide positive electrode material.

[0094] A positive electrode sheet is prepared from a sodium ion oxide positive electrode material, and a button battery is prepared using the sodium sheet as a counter electrode.

[0095] The batteries provided in Examples 1-8 and Comparative Examples 1-2 were subjected to electrochemical performance testing under the following conditions: a charge-discharge voltage of 2.0-4.0 V, with an initial charge-discharge cycle of 0.1C / 0.1C, followed by 50 cycles at 0.5C / 1C. The test results are shown in Table 1.

[0096] Table 1

[0097] From the data results of Example 1 and Example 4, it can be seen that without doping, the rate performance and cycle performance are significantly reduced.

[0098] From the data results of Example 1, Example 5 and Example 6, it can be seen that if the core particle size is too small, the cycle performance will be reduced, while if the particle size is too large, the capacity and rate performance will be affected.

[0099] From the data results of Examples 1, 7 and 8, it can be seen that if the thickness of the coating layer is too thick, the capacity and rate performance will be significantly reduced, while if the thickness is too thin, it will not be conducive to improving the cycle performance.

[0100] From the data results of Example 1 and Comparative Example 1, it can be seen that the non-core-shell structure, that is, the copper element is directly doped into nickel-iron-manganese, cannot achieve a significant improvement in comprehensive performance such as capacity, rate and cycle performance.

[0101] From the data results of Example 1 and Comparative Example 2, it can be seen that the core is nickel-copper-manganese and the coating is nickel-iron-manganese, which not only fails to improve the cycle performance, but accelerates the capacity decay.

[0102] In summary, the sodium ion precursor material provided by the present application has uniform morphology and stable structure. The core is nickel-iron-manganese with high capacity, and the outer coating is nickel-copper-manganese with high stability. It fully utilizes the high capacity characteristics of the iron-based material while also improving its stability. In the preparation process, nickel-iron-manganese is first obtained into balls and then nickel-copper-manganese is precipitated, which overcomes the problem that copper is difficult to precipitate homogeneously with nickel-iron-manganese, and can greatly increase the copper content, thereby improving the rate performance and cycle stability of the sodium ion positive electrode material. The positive electrode in the sodium ion battery is prepared from the precursor material provided in this application, and the core D50 of the precursor is 3 to 18 μm, the thickness of the coating layer is in the range of 0.3 to 1.5 μm, and under a discharge voltage of 2.0-4.0 V, the battery's first discharge specific capacity at 0.1C can reach more than 146.1 mAh / g, and the rate performance at 1C / 0.1C can reach more than 96.1%. The first cycle is tested at 0.1C / 0.1C charge and discharge, and the capacity retention rate after 50 cycles at 0.5C / 1C can reach more than 95.3%.

[0103] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.

Claims

1. A sodium ion precursor material, comprising a core and a coating layer located on the surface of the core; the core comprises nickel-iron-manganese hydroxide, and the coating layer comprises nickel-copper-manganese hydroxide.

2. The sodium ion precursor material according to claim 1, wherein The thickness of the coating layer is 0.3 to 1.5 μm; Optionally, the D50 of the inner core is 3-18 μm.

3. The sodium ion precursor material according to claim 1 or 2, wherein The nickel-iron-manganese hydroxide and the nickel-copper-manganese hydroxide also include doping elements; Optionally, the doping element includes any one of Mg, Al, Zn, Ti, Zr or W, or a combination of at least two thereof; Optionally, the doping amount of the doping element in the sodium ion precursor is 500 to 10000 ppm.

4. A method for preparing the sodium ion precursor material according to any one of claims 1 to 3, the preparation method comprising the following steps: (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent solution to a bottom solution in parallel to perform a coprecipitation reaction to obtain a core; (2) After obtaining the inner core of step (1), the nickel-iron-manganese mixed salt solution is replaced with a nickel-iron-copper mixed salt solution to continue the coprecipitation reaction to obtain the sodium ion precursor material.

5. The method for preparing the sodium ion precursor material according to claim 4, wherein: The nickel-iron-manganese mixed salt solution in step (1) also includes a reducing agent; Optionally, the molar concentration of the nickel-iron-manganese mixed salt solution in step (1) is 0.5 to 2.5 mol / L; Optionally, the pH value of the base solution in step (1) is 9 to 11; Optionally, the base solution in step (1) comprises a precipitant, a complexing agent and water; Optionally, the mass concentration of the complexing agent in the base solution of step (1) is 10 to 20 g / L.

6. The method for preparing the sodium ion precursor material according to claim 4 or 5, wherein: The raw materials added in parallel in step (1) also include a dopant solution; Optionally, the temperature of the coprecipitation reaction in step (1) is 40 to 70° C.; Optionally, the pH value of the coprecipitation reaction in step (1) is 10 to 11; Optionally, the stirring speed of the coprecipitation reaction in step (1) is 200 to 500 rpm.

7. The method for preparing a sodium ion precursor material according to any one of claims 4 to 6, wherein: The nickel-copper-manganese mixed salt solution in step (2) also includes a reducing agent; Optionally, the molar concentration of the nickel-copper-manganese mixed salt solution in step (2) is 0.5 to 2.5 mol / L; Optionally, the raw materials in the coprecipitation reaction process of step (2) also include a dopant solution.

8. The method for preparing a sodium ion precursor material according to any one of claims 4 to 7, wherein: The preparation method comprises the following steps: (1) adding a nickel-iron-manganese mixed salt solution with a molar concentration of 0.5 to 2.5 mol / L, a precipitant solution, a doping agent solution and a complexing agent solution to a base solution in parallel, maintaining a pH value of 10 to 11, and performing a coprecipitation reaction at 40 to 70° C. and 200 to 500 rpm to obtain a core; (2) after obtaining the inner core of step (1), the nickel-iron-manganese mixed salt solution is replaced with a nickel-iron-copper mixed salt solution to continue the coprecipitation reaction to obtain the sodium ion precursor material; Wherein, the nickel-iron-manganese mixed salt solution in step (1) also includes a reducing agent; and the nickel-copper-manganese mixed salt solution in step (2) also includes a reducing agent.

9. A sodium ion oxide positive electrode material, wherein the sodium ion oxide positive electrode material is obtained by mixing and sintering the sodium ion precursor material according to any one of claims 1 to 3 and a sodium source; The sodium ion oxide positive electrode material comprises a core and a coating layer located on the surface of the core; the core comprises nickel-iron-manganese sodium oxide, and the coating layer comprises nickel-copper-manganese sodium oxide.

10. The sodium ion oxide positive electrode material according to claim 9, wherein The sintering temperature is 800-1000°C; Optionally, the sintering time is 10 to 20 hours; Optionally, the nickel-iron-manganese sodium oxide and the nickel-copper-manganese sodium oxide also include doping elements.

11. A sodium ion battery, comprising the sodium ion oxide positive electrode material according to claim 9 or 10.

Citation Information

Patent Citations

  • Preparation method of nickel-aluminum coated nickel-iron-manganese sodium ion precursor material

    CN114291852A

  • Precursor of sodium ion positive electrode material, preparation method and positive electrode material

    CN114956202A

  • Sodium-ion battery positive electrode material, precursor and preparation method

    CN115057482A

  • Precursor for multi-layer coated sodium ion positive electrode material and preparation method of precursor

    CN115448384A

  • Net-shaped copper-doped sodium nickel manganese oxide positive electrode material of sodium-ion battery and preparation method of positive electrode material

    CN115692717A

Cited By

  • P2 / O3 double-phase composite sodium ion battery positive electrode material as well as preparation method and application thereof

    CN119297269A