Multivalent manganese oxide filler and preparation method therefor and use thereof
Through the oxidation reaction and sintering process of Eucalyptus macrophylla leaf extract and potassium permanganate solution, polyvalent manganese oxide filler was prepared, which solved the problems of complex manganese oxide preparation process and poor denitrification effect, and achieved high-efficiency denitrification. Nitrogen and environmentally friendly porous structure filler, suitable for constructed wetland applications.
Patent Information
- Application Number
- PCT/CN2023/137123
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-12-07
- Publication Date
- 2024-10-03
AI Technical Summary
The existing manganese oxide preparation process is complex and not environmentally friendly, and the denitrification effect in constructed wetlands is not high, resulting in unsatisfactory denitrification effects in traditional constructed wetlands.
The Eucalyptus macrophylla leaf extract and potassium permanganate solution are used for oxidation reaction to form a suspension, which is filtered and dried, and then sintered to prepare polyvalent manganese oxide filler. The combination of oxidation reaction and sintering reaction is used to generate II-containing Polyvalent manganese oxide filler of valence, III-valence and IV-valence manganese.
The prepared polyvalent manganese oxide filler has a loose porous structure, which improves the denitrification effect of the constructed wetland and reduces the difficulty of the preparation process, making it suitable for industrial applications. At the same time, the use of Eucalyptus macrophylla leaf extract makes the process cost-effective and environmentally friendly. .
Smart Images

Figure CN2023137123_03102024_PF_FP_ABST
Abstract
Description
A polyvalent manganese oxide filler and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of artificial wetland denitrification, and in particular to a multivalent manganese oxide filler and a preparation method and application thereof. Background Art
[0002] Constructed wetlands are a newly emerging ecological treatment technology. Compared to traditional activated sludge processes, they offer advantages such as lower operating costs, improved wastewater treatment results, ease of operation and maintenance, and significant ecological benefits. They are well-suited for treating decentralized domestic wastewater in rural areas.
[0003] The denitrification mechanism of artificial wetlands is complex and generally includes nitrification and denitrification, plant absorption, substrate adsorption, and volatilization. Nitrification-denitrification is considered the main way of denitrification in artificial wetlands, accounting for more than 50% of denitrification. However, due to the special flooding structure of artificial wetlands, atmospheric reoxygenation (5.77-18.45 gO2m -2 d -1 ) and root oxygen secretion (0.005~12gO2m -2 d -1 ) provides much less oxygen than consumed (450gO2m -2 d -1 The significant gap between oxygen supply and consumption often results in anaerobic or anoxic conditions in constructed wetlands. Furthermore, due to the low organic carbon source in wastewater and the lack of electron acceptors, denitrification in constructed wetlands is also suppressed. Consequently, due to the lack of dissolved oxygen (DO) and electron acceptors in constructed wetlands, nitrification and denitrification are always suppressed, resulting in suboptimal nitrogen removal performance (40-55%) in traditional constructed wetlands, requiring appropriate technologies and processes to address this issue.
[0004] In recent years, studies have shown that mineral oxides such as iron oxide (FeOx) and manganese oxide (MnOx) can act as electron acceptors to mediate nitrogen cycling under anoxic conditions. Compared with FeOx, MnOx has a lower zero charge point (1.5-4.6) and a 5-6 times higher utilization efficiency in microbial metabolism, making it a promising denitrification material. 3+ / Mn 4+ The denitrification process of ) is mainly achieved through two pathways: the coupling of MnOx reduction and nitrification process and the direct mediation of anaerobic ammonium oxidation process (Mnammox), as shown in formulas (1) to (3): 4MnO2+NH4 + +6H + →4Mn 2+ +NO3 - +5H2O (1) 3MnO2+NH4 + +4H + →3Mn2+ +NO2 - +4H2O (2) 3MnO2+2NH4 + +4H + →3Mn 2+ +N2+6H2O (3)
[0005] Currently, the main methods for preparing manganese oxides include hydrothermal synthesis, chemical precipitation, sol-gel, and template methods. These methods have many drawbacks, such as the requirement of high temperature, high pressure, and acidic environments for hydrothermal synthesis, repeated washing requirements for chemical precipitation, the need for precursors such as metal alkoxides for sol-gel methods, and the high cost of template methods.
[0006] Therefore, a low-consumption, low-cost, energy-saving and environmentally friendly, mild-condition, and simple process has become the main goal of current artificial wetland filler production.
[0007] Summary of the Invention
[0008] In order to solve the problem that the existing preparation of manganese oxides is not environmentally friendly, one of the objectives of the present invention is to provide a method for preparing a multivalent manganese oxide filler.
[0009] The technical solution of the present invention to solve the above technical problems is as follows:
[0010] A method for preparing a multivalent manganese oxide filler comprises the following steps:
[0011] Step 1, adding the Eucalyptus globulus leaf extract to a potassium permanganate solution for oxidation reaction, and stirring to form a suspension;
[0012] Step 2: filtering and drying the suspension in step 1 in sequence to obtain a sintering precursor;
[0013] Step 3: sintering the precursor to obtain a polyvalent manganese oxide filler.
[0014] The beneficial effects of the present invention are as follows: a multivalent manganese oxide filler containing II-valent, III-valent, and IV-valent manganese is prepared by combining an oxidation reaction with a sintering reaction, and the filler is loose and porous; in addition, the oxidation reaction and the sintering reaction are combined in the present invention, which reduces the process difficulty of preparing the multivalent manganese oxide and is beneficial to later industrialization to a certain extent.
[0015] On the basis of the above technical solution, the present invention can also be improved as follows:
[0016] Furthermore, the conditions for the oxidation reaction in step 1 are: reaction at room temperature for 2 to 3 hours.
[0017] Furthermore, the solid-liquid ratio of the suspension in step 1 is: (2-3): 50 g / mL.
[0018] Furthermore, the particle size of the Eucalyptus globulus leaf extract in step 1 is 74-100 μm, and the molar concentration of the permanganate solution in step 1 is 0.15-0.3 mol / L.
[0019] Furthermore, the drying conditions in step 2 are: drying temperature of 70-80° C., and drying time of 24-36 hours.
[0020] Furthermore, the sintering conditions in step 3 are: heating rate of 8-12° C. / min, sintering temperature of 600-900° C., sintering atmosphere of air, and sintering time of 3-4 h.
[0021] Furthermore, the sintering conditions in step 3 are: heating rate of 10° C. / min, sintering temperature of 600° C., sintering atmosphere of air, and sintering time of 3 h.
[0022] A second object of the present invention is to provide a multivalent manganese oxide filler prepared according to the first object.
[0023] The third object of the present invention is to provide an application of the multivalent manganese oxide filler in the second object in denitrification of artificial wetlands.
[0024] The present invention has the following beneficial effects:
[0025] 1. The manganese oxide filler prepared in the present invention has a loose and porous structural feature. When used as a filler for artificial wetlands, it has a strong purification function for the environment and also has an efficient denitrification effect. It also promotes the growth and development of wetland vegetation, enabling artificial wetlands to better play their ecological protection function.
[0026] 2. The polyvalent manganese oxide filler of the present invention is prepared based on the extract of Eucalyptus globulus leaves. The extract of Eucalyptus globulus leaves plays the role of reducing agent and template agent in the formation of the polyvalent manganese oxide filler. Specifically, the extract of Eucalyptus globulus leaves is rich in amino acids, proteins, sugars, vitamins, organic amines and quaternary ammonium ions. The reducing sugars and amino acids in the sugars react with potassium permanganate to make MnO4 - The organic amines and quaternary ammonium ions in the extract of Eucalyptus globulus leaves play the role of structural templates in the preparation of multivalent manganese oxide fillers, specifically: (1) structural guidance, by adding organic matter to change the chemical properties of the substance, providing a certain template for the formation of the final filler structure, and then forming a mesoporous material with a specific crystal phase through calcination; (2) playing a space-filling role in the filler skeleton, which can stabilize the final structure; (3) playing a role in balancing the charge of the product skeleton.
[0027] Therefore, the present invention ultimately forms a polyvalent manganese oxide filler with a stable chemical composition and structure, which is conducive to the utilization and growth of microorganisms and has high nitrogen removal efficiency when used in constructed wetlands. Furthermore, the Eucalyptus globulus leaf extract of the present invention can also be extracted from discarded Eucalyptus globulus dead leaves, which has the advantages of a wide raw material source and low cost.
[0028] 3. The present invention combines oxidation reaction with sintering reaction to prepare a polyvalent manganese oxide filler containing II-valent, III-valent, and IV-valent manganese, and the filler is loose and porous. In addition, the present invention combines oxidation reaction with sintering reaction, which reduces the process difficulty of preparing polyvalent manganese oxide and is beneficial to later industrialization to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a SEM image, wherein (a) and (c) are SEM images of the sintered precursor, and (b) and (d) are SEM images of the multivalent manganese oxide filler;
[0030] FIG2 is an EDS spectrum diagram, wherein (a) is an EDS spectrum diagram of the sintered precursor, and (b) is an EDS spectrum diagram of the multivalent manganese oxide filler;
[0031] FIG3 is an FTIR graph of the sintered precursor and the multivalent manganese oxide filler;
[0032] FIG4 is an XPS graph, wherein (a) is an XPS graph of the sintered precursor, and (b) is an XPS graph of the multivalent manganese oxide filler;
[0033] FIG5 is a curve showing the change in ammonia nitrogen concentration after removal by polyvalent manganese oxide fillers;
[0034] FIG6 is a curve showing the change in nitrate concentration after removal by polyvalent manganese oxide fillers;
[0035] FIG7 is a curve showing the change in total nitrogen concentration removed by polyvalent manganese oxide fillers;
[0036] FIG8 is a curve showing the change in chemical oxygen demand (COD) concentration removed by polyvalent manganese oxide fillers;
[0037] FIG9 is a curve showing the change in ammonia nitrogen removal concentration of fillers prepared with different extracts;
[0038] FIG10 is a curve showing the change in nitrate concentration removed by fillers prepared with different extracts;
[0039] Figure 11 shows the change curve of total nitrogen concentration removed by fillers prepared with different extracts. DETAILED DESCRIPTION
[0040] The following describes a multivalent manganese oxide filler, a preparation method thereof, and applications of the present invention in conjunction with examples.
[0041] However, the present invention may be exemplified in many different forms and should not be construed as limited to the specific embodiments set forth herein; rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0042] The inventors have found through extensive research that the existing manganese oxide preparation process is complex and does not meet environmental protection requirements, and that the existing manganese oxide denitrification efficiency is low.
[0043] Based on this, an embodiment of the first aspect of the present invention provides a method for preparing a multivalent manganese oxide filler, which comprises the following steps:
[0044] Step 1, adding the Eucalyptus globulus leaf extract to a potassium permanganate solution for oxidation reaction, and stirring to form a suspension;
[0045] Step 2: filtering and drying the suspension in step 1 in sequence to obtain a sintering precursor;
[0046] Step 3: sintering the precursor to obtain a polyvalent manganese oxide filler.
[0047] The Eucalyptus globulus leaf extract in this embodiment is rich in amino acids, proteins, sugars (including reducing sugars), vitamins, organic amines and quaternary ammonium ions, such as macrocarpon aldehyde A, macrocarpon aldehyde B, macrocarpon aldehyde C, macrocarpon aldehyde D, macrocarpon aldehyde E, n-tricaracon-16,18-dione and flavonoids; therefore, after being mixed with potassium permanganate solution, an oxidation reaction occurs, and the reducing sugars in the Eucalyptus globulus leaf extract work together with the amino acids to convert MnO4 - Reduction generates different low-valent states (such as III and IV manganese).
[0048] Sintering can convert IV manganese in the precursor into manganese of different valence states, and the reaction formulas are as follows (4) to (5): 4MnO2=2Mn2O3+O2 (4) 6Mn2O3=4Mn3O4+O2 (5);
[0049] In addition, the organic amines and quaternary ammonium ions in the extract of Eucalyptus globulus leaves can play the role of structural templates in the formation of polyvalent manganese oxide fillers, specifically: (1) structural guidance, by adding organic matter to change the chemical properties of the substance, providing a certain template for the formation of the final filler structure, and then forming a mesoporous material with a specific crystal phase through calcination; (2) playing a space-filling role in the filler skeleton, which can stabilize the final structure; (3) playing a role in balancing the charge of the product skeleton.
[0050] Specifically, the present invention combines an oxidation reaction with a sintering reaction to produce a multivalent manganese oxide (including manganese II, III, and IV). Furthermore, the multivalent manganese oxide prepared in the present invention has a loose and porous structure, demonstrating a high denitrification effect. Furthermore, combining the oxidation and sintering reactions reduces the complexity of the multivalent manganese oxide preparation process.
[0051] In addition, the Eucalyptus globulus leaf extract in this embodiment is available on the market. The Eucalyptus globulus leaf extract in this embodiment is produced by Shaanxi Suao Biotechnology Co., Ltd.
[0052] In some embodiments, the oxidation reaction in step 1 is carried out at room temperature for 2-3 hours. Under these conditions, potassium permanganate is completely reduced to low-valent manganese oxides by the reducing sugars and amino acids in the Eucalyptus globulus leaf extract. Furthermore, in this embodiment, the stirring speed is typically 400 rpm.
[0053] In addition, in some embodiments, the solid-liquid ratio of the suspension in step 1 is (2-3):50 g / mL. A solid-liquid ratio within this range ensures the yield and effectiveness of the preparation of the polyvalent manganese oxide filler, and avoids excessive amounts of Eucalyptus globulus leaf extract powder when the solid-liquid ratio exceeds this range, ultimately resulting in incomplete reaction with the potassium permanganate solution; and avoids insufficient amounts of Eucalyptus globulus leaf extract powder when the solid-liquid ratio is below this range, resulting in waste of potassium permanganate or overreaction. Preferably, the solid-liquid ratio of the suspension in this embodiment is 3:50 g / mL.
[0054] In addition, in some embodiments, the particle size of the Eucalyptus globulus leaf extract in step 1 is 74 to 100 μm, and the molar concentration of the permanganate solution in step 1 is 0.15 to 0.3 mol / L. First, in this embodiment, the Eucalyptus globulus leaf extract of this particle size and the potassium permanganate solution are more likely to form a suspension, which is conducive to the full oxidation reaction between the Eucalyptus globulus leaf extract and potassium permanganate; and the potassium permanganate solution in this molar concentration range ensures that the potassium permanganate in the suspension with a solid-liquid ratio of (2 to 3): 50 g / mL can completely react with the Eucalyptus globulus leaf extract, avoiding the effect of too much or too little potassium permanganate on the generated multivalent manganese oxides. Preferably, the molar concentration of the potassium permanganate solution in this embodiment is 0.2 mol / L.
[0055] In addition, in some embodiments, the drying conditions in step 2 are: a drying temperature of 70 to 80° C. and a drying time of 24 to 36 hours.
[0056] In addition, in some embodiments, the sintering conditions in step 3 are: a heating rate of 8-12°C / min, a sintering temperature of 600-900°C, a sintering atmosphere of air, and a sintering time of 3-4 hours. Sintering under these conditions is conducive to the formation of MnO2 into oxides of different manganese valences (see the above formulas (4) and (5)), while also avoiding the decomposition of organic matter in the Eucalyptus globulus leaf extract due to excessively high temperatures; and also avoiding the incomplete decomposition of the Eucalyptus globulus leaf extract due to excessively low temperatures, which affects the effect of the conversion of MnO2 into manganese oxides of different valences. Preferably, the sintering conditions in step 3 are: a heating rate of 10°C / min, a sintering temperature of 600°C, a sintering atmosphere of air, and a sintering time of 3 hours. Under these conditions, the organic matter in the Eucalyptus globulus leaf extract that serves as a template can be completely decomposed, thereby increasing the specific surface area of the multivalent manganese oxide filler to a certain extent, while having low energy consumption.
[0057] The embodiment of the second aspect of the present invention provides a multivalent manganese oxide filler prepared according to the embodiment of the first aspect. The multivalent manganese oxide filler of the present invention has a loose and porous structure and also has the characteristics of good denitrification effect.
[0058] The embodiment of the third aspect of the present invention provides an application of the multivalent manganese oxide filler of the embodiment of the second aspect in denitrification in artificial wetlands.
[0059] Example
[0060] Example 1
[0061] A method for preparing a multivalent manganese oxide filler comprises the following steps:
[0062] Step 1: Add a 74 μm eucalyptus globulus leaf extract to a 0.15 mol / L potassium permanganate solution for oxidation reaction, and stir to form a suspension; wherein the oxidation reaction conditions are: reaction at room temperature for 2 hours, a solid-liquid ratio of the suspension of 2:50 g / mL, and a stirring speed of 400 rpm.
[0063] Step 2: Filter, wash and dry the suspension in step 1 in sequence to obtain a sintering precursor; wherein the drying conditions are: temperature of 70° C. and time of 24 hours.
[0064] Step 3: sintering the precursor to obtain a polyvalent manganese oxide filler; wherein the sintering conditions are: a heating rate of 8° C. / min, a sintering temperature of 700° C., a sintering atmosphere of air, and a sintering time of 4 hours.
[0065] Example 2
[0066] A method for preparing a multivalent manganese oxide filler comprises the following steps:
[0067] Step 1: Add a 74 μm eucalyptus globulus leaf extract to a 0.2 mol / L potassium permanganate solution for oxidation reaction, and stir to form a suspension; wherein the oxidation reaction conditions are: reaction at room temperature for 3 hours, the solid-liquid ratio of the suspension is 3:50 g / mL, and the stirring speed is 400 rpm.
[0068] Step 2: Filter, wash and dry the suspension in step 1 in sequence to obtain a sintering precursor; wherein the drying conditions are: temperature of 75° C. and time of 26 hours.
[0069] Step 3: sintering the precursor to obtain a polyvalent manganese oxide filler; wherein the sintering conditions are: a heating rate of 10° C. / min, a sintering temperature of 600° C., a sintering atmosphere of air, and a sintering time of 3 hours.
[0070] Example 3
[0071] A method for preparing a multivalent manganese oxide filler comprises the following steps:
[0072] Step 1: Add a 100 μm eucalyptus globulus leaf extract to a 0.3 mol / L potassium permanganate solution for oxidation reaction, and stir to form a suspension; wherein the oxidation reaction conditions are: reaction at room temperature for 3 hours, the solid-liquid ratio of the suspension is 2.5:50 g / mL, and the stirring speed is 400 rpm.
[0073] Step 2: Filter, wash and dry the suspension in step 1 in sequence to obtain a sintering precursor; wherein the drying conditions are: temperature 80° C. and time 36 hours.
[0074] Step 3: sintering the precursor to obtain a polyvalent manganese oxide filler; wherein the sintering conditions are: a heating rate of 12° C. / min, a sintering temperature of 900° C., a sintering atmosphere of air, and a sintering time of 3 hours.
[0075] Comparative Example 1
[0076] The preparation method of the manganese oxide filler in this example is the same as the preparation method of the multivalent manganese oxide filler in Example 2, except that the Eucalyptus globulus leaf extract is replaced with Eucommia ulmoides leaf extract; the Eucommia ulmoides leaf extract in this example is produced by Shaanxi Suao Biotechnology Co., Ltd.
[0077] Comparative Example 2
[0078] The preparation method of the manganese oxide filler in this embodiment is the same as the preparation method of the polyvalent manganese oxide filler in Example 2, except that the Eucalyptus globulus leaf extract is replaced by Platycladus orientalis leaf extract; the Platycladus orientalis leaf extract in this embodiment is produced by Shaanxi Suoao Biotechnology Co., Ltd.
[0079] Test analysis:
[0080] 1. SEM and EDS test analysis
[0081] (1) The polyvalent manganese oxide filler finally prepared in Example 2 (i.e., the Mn-eucalyptus leaf extract after calcination) and the sintered precursor prepared in step 2 of Example 2 (i.e., the Mn-eucalyptus leaf extract before calcination) were subjected to SEM and EDS testing and analysis.
[0082] The test results are shown in Figures 1 and 2, where (a) and (c) in Figure 1 are SEM images of the sintered precursor, and (b) and (d) are SEM images of the multivalent manganese oxide filler.
[0083] As can be seen in Figures 1 (a) and (b), the calcined polyvalent manganese oxide filler exhibits a distinctly porous structure compared to the sintered precursor. Furthermore, further observation of the magnified SEM images of the sintered precursor and polyvalent manganese oxide filler (i.e., (c) and (d)) reveals that the sintered precursor exhibits some wrinkles and grooves, but is generally compact with few and small voids. In contrast, the polyvalent manganese oxide filler exhibits significantly more wrinkles and pores, resulting in an uneven and relatively loose granular surface.
[0084] In the present invention, the pore structure of the polyvalent manganese oxide filler is the basis for the filler's large specific surface area and good adsorption properties. This pore structure is caused by the volatilization of organic compounds (i.e., the Eucalyptus globulus leaf extract) during calcination. This also suggests that the interaction between the Eucalyptus globulus leaf extract and manganese ions during pyrolysis improves the pore structure of the biomass precursor to a certain extent, achieving a pore expansion effect to a certain extent, increasing the specific surface area and pore volume of the polyvalent manganese oxide filler.
[0085] (2) The sintered precursor and the multivalent manganese oxide filler were tested and analyzed using X-ray energy spectrum. The test results are shown in Figure 2, where (a) is the ESD energy spectrum of the sintered precursor and (b) is the EDS energy spectrum of the multivalent manganese oxide filler.
[0086] Figure 2 shows that elements such as C, O, Na, K, and Mg are evenly distributed throughout the sintered precursor and the multivalent manganese oxide filler. The multivalent manganese oxide filler exhibits a significantly lower proportion of oxygen compared to the sintered precursor, while significantly increasing its Mn content to 64.02%. This further confirms the presence and distribution of Mn on the surface of the multivalent manganese oxide filler, and that calcination significantly increases its surface Mn content.
[0087] In addition, there are small amounts of P and S elements in the polyvalent manganese oxide filler, indicating that calcination promotes the reaction between the Eucalyptus globulus leaf extract and manganese ions, thereby changing the structure and properties of the sintered precursor, resulting in the release of some elements in the material, which is beneficial to the growth of microorganisms, which is consistent with the SEM characterization results.
[0088] 2. Infrared spectroscopy test analysis (FIRT)
[0089] The polyvalent manganese oxide filler finally prepared in Example 2 (i.e., the Mn-eucalyptus leaf extract after calcination) and the sintered precursor prepared in Step 2 of Example 2 (i.e., the Mn-eucalyptus leaf extract before calcination) were subjected to infrared spectroscopy analysis, and the test results are shown in Figure 3.
[0090] As can be seen from Figure 3, 3500~2500cm -1 The absorption band at 2936~2916cm is caused by the stretching vibration of -OH; -1 The absorption band of -CH2 is caused by asymmetric stretching vibration. Compared with the sintered precursor, the absorption band of multivalent manganese oxide filler at 2614.5cm -1 and 1860cm -1 Two new peaks appeared at , corresponding to the stretching vibrations of -COOH and C=O, respectively. This indicates that calcination increases the amount of -COOH and C=O in the filler, and the increased -COOH and C=O are conducive to the attachment and growth of microorganisms, thereby improving the denitrification capacity of the polyvalent manganese oxide filler.
[0091] 3. XPS test analysis
[0092] The multivalent manganese oxide filler finally prepared in Example 2 (i.e., the Mn-eucalyptus leaf extract after calcination) and the sintered precursor prepared in Step 2 of Example 2 (i.e., the Mn-eucalyptus leaf extract before calcination) were subjected to XPS testing and analysis, and the test results are shown in Figure 4; wherein (a) is the XPS graph of the sintered precursor, and (b) is the XPS graph of the multivalent manganese oxide filler.
[0093] Figure 4 shows the Mn 2p spectra of the sintered precursor and the multivalent manganese oxide filler. As can be seen from Figure 4, the double peaks at 641.9eV and 653.40eV are respectively related to the Mn 2p3 / 2 and Mn 2p 1 / 2 The binding energy of Mn 2p 3 / 2 and Mn 2p 1 / 2 The spin energy separation between the double peaks is 11.5 eV. 3 / 2 The main peak at 640.80eV, 641.4eV and 643.3eV is curled into three peaks, which can be attributed to the oxidation states of Mn, MnO, Mn2O3 and MnO2. 1 / 2 The main peak at 652.9eV and 654.5eV is reversed into two peaks, which can be attributed to the oxidation states of Mn, Mn2O3 and MnO. Since the area enclosed by the peak and the horizontal axis is related to the content of the element, it can be seen from the figure that Mn in the multivalent manganese oxide filler is 2+ The content of Mn decreases, 3+ and Mn 4+ This further demonstrates the successful synthesis of multivalent manganese oxides and that calcination changes the content of manganese in different valence states in the filler. In addition, the increase in oxidized manganese (3+, 4+) after calcination also promotes the occurrence of manganese ammonia oxidation under anaerobic conditions, thereby facilitating nitrogen removal in constructed wetlands.
[0094] 4. The denitrification performance of the polyvalent manganese oxide filler prepared in Example 2 was tested using a cylindrical constructed wetland reactor with a height of 50 cm and an inner diameter of 10 cm. During the test, a mixture of the polyvalent manganese oxide filler and gravel was placed 5 to 45 cm from the bottom of the reactor. The water was introduced from the top and out from the bottom. The grass planted in the constructed wetland was windmill grass with an HRT of 5 days.
[0095] In addition, during the test, different groups of artificial wetlands were set up according to the volume of polyvalent manganese oxide filler and gravel in the mixture, specifically:
[0096] In group A (5% Mn-eucalyptus leaf extract (i.e., multivalent manganese oxides)), the volume ratio of multivalent manganese oxide filler to gravel was 5%, and the rest of the constructed wetland reactor was filled with gravel;
[0097] In group B (15% Mn-eucalyptus leaf extract), the volume ratio of polyvalent manganese oxide filler to gravel was 15%, and the rest of the constructed wetland reactor was filled with gravel;
[0098] In group C (25% Mn-eucalyptus leaf extract), the volume ratio of polyvalent manganese oxide filler to gravel was 25%, and the rest of the constructed wetland reactor was filled with gravel;
[0099] In the control group (conventional constructed wetland), the substrate of the constructed wetland reactor was only gravel.
[0100] In addition, the influent water (i.e., simulated raw water) during the test was referenced to general domestic sewage (COD = 210 mg / L, NH4 + -N concentration is 35 mg / L, TN concentration is 35 mg / L), specifically: 2.1675g glucose, 1.3375g ammonium chloride, 0.1g ferrous chloride tetrahydrate, 0.2195g potassium dihydrogen phosphate, 0.2g EDTA-Na, 0.1g calcium chloride dihydrate, 0.6g magnesium chloride hexahydrate, 1g sodium bicarbonate, 2mL trace element concentrate (prepared by zinc sulfate, manganese chloride, cobalt chloride, copper chloride, boric acid, nickel chloride, sodium molybdate) are dissolved in 10L tap water to prepare influent water, wherein the COD concentration in the influent water is 210mg / L, NH4 + The -N concentration was 35 mg / L. Furthermore, during the test, measurements were taken after the system stabilized, with a hydraulic retention time of 5 days and sampling every two days. Each sample was filtered with a 0.45 μm filter and the effluent COD, ammonia nitrogen, nitrate nitrogen, and total nitrogen concentrations were measured.
[0101] The test results are shown in Figures 5 to 8, where Figure 5 is a curve showing the concentration change of ammonia nitrogen removed by polyvalent manganese oxide filler, Figure 6 is a curve showing the concentration change of nitrate removed by polyvalent manganese oxide filler, Figure 7 is a curve showing the concentration change of total nitrogen removed by polyvalent manganese oxide filler, and Figure 8 is a curve showing the concentration change of chemical oxygen demand (COD) removed by polyvalent manganese oxide filler.
[0102] As shown in Figure 5, the polyvalent manganese oxide-filled constructed wetland of the present invention significantly improves ammonia nitrogen removal efficiency compared to conventional constructed wetlands. Furthermore, the higher the polyvalent manganese oxide filler ratio, the better the ammonia nitrogen removal efficiency. This demonstrates that the polyvalent manganese oxide prepared in the present invention has excellent ammonia nitrogen removal performance.
[0103] As can be seen in Figure 6, the experimental group with the highest polyvalent manganese oxide ratio (i.e., Group C) had the highest nitrate content, followed by the experimental groups with 5% (Group A) and 15% (Group B). The control group had the lowest nitrate content, almost 0. This is because the experimental group with the highest ratio had a greater degree of nitrification and manganese ammonia oxidation, resulting in better ammonia nitrogen removal and more intermediate nitrate produced, which corresponds to the above ammonia nitrogen results.
[0104] As shown in Figure 7, the trends in total nitrogen concentration across the experimental groups were similar to those for ammonia nitrogen. The polyvalent manganese oxide-filled constructed wetlands demonstrated significantly better total nitrogen removal than conventional constructed wetlands. Furthermore, the higher the polyvalent manganese oxide ratio, the better the total nitrogen removal. This demonstrates that the polyvalent manganese oxide prepared in this invention exhibits excellent total nitrogen removal performance and is a promising denitrification filler for constructed wetlands.
[0105] As can be seen from FIG8 , all test groups have a good removal effect on COD, and the removal effect of the artificial wetland filled with polyvalent manganese oxide is better than that of the conventional artificial wetland, indicating that the polyvalent manganese oxide prepared by the present invention has good COD removal performance.
[0106] 5. The properties of the multivalent manganese oxide filler in Example 2 and the manganese oxide fillers prepared in Comparative Examples 1 and 2 were tested using the same testing method as in 1 above, except that:
[0107] During the test, different groups were set according to the different fillers in the mixture (mixture of fillers and gravel) placed in the section 5 to 45 cm from the bottom of the reactor, specifically:
[0108] Group 1 (25% Mn-eucalyptus leaf extract): the volume ratio of the multivalent manganese oxide filler prepared in Example 2 to gravel was 25%, and the rest of the reactor was filled with gravel;
[0109] Group 2 (25% Mn-eucommia leaf extract), the volume ratio of the manganese oxide filler prepared in Comparative Example 1 to gravel was 25%, and the rest of the reactor was filled with gravel;
[0110] Group 3 (25% Mn-Orientalis orientalis leaf extract), the volume ratio of the manganese oxide filler prepared in Comparative Example 2 to gravel was 25%, and the rest of the reactor was filled with gravel;
[0111] In the control group (conventional constructed wetland), the substrate of the constructed wetland reactor was only gravel.
[0112] The water inlet and water inlet method in this test are the same as those in the above 1.
[0113] The test results are shown in Figures 9 to 11, where Figure 9 is a curve showing the concentration change of ammonia nitrogen removed by fillers prepared with different extracts, Figure 10 is a curve showing the concentration change of nitrate removed by fillers prepared with different extracts, and Figure 11 is a curve showing the concentration change of total nitrogen removed by fillers prepared with different extracts.
[0114] As can be seen from Figure 9, the manganese oxide artificial wetlands prepared with different extracts have better ammonia nitrogen removal effects than conventional artificial wetlands, indicating that the fillers prepared by the method of the present invention have a certain effect on the denitrification of artificial wetlands. Among them, the ammonia nitrogen removal effect of the multivalent manganese oxide (i.e., Mn-eucalyptus leaf extract) is significantly better than the manganese oxide filler prepared with Eucommia ulmoides leaf extract (i.e., Mn-Eucommia ulmoides leaf extract) and the manganese oxide filler prepared with Platycladus orientalis leaf extract (i.e., Mn-Platycladus orientalis leaf extract), indicating that the type of extract has a certain influence on the denitrification of artificial wetlands. The principle is that the organic amines and quaternary ammonium ions rich in the Eucalyptus globulus leaf extract in the present invention act as templates in the preparation process of the multivalent manganese oxide, making the multivalent manganese oxide prepared by the present invention have a loose, porous and porous structure, increasing the specific surface area of the multivalent manganese oxide filler in the present invention and improving its denitrification efficiency.
[0115] As can be seen from Figure 10, the nitrate content in the first polyvalent manganese oxide test group (i.e., 25% Mn-eucalyptus leaf extract) was the highest, followed by groups 2 (i.e., 25% Mn-eucommia leaf extract) and 3 (i.e., 25% Mn-orientalis leaf extract). The control group had the lowest nitrate content, almost 0. This is because the polyvalent manganese oxide nitrification process and the manganese ammoxidation process proceed to a greater extent, resulting in better ammonia nitrogen removal and more intermediate nitrate generated, which corresponds to the above ammonia nitrogen results.
[0116] As can be seen from Figure 11, the trend of change in total nitrogen concentration in each test group is similar to that of ammonia nitrogen. The removal effect of total nitrogen in the artificial wetland filled with polyvalent manganese oxide (i.e., 25% Mn-eucalyptus leaf extract) in Group 1 is significantly better than that in Group 2 (i.e., 25% Mn-Eucommia ulmoides leaf extract) and Group 3 (i.e., 25% Mn-Platycladus orientalis leaf extract), indicating that the polyvalent manganese oxide prepared by the present invention has good removal performance for total nitrogen.
[0117] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a multivalent manganese oxide filler, characterized in that: The following steps are involved: Step 1, adding the Eucalyptus globulus leaf extract to a potassium permanganate solution for oxidation reaction, and stirring to finally form a suspension; Step 2, filtering and drying the suspension in step 1 in sequence to obtain a sintering precursor; Step 3: sintering the sintering precursor to obtain a polyvalent manganese oxide filler.
2. The preparation method according to claim 1, characterized in that: The conditions for the oxidation reaction in step 1 are: reacting at room temperature for 2 to 3 hours.
3. The preparation method according to claim 2, characterized in that: The solid-to-liquid ratio of the suspension in step 1 is: (2-3): 50 g / mL.
4. The preparation method according to claim 3, characterized in that: The particle size of the Eucalyptus globulus leaf extract in step 1 is 74-100 μm, and the molar concentration of the permanganate solution in step 1 is 0.15-0.3 mol / L.
5. The preparation method according to claim 4, characterized in that: The drying conditions in step 2 are: drying temperature of 70-80° C. and drying time of 24-36 hours.
6. The preparation method according to claim 5, characterized in that: The sintering conditions in step 3 are: heating rate of 8-12° C. / min, sintering temperature of 600-900° C., sintering atmosphere of air, and sintering time of 3-4 hours.
7. The preparation method according to claim 6, characterized in that: The sintering conditions in step 3 are: heating rate of 10° C. / min, sintering temperature of 600° C., sintering atmosphere of air, and sintering time of 3 h.
8. A multivalent manganese oxide filler prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the multivalent manganese oxide filler according to claim 8 in denitrification of artificial wetlands.
Citation Information
Patent Citations
Green preparation method of manganese dioxide
CN107500361A
Method for carrying out reduction acidolysis-leaching and simultaneously removing iron to treat oxidized manganese ore
CN108660326A
Wetland substrate preparation method and artificial wetland system
CN115093031A
Multivalent manganese oxide filler as well as preparation method and application thereof
CN116177742A
Media of constructed wetland for the treatment of municipal wastewater and preparation methods thereof
KR100845521B1