Liquid crystal polyester and preparation method therefor and use thereof
By introducing 2,6-naphthylene and 4,4-diphenyl ether structures, combined with 1,4-phenylene, the melting point and crystallization temperature of liquid crystal polyester are reduced, solving the problem of high melting point and processing problems of existing liquid crystal polyester. To solve the problem of poor performance, its foaming resistance and heat resistance have been significantly improved.
Patent Information
- Application Number
- PCT/CN2024/081356
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
The melting point of existing foam-resistant liquid crystal polyester is relatively high, resulting in poor processing performance. During the lead-free reflow soldering process, it is easy to cause material degradation and uneven shrinkage of parts, resulting in warpage and deformation.
The 2,6-naphthylene structure with a side-step effect and the 4,4-diphenyl ether group with a bent structure are used to replace the easily rotated biphenyl structure and combined with the 1,4-phenylene group to form a low melting point and Liquid crystal polyester with low crystallization temperature reduces chain segment movement and the generation of small molecules, improving foaming resistance and stability.
It achieves the low melting point, low foaming rate and excellent thermal weight loss resistance of liquid crystal polyester. The average foaming rate is as low as 10%, the melting point is 360°C and below, and the thermal weight loss rate in 60 minutes at 300°C is as low as 0.3%.
Smart Images

Figure PCTCN2024081356-FTAPPB-I100001 
Figure PCTCN2024081356-FTAPPB-I100002 
Figure PCTCN2024081356-FTAPPB-I100003
Abstract
Description
Liquid crystal polyester and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of engineering plastics, in particular to a liquid crystal polyester and a preparation method and application thereof. Background Art
[0002] The rapid development of miniaturization and high frequency of electronic and electrical equipment has promoted the development of electronic component density, miniaturization and high-density assembly technology. In particular, the use of surface mount technology (SMT) connectors has placed higher requirements on the temperature resistance and dimensional stability of the plastic materials used. In order to meet environmental protection requirements, lead-free reflow soldering is widely adopted, which places higher requirements on the blister resistance of the materials used at the high peak temperatures in the reflow soldering process. The rigid chain structure and orderly arrangement of molecules of thermotropic liquid crystal polyester (LCP) give it excellent physical and mechanical properties. It excels in mechanical properties, dielectric properties, self-flammability (without the addition of flame retardants), and heat resistance, and is widely used in connector materials using lead-free reflow soldering.
[0003] Conventional LCPs, in order to meet the requirements for blister resistance during lead-free reflow soldering, generally achieve this by increasing the resin's melting point and crystallization temperature, reducing the chain segment mobility at the lead-free reflow soldering processing temperature, and inhibiting the diffusion of residual small molecules. However, increasing the resin's melting point and crystallization temperature increases the processing temperature required to meet melt fluidity during injection molding. This can easily cause resin degradation during processing, leading to deterioration of mechanical properties. Furthermore, it can also cause the external cooling rate of the molded part to be too rapid, resulting in uneven shrinkage and warping of the part.
[0004] Therefore, it is necessary to provide a thermotropic liquid crystal polyester having both a lower melting point and better anti-blistering performance.
[0005] Summary of the Invention
[0006] The purpose of the present invention is to provide a liquid crystal polyester having a lower melting point, better mechanical properties and blister resistance in order to solve the defects of the existing blister-resistant liquid crystal polyester having a high melting point and poor processing and mechanical properties.
[0007] Another object of the present invention is to provide a method for preparing the liquid crystal polyester.
[0008] Another object of the present invention is to provide use of the liquid crystal polyester in preparing blister-resistant and / or heat-resistant electronic devices.
[0009] To achieve the above object, the present invention adopts the following technical solutions:
[0010] A liquid crystal polyester comprising repeating units represented by formula I, formula II and formula III:
[0011] —O—Ar1—O— Formula I;
[0012] —OC—Ar2—CO— Formula II;
[0013] —O—Ar3—CO— Formula III;
[0014] Among them, Ar1 is at least one of 1,4-phenylene, 1,3-phenylene, 4,4-biphenylene or 4,4-diphenylether; Ar2 is at least one of 1,4-phenylene, 1,3-phenylene, 2,6-naphthylene or 4,4-diphenylether; Ar3 is at least one of 2,6-naphthylene or 1,4-phenylene; and the liquid crystal polyester contains 1,4-phenylene, 2,6-naphthylene and 4,4-diphenylether at the same time.
[0015] It should be noted that the repeating unit of Formula I corresponds to an aromatic diphenol monomer, the repeating unit of Formula II corresponds to an aromatic dicarboxylic acid monomer, and the repeating unit of Formula III corresponds to a hydroxyaromatic carboxylic acid monomer. Regarding the ratios in Formulas I through III: the monomer of Formula I and the monomer of Formula II undergo dehydration and condensation to form a polyester; Formula III can react with Formulas I and II, or with Formula III with different Ar3 structural units; in the polyester structures formed by Formulas I through III, the number of —O— and —CO— is equal.
[0016] The present invention simultaneously selects and introduces a 2,6-naphthylene structure with a "side-step effect" and a 4,4-diphenyl ether group with a bent structure, and replaces the biphenyl structure that is easy to rotate with a p-phenylene structure (i.e., a structure containing 1,4-phenylene) that is easily sublimated. The three cooperate with each other. On the one hand, they can increase the energy barrier of chain segment movement at high temperature, reduce the movement of molecular chain ends at lead-free reflow soldering temperature, inhibit the ester exchange reaction at the chain end, and jointly reduce the generation of vaporized small molecules, thereby avoiding blistering; on the other hand, the 2,6-naphthylene structure and the 4,4-diphenyl ether group can also play a role in lowering the melting point and crystallization temperature of liquid crystal polyester. In addition, the inventors have creatively discovered that the existing anti-foaming liquid crystal polyesters all contain a relatively high content of biphenyl monomers. When a 4,4-diphenyl ether group is introduced, the content of biphenyl monomers can be significantly reduced (≤5 mol%), and even no biphenyl monomers can be added. It can also significantly inhibit the movement of molecular chains, reduce the generation of small molecules, and improve the anti-foaming stability of the prepared liquid crystal polyester, with an average foaming rate as low as 10% or less.
[0017] Preferably, based on all repeating units of the liquid crystal polyester, any one or more of the following conditions are met:
[0018] (1) The content of structural units containing 1,4-phenylene is greater than 70 mol%, preferably greater than 75 mol%;
[0019] (2) the content of the structural unit containing 2,6-naphthylene is ≥8 mol %, preferably ≥10 mol %;
[0020] (3) The content of the structural unit containing a 4,4-diphenyl ether group is ≥ 0.2 mol %, preferably ≥ 0.5 mol %.
[0021] Preferably, based on all repeating units of the liquid crystal polyester, the following conditions are satisfied:
[0022] 0 mol%≤the content of the structural unit containing 1,3-phenylene≤1.2 mol%, preferably ≤1 mol%;
[0023] The content of the structural unit containing 4,4-biphenyl group is 0 mol%≤5 mol%, preferably ≤1 mol%.
[0024] Preferably, based on all repeating units of the liquid crystal polyester, the following conditions are satisfied:
[0025] The content of the structural unit containing 1,4-phenylene is 79 to 90 mol%;
[0026] Or, the content of the structural unit containing 2,6-naphthylene is 10 to 20 mol%;
[0027] Alternatively, the content of the structural unit containing a 4,4-diphenyl ether group is 0.5 to 1.5 mol%.
[0028] When the amount of the above groups is within the above range, the obtained liquid crystal polyester has a relatively low melting point, foaming rate and thermal weight loss rate.
[0029] Further preferably, the amount of each repeating unit in the liquid crystal polyester, based on all the repeating units of the liquid crystal polyester (i.e., the sum of the mole percentages of the repeating units represented by Formula I, Formula II, and Formula III is 100 mol%), satisfies at least one of the following conditions:
[0030] 1) In the repeating units represented by formula I, the content of structural units containing 1,4-phenylene groups is 10 mol% or less and less than 20 mol%, or the content of structural units containing 1,3-phenylene groups is 0 mol% or less and less than 0.5 mol%, or the content of structural units containing 4,4-biphenyl groups is 0 mol% or less and less than 5 mol%, or the content of structural units containing 4,4-diphenyl ether groups is 0 mol% or less and less than 1 mol%;
[0031] 2) In the repeating units represented by formula II, the content of structural units containing 1,4-phenylene groups is 12 mol% or less and less than 20 mol%, or the content of structural units containing 1,3-phenylene groups is 0 mol% or less and less than 1 mol%, or the content of structural units containing 2,6-naphthylene groups is 0 mol% or less and less than 0.5 mol%, or the content of structural units containing 4,4-diphenyl ether groups is 0 mol% or less and less than 1 mol%;
[0032] 3) In the repeating units represented by formula III, the content of the structural units containing 1,4-phenylene is 40 mol% or less and 60 mol% or the content of the structural units containing 2,6-naphthylene is 8 mol% or less and 20 mol% or less.
[0033] More preferably, based on all the repeating units of the liquid crystal polyester (i.e., the sum of the mole percentages of the repeating units represented by Formula I, Formula II, and Formula III is 100 mol%), at least one of the following conditions is satisfied:
[0034] (1) In the repeating units represented by formula I, the content of structural units containing 1,4-phenylene groups is 15.9 mol% or less and 18 mol% or less, or the content of structural units containing 1,3-phenylene groups is 0 mol% or less and 0.6 mol% or less, or the content of structural units containing 4,4-biphenyl groups is 0 mol% or less and 0.5 mol% or less, or the content of structural units containing 4,4-diphenyl ether groups is 0 mol% or less and 0.5 mol% or less;
[0035] (2) In the repeating units represented by formula II, the content of structural units containing 1,4-phenylene groups is 12 mol% or less and less than 15 mol%, or the content of structural units containing 1,3-phenylene groups is 0 mol% or less and less than 0.6 mol%, or the content of structural units containing 2,6-naphthylene groups is 0 mol% or less and less than 0.5 mol%, or the content of structural units containing 4,4-diphenylether groups is 0.5 mol% or less and less than 1 mol%;
[0036] (3) In the repeating units represented by formula III, the structural units of 1,4-phenylene are 50 mol% or less and 55 mol% or less, and the structural units of 2,6-naphthylene are 13 mol% or less and 16 mol% or less.
[0037] Within the above monomer range, the obtained liquid crystal polyester has a low melting point and particularly excellent anti-foaming performance.
[0038] The melting point of the liquid crystal polyester is 328-360°C, and the melting point is measured by DSC. The temperature is increased from room temperature (20-30°C) at a heating rate of 20°C / min to a maximum temperature 30°C higher than the melting point, and then the temperature is maintained at this temperature for 3 minutes and then cooled to room temperature at a rate of 20°C / min. After the test sample is maintained at room temperature for 3 minutes, it is heated again at a heating rate of 20°C / min to a maximum temperature 30°C higher than the melting point to obtain a second melting curve of the liquid crystal polyester. The melting peak of this curve is selected as the melting point.
[0039] The crystallization temperature of the liquid crystal polyester is less than 300°C. The crystallization temperature is measured by DSC. The temperature is raised from room temperature to a maximum temperature 30°C higher than the melting point at a heating rate of 20°C / min, and then the temperature is kept at this temperature for 3 minutes and then cooled to room temperature at a rate of 20°C / min to obtain a crystallization curve of the liquid crystal polyester. The crystallization peak of this curve is selected as the crystallization temperature.
[0040] The melt viscosity of the liquid crystal polyester is 10-30 Pa.s, and the melt viscosity is tested by a capillary rheometer at a test temperature of 0-30°C above the melting point and a shear rate of 1000s. -1 , measured using a die with an inner diameter of 1 mm and a length of 40 mm.
[0041] The liquid crystal polyester has excellent foaming resistance and stability, and the average foaming rate is 10% or less.
[0042] The liquid crystal polyester has a thermal weight loss rate of ≤0.3% at 300°C for 60 minutes, and can be as low as 0.21%. The thermal weight loss rate is measured using a TGA (thermogravimetric analyzer) in a nitrogen atmosphere. The sample is heated to 150°C at a rate of 20°C / min, held at 150°C for 10 minutes, then heated to 300°C at a rate of 20°C / min, and held at 300°C for 60 minutes. The thermal weight loss rate (%) at 300°C for 60 minutes = 100% - sample mass at 300°C for 60 minutes / mass at 300°C for 0 minutes * 100%.
[0043] The present invention also protects a method for preparing the above-mentioned liquid crystal polyester. The method for preparing the liquid crystal polyester comprises the following steps:
[0044] S1. A catalytic acylation reaction of a repeating unit monomer of formula III and a repeating unit monomer of formula I with an acylating agent;
[0045] S2. The acylation reaction product of step S1 is subjected to melt polycondensation and reduced pressure polycondensation under catalysis with a repeating unit monomer of formula II to obtain a prepolymer;
[0046] S3. The prepolymer obtained in step S2 is cooled and granulated, and solid-phase polymerization is performed under vacuum conditions to obtain the liquid crystal polyester.
[0047] In the present invention, the hydroxyl group is first acylated, and the acyloxy group obtained after the acylation is further subjected to polycondensation and polymerization with the carboxyl group to obtain the liquid crystal polyester.
[0048] Preferably, the ratio of the molar amount A of the repeating unit monomer of formula I in step S1 to the molar amount B of the repeating unit monomer of formula II in step S2 is A:B=(1.03-1.6):1.
[0049] In certain preferred embodiments, by controlling the dosage ratio of the repeating unit monomer of formula I and the repeating unit monomer of formula II, the ratio of the terminal reaction groups (carboxyl and acyloxy) in the prepolymer molecules formed at the end of the prepolymerization reaction can be unbalanced, thereby being able to maintain the viscosity growth during the solid-phase polymerization (thickening stage) while the growth rate (of the molecular chain) is slower and more controllable, which not only reduces the residual gas, but also extends the deashing time of small molecules and reduces the content of small molecules, thereby further avoiding the gasification of small molecules at the reflow temperature to generate bubbles, and further improving the foaming resistance of the liquid crystal polyester.
[0050] Because aromatic diphenol monomers readily volatilize during polymerization, an excess of aromatic diphenol monomer (i.e., the molar amount of the repeating unit monomer of Formula I is greater than the molar amount of the repeating unit monomer of Formula II) can both slow solid-phase polymerization and remove more gas during volatilization, ensuring excellent anti-blistering properties of the polyester. However, an excess of carboxylic acid groups, coupled with the volatilization of the aromatic diphenol monomer, can result in a low polyester yield, leaving more small-molecule monomers in the resulting polyester, and increasing the thermal weight loss rate of the polyester material.
[0051] Preferably, the acylation reaction in step S1 is carried out in an inert atmosphere, wherein the inert atmosphere is an atmosphere formed by at least one of nitrogen, helium, argon or carbon dioxide. In order to suppress the occurrence of side reactions, the inert atmosphere is preferably an atmosphere formed by carbon dioxide gas.
[0052] The temperature of the acylation reaction is 100-180° C.; the time of the acylation reaction is 0.5-3 hours; and the pressure of the acylation reaction is 0.1-0.2 MPa.
[0053] The acylating agent is a conventional acylating agent in the art, including but not limited to at least one of acetic anhydride, propionic anhydride, butyric anhydride, or valeric anhydride, preferably acetic anhydride. The molar amount of the acylating agent is greater than the total molar amount of the hydroxyaromatic carboxylic acid monomer and the aromatic diphenol monomer. The molar amount of the acylating agent is preferably 1.01 to 1.03 times the total molar amount of the hydroxyaromatic carboxylic acid monomer and the aromatic diphenol monomer.
[0054] In step S2., before carrying out the melt polycondensation reaction, the pressure of the reaction system needs to be reduced to normal pressure (100-101 kPa) before adding the repeating unit monomer of formula II. During the melt polycondensation reaction, the alkyl acid (the corresponding alkyl acid formed after the acylating agent reacts), unreacted acylating agent, and a small amount of hydroquinone acylate need to be discharged. The amount of alkyl acid received is used to determine whether the reaction reaches more than 90% of the theoretical value. When the melt polycondensation reaction reaches more than 90% of the theoretical value, the reduced pressure polycondensation is carried out again.
[0055] The reaction temperature of the melt polycondensation is 200-400° C.; the temperature of the reduced pressure polycondensation is 300-400° C.; and the pressure of the reduced pressure polycondensation is 1-10 kPa.
[0056] In step S3, the conditions for the solid phase polymerization are: vacuum degree of 0.1 Pa to 50 kPa, temperature of 160 to 350° C., and polymerization time of 0.5 to 40 h.
[0057] Preferably, the acylation reaction and melt polycondensation are carried out in the presence of a catalyst, which is a conventional polyester polymerization catalyst in the art, and is a metal salt catalyst, including but not limited to at least one of potassium acetate, sodium acetate, magnesium acetate, zinc acetate, antimony trioxide, or tetrabutyl titanate. The catalyst is added in an amount of 50 to 200 ppm based on the total amount of monomers.
[0058] The above reaction is carried out in a vertical polymerization tank equipped with a stirrer. The stirring blades can be turbine blades, double screw blades or multi-stage paddle blades, preferably double screw blades.
[0059] The application of the liquid crystal polyester in the preparation of blister-resistant and / or heat-resistant electronic devices is also within the scope of the present invention. Such electronic devices include, but are not limited to, sensors, LED lamps, connectors, sockets, resistors, relay housings, relay bases, relay bobbins, switches, coil bobbins, capacitors, variable capacitor housings, optical pickups, resonators, various terminal blocks, transformers, plugs, printed wiring boards, tuners, speakers, microphones, headphones, small motors, head mounts, power modules, housings, semiconductors, LCD components, FDD brackets, FDD chassis, HDD components, motor brush holders, parabolic antennas, and computer-related components.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] The present invention simultaneously introduces a 2,6-naphthylene structure with a "side-step effect" and a 4,4-diphenyl ether group with a kinked structure, replacing the easily rotatable biphenyl structure with a readily sublimable para-phenylene structure (i.e., a structure containing 1,4-phenylene). The three elements work together to lower the melting point and crystallization temperature while reducing the generation of vaporized small molecules, thereby preventing blistering. The introduction of the 4,4-diphenyl ether group also significantly reduces the content of biphenyl monomers while significantly improving the blister resistance of the liquid crystal polyester during processing.
[0062] The liquid crystal polyester prepared by the present invention has excellent foaming resistance and stability, with an average foaming rate as low as 10% or less; and a melting point of 360°C or less, which can be as low as 328°C; and also has excellent heat-weight loss resistance, with a weight loss rate as low as 0.3% or less after 60 minutes at 300°C. DETAILED DESCRIPTION
[0063] For better explanation of the purpose, technical scheme and advantage of the present invention, the present invention will be further described below in conjunction with specific embodiment, but embodiment does not limit the present invention in any form.Unless otherwise stated, the reagent, method and equipment adopted in the present invention are conventional reagents, methods and equipment in the art.Unless otherwise stated, the reagents and materials used in the present invention are commercially available.
[0064] The following raw materials are selected in the embodiments of the present invention:
[0065] Hydroquinone: Yingchuansheng Chemical;
[0066] Resorcinol: Shandong Tianshili Biotechnology Co., Ltd.
[0067] 4,4′-dihydroxydiphenyl ether: Zhengzhou Four Seasons Chemical Products Co., Ltd.
[0068] 4,4′-Biphenylenediphenol: Shanghai Yuanye Biotechnology Co., Ltd.;
[0069] 2,6-Naphthalenediol: Beijing Jianqiang Weiye Technology Co., Ltd.;
[0070] 4-Hydroxybenzoic acid: Tianjin Yifang Technology Co., Ltd.;
[0071] 3-Hydroxybenzoic acid: Chengdu Yuanda Chemical Co., Ltd.;
[0072] 6-Hydroxy-2-naphthoic acid: Shandong Lifan Chemical Co., Ltd.
[0073] Terephthalic acid: Shanghai Kaiyin Chemical Co., Ltd.;
[0074] Isophthalic acid: Shandong Fengtai Chemical Technology Co., Ltd.
[0075] 2,6-Naphthalene dicarboxylic acid: Tesco Chemical (Hubei) Co., Ltd.;
[0076] 4,4′-Diphenyl ether dicarboxylic acid: Hubei Jiufenglong Chemical Co., Ltd.
[0077] Catalyst potassium acetate: Sinopharm Group;
[0078] Acylating agent acetic anhydride: Nanjing Zhuocheng Petrochemical Co., Ltd.
[0079] Examples 1 to 15, Comparative Examples 1 to 6
[0080] The liquid crystal polyesters of the embodiments and comparative examples of the present invention, the monomers and the dosage formulas are shown in Table 1, and are prepared according to a preparation method comprising the following steps:
[0081] S1. Acylation reaction:
[0082] In a vertical polymerization tank equipped with twin propeller blades, a hydroxyaromatic carboxylic acid monomer (a monomer corresponding to the repeating unit of Formula III), an aromatic diphenol monomer (a monomer corresponding to the repeating unit of Formula I), and acetic anhydride (the molar amount of acetic anhydride is 1.03 times the total molar amount of the hydroxyaromatic carboxylic acid monomer and the aromatic diphenol monomer) are added in proportion, and then carbon dioxide gas is introduced, the pressure is increased to 0.12 MPa, and the reaction is stirred at 120° C. for 3 hours to obtain an acylated monomer;
[0083] S2. Preparation of liquid crystal polyester prepolymer:
[0084] Step S1. After the reaction is completed, the pressure in the vertical polymerization tank is reduced to atmospheric pressure (0.1 MPa), and then an aromatic dicarboxylic acid monomer (monomer corresponding to the repeating unit shown in Formula II) is added. The temperature is raised to 300° C., and a melt polycondensation reaction is carried out under these conditions. During the reaction, acid (product of the reaction of the acylating agent), unreacted anhydride molecules (acylating agent), and a small amount of acylate are discharged from the distillation column of the vertical polymerization tank. When the amount of acid collected reaches more than 90% of the theoretical value, the pressure in the polymerization tank is reduced to 1 kPa, and the temperature of the reaction system is raised to 300-400° C., and polycondensation is carried out under reduced pressure to obtain a prepolymer.
[0085] S3. Solid-phase polymerization of prepolymer:
[0086] The prepolymer obtained in step S2 is cooled and granulated, and solid-phase polymerization is carried out at 280° C. under a vacuum condition of 10 Pa until a stable melt viscosity is reached, and then the temperature is lowered to obtain the liquid crystal polyester.
[0087] Table 1 Raw material formula of liquid crystal polyester in the embodiment
[0088] Table 2 Raw material formula of liquid crystal polyester of comparative example
[0089] The properties of the prepared liquid crystal polyester were characterized. The specific test items and test methods are as follows. The test results are detailed in Table 3:
[0090] 1. Melting point: Measured by DSC: From room temperature, the temperature is increased at a heating rate of 20°C / min to a maximum temperature of 30°C above the melting point. After holding at this temperature for 3 minutes, the temperature is then lowered to room temperature at a rate of 20°C / min. The test sample is held at room temperature for 3 minutes and then heated again at a heating rate of 20°C / min to a maximum temperature of 30°C above the melting point. The second melting curve of the liquid crystal polyester is obtained. The temperature corresponding to the melting peak of this curve is the melting point.
[0091] 2. Crystallization temperature: measured by DSC. The temperature is raised from room temperature at a heating rate of 20°C / min to a maximum temperature of 30°C above the melting point, then maintained at this temperature for 3 minutes and then cooled to room temperature at a rate of 20°C / min to obtain a crystallization curve of the liquid crystal polyester. The temperature corresponding to the crystallization peak of this curve is the crystallization temperature.
[0092] 3. Melt viscosity: tested by capillary rheometer, the test temperature is 0-30℃ above the melting point, the shear rate is 1000s -1 , measured using a die with an inner diameter of 1 mm and a length of 40 mm.
[0093] 4. Foaming Rate: Liquid crystal polyester or its combination is extruded at a constant temperature, 5°C above the melting temperature of the liquid crystal polyester, at an injection speed of 60 mm / s into thin sheet specimens 1.0 mm thick and 60 mm long and wide. Samples are taken for injection molding 1 minute after polymerization, 20 minutes after polymerization, and at the end of the polymerization. Ten specimens are obtained from each injection molding cycle. Each set of ten specimens is baked in a 260°C oven for 5 minutes. The specimens are then removed and observed for bubble formation on the surface of each specimen. Foaming Rate = Number of Foamed Sheets / 10. The lower the foaming rate, the better the anti-foaming properties.
[0094] 5.300℃, 60min thermal weight loss rate: Determined by TGA (thermal gravimetric analyzer), with nitrogen atmosphere, the sample was heated to 150℃ at a rate of 20℃ / min and kept at 150℃ for 10min, then heated to 300℃ at a rate of 20℃ / min and kept at 300℃ for 60min; thermal weight loss rate at 300℃ for 60min (%) = 100% - mass of sample at 300℃ for 60min / mass at 300℃ for 0min * 100%.
[0095] Table 3 Performance test results of the embodiments and comparative examples
[0096] From the results in the table above we can see that:
[0097] The results of Examples 1 to 15 show that the liquid crystal polyesters of the present invention having a specific unit structure have excellent properties, with a melting point of 360°C or below, and can be as low as 328°C, which is more conducive to processing; the crystallization temperature is below 300°C, and can be as low as 270°C; the melt viscosity is within an appropriate range (10 to 30 Pa·s), and during processing, it has good foaming resistance and stability, with an average foaming rate (the average foaming rate of samples in the mixing section, homogenization section, and discharge port of the extruder, and injection molding tests are performed on samples taken 1 minute, 20 minutes, and at the end of the polymerization) of 10% or less; it also has good heat loss resistance, and the weight loss rate is 0.3% or less after 60 minutes at 300°C.
[0098] When the molar amount of the aromatic diphenol monomer exceeds the molar amount of the aromatic dicarboxylic acid monomer, better anti-blistering properties are achieved. This is because aromatic diphenol monomers readily volatilize during polymerization. Therefore, an excess of aromatic diphenol monomers not only ensures a slower solid-phase polymerization rate but also removes more gas during volatilization, ensuring the polyester's excellent anti-blistering properties. However, when the carboxylic acid groups are excessive (as in Example 8), the volatilization of the aromatic diphenol monomers leads to a low polyester yield, resulting in a high amount of small-molecule monomers remaining in the resulting polyester. While the anti-blistering stability meets the requirements, the thermal weight loss rate is high.
[0099] The comparison results of Example 3 and Comparative Examples 1 to 4 show that the liquid crystal polyester has excellent performance. It requires the synergistic effect between the three structures of 1,4-phenylene, 2,6-naphthylene and 4,4-diphenyl ether in the polyester molecular chain. In particular, the introduction of the 4,4-diphenyl ether group can significantly reduce the content of biphenyl repeating units. Even without adding biphenyl monomers, it can significantly inhibit the movement of the molecular chain and reduce the production of small molecules. Without any of these (such as Comparative Examples 1 to 3), the anti-foaming performance of the liquid crystal polyester will be significantly reduced or the melting point will be significantly increased. In addition, the liquid crystal polyester molecular chain of Comparative Example 4 does not contain 4,4-diphenyl ether groups or biphenyl groups, and its anti-foaming performance is significantly poor or its melting point is still high.
[0100] Compared with Example 1, in Comparative Example 5, a 2,6-naphthylene group is connected to Ar1, and in Comparative Example 6, a 4,4-diphenyl ether group is connected to Ar3. The melting point and crystallization temperature of the prepared liquid crystal polyester are still relatively high, and the foaming resistance is also poor. It can be seen that the relative position of the group in the molecular chain has a greater influence on the performance of the liquid crystal polyester.
[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A liquid crystal polyester, characterized in that: It includes repeating units represented by formula I, formula II and formula III: —O—Ar1—O—Formula I; —OC—Ar2—CO—Formula II; —O—Ar3—CO—Formula III; Ar1 is at least one of 1,4-phenylene, 1,3-phenylene, 4,4-biphenylene or 4,4-diphenyl ether; Ar2 is at least one of 1,4-phenylene, 1,3-phenylene, 2,6-naphthylene or 4,4-diphenylether; Ar3 is at least one of 2,6-naphthylene or 1,4-phenylene; The liquid crystal polyester contains 1,4-phenylene, 2,6-naphthylene and 4,4-diphenyl ether groups at the same time.
2. The liquid crystal polyester according to claim 1, characterized in that: Based on all repeating units of the liquid crystal polyester, any one or more of the following conditions are met: The content of structural units containing 1,4-phenylene is >70 mol%, preferably >75 mol%; The content of the structural unit containing 2,6-naphthylene is ≥8 mol %, preferably ≥10 mol %; The content of the structural unit containing a 4,4-diphenyl ether group is ≥ 0.2 mol %, preferably ≥ 0.5 mol %.
3. The liquid crystal polyester according to claim 2, characterized in that: Based on all repeating units of the liquid crystal polyester, any one or more of the following conditions are met: The content of the structural unit containing 1,4-phenylene is 79 to 90 mol%; The content of the structural unit containing 2,6-naphthylene is 10 to 20 mol%; The content of the structural unit containing 4,4-diphenyl ether group is 0.5 to 1.5 mol%; 0 mol%≤the content of the structural unit containing 1,3-phenylene≤1.2 mol%, preferably≤1 mol%; 0 mol%≤the content of the structural unit containing 4,4-biphenyl group≤5 mol%, preferably≤1 mol%.
4. The liquid crystal polyester according to claim 2 or 3, characterized in that: Based on all repeating units of the liquid crystal polyester, any one or more of the following conditions are met: (1) In the repeating units represented by formula I, the content of the structural units containing 1,4-phenylene groups is 15.9 mol% or less and 18 mol% or less, the content of the structural units containing 1,3-phenylene groups is 0 mol% or less and 0.6 mol% or less, or the content of the structural units containing 4,4-biphenyl groups is 0 mol% or less and 0.5 mol% or less, or the content of the structural units containing 4,4-diphenyl ether groups is 0 mol% or less and 0.5 mol% or less; (2) In the repeating unit represented by formula II, the content of the structural unit containing 1,4-phenylene is ≤ 12 mol% 15 mol%, or 0 mol%≤the content of the structural unit containing 1,3-phenylene≤0.6 mol%, or 0 mol%≤the content of the structural unit containing 2,6-naphthylene≤0.5 mol%, or 0.5 mol%≤the content of the structural unit containing 4,4-diphenyl ether≤1 mol%; (3) In the repeating units represented by formula III, 50 mol% or less of the structural units of 1,4-phenylene or less than 55 mol% and 13 mol% or less of the structural units of 2,6-naphthylene or less than 16 mol%; The sum of the mole percentages of the repeating units represented by Formula I, Formula II, and Formula III is 100 mol%.
5. The liquid crystal polyester according to claim 1, characterized in that: The repeating unit monomer of formula I is an aromatic diphenol monomer, the repeating unit monomer of formula II is an aromatic dicarboxylic acid monomer, and the repeating unit monomer of formula III is a hydroxy aromatic carboxylic acid monomer.
6. The liquid crystal polyester according to claim 1, characterized in that: Any one or more of the following conditions are met: (1) The average foaming rate of the liquid crystal polyester is 10% or less; (2) The melting point of the liquid crystal polyester is 328 to 360°C; (3) Crystallization temperature ≤ 300°C; (4) The thermal weight loss rate maintained at 300°C for 60 minutes is ≤0.3%.
7. The method for preparing a liquid crystal polyester according to any one of claims 1 to 6, characterized in that: The steps include: S1. Acylation reaction of a repeating unit monomer of formula III, a repeating unit monomer of formula I and an acylating agent under catalysis; S2. The acylation reaction product of step S1 is subjected to melt polycondensation and reduced pressure polycondensation with a repeating unit monomer of formula II under catalysis to obtain a prepolymer; S3. The prepolymer obtained in step S2 is cooled and granulated, and solid phase polymerization is performed under vacuum conditions to obtain the liquid crystal polyester.
8. The method for preparing a liquid crystal polyester according to claim 6, wherein: The ratio of the molar amount A of the repeating unit monomer of formula I in step S1. to the molar amount B of the repeating unit monomer of formula II in step S2. is A:B=(1.03-1.6):
1.
9. The method for preparing a liquid crystal polyester according to claim 6, wherein: The acylation reaction and melt polycondensation are carried out under the action of a catalyst, and the catalyst is at least one of potassium acetate, sodium acetate, magnesium acetate, zinc acetate, antimony trioxide or tetrabutyl titanate.
10. Use of the liquid crystal polyester according to any one of claims 1 to 5 in the preparation of blister-resistant and / or heat-resistant electronic devices.
Citation Information
Patent Citations
Optically anisotropic melt forming aromatic copolyesters based on t-butylhydroquinone
CN1046914A
Thermoplastic liquid crystal polymer and film of same
CN110446738A
Liquid crystal polymer resin and complex thereof
CN110540635A
Liquid crystal polyester as well as preparation method and application thereof
CN116589667A
Optically anisotropic melt forming aromatic copolyesters based on t-butylhydroquinone
CN87101652A
Cited By
Low-alpha ray spherical alumina / liquid crystal polymer 5G base station substrate material
CN121108699A
Low-alpha radiation spheroid alumina / liquid crystal polymer 5g base station substrate material