High-rate current collector and preparation method therefor
By using a combination of conductive material A and conductive material B in the current collector, the conductive adhesive wraps the conductive material A, and adds barium carbonate, which solves the problems of reduced conductive performance and increased water absorption in the existing current collector conductive primer technology, and achieves The low water absorption and high conductivity of the high conductivity and low water absorption nano-coated carbon current collector improve the safety and conductivity of lithium batteries.
Patent Information
- Application Number
- PCT/CN2024/082652
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
In the existing current collector conductive primer technology, cheap conductive agents and water-based binders lead to a decrease in conductivity and an increase in water absorption, which affects the overall effect of the electrode and poses safety risks especially during high-rate charge and discharge.
Using high conductivity and low water absorption nano-coated carbon current collector, through the combination of conductive material A and conductive material B, conductive glue wraps conductive material A, combined with barium carbonate to enhance safety, prepare a nano conductive layer, reduce water absorption and improve conductive performance.
It achieves low water absorption and high conductivity, improves the safety and conductivity of lithium batteries, reduces production costs, and prevents high-temperature fires in high-magnification scenarios.
Smart Images

Figure CN2024082652_03102024_PF_FP_ABST
Abstract
Description
A high-rate current collector and preparation method thereof Technical Field
[0001] The present application relates to the field of lithium battery technology, for example, a high-conductivity, low-water-absorption nano-carbon-coated current collector and a preparation method thereof. Background Art
[0002] With the large-scale application of lithium-ion batteries in various fields such as consumer electronics and electric vehicles, the market has also put forward higher requirements on the energy density, cycle life and safety of lithium-ion batteries. For example, the conductive primer technology of the current collector can not only effectively reduce the contact resistance between the electrode material and the current collector, but also increase the adhesion between the electrode material and the current collector, thereby ensuring that the internal resistance of the battery is reduced while extending the battery life.
[0003] In the existing current collector conductive primer technology, cheap conductive agents and water-based adhesives are usually used as coating materials. Since the surface of this conductive agent is rough and porous, it has an adsorption effect on moisture in the air. In addition, the water-based adhesive also has a certain water absorption capacity. After absorbing moisture, it will reduce the peeling performance between the electrode active material and the current collector, thereby reducing the conductive performance of the current collector or battery, and ultimately affecting the overall effect of the electrode.
[0004] Summary of the Invention
[0005] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0006] The present application provides a high-conductivity, low-water-absorption nano-carbon-coated current collector and a preparation method thereof to solve the technical problems mentioned in the above background technology.
[0007] The present application discloses a high-conductivity, low-water-absorption nano-carbon-coated current collector, comprising a conductive base layer and a nano-conductive layer, wherein the nano-conductive layer is located on any surface of the conductive base layer, wherein the components of the nano-conductive layer include a conductive material A, a conductive glue, a conductive material B, and a binder, and the oil absorption value of the conductive material A is greater than the oil absorption value of the conductive material B, the particle size of the conductive material A is greater than the particle size of the conductive material B, and the conductive glue is a solvent glue.
[0008] In one embodiment, the oil absorption value of the conductive material A is ≥300 ml / 100 g and the particle size is 0.5-1 μm, and the oil absorption value of the conductive material B is ≤100 ml / 100 g and the particle size is <0.5 μm.
[0009] In one embodiment, the conductive material A includes conductive carbon black, and the conductive material B includes at least one of graphene, conductive carbon black, and carbon nanotubes.
[0010] In one embodiment, the solid content of the conductive adhesive is 0.5-10%, and the conductive adhesive includes at least one of a polyaniline solution and a polythiophene solution.
[0011] In one embodiment, the adhesive includes at least one of a modified polyacrylic acid adhesive and a polyacrylic acid adhesive.
[0012] Wherein, the content of the conductive adhesive is less than 10 wt%.
[0013] In one embodiment, the nano-conductive layer further comprises barium carbonate.
[0014] In one embodiment, the water absorption of the high-conductivity, low-water-absorption nano-carbon-coated current collector is 123-242 ppm.
[0015] The present application also discloses a method for preparing a highly conductive and low-water-absorption nano-carbon-coated current collector, comprising the following steps: step a: first drying the conductive material A and adding it to the conductive glue and stirring evenly, then filtering and drying it again, and finally grinding and refining it to obtain the low-water-absorption conductive material; step b: coating the low-water-absorption conductive material and the conductive material B obtained in step a onto the conductive base layer.
[0016] In one embodiment, the weight ratio of the conductive material A to the conductive adhesive is 1-5:1, and the weight ratio of the conductive material A to the conductive material B is 8-10:0.5-1.5.
[0017] In one embodiment, in step b, the low water absorption conductive material obtained in step a, the conductive material B, the modified polyacrylic acid binder and the wetting agent are first mixed and dispersed to obtain a low water absorption and high conductivity slurry, and then the low water absorption and high conductivity slurry is coated on the conductive base layer to form a high conductivity and low water absorption coating, that is, the obtained nano-conductive layer on the surface of the conductive base layer is a high conductivity and low water absorption coating.
[0018] In one embodiment, step b further comprises mixing and dispersing barium titanate into a low water absorption and high conductivity slurry.
[0019] In one embodiment, the thickness of the highly conductive and low water absorption coating is 0.8-1.2 μm.
[0020] In one embodiment, in step b, the conductive material B, the polyacrylic acid binder and the wetting agent are first mixed and dispersed to obtain a highly conductive slurry, and the highly conductive slurry is applied to the conductive base layer to form a highly conductive coating. Then, the low water absorption conductive material, the modified polyacrylic acid binder and the wetting agent obtained in step a are mixed and dispersed to obtain a low water absorption conductive slurry, and the low water absorption conductive slurry is applied to the high conductive coating to form a low water absorption coating, that is, the obtained nano-conductive layer on the surface of the conductive base layer includes a highly conductive coating and a low water absorption coating.
[0021] In one embodiment, step b further includes mixing and dispersing barium titanate into a low water absorption conductive paste.
[0022] In one embodiment, the thickness ratio of the highly conductive coating to the low water absorption coating is 0.3-0.5:0.5-0.6.
[0023] In one embodiment, the drying method is vacuum drying, and the drying temperature is 50-80°C.
[0024] Compared with related technologies, the high-conductivity, low-water-absorption nano-carbon-coated current collector of this application has the following advantages:
[0025] By selecting raw materials such as conductive material A, conductive glue and conductive material B, the dried conductive material A is wrapped with conductive glue, so that the particles of conductive material A are partially wrapped by the conductive glue, thereby blocking the water absorption performance of part of the conductive material A, but at the same time the conductivity is reduced. In order to enhance the conductivity, conductive material B is added. In addition, by adding barium carbonate, the safety during high-rate charge and discharge can also be enhanced, so that the prepared high-conductivity and low-water-absorption nano-carbon-coated current collector includes a conductive base layer and a nano-conductive layer, which has low water absorption, high conductivity and safety, low production cost and simple method.
[0026] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation to the technical solution of this article.
[0028] FIG1 is a schematic diagram of the structure of a high-conductivity, low-water-absorption nano-carbon-coated current collector according to an embodiment of the present application;
[0029] FIG2 is a schematic diagram of the structure of a high-conductivity, low-water-absorption nano-carbon-coated current collector according to another embodiment of the present application.
[0030] Among them, 1. conductive base layer, 2. high conductive low water absorption coating, 3. high conductive coating, 4. low water absorption coating. DETAILED DESCRIPTION
[0031] The technical solution of this application is described in detail below through specific embodiments.
[0032] In the embodiment of the present application, by selecting raw materials such as conductive material A, conductive glue and conductive material B, the prepared current collector has both low water absorption and high conductivity, that is, a high-conductivity and low-water-absorption nano-carbon-coated current collector is obtained. The principle is that the particle size of conductive material A is large and has strong water absorption. If conductive material A is used directly as the raw material for the current collector coating, the coating will absorb a large amount of water. The particle size of conductive material B is small and the water absorption is low, but the selling price of conductive material B is much higher than that of conductive material A. If conductive material B is used directly as the raw material for the current collector coating, the production cost will be directly increased. At the same time, the cost is much higher than the product value. Therefore, this application wraps the dried conductive material A with conductive glue, so that the particles of conductive material A are partially wrapped by the conductive glue (it should be noted that "partial wrapping" refers to the wrapping area of each particle of conductive material A wrapped by conductive glue, and the wrapping area is related to the dryness, oil absorption value and particle size of conductive material A, as well as the type, solid content and content of conductive glue), thereby blocking the water absorption performance of part of the conductive material A, but at the same time the conductive performance is reduced. In order to enhance the conductivity, conductive material B is added. The preparation steps are as follows:
[0033] Step a: First, dry the conductive material A, add it to the conductive glue, stir evenly, filter it, dry it again, and finally grind it to obtain a low water absorption conductive material;
[0034] Step b: coating the low water absorption conductive material and conductive material B obtained in step a onto a conductive base layer.
[0035] In addition, since the addition of conductive material B enhances conductivity, it is easy to cause high-temperature fire when used in high-rate charging and discharging scenarios. In order to enhance safety in high-rate charging and discharging scenarios, barium carbonate can also be added to reduce conductivity by increasing resistance when the temperature is too high, thereby preventing high-temperature fire.
[0036] Please refer to the following Examples 1-8 for details, wherein Examples 1-5 refer to FIG1 , and Examples 6-10 refer to FIG2 .
[0037] Example 1
[0038] Select materials:
[0039] Conductive material A, 10kg conductive carbon black, oil absorption value 350ml / 100g, particle size 0.75μm; conductive glue, 3kg polyaniline butyl acetate solution, solid content 12%, content 9.5wt%, molecular weight 9500Da; conductive material B, 4kg graphene, oil absorption value 80ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%; wetting agent, 2kg water; conductive base layer 1, 10μm thick aluminum current collector.
[0040] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0041] Step a: First, 10 kg of conductive material A is vacuum dried at 80°C for 6 hours, then added to 3 kg of conductive glue and stirred for 2 hours, then filtered and vacuum dried again at 80°C for 4 hours, and finally ground and refined to obtain a low water absorption conductive material;
[0042] Step b: First, the low-water-absorption conductive material obtained in step a, 4 kg of conductive material B, 5 kg of binder and 2 kg of wetting agent are mixed and dispersed for 1 hour to obtain a low-water-absorption and high-conductivity slurry, and then the low-water-absorption and high-conductivity slurry is applied to both surfaces of a 10 μm thick conductive base layer 1 by a coater and dried at 90°C to form a high-conductivity and low-water-absorption coating 2. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 is a high-conductivity and low-water-absorption coating 2.
[0043] In this embodiment, the weight ratio of conductive material A to conductive adhesive is 10:3, and the weight ratio of conductive material A to conductive material B is 2.5:1. The total thickness of the high-conductivity, low-water-absorption coating 2 of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1.2 μm, that is, the thickness of the nano-conductive layer is 1.2 μm.
[0044] Example 2
[0045] Select materials:
[0046] Conductive material A, 9 kg conductive carbon black, oil absorption value 325 ml / 100 g, particle size 0.75 μm; conductive adhesive, 3 kg polythiophene butyl acetate solution, solid content 4.8%, content 9.2 wt%, molecular weight 9300 Da; conductive material B, 1 kg carbon nanotubes, oil absorption value 75 ml / 100 g, particle size 0.4 μm; binder, 5 kg modified polyacrylic acid binder, content 25 wt%; wetting agent, 1 kg water; conductive base layer 1, 10 μm thick aluminum foil.
[0047] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0048] Step a: First, 9 kg of conductive material A is vacuum dried at 65°C for 2.5 hours, then added to 3 kg of conductive glue and stirred for 2 hours. After filtering, the mixture is vacuum dried again at 65°C for 1.5 hours, and finally ground and refined to obtain a low water absorption conductive material.
[0049] Step b: First, the low-water-absorption conductive material obtained in step a, 1 kg of conductive material B, 5 kg of binder and 1 kg of wetting agent are mixed and dispersed for 0.5 h to obtain a low-water-absorption and high-conductivity slurry, and then the low-water-absorption and high-conductivity slurry is applied to both surfaces of a 10 μm thick conductive base layer 1 by a coating machine to form a high-conductivity and low-water-absorption coating 2, that is, the obtained nano-conductive layer on the surface of the conductive base layer 1 is a high-conductivity and low-water-absorption coating 2.
[0050] In this embodiment, the weight ratio of conductive material A to conductive adhesive is 3:1, and the weight ratio of conductive material A to conductive material B is 9:1. The total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1 μm, that is, the thickness of the high-conductivity, low-water-absorption coating 2 is 1 μm.
[0051] Example 3
[0052] Select materials:
[0053] Conductive material A, 10kg conductive carbon black, oil absorption value 300ml / 100g, particle size 1μm; conductive glue, 2kg polythiophene butyl acetate solution, solid content 0.5%, content 5.3wt%, molecular weight 4700Da; conductive material B, 1.5kg conductive carbon black, oil absorption value 100ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%; wetting agent, 1kg water; conductive base layer 1, 10μm thick copper current collector.
[0054] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0055] Step a: First, 10 kg of conductive material A is vacuum dried at 50°C for 3 hours, then added to 2 kg of conductive glue and stirred for 3 hours, then filtered and vacuum dried again at 50°C for 2 hours, and finally ground and refined to obtain a low water absorption conductive material;
[0056] Step b: First, the low-water-absorption conductive material obtained in step a, 1.5 kg of conductive material B, 5 kg of binder and 1 kg of wetting agent are mixed and dispersed for 0.5 h to obtain a low-water-absorption and high-conductivity slurry, and then the low-water-absorption and high-conductivity slurry is applied to both surfaces of a 10 μm thick conductive base layer 1 by a coater and dried at 100° C. to form a high-conductivity and low-water-absorption coating 2, that is, the obtained nano-conductive layer on the surface of the conductive base layer 1 is a high-conductivity and low-water-absorption coating 2.
[0057] In this embodiment, the weight ratio of conductive material A to conductive adhesive is 5:1, the weight ratio of conductive material A to conductive material B is 10:1.5, and the total thickness of the nano-conductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1.2 μm, that is, the thickness of the high-conductivity, low-water-absorption coating 2 is 1.2 μm.
[0058] Example 4
[0059] Select materials:
[0060] Conductive material A, 8kg conductive carbon black, oil absorption value 300ml / 100g, particle size 0.5μm; conductive adhesive, 2kg polyaniline butyl acetate solution, solid content 10%, content 7.2wt%, molecular weight 8200Da; conductive material B, 0.5kg conductive carbon black, oil absorption value 50ml / 100g, particle size 0.3μm; binder, 5kg modified polyacrylic acid binder, content 25wt%; wetting agent, 2kg water; conductive base layer 1, 10μm thick aluminum foil.
[0061] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0062] Step a: First, 8 kg of conductive material A is vacuum dried at 80°C for 3 hours, then added to 2 kg of conductive glue and stirred for 2 hours, then filtered and vacuum dried again at 80°C for 2 hours, and finally ground and refined to obtain a low water absorption conductive material;
[0063] Step b: First, the low-water-absorption conductive material obtained in step a, 0.5 kg of conductive material B, 5 kg of binder and 2 kg of wetting agent are mixed and dispersed for 0.5 h to obtain a low-water-absorption and high-conductivity slurry, and then the low-water-absorption and high-conductivity slurry is applied to both surfaces of a 10 μm thick conductive base layer 1 by a coater and dried at 90°C to form a high-conductivity and low-water-absorption coating 2. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 is a high-conductivity and low-water-absorption coating 2.
[0064] In this embodiment, the weight ratio of conductive material A to conductive adhesive is 4:1, and the weight ratio of conductive material A to conductive material B is 16:1. The total thickness of the nano-conductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 0.8 μm, that is, the thickness of the high-conductivity, low-water-absorption coating 2 is 0.8 μm.
[0065] Example 5
[0066] Select materials:
[0067] Conductive material A, 9kg conductive carbon black, oil absorption value 325ml / 100g, particle size 0.75μm; conductive adhesive, 3kg polythiophene butyl acetate solution, solid content 4.8%, content 9.2wt%, molecular weight 9300Da; conductive material B, 1kg carbon nanotubes, oil absorption value 75ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%; wetting agent, 1kg water; 0.5kg barium carbonate; conductive base layer 1, 10μm thick aluminum foil.
[0068] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0069] Step a: First, 9 kg of conductive material A is vacuum dried at 65°C for 2.5 hours, then added to 3 kg of conductive glue and stirred for 2 hours. After filtering, the mixture is vacuum dried again at 65°C for 1.5 hours, and finally ground and refined to obtain a low water absorption conductive material.
[0070] Step b: First, the low water absorption conductive material obtained in step a, 1 kg of conductive material B, 5 kg of binder, 0.5 kg of barium carbonate and 1 kg of wetting agent are mixed and dispersed for 0.5 h to obtain a low water absorption and high conductivity slurry, and then the low water absorption and high conductivity slurry is coated on both surfaces of a 10 μm thick conductive base layer 1 by a coating machine to form a high conductive and low water absorption coating 2, that is, the obtained nano conductive layer on the surface of the conductive base layer 1 is a high conductive and low water absorption coating 2.
[0071] In this embodiment, the weight ratio of conductive material A to conductive adhesive is 3:1, and the weight ratio of conductive material A to conductive material B is 9:1. The total thickness of the nano-conductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1.1 μm, that is, the thickness of the high-conductivity, low-water-absorption coating 2 is 1.1 μm.
[0072] Example 6
[0073] Select materials:
[0074] Conductive material A, 10kg conductive carbon black, oil absorption value 350ml / 100g, particle size 0.75μm; conductive glue, 2.5kg polyaniline solution, solid content 12%, content 9.5wt%, molecular weight 9500Da; conductive material B, 4kg graphene, oil absorption value 80ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%, 2.5kg polyacrylic acid binder, content 25wt%; wetting agent, 2.5kg water; conductive base layer 1, 8μm thick aluminum current collector.
[0075] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0076] Step a: First, 10 kg of conductive material A is vacuum dried at 80°C for 6 hours, then added to 2.5 kg of conductive glue and stirred for 2 hours, then filtered and vacuum dried again at 80°C for 4 hours, and finally ground and refined to obtain a low water absorption conductive material;
[0077] Step b: First, 4 kg of conductive material B, 2.5 kg of polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 2 hours to obtain a highly conductive slurry, and the highly conductive slurry is applied to both surfaces of an 8 μm thick conductive base layer 1 by a coater, and then dried at 90°C to form a highly conductive coating 3. Then, the low-water-absorption conductive material obtained in step a, 5 kg of modified polyacrylic acid binder and 1.5 kg of wetting agent are mixed and dispersed for 1 hour to obtain a low-water-absorption conductive slurry, and the low-water-absorption conductive slurry is applied to the surface of the high-conductive coating 3 by a coater, and then dried at 90°C to form a low-water-absorption coating 4. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 includes a highly conductive coating 3 and a low-water-absorption coating 4.
[0078] In this embodiment, the weight ratio of conductive material A and conductive glue is 4:1, and the weight ratio of conductive material A and conductive material B is 2.5:1. The total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1.1 μm, that is, the thickness of the high-conductive coating 3 is 0.5 μm, and the thickness of the low-water-absorption coating 4 is 0.6 μm.
[0079] Example 7
[0080] Select materials:
[0081] Conductive material A, 9kg conductive carbon black, oil absorption value 325ml / 100g, particle size 0.75μm; conductive adhesive, 3.6kg polythiophene butyl acetate solution, solid content 4.8%, content 9.2wt%, molecular weight 9300Da; conductive material B, 1kg carbon nanotubes, oil absorption value 75ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%, 2.5kg polyacrylic acid binder, content 25wt%; wetting agent, 2kg water; conductive base layer 1, 8μm thick aluminum foil.
[0082] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0083] Step a: First, 9 kg of conductive material A was vacuum dried at 65°C for 2.5 hours, then added to 3.6 kg of conductive glue and stirred for 2 hours. After filtering, the mixture was vacuum dried again at 65°C for 1.5 hours, and finally ground and refined to obtain a low water absorption conductive material.
[0084] Step b: First, 1 kg of conductive material B, 2.5 kg of polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 2 hours to obtain a highly conductive slurry, and the highly conductive slurry is applied to both surfaces of an 8 μm thick conductive base layer 1 by a coater, and then dried at 90°C to form a highly conductive coating 3. Then, the low water absorption conductive material obtained in step a, 5 kg of modified polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 0.5 hours to obtain a low water absorption conductive slurry, and the low water absorption conductive slurry is applied to both surfaces of the high conductive coating 3 by a coater, and then dried at 90°C to form a low water absorption coating 4. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 includes a highly conductive coating 3 and a low water absorption coating 4.
[0085] In this embodiment, the weight ratio of conductive material A and conductive glue is 2.5:1, the weight ratio of conductive material A and conductive material B is 9:1, and the total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 0.9 μm, that is, the thickness of the high-conductive coating 3 is 0.4 μm, and the thickness of the low-water-absorption coating 4 is 0.5 μm.
[0086] Example 8
[0087] Select materials:
[0088] Conductive material A, 8kg conductive carbon black, oil absorption value 300ml / 100g, particle size 0.5μm; conductive glue, 4kg polythiophene butyl acetate solution, solid content 0.5%, content 5.3wt%, molecular weight 4700Da; conductive material B, 0.5kg conductive carbon black, oil absorption value 50ml / 100g, particle size 0.3μm; binder, 5kg modified polyacrylic acid binder, content 25wt%, 2.5kg polyacrylic acid binder, content 25wt%, conductive base layer 1, 8μm thick copper current collector.
[0089] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0090] Step a: First, 8 kg of conductive material A is vacuum dried at 50°C for 3 hours, then added to 4 kg of conductive glue and stirred for 3 hours, then filtered and vacuum dried again at 50°C for 2 hours, and finally ground and refined to obtain a low water absorption conductive material;
[0091] Step b: First, 0.5 kg of conductive material B, 2.5 kg of polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 2 hours to obtain a highly conductive slurry, and the highly conductive slurry is applied to both surfaces of an 8 μm thick conductive base layer 1 by a coater, and then dried at 90°C to form a highly conductive coating 3. Then, the low water absorption conductive material obtained in step a, 5 kg of modified polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 0.5 hours to obtain a low water absorption conductive slurry, and the low water absorption conductive slurry is applied to both surfaces of the high conductive coating 3 by a coater, and then dried at 90°C to form a low water absorption coating 4. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 includes a highly conductive coating 3 and a low water absorption coating 4.
[0092] In this embodiment, the weight ratio of conductive material A and conductive glue is 2:1, and the weight ratio of conductive material A and conductive material B is 16:1. The total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 0.8 μm, that is, the thickness of the high-conductive coating 3 is 0.3 μm, and the thickness of the low-water-absorption coating 4 is 0.5 μm.
[0093] Example 9
[0094] Select materials:
[0095] Conductive material A, 10 kg conductive carbon black, oil absorption value 300 ml / 100 g, particle size 1 μm; conductive adhesive, 3.3 kg polyaniline solution, solid content 10%, content 7.2 wt%, molecular weight 8200 Da; conductive material B, 1.5 kg conductive carbon black, oil absorption value 100 ml / 100 g, particle size 0.4 μm; binder, 5 kg modified polyacrylic acid binder, content 25 wt%, 2.5 kg polyacrylic acid binder, content 25 wt%; wetting agent, 2.5 kg water; conductive base layer 1, 8 μm thick aluminum foil.
[0096] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0097] Step a: First, 10 kg of conductive material A was vacuum dried at 80°C for 3 hours, then added to 3.3 kg of conductive glue and stirred for 2 hours. After filtering, the mixture was vacuum dried again at 80°C for 2 hours, and finally ground and refined to obtain a low water absorption conductive material.
[0098] Step b: First, 1.5 kg of conductive material B, 2.5 kg of polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 2 hours to obtain a highly conductive slurry, and the highly conductive slurry is applied to both surfaces of an 8 μm thick conductive base layer 1 by a coater, and then dried at 90°C to form a highly conductive coating 3. Then, the low water absorption conductive material obtained in step a, 5 kg of modified polyacrylic acid and 1.5 kg of wetting agent are mixed and dispersed for 0.5 hours to obtain a low water absorption conductive slurry, and the low water absorption conductive slurry is applied to both surfaces of the high conductive coating 3 by a coater, and then dried at 90°C to form a low water absorption coating 4. That is, the obtained nano-conductive layer on the surface of the conductive base layer 1 includes a highly conductive coating 3 and a low water absorption coating 4.
[0099] In this embodiment, the weight ratio of conductive material A and conductive glue is 3:1, the weight ratio of conductive material A and conductive material B is 20:3, and the total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1 μm, that is, the thickness of the high-conductive coating 3 is 0.5 μm, and the thickness of the low-water-absorption coating 4 is 0.5 μm.
[0100] Example 10
[0101] Select materials:
[0102] Conductive material A, 9kg conductive carbon black, oil absorption value 325ml / 100g, particle size 0.75μm; conductive adhesive, 3.6kg polythiophene butyl acetate solution, solid content 4.8%, content 9.2wt%, molecular weight 9300Da; conductive material B, 1kg carbon nanotubes, oil absorption value 75ml / 100g, particle size 0.4μm; binder, 5kg modified polyacrylic acid binder, content 25wt%, 2.5kg polyacrylic acid binder, content 25wt%; wetting agent, 2kg water; 0.5kg barium carbonate; conductive base layer 1, 8μm thick aluminum foil.
[0103] Preparation of high conductivity and low water absorption nano-carbon-coated current collector:
[0104] Step a: First, 9 kg of conductive material A was vacuum dried at 65°C for 2.5 hours, then added to 3.6 kg of conductive glue and stirred for 2 hours. After filtering, the mixture was vacuum dried again at 65°C for 1.5 hours, and finally ground and refined to obtain a low water absorption conductive material.
[0105] Step b: First, 1 kg of conductive material B, 2.5 kg of polyacrylic acid binder and 1 kg of wetting agent are mixed and dispersed for 2 hours to obtain a highly conductive slurry, and the highly conductive slurry is applied to both surfaces of an 8 μm thick conductive base layer 1 by a coater, and then dried at 90°C to form a highly conductive coating 3. Then, the low-water-absorbing conductive material obtained in step a, 5 kg of modified polyacrylic acid binder, 0.5 kg of barium carbonate and 1 kg of wetting agent are mixed and dispersed for 0.5 hours to obtain a low-water-absorbing conductive slurry, and the low-water-absorbing conductive slurry is applied to both surfaces of the high-conductive coating 3 by a coater, and then dried at 90°C to form a low-water-absorbing coating 4. The obtained nano-conductive layer on the surface of the conductive base layer 1 includes a highly conductive coating 3 and a low-water-absorbing coating 4.
[0106] In this embodiment, the weight ratio of conductive material A and conductive adhesive is 2.5:1, the weight ratio of conductive material A and conductive material B is 9:1, and the total thickness of the nanoconductive layer of the prepared high-conductivity, low-water-absorption nano-carbon-coated current collector is 1 μm, that is, the thickness of the high-conductive coating 3 is 0.4 μm, and the thickness of the low-water-absorption coating 4 is 0.6 μm.
[0107] Comparative Example 1
[0108] 10 kg of conductive carbon black with an oil absorption value of 500 ml / 100 g and a particle size of 2 μm was selected, as was 5 kg of modified polyacrylic acid binder with a content of 25 wt % and a 10 μm thick aluminum current collector.
[0109] The steps for preparing the current collector are as follows: first, 10 kg of conductive carbon black is vacuum dried at 20°C for 10 hours, then added to 5 kg of modified polyacrylic acid binder and stirred for 1 hour to obtain a slurry. The slurry is then coated on both surfaces of a 10 μm thick aluminum current collector using a coater and dried at 50°C to form a conductive coating.
[0110] In this comparative example, the thickness of the conductive coating layer was 1 μm.
[0111] Comparative Example 2
[0112] Select 10kg of conductive carbon black with an oil absorption value of 500ml / 100g and a particle size of 2μm, select 10kg of graphene with an oil absorption value of 200ml / 100g and a particle size of 1μm, select 5kg of polyacrylic acid binder with a content of 25wt%, and an 8μm thick copper current collector.
[0113] The steps for preparing the current collector are as follows: first, 10 kg of conductive carbon black is vacuum dried at 20°C for 10 h, then the dried conductive carbon black and 10 kg of graphene are added to 5 kg of polyacrylic acid binder and stirred for 1 h to obtain a slurry, and then the slurry is coated on both surfaces of an 8 μm thick copper current collector through a coater and dried at 50°C to form a conductive coating.
[0114] In this comparative example, the thickness of the conductive coating layer was 1 μm.
[0115] Performance Testing
[0116] The performance of the above Examples 1-10 and Comparative Examples 1-2 were tested, and the test results are shown in Table 1 below.
[0117] Table 1 Performance test
[0118] Through testing under different humidity environments, in terms of water absorption, compared with the comparative example, Examples 1-10 of the embodiments of the present application have very low water absorption, especially the higher the humidity, the greater the difference in water absorption between Examples 1-10 and Comparative Example 1-2. For example: in an environment with a humidity of 20%, the difference in water absorption between Example 2 and Comparative Example 1 is 331ppm, and in an environment with a humidity of 20%, the difference in water absorption between Example 2 and Comparative Example 1 is 1126ppm. In terms of coating peeling force, compared with the comparative example, Examples 1-10 of the embodiments of the present application have higher peeling force, and in an environment with higher humidity, Examples 1-10 still have strong peeling force.
[0119] In summary, it can be seen that when the high-conductivity, low-water-absorption nano-carbon-coated current collector prepared by the present application is used in a lithium battery, due to the low water absorption performance of the nano-conductive layer, when water is generated in the electrolyte of the battery, the peeling force between the nano-conductive layer and the conductive base layer is less affected, and therefore the conductive performance of the current collector or the battery is less affected.
[0120] The above description is only a preferred embodiment of the present application and is not intended to limit the application. Any modifications, equivalent replacements, improvements, etc. made within the design concept of the present application should be included in the scope of protection of the present application.
Claims
1. A high-conductivity, low-water-absorption nano-carbon-coated current collector, wherein: The high-conductivity, low-water-absorption nano-carbon-coated current collector comprises a conductive base layer and a nano-conductive layer, wherein the nano-conductive layer is located on any surface of the conductive base layer; Among them, the components of the nano conductive layer include conductive material A, conductive glue, conductive material B and adhesive, and the oil absorption value of the conductive material A is greater than the oil absorption value of the conductive material B, the particle size of the conductive material A is greater than the particle size of the conductive material B, and the conductive glue is a solvent glue.
2. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 1, wherein: The oil absorption value of the conductive material A is ≥300 ml / 100 g and the particle size is 0.5-1 μm, and the oil absorption value of the conductive material B is ≤100 ml / 100 g and the particle size is <0.5 μm.
3. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 2, wherein: The conductive material A includes conductive carbon black, and the conductive material B includes at least one of graphene, conductive carbon black and carbon nanotubes.
4. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 1, wherein: The solid content of the conductive adhesive is 0.5-10%, and the conductive adhesive comprises at least one of a polyaniline solution and a polythiophene solution.
5. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 1, wherein: The adhesive includes at least one of a modified polyacrylic acid adhesive and a polyacrylic acid adhesive.
6. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 1, wherein: The nano-conductive layer also includes barium carbonate.
7. The high-conductivity, low-water-absorption nano-carbon-coated current collector according to any one of claims 1 to 6, wherein: The water absorption of the high-conductivity and low-water-absorption nano-carbon-coated current collector is 123-242 ppm.
8. A method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to any one of claims 1 to 7, wherein: The preparation method comprises the following steps: Step a: First dry the conductive material A, add it to the conductive glue and mix it evenly, then filter it and dry it again. Dry, and finally grind and refine to obtain low water absorption conductive material; Step b: coating the low water absorption conductive material and conductive material B obtained in step a onto a conductive base layer.
9. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 8, wherein: The weight ratio of the conductive material A to the conductive adhesive is 1-5:1, and the weight ratio of the conductive material A to the conductive material B is 8-10: 0.5-1.5。 10. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 9, wherein: In step b, the low water absorption conductive material, conductive material B, modified polyacrylic acid binder and wetting agent obtained in step a are first mixed and dispersed to obtain a low water absorption and high conductivity slurry, and then the low water absorption and high conductivity slurry is coated on a conductive base layer to form a high conductivity and low water absorption coating, that is, the nano conductive layer on the surface of the conductive base layer is the high conductivity and low water absorption coating.
11. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 10, wherein: Step b also includes mixing and dispersing barium titanate into the low water absorption and high conductivity slurry.
12. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 11, wherein: The thickness of the high-conductivity and low-water-absorption coating is 0.8-1.2 μm.
13. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 8, wherein: In step b, the conductive material B, the polyacrylic acid binder and the wetting agent are first mixed and dispersed to obtain a high conductive slurry, and the high conductive slurry is applied to the conductive base to form a high conductive coating. Then, the low water absorption conductive material, the modified polyacrylic acid binder and the wetting agent obtained in step a are mixed and dispersed to obtain a low water absorption conductive slurry, and the low water absorption conductive slurry is applied to the high conductive coating to form a low water absorption coating, that is, the obtained nano conductive layer on the surface of the conductive base includes a high conductive coating and a low water absorption coating.
14. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 13, wherein: Step b also includes mixing and dispersing barium titanate into the low water absorption conductive slurry.
15. The method for preparing a high-conductivity, low-water-absorption nano-carbon-coated current collector according to claim 14, wherein: The thickness ratio of the high conductive coating to the low water absorption coating is 0.3-0.5:0.5-0.6.
Citation Information
Patent Citations
Current collector and manufacturing method thereof
CN110676463A
Current collector conductive coating and preparation method thereof
CN110718674A
Battery current collector and preparation method thereof
CN112820881A
Preparation method of positive electrode slurry, positive electrode plate and lithium ion battery
CN114284465A
Composite structure flexible current collector and preparation method thereof
CN114784291A