Process for manufacturing an association of piezoelectric and magnetostrictive materials to obtain a magnetoelectric composite material exhibiting a self-biasing behavior

The composite material, formed by stacking magnetostrictive and piezoelectric layers with specific thicknesses and grown using cathode sputtering, achieves self-polarization and high magnetoelectric output, addressing the limitations of conventional composites and enabling efficient, lead-free, and fatigue-resistant magnetoelectric devices for medical and monitoring applications.

WO2024200842A1PCT designated stage expired Publication Date: 2024-10-03CENT NAT DE LA RECH SCI (C N R S) +1

Patent Information

Application Number
PCT/EP2024/058807
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing magnetoelectric composites face challenges in achieving self-polarization, which is essential for reducing the dependency on external magnetic fields, particularly in implantable medical devices, due to the limitations of thin nickel layers and structural fatigue in conventional bonding methods.

Method used

A composite material is developed by stacking layers of magnetostrictive and piezoelectric materials with specific thickness ranges, where the magnetostrictive layers are grown using cathode sputtering to create a strong bond, inducing significant deformation and self-polarization effects without the need for external magnetic fields.

Benefits of technology

The composite material achieves high magnetoelectric output and self-polarization, enabling efficient operation of magnetoelectric devices without lead or rare earths, with improved structural integrity and reduced fatigue, suitable for medical and infrastructure monitoring applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024058807_03102024_PF_FP_ABST
    Figure EP2024058807_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a process for manufacturing a composite material by cathode sputtering thin layers of magnetostrictive materials onto opposite surfaces of a substrate made of piezoelectric material, said material comprising a stack of layers in the following order: a first layer comprising the magnetostrictive material, of a thickness of 1 to 50 μm; a second layer comprising the piezoelectric material, of a thickness of less than 1 mm; and a third layer comprising said magnetostrictive material, of a thickness of 1 to 50 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Description Title of the invention: METHOD FOR PRODUCING A COMBINATION OF PIEZOELECTRIC AND MAGNETOSTRICTIVE MATERIALS TO OBTAIN A MAGNETOELECTRIC COMPOSITE MATERIAL EXHIBITING SELF-POLARIZED BEHAVIOR

[0001] The present invention relates to the field of laminar composite materials comprising a piezoelectric substrate associated with layers of magnetostrictive materials.

[0002] Bibliographic references in the following text are noted in the description text as follows: [] ; and listed in the reference table. State of the art

[0003] Magnetoelectric (ME) composites open up perspectives in different fields of engineering to design sensors, transducers, filters and other devices based on the change of electric polarization induced by an exciting magnetic field (forward ME effect) or by the change of M (magnetization) induced by an exciting electric field (reverse ME effect). For example, the possibility of harvesting electrical energy from an external exciting magnetic field to integrated medical devices is particularly interesting [1].

[0004] The term "magnetoelectric", hereinafter used by its acronym "ME"; defines the ability of a material to vary its state of magnetization under the action of an electric field and to vary its state of electric polarization under the action of a magnetic field, generally composed of a static polarization component and a small signal dynamic component.

[0005] Furthermore, the use of a micro-energy source ME to power a sensor in the biomedical field through the human body is known. This application is achievable by employing a small-signal dynamic magnetic field operating in a range frequency where there is no absorption by the human body (about 100 kHz) [2],

[0006] ME devices incorporating laminar composites made of ferroelectric (FE) materials (e.g., BaTiOa, Pb(Zr, Ti)Oa, Pb(Mg, Nb)Oa, PbTiOa) bonded to ferromagnetic (FM) and magnetostrictive materials (e.g., CoFe2O4, Terfenol-D, Galfenol) leading to efficient cross-coupling via intense elastic mechanical deformation upon application of a magnetic field, i.e., magnetoelastic coupling, are common [3]. Self-polarization conditions are difficult to obtain but they allow ME composites to no longer depend on the static component of the excitation magnetic field.

[0007] The term "magnetostrictive" defines a material exhibiting a magnetostriction property, which characterizes the ability of a material to deform depending on the orientation of its magnetization, for example under the influence of a magnetic field.

[0008] The term "self-bias" defines the ability to obtain a usable magnetoelectric coefficient without the need to impose an external continuous magnetic field, which greatly simplifies the technology of ME devices and facilitates their use for implantable medical device purposes.

[0009] Due to their magnetic properties, nickel (Ni) films are good candidates for magnetoelastic actuation by coupling with substrates that exhibit structural anisotropy in the plane parallel to the surfaces, such as LiNbOa. Usually, nickel films are composed of randomly distributed crystals (so-called polycrystalline film). Nevertheless, the magnetization and magnetostriction curves can exhibit anisotropic behaviors when an external extensive (positive) or compressive (negative) stress is applied along the x- and y-directions of the plane. An example of magnetic anisotropic F control of nickel films deposited on LiNbOa is known from [4]. However, the nickel layers in [4] are too thin, at most 100 nm, for to be able to obtain, following the application of an external excitation magnetic field, sufficient deformation of the LiNbOa which carries the Nickel layers on its faces. In fact, the Ni layers are deposited by a laboratory technique well suited to studies of very thin layers (electron beam evaporation), therefore not allowing sufficient deformation to be obtained. Description of the invention

[0010] To overcome the drawbacks of the aforementioned state of the art, the present invention relates to a composite material, comprising the stacking of layers on top of each other in the following order: • a first layer comprising a magnetostrictive material with a thickness of 1 to 50 pm; • a second layer comprising a piezoelectric material with a thickness of less than 1 mm; and • a third layer comprising said magnetostrictive material with a thickness of 1 to 50 pm.

[0011] The inventors have shown in a completely fortuitous manner that the association of such layers in these thickness ranges makes it possible to obtain sufficient deformation of the piezoelectric material by the magnetoelectric material under self-polarization conditions. Such a composite material integrating relatively thick magnetostrictive layers inducing significant longitudinal deformations of the piezoelectric layer makes it possible to obtain a high ME output (-100 V / (cm Oe)) in the -100-400 kHz regime.

[0012] Advantageously, the magnetostrictive material is selected from the following materials: nickel (Ni), iron (Fe), metal alloys comprising Ni, metal alloys comprising Fe, Fe-based oxides and cobalt (Co)-based oxides, such as CoFe2O4.

[0013] Advantageously, the piezoelectric material is selected from materials comprising at least one of the elements chosen from N (nitrogen), Fe, Nb (niobium), Bi (bismuth), Li (lithium), Ti (titanium), Ba (barium), Pb (lead), Al (aluminum), Mg (magnesium), O (oxygen) and Zn (zinc); preferably selected from LiNbOa, ZnO, BaTiOa, BiFcOa, LiTaOa, lead zirconate titanate (PZT), lead magnesium niobate - lead titanate (PMN-PT), or even aluminum nitride (AIN).

[0014] The inventors have shown that materials incorporating such stacks, for example Ni / LiNbCh / Ni, enable efficient self-polarized magnetoelectric devices without lead and without rare earths. The sputtering growth of these tri-layers ensures a tight and strong physical bond between the magnetostrictive layers and the piezoelectric. This is an advantage over conventional laminar composites, for which the magnetostrictive layers are bonded using epoxy to the piezoelectric material, which makes the composites prone to structural fatigue and material aging. In the case of Ni / LiNbCL / Ni, the residual stresses are due to the mismatch of the thermal expansion coefficient of Ni and LiNbOa which, in turn, induces a significant magnetic anisotropy and consequently a self-polarization effect of the composite material

[0011] .

[0015] PZTs, being lead zirconate titanoates, are chemical compounds with the formula PbZr x Tii- x O3 (0 < x < 1) and these are perovskite structure ceramics. PZTs can be of the PZT-5A, PZT-5H or PZT-5J type.

[0016] PMN-PTs, being magnesium lead niobate - lead titanate, are compounds of formula xPb(Mgi / 3Nb2 / 3)O3-(lx)PbTiO3 (0 < x < 1), such as those described in article [5].

[0017] Aluminum nitride of formula AIN, whose IUPAC name is azanylidinealumane, is identified by a CAS number: 24304-00-5.

[0018] Advantageously, the piezoelectric material is selected from 36° Y-cut LiNbCL; 163° Y-cut LiNbCL; Y-cut LiNbCL; Y-cut LiTaCL; 36° Y-cut LiTaCL and 163° Y-cut LiTaCL, and preferably from 36° Y-cut LiNbO3; 163° Y-cut LiNbO3; 36° Y-cut LiTaO3 and 163° Y-cut LiTaCL. The inventors have demonstrated that the crystalline orientation of the substrate, in particular 36° Y-cut and 163° Y-cut, induces a stress spontaneously anisotropic residual in the magnetoelectric layers during cooling after growth, as evidenced by X-ray diffraction and magnetometry measurements, described in the experimental section below.

[0019] The cutting angle of the LiNbOa crystal and that of LiTaOa are defined with respect to an orthonormal coordinate system (X,Y,Z) which we define as follows: the Z direction is parallel to the ternary rotation axis present in these two crystals (space group R3c)[Wong, K.K. (2002). Properties of Lithium Niobate. London, United Kingdom: INSPEC. p. 8. ISBN 0-85296-799-3.] The lattice is defined by the usual basis vectors of a Bravais lattice of the hexagonal crystal family: (a, b, c), with c parallel to Z. We define X and Y as the two directions perpendicular to Z such that X is parallel to the vector a and Y is perpendicular to X. Consequently, the so-called Y-cut indicates that the crystal is cut with the Y axis parallel to the surface normal. The 163° Y-cut indicates that the crystal is cut at the plane rotated 163° from the Y-plane around the X-axis (counterclockwise rotation).The 36° Y-cut indicates that the crystal is cut at the plane rotated 36° from the Y plane around the X axis (counterclockwise rotation).

[0020] Advantageously, the thickness of each layer comprising the magnetostrictive material is 5 to 35 μm.

[0021] Advantageously, the thickness of the layer comprising the piezoelectric material is 100 to 500 μm.

[0022] The present invention also relates to a method of manufacturing the composite material according to the invention comprising at least one step of depositing one of the layers selected between the first and third layers designated as thin layers, on the second layer designated as substrate, implementing the cathode sputtering technique.

[0023] Advantageously, the manufacturing method according to the present invention comprises the following steps: a- cleaning the surfaces of the substrate, preferably chosen from a double-sided polished LiNbOa plate, in an ultrasonic bath with acetone, then with isopropanol; b- introducing the substrate into a cathode sputtering deposition device;

[0024] c- once the vacuum is established, create in-situ in the growth frame a surface cleaning plasma of the aforementioned substrate; and d- spray a thin layer of magnetostrictive material, preferably a Ni film, at a pressure of 10-3 to 10-1 mbar, with a power of 100 to 1000 W (i.e. between 1 W / cm 2 and 13 W / cm 2 ). The temperature imposed on the substrate during this step of deposition of the magnetostrictive material can vary from room temperature up to 600°C.

[0025] e- repeat steps b-, c- and d- previously described on the opposite face of the LiNbO3 plate.

[0026] Advantageously, the cathode sputtering device is an SCM400 frame, comprising a magnetron, formerly marketed by the company Alcatel. The mode used is an RF mode (13.56 MHz) under Ar gas.

[0027] Advantageously, the Ni sputtering in steps d- and e- is carried out while maintaining a bare surface, preferably 0.5 to 1.5 mm wide, on the edges of the LiNbOa substrate plate. The objective being that the two opposite faces do not end up in short circuit after the Ni deposits.

[0028] The present invention also relates to a magnetoelectric transducer comprising the composite material according to the invention, and a magnetic field source.

[0029] The present invention also relates to a use of a magnetoelectric transducer according to the invention, to obtain a potential difference between the first and third layers comprising the magnetostrictive material by applying a dynamic small signal magnetic field in the direction of the planes of the layers at a frequency of 100 to 400 kHz. This dynamic magnetic field has a sufficiently low amplitude so that we remain in a linear approximation. This is our case here because the magnetic field has an amplitude of 1 Oe = 0.1 mT and the response of the magnetostrictive material is linear.

[0030] The present invention also relates to a magnetoelectric device comprising a magnetoelectric transducer according to the invention, for generating an electric voltage without applying a so-called static continuous magnetic field. Such behavior of the device is attributed to so-called self-bias phenomena corresponding to the English term "self-bias".

[0031] Such a device can be advantageously used to power electronic microsystems for monitoring deformations in construction infrastructures, or in the medical field, used in a medical implant.

[0032] The present invention is also described in the detailed description which follows, using the experimental part which details certain embodiments using examples, given solely for illustrative purposes and which should not be considered as limiting, and the figures briefly described in the part which follows. Brief description of the figures

[0033] [Fig.l] - Figure 1 shows illustrations of the different sections of the monocrystalline substrate LiNbOa;

[0034] [Fig.2] - Figure 2 represents the XRD patterns of the deposited nickel films (Cu target with a monochromator wavelength λ = 1.54 Å);

[0035] [Fig.3] - Figure 3 represents the characterization of the Ni / LiNbCL / Ni tri-layer with magnetic fields applied along the x or y axes

[0036] [Fig.4] - Figure 4 represents an ME resonance measurement carried out to determine the electromechanical resonance (EMR) frequency of each sample in their two in-plane directions; two different LiNbOa sections are studied: (YX1) 36° (a) and (YX1) 163° (b);

[0037] [Fig.5] - Figure 5 represents the ME coefficient as a function of the HDC for the samples Ni / (YX1) 36° Y-cut LiNbOa / Ni and Ni / (YX1) 36° Y-cut LiNbCE / Ni in the x and y directions, the measurements are carried out at the electromechanical resonance (EMR) frequency of each sample;

[0038] [Fig.6] - Figure 6 represents the magnetization of Nickel films in a three-layer sample and in the free state;

[0039] [Fig.7] - Figure 7 represents the hysteresis loops ME and curves (dM 2 / dH)-H of tri-layer samples;

[0040] [Fig.8] - Figure 8 represents the VSM magnetization cycles measured at different temperatures in both directions of a Ni / (YX1) 36° Y-cut LiNbCE / Ni tri-layer. ; and

[0041] [Fig.9] - Figure 9 represents the XRD patterns in the plane of the (311) peak of Ni from a sample integrating the (YX1) 36° Y-cut LiNbOa (Cu target without monochromator, Å of K_a= 1.5419 Â). Experimental Part

[0042] Materials and methods In the context of the invention, the diffractometer used for X-ray diffraction is a Rigaku “Smartlab®” multi-configuration 5-circle diffractometer with rotating anode, suitable for thin films allowing diffraction under grazing incidence and other high-resolution measurements.

[0043] Two commercial monocrystalline substrates (supplied on specific request from NEYCO®) LiNbOa polished on both sides, cut in a 36° Y-cut - “36° Y-cut” (20x5x0.1 mm 3) and cut in Y at 163° - “163° Y-cut” (10x5x0.1 mm 3 ) were used to deposit thick polycrystalline Ni films on each side by RF magnetron sputtering. A high purity Ni target (Ni > 99.95%) was used. The “a” axis is identified by the (210) peak of the single-crystal LiNbOa substrates using in-plane X-ray diffraction (XRD). It is observed that the “a” axes of both LiNbOa substrates are parallel to their x (length) directions. As shown in Figure 1, the 36° Y-cut (36° Y-cut ) and the 163° Y-cut (163° Y- cut) can also be designated as (YX1) 36° and (YX1) 163° respectively according to the IEEE standard [ANSI / IEEE Std 176-1987 An American National Standard IEEE Standard on Piezoelectricity, 74]. Before deposition, the LiNbOa substrates were chemically cleaned (ultrasonic bath with first acetone and then isopropanol) before being introduced into the sputtering deposition machine, and the substrate surfaces were cleaned in situ using an argon plasma. Nickel films with a thickness of 5 to 35 μm were deposited on both sides under a pressure of 10' 1 mbar with a power between 100 and 500 W. The ultimate vacuum of the spray chamber is 10' 7mbar. The depositions were carried out under argon atmosphere, at room temperature or at 200°C. The distance between the target and the substrate support is 65 mm. A distance of 1 mm between the edges of the LiNbOa substrate and the edges of the nickel film was kept to avoid short-circuiting the deposited nickel films. The two faces of the same sample are assumed to be symmetrical, with the same amount of Ni.

[0044] The XRD patterns of the deposited nickel films (arbitrary side) of the two samples are shown in Figure 2, and compared with the pattern of the reference polycrystalline Ni target. The nickel films deposited on the LiNbOa substrate are polycrystalline. Results and discussion

[0045] Characterization of magnetoelectric (ME) behavior

[0046] As shown in Figure 1, the ME behaviors of Ni / LiNbOa / Ni samples are characterized in the so-called LT mode, where the external magnetic field is applied longitudinally in the x- or y-plane direction, and the output electric voltage is transversely polarized in the z-direction. According to the studies published in [6-7], the ME coefficient aE is mainly determined by the transverse piezoelectric constants d_31 A P, thus, the cuts (YX1) 36° and (YX1) 163° are chosen with high values ​​[8], i.e. d_31 A P ~ 18 pC / N for the first and d_31 A P ~ -20 pC / N for the second respectively, favoring the ME effect along the x and y directions of the experimental setup, respectively (see Figure 3).

[0047] The ME coefficient characterization was performed using the same setup as described in [2]. A 100-turn copper coil was used to apply a small harmonic magnetic signal Hac of 1 Oe = 0.1 mT in RMS. This field was driven by an alternating current from a Rohde & Schwarz® HM8150 arbitrary waveform generator. Simultaneously, a static magnetic field of HDC bias is superimposed in the same direction as Hac by setting the distance “d” between two blocks of permanent magnets mounted on a movable rail and previously calibrated with a Gaussmeter in the middle of the copper coil. The ME samples were inserted in the middle of the coil to apply the superimposed magnetic field during the ME coefficient characterization. They were mounted in a sample holder composed of plastic plates printed by a 3D printer and two separate conductive wires.The plastic plates were used to align the length or width direction of the ME samples with the applied magnetic field; the wires are brought into electrical contact with the Ni films on both sides of the ME sample. Then the ME output voltage (MEV) generated between the Ni layers of a ME sample is measured using a Keysight® MSO7054A digital oscilloscope. From these results, the ME coefficient aE is obtained using the formula (A) where t. p is the thickness of the piezoelectric substrate:

[0048] [FORMULA A] aE = VME / .Hac x tp)

[0049] In order to clearly study the ME aE behaviors as a function of HDC value of Ni / LiNbOs / Ni samples, the Hac frequency is set close to the electromechanical resonance frequency (EMR) of each sample to obtain a remarkable magnitude of the VME output voltage. This frequency or EMR is calculated using the following equation according to the formula (B) [9], where Z is the length of the piezoelectric substrate, y is the average Youg modulus and p is the average volume density of the ME composite.

[0050] [FORMULA B]

[0051] The measurements are shown in Figure 4: the first harmonics obtained are approximately 160 kHz and 320 kHz for the samples with the 20 mm long (YX1) 36° substrate and the 10 mm long (YX1) 163° substrate [9], respectively. The electromechanical resonance (EMR) frequency corresponding to the maximum of the VME is identified by ME voltage measurements performed by sweeping the Hac signal frequency. Then, the ME coefficient characterization is performed by sweeping the HDC first from -710 Oe = -71 mT to 710 Oe = 71mT, and then from 71 to -71 mT. The direction of HDC is changed by swapping the permanent magnets in the position of HDC~0 mT (see Figure 4).

[0052] As shown in Figure 5, each measurement exhibits a maximum ME response at the optimal bias magnetic field, Hbias. It is noted that the Hbias values ​​in the x direction are much smaller than those in the y direction, where x is parallel to the al axis in the trigonal system of LiNbOa and y is the axis perpendicular to x, in the plane: for the Ni / (YX1) 36° Y-cut LiNbOa / Ni, Hbias is equal to ±37 Oe = ± 3.7 mT and ±149 Oe = ± 14.9 mT in the x and y directions, respectively. For the Ni / (YX1) 163° Y-cut LiNbOa / Ni, Hbias is equal to ±106 Oe = ± 10.6 mT and ±238 Oe = ±23.8 mT in the x and y directions, respectively.

[0053] In Figure 5 (Figures 5a and 5b) a "self-polarized" behavior is shown for Hac parallel to the x direction. Interestingly, at HDC = 0, aE is at 94.20% of its maximum value for the sample grown on the (YX1) 36° LiNbOa substrate and at 80% for the one grown on the (YX1) 163° LiNbOa substrate. Moreover, the self-polarized behavior self-bias is greatly reduced in the y direction, where aE values ​​are less than 40% of their maximum values.

[0054] Measurements of magnetic anisotropies: role played by the LiNbCh substrate

[0055] In the following, we relate the ME response of our devices to the intrinsic magnetic properties of Ni films and show the important role played by the LiNbOa substrate. For this purpose, magnetic hysteresis loops are collected using a vibrating sample magnetometer (VSM) available on a Quantum Design® Physical Property Measurement System (PPMS).

[0056] The magnetization (M) was measured at 300K as a function of the HDC from 2 kOe = 200 ni T to 500 Oe = 50 ni T (step = 10 Oe = 1 mT), then from 500 Oe = 50 mT to -500 Oe = -50 mT with high accuracy (step = 2 Oe = 0.2 mT), after from -500 Oe = -50 mT to -2 kOe = -200mT, and finally a reverse repetition. An accurate determination of the coercive field was attempted during these measurements. Before mounting each sample, an oscillating field from 10 kOe = 1 T to zero was applied to reduce the residual magnetic field in the solenoid to less than 5 Oe = 0.5 mT.

[0057] The samples were laser cut into 5 x 5 mm pieces 2 to fit the VSM sample holder. After measuring the magnetization of the tri-layer sample, self-supporting Ni films whose magnetization was measured by VSM were isolated. As shown in Figure 6, anisotropic behavior of the magnetization is observed on the tri-layer samples, with higher remanence and lower saturation field in the x direction compared to the y direction. Interestingly, the anisotropy is larger in the tri-layer samples than in the isolated Ni films. The anisotropy is greatly reduced in the self-supporting films, indicating the important role played by the residual stress imposed by the substrate. This allows us to deduce that the LiNbOa substrates induce anisotropic internal stress and a consequent magnetic anisotropy.

[0058] Relationship between magnetic anisotropies and ME

[0059] In order to relate the magnetic anisotropy to the ME anisotropic response, we compare the M(H) cycles with the field dependence aE. Indeed, the ME coupling combines the piezomagnetic and piezoelectric effects, both effects are assumed to be linear

[0010] . The ME coefficient can be written as the product of the gradients of the piezomagnetic and piezoelectric effects: aE = \dT / dS X dD / dT X dE / dD | X dS / dH , where T is the stress, D is the displacement field, E is the electric field, S is the strain. Thus, the magnetic field dependence of the ME coefficient is such that aE oc dS / dH = d / dH, where A is the strain due to magnetostriction. Since A oc M2 , finally the relationship obtained by the inventors is aE oc dM2 / dH as the relationship relating the ME response and the magnetization.

[0060] As shown in Figure 7, we find good agreement between the dependence of H on (dM 2 / dH) and the ME hysteresis loop (sign permutation of a_E at antiresonances), attesting that the ME anisotropy behavior reflects the magnetic anisotropy of the nickel films in contact with the LiNbOa substrates.

[0061] Origin of magnetic and ME anisotropies

[0062] The results presented in this section show that the origin of the magnetic anisotropy lies in the difference between the coefficient of thermal expansion (CTE) of Ni and that of LiNbOa. The thicknesses of the two Ni layers are 10 pm each and that of the LiNbOa substrate is 100 pm. Similar effects were observed for Ni thicknesses of 35 pm. Indeed, the samples are heated during deposition due to plasma exposure and the deposition temperature imposed on the substrate, and then cooled to room temperature (~ 300K) after the sputtering growth procedure.Thus, the nickel films of the tri-layer samples are subject to residual stresses or related to the effects of thermal expansion, i.e., the very general formula or, ij = Ce, ijkl (as — af )kl AT , where as and af are respectively the thermal expansion coefficients of the LiNbOa substrate and the Ni film, AT the difference between the. room temperature and the temperature during the sputtering deposition process, and Ce, ijkl is the elastic tensor of the nickel film. The experiments presented below investigate the in-plane biaxial (residual) stress induced in nickel films, i.e., gold, xx and gold, yy . Since the CTE of the LiNbOa substrate in the x direction is higher than the CTE of nickel, as shown in Table 1 (as — af > 0), a negative (compressive) residual stress develops upon cooling of the sample. On the other hand, the coefficient of thermal expansion of the LiNbOa substrate in the y direction is lower than the CTE of nickel, as shown in Table 1 (as — af < 0) leading to a positive (extensional) residual stress under cooling condition. Thus, the residual stress is anisotropic at room temperature leading to the observed magnetic anisotropy.Indeed, the order of magnitude of the residual stress can be evaluated by considering an estimated ri T of -100 K due to the growth procedure and a Young's modulus of Nickel Ce = 207 GPa. It turns out that the expected residual stress, gold, will be of the order of 50 MPa, with opposite signs in the x and y directions.

[0063] [Table 1] a in the x direction a in the direction [K' 1 ] y [K' 1 ] Nickel 13xl0' 6 13xl0' 6 (YX1) 36° LiNbO3 15.4xl0' 6 10.23xl0' 6 (YX1) 163° LiNbO3 15.4xl0' 6 10.9xl0' 6 Table 1: CTE of nickel af and LNO as substrates

[0064] Probing stress-induced magnetic anisotropy through magnetic and structural measurements

[0065] The inventors also carried out the following experiments in order to determine the most suitable conditions in order to obtain the ideal deformation induced by phenomena linked to magnetic anisotropy.

[0066] M(H) curves at different temperatures:

[0067] Figure 8 shows the magnetization cycles measured by 5 VSM in the x and y directions, as a function of temperature. Magnetization cycles are found to be strongly temperature dependent in the y direction: magnetic remanence is higher at 400K than at 200K. In the x direction, high remanence is found at all temperatures probed. This indicates that residual stress is released by heating, leading to a more isotropic magnetic behavior at 400K. This behavior is related to that observed in Figure 6 where the magnetization cycles of the free-standing films are strongly modified in the y direction compared to the cycles measured for the same layer when it was still in contact with the5 substrate.

[0068] Determination of residual stresses by the X-ray diffraction method:

[0069] The existence of residual stresses is confirmed by a direct and quantitative determination of the changes in the atomic spacing of the nickel film by XRD phi-scan along the x and y directions. We compare the atomic spacing corresponding to the (311) peak, d311, in the nickel film deposited on LiNbOa with the free nickel film after removal from the substrate. As shown in Figure 9, by a fit of the measured (311) peaks using the Pseudo-Voigt function,5 the value of d311 can be estimated in the x and y directions. The measured negative (positive) change in the atomic spacing indicates a negative (positive) residual stress in x (y).

[0070] [Table 2] Neither tri-layered Nor isolated Neither tri-layered Nor isolated (x-direction) (x-direction) (y-direction) (y-direction)6 [degree] 93.0401 93.0127 92.9828 93.0318 cu [À] 1.0625 1.0627 1.0630 1.0626 Change -0.0002 0.0004 atomic space [Â] Table 2. Estimation of atomic spacing variation References

[0071] Table 3 below lists the references cited previously in the text: 5 [Table 3]

Claims

Claims 1. A method of manufacturing a composite material comprising stacking the layers on top of each other in the following order: - a first layer comprising a magnetostrictive material with a thickness of 1 to 50 pm; - a second layer comprising a piezoelectric material with a thickness of less than 1 mm; and - a third layer comprising said magnetostrictive material with a thickness of 1 to 50 μm; said manufacturing method comprising the following steps, after providing a substrate provided with surfaces and intended to form the second layer: a) cleaning the surfaces of the substrate in an ultrasonic bath with acetone, then with isopropanol; b) introducing the substrate into a cathode sputtering deposition apparatus, said apparatus being provided with a growth frame; c) once the vacuum has been established in said apparatus, making in situ in the growth frame a surface cleaning plasma of the substrate; d) spraying a thin layer of magnetostrictive material onto a surface of the substrate to form said first layer, at a pressure of 10' 3 at 10' 1 mbar, with a power of 100 to 1000 W or between 1 W / cm 2 and 13 W / cm 2 ; e) repeating steps b), c) and d) on the opposite surface of the substrate to form said third layer.

2. A method of manufacturing a composite material according to claim 1, wherein the magnetostrictive material is selected from Ni, Fe, metal alloys comprising Ni, metal alloys comprising Fe, Fe-based oxides and Co-based oxides.

3. Method for manufacturing a composite material according to claim 1 or 2, in which the piezoelectric material is selected from materials comprising at least one of the elements chosen from N, Fe, Nb, Bi, Li, Ti, Ba, Pb, Al, Mg, O and Zn.

4. Method for manufacturing a composite material according to one of claims 1 to 3, in which the piezoelectric material is selected from: LiNbOa, ZnO, BaTiOa, BiFcOa, LiTaOa, a lead zirconate titano (PZT), a lead magnesium niobate - lead titanate (PMN-PT), or even aluminum nitride (AIN).

5. A method of manufacturing a composite material according to one of claims 1 to 3, wherein the piezoelectric material is selected from 36° Y-cut LiNbO3; 163° Y-cut LiNbO3; Y-cut LiNbCh; Y-cut LiTaO3; 36° Y-cut LiTaO3 and 163° Y-cut LiTaO3.

6. Method for manufacturing a composite material according to one of claims 1 to 5, in which the thickness of each layer comprising the magnetostrictive material is 5 to 35 μm.

7. Method for manufacturing a composite material according to one of claims 1 to 6, in which the thickness of the layer comprising the piezoelectric material is 100 to 500 μm.

Citation Information

Patent Citations

  • Micro-cavity magnetic sensitive device and preparation method thereof

    CN115548210A

Cited By

  • Forceps control system based on transducer device, preparation method and control method

    CN119633917A

  • Transducer device-based tweezer manipulation system, preparation method and manipulation method

    CN119633917B