Coke production method
By calculating and adjusting the interfacial tension in coal blends using specific formulas, the method addresses the challenge of using coal blends with abnormal surface tensions, ensuring high coke strength and expanding raw material utilization in blast furnace coke production.
Patent Information
- Application Number
- PCT/JP2023/040108
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-11-07
- Publication Date
- 2024-10-03
AI Technical Summary
The existing methods for producing blast furnace coke struggle to maintain high strength when using coal blends with carbon materials having abnormal surface tensions, limiting the range of usable raw materials and leading to decreased coke strength.
A method involving the calculation of interfacial tension using specific formulas to determine the blending ratios of coal and carbon materials in both molded and powdered coal mixtures, ensuring the interfacial tension of the powdered coal mixture is less than 0.03 mN/m, thereby suppressing the decrease in coke strength.
This approach allows for the use of a wider range of coal and carbon materials, including those with abnormal surface tensions, stabilizing coke production and expanding resource availability by maintaining high coke strength.
Smart Images

Figure JP2023040108_03102024_PF_FP_ABST
Abstract
Description
Coke manufacturing method
[0001] The present invention relates to a coke manufacturing method, and more particularly to a method for adjusting the blending of raw materials into briquettes in a coke manufacturing method in which a portion of raw coal is carbonized as briquettes.
[0002] Blast furnace coke is used in the blast furnace as a reducing agent, a heat source, and a support material to maintain gas permeability and liquid permeability. Stable operation of the blast furnace requires ensuring gas permeability and liquid permeability within the furnace, which requires coke with excellent properties such as strength, particle size, and post-reaction strength. Among these, coke strength, such as rotational strength, is a particularly important property for blast furnace coke.
[0003] Blast furnace coke is produced by carbonizing coal in a carbonization furnace to soften and melt the coal particles and bond them together. Therefore, to produce high-strength coke, caking coal with excellent thermoplasticity is required. However, in recent years, caking coal suitable for coke production has been depleted. Therefore, there is a demand for expanded use of coal with poor thermoplasticity that has not been used in coke production until now, as well as carbon materials other than coal. Carbon materials other than coal include biomass such as wood pellets and oil palm residue, torrefied biomass obtained by torrefaction, biomass carbon material obtained by heat treatment of biomass, plastics, etc. In recent years, CO 2 Due to the growing need to reduce emissions, there is a demand to use biomass-derived carbon materials and waste plastics in coke production.
[0004] When producing blast furnace coke, a coal blend containing multiple types of coal is used. Therefore, methods for estimating the coke strength of coke produced using a coal blend as a raw material have been studied. In recent years, it has been discovered that the surface tension of coal in a thermoplastic state affects the adhesive strength of the coal. Patent Document 1 discloses a coal blending method and a coke production method that use surface tension and interfacial tension calculated from the surface tension. Patent Document 1 calculates the interfacial tension between different coal particles based on the surface tension of heat-treated coal (semi-coke) obtained by heat treating coal (hereinafter referred to as the surface tension of coal), and manages the coal blend based on the magnitude of the interfacial tension.
[0005] Coke is produced by carbonizing coal, softening and melting it, and fusing it together. Therefore, it is believed that the adhesive strength between coal particles affects the coke strength of the resulting coke. Generally, the adhesive strength between coal particles improves as the interfacial tension at the adhesive interface decreases. Since the unit of interfacial tension is mN / m, it can be considered as the free energy present at the interface. In other words, the presence of interfacial tension means that free energy exists at the interface that can act as a force. Therefore, it is believed that high interfacial tension makes fracture at the adhesive interface more likely to occur. According to Patent Document 1, if the interfacial tension of a coal blend exceeds 0.03 mN / m, the coke strength of the resulting coke decreases significantly, so it is preferable to keep the interfacial tension of the coal blend at 0.03 mN / m or less.
[0006] International Publication No. 2013 / 054526
[0007] MCWilliams and DW Fuerstenau, International Journal of Mineral Processing, 20(1987), p.153-157
[0008] According to Patent Document 1, in order to obtain high-strength coke, it is preferable to blend coals so that the interfacial tension of the coal blend is low. Therefore, to produce high-strength coke, it is effective to use coals with similar surface tension values in the coal blend. However, this method makes it difficult to use coals with too high or too low surface tensions. Patent Document 1 does not disclose a method for preventing a decrease in coke strength when using coals or carbonaceous materials with surface tensions that are significantly different from the weighted average surface tensions of the coals and carbonaceous materials contained in the coal blend, which poses a problem of limiting the range of usable coal resources.
[0009] Expanding the range of coal resources that can be used as coke raw materials would offer significant benefits in terms of stable procurement of raw materials and expanded application of difficult-to-use raw materials. Therefore, there has been a demand for a coke manufacturing method that can suppress a decrease in the coke strength of the produced coke, even when producing coke using a coal blend that contains coal or carbonaceous materials whose surface tension is too high or too low compared to the average surface tension of the coal blend. Hereinafter, coal or carbonaceous materials whose surface tension is too high or too low compared to the average surface tension of the coal blend will be referred to as "coal materials with abnormal surface tension."
[0010] The present invention has been made in consideration of the above circumstances, and its object is to provide a coke manufacturing method that can suppress a decrease in the coke strength of the produced coke, even when coke is produced using a coal blend that contains a carbonaceous material with abnormal surface tension.
[0011] The means for solving the above problems are as follows: [1] A method for producing coke by carbonizing a coal blend obtained by blending briquettes containing multiple brands of coal and a powder coal mixture containing multiple brands of powdered coal, wherein the interfacial tension γ of the coal blend is calculated using the surface tension of heat-treated coal obtained by heat-treating each brand of coal contained in the coal blend, the blending ratio of each brand of coal, and the following formula (1) or the following formula (2): inter and the interfacial tension of the powder coal mixture γ p But γ inter>γ p and γ p and determining the brand and blending ratio of coal to be blended in the briquettes and the powder coal mixture so as to satisfy the following condition: [2] A carbon material is blended into at least one of the briquettes and the powder coal mixture, and each brand of coal contained in the blended coal is heat-treated to obtain a surface tension of the heat-treated coal and the carbon material, and the blending ratio of each brand of coal and the carbon material, and the interfacial tension γ of the blended coal is calculated using the following formula (3) or (4) instead of the formulas (1) and (2). iter and the interfacial tension of the powder coal mixture γ p But γ inter >γ p and γ p The method for producing coke according to [1], wherein the brand and blending ratio of coal to be blended in the briquettes and the powdered coal mixture, and the type and blending ratio of the carbon material to be blended in the briquettes and the powdered coal mixture are determined so as to satisfy a β-value of 0.03 or less.
[0012] According to the present invention, even when coke is produced using a coal blend containing carbonaceous materials with abnormal surface tension, it is possible to suppress a decrease in the coke strength of the produced coke. As a result, a wide range of coals or carbonaceous materials, including carbonaceous materials with abnormal surface tension that could not be used in the past, can be used as coke raw materials, which contributes to stable procurement of raw materials and expansion of resources.
[0013] FIG. 1 shows the interfacial tension γ of the powder coal mixtures of Examples 1 to 3 and Comparative Examples 2 and 3. p 2 is a graph showing the relationship between the interfacial tension γ of the powder coal mixtures of Examples 4 to 7 and Comparative Examples 5 and 6. p 1 is a graph showing the relationship between the amount of coke strength increase and the amount of coke strength increase.
[0014] In order to solve the above-mentioned problems, the inventors of the present invention have studied a method for producing coke by using briquettes, which are formed by briquetting coal, as part of a coal blend, and carbonizing a coal blend containing the briquettes, unbriquetted powdered coal, and a carbon material (hereinafter referred to as a powdered coal mixture). Patent Document 1 discloses that a coal blend not containing briquettes has a suitable upper limit for the interfacial tension. However, in a briquette, particles such as coal are arranged closer to each other than in powdered coal, making adhesion between particles more likely than in powdered coal. Therefore, the suitable upper limit for the interfacial tension may change when the coal is briquetted.
[0015] As a result of extensive research, the inventors have confirmed that the interfacial tension of coal contained in a briquette has a smaller effect on coke strength than the interfacial tension of coal contained in a powdered coal. Specifically, they have found that when a coal blend containing a briquette and a powdered coal mixture is used, the interfacial tension of the powdered coal mixture becomes dominant when a carbonaceous material with abnormal surface tension is blended into the briquette. As a result, they have found that the decrease in coke strength due to the blending of a carbonaceous material with abnormal surface tension in the coal blend can be suppressed. Specifically, even when the interfacial tension of the entire coal blend is high, if the interfacial tension of the powdered coal mixture is reduced by blending a large amount of a carbonaceous material with abnormal surface tension in the briquette, the interfacial tension of the powdered coal mixture becomes dominant, thereby suppressing the decrease in coke strength of the coke produced by carbonizing the coal blend. Based on this finding, the present invention has been completed. The present invention will be described in detail below through embodiments of the present invention.
[0016] The effect of coal surface tension on coke strength is described in detail in Patent Document 1. In the coke manufacturing method according to this embodiment, first, the surface tension of the heat-treated coal or carbon material contained in the coal blend that is the raw material for the coke is determined. The measurement of the surface tension may be performed by the same method as that described in Patent Document 1. An outline of the method for measuring the surface tension is given below.
[0017] Known methods for measuring the surface tension of coal and carbonaceous materials include the sessile drop method, capillary rise method, maximum bubble pressure method, liquid gravity method, hanging drop method, ring method, plate method, expansion / contraction method, sliding method, and film flotation method. Because coal is composed of various molecular structures, its surface tension is expected to vary. For this reason, it is preferable to use a method that can evaluate the distribution of surface tension, such as the film flotation method described in Non-Patent Document 1. The film flotation method can be similarly applied to coal, carbonaceous materials, and semi-coke obtained by carbonizing them, and the surface tension distribution can be determined using a finely pulverized coal sample. The average value of the obtained surface tension distribution can be used as the surface tension of the coal sample.
[0018] Because adhesion of coal particles occurs when coal is in a softened and molten state during thermal carbonization, it is preferable to use heat-treated coal (semi-coke) as the coal sample for measuring surface tension. However, since no method for measuring the surface tension of molten coal at high temperatures is known, the present embodiment also measures the surface tension of heat-treated coal or carbon material using the method disclosed in Patent Document 1.
[0019] The heat treatment temperature for the coal sample is preferably within the range of 350°C to 800°C, which corresponds to the temperature at which coal begins to thermoplasticize and melt, and then adheres and solidifies to complete coking. In particular, it is more preferable to use semi-coke that has been heated to a temperature within the range of 350°C to 550°C, which is the temperature at which coal thermoplasticizes and melts, as this temperature contributes to adhesion. Of these, it is particularly preferable to use semi-coke that has been heated to a temperature within the range of 480°C to 520°C.
[0020] The heating of the coal sample is preferably carried out in an inert gas atmosphere, such as nitrogen, argon, or helium, which does not react with coal or carbon materials. The heating rate is preferably determined based on the heating rate used when producing coke in a coke oven; for example, the sample may be heated at a heating rate of 3°C / min. Furthermore, the sample heated to the target temperature is preferably rapidly cooled at a cooling rate of 10°C / sec or more in order to maintain the molecular structure at the target temperature, and the cooling method is preferably liquid nitrogen.
[0021] For carbon materials other than coal, it is also preferable to measure the surface tension of a sample that has been heat-treated in advance. Note that for carbon materials in which organic matter has been carbonized (semi-carbonized) in advance, the surface tension may be measured without prior heat treatment if the carbonization temperature exceeds the heat treatment temperature of coal.
[0022] Next, the briquettes will be described. In the coke manufacturing method according to this embodiment, a portion of the blended coal charged into the coke oven is briquetted. Briquettes can be formed by methods such as granulation, crimping, molding, adhesion, and kneading, and a combination of these methods may be used to form the briquettes. One example of a briquette is a briquette (briquetted coal) obtained by mixing multiple coals and carbon materials, adding a binder as needed, kneading the mixture in a kneader, and then compacting and molding the mixture in a double-roll molding machine. Examples of binders that can be used include water, coal-based binders (coal tar pitch, solvent-refined coal, tar, tar slag, etc.), petroleum-based binders (asphalt, asphalt pitch, propane-deasphalted asphalt, etc.), and organic binders (starch, molasses, synthetic polymer compounds, resins, etc.). The particle size of the coal used for briquetting is preferably adjusted by pulverization so that the ratio of particles of 3 mm or less is 70 to 100% by mass.
[0023] The bulk density of the molded product is 0.8 g / cm 3 It is preferable that the density is 0.9 g / cm or more. 3 More preferably, it is 1.0 g / cm or more. 3Increasing the bulk density of the briquettes improves the adhesiveness of even the carbonaceous material with abnormal surface tension to the surrounding coal and carbon materials, thereby suppressing a decrease in the coke strength of the produced coke.
[0024] Next, the powdered coal mixture will be described. In the coke manufacturing method according to this embodiment, the portion of the blended coal charged into the coke oven other than the briquettes is referred to as the powdered coal mixture. The coal constituting the powdered coal mixture is also preferably pulverized and adjusted in particle size so that the ratio of particles of 3 mm or less is 70 to 100 mass %. Furthermore, before charging into the coke oven, the moisture content may be adjusted by humidity control and drying. A carbon material may be blended into the powdered coal mixture.
[0025] Next, a method for calculating the interfacial tension will be described. In the coke manufacturing method according to this embodiment, the blending composition of the briquettes and the powder coal mixture is determined based on the interfacial tension calculated from the surface tension. The interfacial tension can be calculated based on the method described in Patent Document 1, and the method for measuring the interfacial tension will be outlined below.
[0026] It is preferable to measure the interfacial tension between coal particles directly at the interface between different coal particles, but such measurement is very difficult using existing technology. Therefore, it is preferable to measure it using the method described in Patent Document 1, which discloses the effect on coke strength. The interfacial tension between coal particles can be calculated using the surface tension of each coal or carbon material constituting the coal blend, the blending ratio, and the following equation (1).
[0027]
[0028] The surface tension of each heat-treated coal is the surface tension of heat-treated coal heated to the same temperature. i The blending ratio w i is the ratio of each brand (coal) contained in the blended coal to the total mass of the blended coal. i The interfacial tension between two different brands can be calculated using the following formula (5):
[0029] In the above equation (5), β is a constant, and Li and Neumann define its value as β = 0.0001247 [(m 2・mJ) 2 ]
[0030] The blending ratio may be calculated based on the ratio at the time of heat treatment, taking into account the difference in yield of each coal at the time of heat treatment. However, there is no significant difference in determining the blending composition whether it is calculated based on the blending ratio in the coal blend or the ratio in the heat-treated product. In addition, the interfacial tension γ of the powder coal mixture (the remainder of the coal blend excluding the briquettes) p Regarding the above, if the individual coal brands present in the powder coal mixture and their blending ratios are determined, it can be calculated similarly using the above formula (1).
[0031] The interfacial tension of the coal blend can also be calculated using the following formula (2): It is shown in Patent Document 1 that the calculation results of the above formula (1) and the following formula (2) agree with each other.
[0032]
[0033] Furthermore, the following formulas (3) and (4) are extensions of the above formulas (1) and (2) for calculating the interfacial tension of a coal blend so as to include a carbon material. The calculation concepts of the following formulas (3) and (4) are the same as those of the above formulas (1) and (2). The interfacial tension of a coal blend containing a carbon material can be calculated using the following formulas (3) and (4).
[0034]
[0035]
[0036] Next, a method for determining the blending composition of the briquettes and the powder coal mixture will be described. In the coke manufacturing method according to this embodiment, the interfacial tension γ p is the interfacial tension of the entire coal blend γ inter and the interfacial tension of the powder coal mixture γ p The blending composition of the briquettes and the powder coal mixture is determined so that the value of the blended coal powder is less than 0.03. Here, the blending composition refers to the brand and blending ratio of the blended coals and the type and blending ratio of the blended carbon materials.
[0037] It should be noted that Patent Document 1 discloses that although the surface tension of heat-treated coal changes when the heat treatment temperature of the coal is changed, the tendency of change is the same regardless of the brand of coal, and the value of the interfacial tension between coals hardly changes. p The preferred range can be determined regardless of the heat treatment temperature of the coal.
[0038] The blending ratio of a certain coal brand in a coal blend is the sum of the product of the blending ratio of the briquettes of the coal blend and the blending ratio of a certain coal brand in the briquettes, and the product of the blending ratio of the powder coal mixture in the coal blend and the blending ratio of a certain coal brand in the powder coal mixture. Therefore, for example, if the blending composition of the coal blend is determined, and the blending ratio of the briquettes of the coal blend and the blending ratio of the coal brands in the briquettes are determined, the blending ratio of the powder coal mixture can also be determined.
[0039] The inventors have found that the effect of the interfacial tension of the briquettes on coke strength is less than that of the interfacial tension of the powder coal mixture, and that when a carbonaceous material with abnormal surface tension is blended into the briquettes, the effect of the interfacial tension of the powder coal mixture becomes dominant. Therefore, it can be seen that a decrease in coke strength of the produced coke can be suppressed more effectively by using a coal blend in which the blending composition of the briquettes and the powder coal mixture is changed so that the interfacial tension of the powder coal mixture is smaller than that of the coal blend, than by using a coal blend in which the blending composition of the briquettes and the powder coal mixture is the same.
[0040] That is, rather than making the blending composition of the briquettes and the powdered coal mixture the same, it is preferable to change the blending composition of both and determine the blending composition so as to reduce the interfacial tension of the powdered coal mixture. This technical idea can be expressed mathematically as γ inter >γ p γ inter >γ p is likely to cause a decrease in coke strength. inter This indicates that the present invention is suitable for application to a coal blend with a high
[0041] According to the suggestion of Patent Document 1, the interfacial tension γ of the coal blend calculated using the formula (1) or (2) inter If the interfacial tension γ of the powder coal mixture, which affects the coke strength, is 0.03 or more, there is a concern that the coke strength may decrease.p It can be seen that if the blending composition is determined so that coal with abnormal surface tension in the coal blend is included in the briquette so that the value of α is less than 0.03, the decrease in coke strength can be suppressed and the coke strength can be improved compared to when the blending ratio of coal with abnormal surface tension is the same between the briquette and the powder coal mixture.
[0042] Here, the content of the briquettes in the entire coal blend is preferably within a range of 10% by mass or more and 50% by mass or less. If the briquettes account for less than 10% by mass of the entire coal blend, the effect of expanding the range of usable coal resources becomes small, which is not preferable. Furthermore, if the briquettes account for more than 50% by mass of the entire coal blend, the cost of briquetting the briquettes increases, which is not preferable. It is more preferable that the blending ratio of the briquettes is within a range of 15% by mass or more and 40% by mass or less of the entire coal blend.
[0043] Regarding the blending composition in the briquettes, if the fluidity of the raw materials for the briquettes is too low, it may be undesirable because it will result in many defects in the briquette-derived portions of the produced coke. The lower limit of the fluidity of the raw materials for the briquettes varies depending on the blending amount of the briquettes and the composition of the coal and carbon material used in the briquettes, but it is preferable that the average log MF, which is the common logarithm of the Gieseler fluidity MF of each coal and carbon material blended in the briquettes and is based on the content of each coal and carbon material in the briquettes, is 1.4 or more.
[0044] Finally, the carbonization of the coal blend will be described. The coal blend, which is produced by mixing the briquettes and the powder coal mixture, is charged into a coke oven and carbonized to produce coke. The coal blend can be carbonized at a temperature of approximately 900°C or higher using a general chamber-type coke oven.
[0045] Next, an example in which coke was produced by applying the coke production method according to this embodiment will be described. The properties of the coal and carbon material used in this example are shown in Table 1.
[0046]
[0047] In Table 1 above, A to H are coals, and I is biomass (palm kernel shells) carbonized at 500° C. Among these, coal A and carbon material I have a surface tension γ that is higher than the average for the entire coal blend, and in this blending configuration, coal A and carbon material I can be said to be carbon materials with abnormal surface tension.
[0048] Ro is the average maximum reflectance of coal vitrinite measured according to JIS M8816:1992. logMF is the common logarithm of the Gieseler maximum fluidity of coal measured according to JIS M8801:2008. The maximum fluidity MF of I was 0 ddpm. γ is the surface tension of heat-treated coal or carbon material heat-treated at 500°C, and is the average value of the surface tension distribution determined using the film flotation method described in Patent Document 1.
[0049] A coal blend containing a briquette and a powder coal mixture was prepared using several brands of coal listed in Table 1. Each coal was pulverized so that the ratio of particles of 3 mm or less was 100% by mass. The briquette was prepared by adding 4.0 parts and 6.5 parts of tar pitch and tar slag as binders to 100 parts of the briquette raw material, respectively, and mixing them. The briquette was then compressed in a double-roll molding machine to a volume of 34 cm. 3 The molded charcoal was produced.
[0050] The briquetted coal was blended with a non-briquette powder coal mixture to prepare a coal blend. 3 The mixture was packed into a carbonization can so that the blended coals would become 100% by mass, and carbonized in an electric furnace at a furnace wall temperature of 1050°C for 6 hours, followed by cooling under nitrogen to produce coke. The coal blending composition (mass % relative to the total coal blend), the interfacial tension of the briquettes or powder coal mixture, the average log MF, and the coke strength DI (150 / 15) of the produced coke are shown in Table 2 below. The interfacial tension was calculated using the surface tension of each coal, the blending ratio, and the above formula (2). The average log MF was calculated by averaging the log MF of each coal weighted by the blending ratio of each coal. The coke strength was the drum strength index DI (150 / 15) measured using the rotational strength test method specified in JIS K2151:2004.
[0051]
[0052] Comparative Example 1 is an example in which the briquettes and the powder coal mixture are blended in the same manner. Therefore, the interfacial tension in this example is the interfacial tension γ inter In Examples 1 to 3 and Comparative Examples 2 and 3, the blending ratio of the briquettes and the powder coal mixture was different, and the values of the interfacial tension and the average logMF were shown for each blending ratio. The blending ratio of the briquettes in the coal blend was the total blending ratio of each coal brand blended in the briquettes, and was adjusted to be within the range of 30% by mass to 35% by mass. In the case of the same blending ratio as in Comparative Example 1, the blending ratio of the briquettes was 30% by mass.
[0053] FIG. 1 shows the interfacial tension γ of the powder coal mixtures of Examples 1 to 3 and Comparative Examples 2 and 3. p The horizontal axis of Fig. 1 is the interfacial tension γ of the powder coal mixture. p The vertical axis represents the coke strength DI (150 / 15) (-) (mN / m), and the horizontal axis represents the coke strength DI (150 / 15) (-). Note that (-) means that the value is dimensionless. The dashed line in Figure 1 represents the coke strength of Comparative Example 1.
[0054] As shown in Figure 1 and Table 2, γ inter >γ p and γ p The coke strengths of the cokes produced in Examples 1 to 3, which satisfied the condition <0.03, were higher than that of the coke produced in Comparative Example 1, in which the blending ratio of the briquettes and the powder coal mixture was the same. If the blending ratios of the briquettes and the powder coal mixture were different, it was thought that not only the interfacial tension of the powder coal mixture but also adhesion at the boundary between the briquettes or the powder coal mixture could become a problem. However, from the results of Figure 1 and Table 2, it can be seen that the strength of the produced coke is not dependent on the interfacial tension of the powder coal mixture, but on the interfacial tension γ p Furthermore, it was confirmed that the influence of the interfacial tension γ p It was also confirmed that under the condition that the tensile strength was less than 0.03 mN / m, a coke strength equal to or greater than that obtained when the same blending was used (Comparative Example 1) was obtained.
[0055] In addition, from the above results, it can be seen that under the condition that the blending composition of the entire coal blend (the type and blending ratio of the coal brand or carbon material used) is the same, γ inter >γ p and γ pIt can be seen that high-strength coke can be obtained by determining the blending composition of the briquettes and the powder coal mixture so that the γ value of the powder coal mixture satisfies the above equation. For example, the blending composition of the briquettes and the powder coal mixture can be determined by determining the blending composition of the entire coal blend in advance, and then determining the blending composition of the briquettes and the powder coal mixture without changing the blending composition of the entire coal blend. In this case, by blending the briquettes so that more carbonaceous materials with abnormal surface tension are included in the briquettes, the γ value of the powder coal mixture can be reduced. p becomes smaller, which means that γ inter >γ p and γ p <0.03 can be achieved.
[0056] Examples 4 to 7 are examples of coke production using coal blends in which a carbon material is blended with multiple brands of coal. Conditions other than the blending composition were the same as those of Examples 1 to 3. Biomass carbonized at 500°C was used as the carbon material. The properties of this biomass are shown as Brand I in Table 1. The blending compositions, interfacial tensions of the briquettes or powder coal mixtures, average log MF, coke strength DI (150 / 15) and coke strength increase ΔDI (150 / 15) of the produced cokes for Examples 4 to 7 are shown in Tables 3 and 4 below.
[0057]
[0058]
[0059] Inventive Examples 4 and 5 and Comparative Examples 4 to 6 are examples of producing coke using a coal blend containing 3 mass % of carbon material I. Inventive Examples 6 and 7 and Comparative Example 7 are examples of producing coke using a coal blend containing 5 mass % of carbon material I. Comparative Examples 4 and 7 are examples in which the briquettes and the powder coal mixture were blended in the same proportions. The interfacial tensions of Comparative Examples 4 and 7 were the interfacial tensions of the coal blends. γinterSince the coke strength of the cokes produced in Comparative Examples 4 and 7 was different, ΔDI is shown for each of the invention examples and comparative examples. ΔDI is the increase in coke strength, and in Table 3, it is the value obtained by subtracting the coke strength of Comparative Example 4 from the coke strengths of Invention Examples 4 and 5 and Comparative Examples 5 and 6, while in Table 4, it is the value obtained by subtracting the coke strength of Comparative Example 7 from the coke strengths of Invention Examples 6 and 7. Note that the average logMF in Tables 3 and 4 was calculated assuming that the logMF of carbon material I was 0.
[0060] FIG. 2 shows the interfacial tension γ of the powder coal mixtures of Examples 4 to 7 and Comparative Examples 5 and 6. p 2 is a graph showing the relationship between the interfacial tension γ of the powder coal mixture and the increase in coke strength. p 2, the vertical axis represents the coke strength increase ΔDI(150 / 15)(−), and the black circles represent the results in Table 3, and the white circles represent the results in Table 4.
[0061] As shown in FIG. p It was confirmed that the coke strength tends to decrease as γ increases. p From these results, it was found that when the γ value was 0.03 or more, the coke strength decreased significantly. Even if the blend contains coals with abnormal surface tension (coal A and carbon material I), which are difficult to use as normal coke raw materials, and the interfacial tension of the coal blend increases, it is possible to form a part of the coal blend into a briquette and use the γ inter >γ p and γ p It was confirmed that by determining the blending composition so as to satisfy the condition of <0.03, it is possible to suppress a decrease in the coke strength of the produced coke and to realize the production of high-strength coke.
[0062] From these results, it can be seen that even when coke is produced using a coal blend containing coal with abnormal surface tension, γ inter >γ p and γ pIt was confirmed that by determining the blending composition so that the ratio satisfies <0.03, it is possible to suppress the decrease in coke strength of the produced coke and realize the production of high-strength coke. This means that a wide range of coals or carbonaceous materials, including carbonaceous materials with abnormal surface tension that could not be used in the past, can be used as coke raw materials, which will contribute to the stable procurement of raw materials and the expansion of resources.
Claims
1. A method for producing coke by carbonizing a coal blend obtained by blending a briquettes containing multiple brands of coal and a powdered coal mixture containing multiple brands of powdered coal, the method comprising the steps of: calculating the surface tension of heat-treated coal obtained by heat-treating each brand of coal contained in the coal blend; the blending ratio of each brand of coal; and the interfacial tension γ of the coal blend calculated using the following formula (1) or the following formula (2): inter and the interfacial tension of the powder coal mixture γ p But, γ inter >γ p And γ p and determining the brands and blending ratios of coal to be blended in the briquettes and the powder coal mixture so as to satisfy the following:
2. Blending a carbon material into at least one of the briquettes and the powdered coal mixture, and calculating the surface tension of the heat-treated coal and the carbon material obtained by heat-treating each brand of coal contained in the blended coal, the blending ratio of each brand of coal and the carbon material, and the interfacial tension γ of the blended coal calculated using the following formula (3) or (4) instead of the formulas (1) and (2). iter and the interfacial tension of the powder coal mixture γ p But, γ inter >γ p And γ p The method for producing coke according to claim 1, wherein the brand and blending ratio of the coal to be blended in the briquettes and the powdered coal mixture, and the type and blending ratio of the carbon material to be blended in the briquettes and the powdered coal mixture are determined so as to satisfy the following:
Citation Information
Patent Citations
Estimation of fluidity or the like of noncaking or slightly caking coal
JP1996176553A
Method for estimating coke strength for coal blend and method for producing coke
JP2005281355A