Steel sheet, member, and methods for producing same
The steel plate composition and processing method achieve high tensile strength, dimensional accuracy, and wide shear angle range, addressing the limitations of current steel plates for automobile parts and contributing to improved crashworthiness and reduced emissions.
Patent Information
- Application Number
- PCT/JP2023/041852
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-11-21
- Publication Date
- 2024-10-03
AI Technical Summary
Current steel plates used in automobile parts lack the combination of high tensile strength (TS) of 1180 MPa or more, excellent dimensional accuracy, and a wide range of shear angles, which are essential for improved crashworthiness and reduced emissions.
A steel plate composition with an area fraction of tempered martensite of 83% or more, total area fraction of ferrite and bainitic ferrite between 5% and 15%, and prior austenite grain boundary occupancy of 20% or more, along with specific heating and cooling processes, ensures the desired properties.
The steel plate achieves a TS of 1180 MPa or more, excellent dimensional accuracy, and a wide range of shear angles, enhancing crashworthiness and fuel efficiency while reducing CO2 emissions.
Smart Images

Figure JP2023041852_03102024_PF_FP_ABST
Abstract
Description
Steel plates and components, and their manufacturing methods
[0001] The present invention relates to a steel plate, a member made from the steel plate, and a method for manufacturing the same.
[0002] CO emissions from lighter automobile bodies 2 In order to achieve both reduced emissions and improved crashworthiness, efforts are being made to increase the strength of steel sheets used in automobile parts. Furthermore, new regulations are being introduced one after another. Therefore, the use of steel sheets with a tensile strength (TS) of 1180 MPa or more is increasing in the main structural parts of automobiles (hereinafter referred to as automotive frame parts).
[0003] Steel sheets used as raw materials for automobile parts are also required to have excellent dimensional accuracy when formed into parts (hereinafter simply referred to as dimensional accuracy). For example, in automobile frame parts such as bumpers, it is possible to suppress springback and improve dimensional accuracy by controlling the yield ratio (hereinafter also referred to as YR) of the steel sheet within a certain range.
[0004] For example, Patent Document 1 discloses a steel sheet used as a material for automobile parts, which describes a steel sheet having a composition containing, in mass %, C: 0.09% or more and 0.37% or less, Si: more than 0.70% and 2.00% or less, Mn: 2.60% or more and 3.60% or less, P: 0.001% or more and 0.100% or less, S: 0.0200% or less, Al: 0.010% or more and 1.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities, wherein the area fraction of martensite having a carbon concentration of more than 0.7 × [%C] and less than 1.5 × [%C] is 55% or more, and the area fraction of tempered martensite having a carbon concentration of 0.7 × [%C] or less is 5% or more and 40% or less, "A high-strength steel plate having a steel structure in which the ratio of the carbon concentration in the retained austenite to the volume fraction of the retained austenite is 0.05 or more and 0.40 or less, the martensite and the tempered martensite each have an average crystal grain size of 5.3 μm or less, the steel structure further has a softened surface layer thickness of 10 μm or more and 100 μm or less, and the tensile strength is 1180 MPa or more. Here, [% C] indicates the content (mass %) of the component element C in the steel."
[0005] Patent Document 2 states that "a steel sheet containing, by mass%, C: 0.15% or more and 0.40% or less, Si: 1.5% or less, Mn: 0.9 to 1.7%, P: 0.03% or less, S: less than 0.0020%, sol. Al: 0.2% or less, N: less than 0.0055%, and O: 0.0025% or less, and satisfying the relationship of the following formula (1), with the balance being Fe and unavoidable impurities; the area ratio of tempered martensite and bainite to the entire structure is 95% or more and 100% or less in total; the steel sheet is composed of one or more inclusion particles having a major axis of 0.3 μm or more that are elongated and / or distributed in a point-like pattern in the rolling direction, and when the inclusion particles are composed of two or more, the distance between the inclusion particles is 30 μm or less; the number of inclusion groups having a total length in the rolling direction of more than 120 μm is 0.8 or less per mm2; The aspect ratio is 2.5 or less, and the major axis is 0.20 μm or more and 2 μm or less, and the number of Fe-based carbides is 3500 / mm 2carbides having a diameter of 10 to 50 nm distributed inside the tempered martensite and / or the bainite are 0.7 × 107 particles / mm 2 or more, and has a structure in which the average grain size of prior γ grains is 18 μm or less, and has a thickness of 0.5 to 2.6 mm, a tensile strength of 1320 MPa or more, and has excellent delayed fracture resistance. 5 [%S] + [%N] < 0.0115...(1) where [%S] and [%N] are the S and N contents (mass%) in the steel, respectively. Here, excellent delayed fracture resistance means that the delayed fracture time when subjected to cold press forming involving shearing or punching is as follows: Tensile strength: more than 200 hours for tensile strength of 1320 MPa or more and less than 1530 MPa, 24 hours or more for tensile strength of 1530 MPa or more and less than 1550 MPa, 12 hours or more for tensile strength of 1550 MPa or more and less than 1570 MPa, 9 hours or more for tensile strength of 1570 MPa or more and less than 1610 MPa, 1.0 hours or more for tensile strength of 1610 MPa or more and less than 1960 MPa, and 0.2 hours or more for tensile strength of 1960 MPa or more. The delayed fracture time is the time from the start of immersion to the onset of microcracks when immersed in hydrochloric acid (hydrogen chloride aqueous solution) of pH 1 at an aqueous solution temperature of 20°C.
[0006] Patent Document 3 describes a steel having a composition containing, by mass%, C: 0.12% or more and 0.40% or less, Si: 0.01% or more and 1.5% or less, Mn: more than 1.7% and 3.5% or less, P: 0.05% or less, S: 0.010% or less, sol. Al: 1.00% or less, N: 0.010% or less, B: 0.0002% or more and 0.0050% or less, and one or two of Nb and Ti in a total amount of 0.010% or more and 0.080% or less, with the balance being Fe and unavoidable impurities, and a steel structure having an area fraction of martensite of 70% or more, an area fraction of bainite of 30% or less, and a total area fraction of ferrite and retained austenite of 10% or less, The number density of carbides with a major axis of 0.5 μm or more at a position of 1 / 4 of the plate thickness of the steel plate is 60,000 pieces / mm2 The number density of inclusion particles having a circle equivalent diameter of 4.0 μm or more in the range of 1 / 4 to 3 / 4 of the plate thickness of the steel plate is 10 particles / mm 2 30 pieces / mm or more 2 The number density of inclusion particles having a circle equivalent diameter of 4.0 μm or more in the range from the surface of the steel plate to 1 / 4 of the plate thickness is 27 particles / mm 2 The disclosure states that "a steel plate having a tensile strength of 1,310 MPa or more and a modulus of elasticity of 1,310 MPa or more."
[0007] Patent No. 6747612 Patent No. 6112261 Patent No. 7001197
[0008] Automotive parts, particularly automotive frame parts, often have end faces (hereinafter also referred to as sheared end faces) formed by shearing. Therefore, steel sheets used as raw materials for automotive parts are also required to have excellent delayed fracture resistance after shearing. Delayed fracture is a phenomenon that leads to fracture in the following manner. Specifically, when a part is subjected to high stress due to forming or other processes and then placed in a hydrogen penetration environment, hydrogen penetrates into the part. The hydrogen that penetrates into the part reduces interatomic bonding strength and causes local deformation. This causes microcracks to form in the part, which then propagate and lead to fracture.
[0009] Delayed fracture resistance is affected by the shape of the sheared edge. The shape of the sheared edge is also affected by the shear angle used during shearing (hereinafter simply referred to as the shear angle). In other words, delayed fracture resistance is affected by the shear angle. For example, even for parts made from the same steel plate, delayed fracture resistance decreases if the shear angle is outside the appropriate range. The shear angle is the angle (opening angle) between the upper and lower blades used in shearing.
[0010] Steel sheets used as raw materials for automotive parts are sheared at various shear angles depending on the required dimensional accuracy, productivity, equipment limitations, etc. Therefore, there is a demand for a wide range of appropriate shear angles for delayed fracture (i.e., the range of shear angles at which excellent delayed fracture resistance can be obtained in the steel sheet after shearing, hereinafter also referred to as shear angle range), i.e., an excellent shear angle range.
[0011] However, no consideration is given to the shear angle range in any of the steel sheets disclosed in Patent Documents 1 to 3. Therefore, there is currently a demand for the development of a steel sheet having a TS of 1180 MPa or more and also excellent in dimensional accuracy and shear angle range.
[0012] The present invention has been developed in view of the above-mentioned current situation, and aims to provide a steel sheet having a TS of 1180 MPa or more and excellent dimensional accuracy and shear angle range, together with an advantageous manufacturing method thereof. Another aim of the present invention is to provide a member made from the above-mentioned steel sheet and a manufacturing method thereof.
[0013] Here, TS is measured by a tensile test in accordance with JIS Z 2241:2022. Excellent dimensional precision means that YR is 65% or more and 85% or less. Here, YR is calculated by the following formula: YR = 100 × YS / TS, where YS is the yield stress and, like TS, is measured by a tensile test in accordance with JIS Z 2241:2022. Excellent shear angle range means that the appropriate range of shear angle at which delayed fracture does not occur when the load stress is 1000 MPa is 0 to 0.5° or more. Details of the measurement methods are as described in the examples below.
[0014] To achieve the above-mentioned object, the inventors conducted extensive research and obtained the following findings. (A) To obtain a TS of 1180 MPa or more, it is important that the area fraction of tempered martensite is 83% or more and that the total area fraction of ferrite and bainitic ferrite is less than 15%. This makes it possible to obtain a TS of 1180 MPa or more while ensuring the required properties. (B) To obtain excellent dimensional accuracy, it is important that the total area fraction of ferrite and bainitic ferrite is 5% or more. This makes it possible to obtain excellent dimensional accuracy while ensuring the required properties. (C) To obtain excellent shear angle range, it is important that the area fraction of retained austenite is less than 3% and that the occupancy rate of prior austenite grain boundaries by ferrite and bainitic ferrite is 20% or more. This makes it possible to obtain an excellent shear angle range while ensuring the required properties. The present invention was completed based on the above findings and further research.
[0015] That is, the gist of the present invention is as follows: 1. A steel sheet having a chemical composition, in mass%, of C: 0.030% or more and 0.500% or less, Si: 0.010% or more and 2.500% or less, Mn: 0.10% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, N: 0.0100% or less, O: 0.0100% or less, and Al: 1.000% or less, with the balance being Fe and unavoidable impurities, and a microstructure in which an area fraction of tempered martensite is 83% or more, an area fraction of retained austenite is less than 3%, a total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%, and an occupancy rate of prior austenite grain boundaries by the ferrite and the bainitic ferrite is 20% or more.
[0016] 2. The composition further contains, in mass %, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less. 2. The steel sheet according to 1 above, containing at least one selected from the following:
[0017] 3. The steel sheet according to 1 or 2 above, which has a plating layer on the surface.
[0018] 4. A member made using the steel plate according to any one of 1 to 3 above.
[0019] 5. A method for manufacturing the steel plate according to any one of 1 to 3 above, comprising: a preparation step of preparing a base steel plate having the chemical composition according to 1 or 2 above; a heating step of heating the base steel plate under conditions of an average heating rate of 5.0°C / s or less in a temperature range of 700°C to 750°C, and a maximum attainable temperature T1 of 800°C or more and 900°C or less; a first cooling step of cooling the base steel plate under conditions of an average cooling rate of 0.10°C / s or more and 5.00°C / s or less in a temperature range from the maximum attainable temperature T1 to an intermediate holding temperature T2; an intermediate holding step of holding the base steel plate under conditions of an intermediate holding temperature T2 of 600°C or more and 750°C or less, an intermediate holding time t2 of 1.0 second or more and 2000.0 seconds or less, and a tension applied to the base steel plate of 5 MPa or more; and a second cooling step of cooling the base steel sheet to a second cooling end temperature under the condition of an average cooling rate of 300°C / s or more in a temperature range of 100°C to 300°C; and a tempering step of tempering the base steel sheet under the conditions of a tempering temperature T3 of 100°C to 400°C and a tempering time t3 of 10 seconds to 10,000 seconds.
[0020] 6. The method for producing a steel sheet according to 5 above, further comprising a plating step of plating the base steel sheet between the intermediate holding step and the second cooling step, or after the tempering step.
[0021] 7. A method for manufacturing a component, comprising a step of subjecting the steel plate according to any one of 1 to 3 above to at least one of forming and joining to form a component.
[0022] According to the present invention, a steel sheet having a TS of 1180 MPa or more and excellent dimensional accuracy and shear angle flexibility can be obtained. Furthermore, the steel sheet of the present invention can be applied to a wider range of automotive parts, which can further improve fuel efficiency by reducing the weight of the automobile body, and can also reduce CO 2 This can make a significant contribution to reducing emissions, and therefore has great industrial value.
[0023] FIG. 2 is a schematic diagram for explaining the definition of the prior γ grain boundary occupancy rate.
[0024] The present invention will be described based on the following embodiments. [1] Steel Sheet First, the chemical composition of a steel sheet according to one embodiment of the present invention will be described. Note that although the unit of chemical composition is always "mass %", hereinafter, unless otherwise specified, it will be simply expressed as "%".
[0025] [C: 0.030% or more and 0.500% or less] C is one of the important basic components of steel. In particular, in a steel sheet according to one embodiment of the present invention, C is an important element that affects the area fraction of tempered martensite. If the C content is less than 0.030%, the area fraction of tempered martensite decreases, making it difficult to achieve a TS of 1180 MPa or more. On the other hand, if the C content exceeds 0.500%, the tempered martensite becomes embrittled, making it difficult to achieve an excellent shear angle range. Therefore, the C content is set to 0.030% or more and 0.500% or less. The C content is preferably set to 0.050% or more, more preferably 0.100% or more. The C content is preferably set to 0.400% or less, more preferably 0.350% or less.
[0026] [Si: 0.010% or More and 2.500% or Less] Si is one of the important basic components of steel. In particular, in a steel sheet according to one embodiment of the present invention, Si suppresses carbide formation during annealing and promotes the formation of retained austenite. That is, Si is an important element that affects the area fraction of retained austenite. If the Si content is less than 0.010%, it becomes difficult to achieve a TS of 1180 MPa or more. On the other hand, if the Si content exceeds 2.500%, the amount of retained austenite increases excessively, making it difficult to achieve excellent shear angle range. Therefore, the Si content is set to 0.010% or more and 2.500% or less. The Si content is preferably set to 0.050% or more, more preferably 0.100% or more. The Si content is preferably set to 2.000% or less, more preferably 1.200% or less.
[0027] [Mn: 0.10% or More and 5.00% or Less] Mn is one of the important basic components of steel. In particular, in a steel sheet according to one embodiment of the present invention, Mn is an important element that affects the area fraction of tempered martensite and the shear angle range. If the Mn content is less than 0.10%, the area fraction of tempered martensite decreases, making it difficult to achieve a TS of 1180 MPa or more. On the other hand, if the Mn content exceeds 5.00%, the tempered martensite becomes embrittled, making it difficult to achieve an excellent shear angle range. Therefore, the Mn content is set to 0.10% or more and 5.00% or less. The Mn content is preferably set to 0.50% or more, more preferably 0.80% or more. The Mn content is preferably set to 4.50% or less, more preferably 4.00% or less.
[0028] [P: 0.100% or less] P segregates at prior austenite grain boundaries, embrittling the grain boundaries and becoming the starting point for delayed fracture. Therefore, if the P content is excessive, it becomes difficult to achieve excellent shear angle range. Therefore, the P content is set to 0.100% or less. The P content is preferably set to 0.070% or less. There is no particular lower limit for the P content. However, P is a solid solution strengthening element and can increase the strength of the steel sheet. Therefore, the P content is preferably set to 0.001% or more.
[0029] [S: 0.0200% or less] S exists as sulfides and becomes the starting point of delayed fracture. Therefore, if the S content is excessive, it becomes difficult to achieve excellent shear angle range. Therefore, the S content is set to 0.0200% or less. The S content is preferably set to 0.0050% or less. There is no particular lower limit for the S content. However, due to constraints in production technology, the S content is preferably set to 0.0001% or more.
[0030] [N: 0.0100% or less] N exists as nitrides and becomes the starting point of delayed fracture. Therefore, if the N content is excessive, it becomes difficult to achieve an excellent shear angle range. Therefore, the N content is set to 0.0100% or less. The N content is preferably set to 0.0050% or less. There is no particular lower limit for the N content. However, due to constraints in production technology, the N content is preferably set to 0.0001% or more.
[0031] [O: 0.0100% or less] O exists as an oxide and becomes the starting point of delayed fracture. Therefore, if the O content is excessive, it becomes difficult to achieve excellent shear angle range. Therefore, the O content is set to 0.0100% or less. The O content is preferably set to 0.0050% or less. There is no particular lower limit for the O content. However, due to constraints in production technology, the O content is preferably set to 0.0001% or more.
[0032] [Al: 1.000% or less] Al exists as an oxide and becomes the starting point of delayed fracture. Therefore, if the Al content is excessive, it becomes difficult to achieve an excellent shear angle range. Therefore, the Al content is set to 1.000% or less. The Al content is preferably set to 0.500% or less. There is no particular lower limit for the Al content. However, due to constraints in production technology, the Al content is preferably set to 0.001% or more.
[0033] The basic component composition of a steel sheet according to one embodiment of the present invention has been described above, but the steel sheet according to one embodiment of the present invention has a component composition containing the above basic components, with the balance other than the above basic components including Fe (iron) and unavoidable impurities. Here, the steel sheet according to one embodiment of the present invention preferably has a component composition containing the above basic components, with the balance consisting of Fe and unavoidable impurities. In addition to the above basic components, the steel sheet according to one embodiment of the present invention may contain, as an optional additional element, at least one element selected from the following, either alone or in combination: Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and Bi: 0.200% or less The effects of the present invention can be obtained as long as the optional elements are contained in an amount equal to or less than the upper limit, so no lower limit is set. Furthermore, when the optional elements are contained in an amount less than the preferred lower limit described below, the elements are considered to be contained as inevitable impurities.
[0034] [Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less] When the Ti, Nb, and V contents are each 0.200% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Ti, Nb, and V are contained, their contents are preferably 0.200% or less. The contents of Ti, Nb, and V are more preferably 0.100% or less. There are no particular lower limits for the contents of Ti, Nb, and V. However, Ti, Nb, and V form fine carbides, nitrides, or carbonitrides during hot rolling or annealing, thereby increasing the strength of the steel sheet. Therefore, the contents of Ti, Nb, and V are preferably 0.001% or more.
[0035] [Ta: 0.10% or less, W: 0.10% or less] When the Ta and W contents are each 0.10% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Ta and W are contained, their contents are preferably 0.10% or less. The Ta and W contents are more preferably 0.08% or less. There are no particular lower limits for the Ta and W contents. However, Ta and W increase the strength of the steel sheet by forming fine carbides, nitrides, or carbonitrides during hot rolling or annealing. Therefore, the Ta and W contents are preferably 0.01% or more.
[0036] [B: 0.0100% or less] If the B content is 0.0100% or less, cracks will not form inside the steel sheet during casting or hot rolling, and will not become the starting point for delayed fracture. Therefore, the shear angle range will not be reduced. Therefore, when B is contained, its content is preferably 0.0100% or less. The B content is more preferably 0.0080% or less. There is no particular lower limit for the B content. However, B is an element that segregates to austenite grain boundaries during annealing and improves hardenability. Therefore, the B content is preferably 0.0003% or more.
[0037] [Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less] When the Cr, Mo, and Ni contents are each 1.00% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Cr, Mo, and Ni are contained, their contents are preferably 1.00% or less. The Cr, Mo, and Ni contents are each more preferably 0.80% or less. There are no particular lower limits for the Cr, Mo, and Ni contents. However, Cr, Mo, and Ni are elements that improve hardenability. Therefore, the Cr, Mo, and Ni contents are preferably 0.01% or more.
[0038] [Co: 0.010% or less] If the Co content is 0.010% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Co is contained, the content is preferably 0.010% or less. The Co content is more preferably 0.008% or less. There is no particular lower limit for the Co content. However, Co is an element that improves hardenability. Therefore, the Co content is preferably 0.001% or more.
[0039] [Cu: 1.00% or less] If Cu is 1.00% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Cu is contained, its content is preferably 1.00% or less. The Cu content is more preferably 0.80% or less. There is no particular lower limit for the Cu content. However, Cu is an element that improves hardenability. Therefore, the Cu content is preferably 0.01% or more.
[0040] [Sn: 0.200% or less] If the Sn content is 0.200% or less, cracks will not form inside the steel sheet during casting or hot rolling, and they will not become the starting point for delayed fracture. Therefore, the shear angle range will not be reduced. Therefore, when Sn is contained, its content is preferably 0.200% or less. The Sn content is more preferably 0.100% or less. There is no particular lower limit for the Sn content. However, Sn is an element that improves hardenability and generally also improves corrosion resistance. Therefore, the Sn content is preferably 0.001% or more.
[0041] [Sb: 0.200% or less] If the Sb content is 0.200% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Sb is contained, its content is preferably 0.200% or less. The Sb content is more preferably 0.100% or less. There is no particular lower limit for the Sb content. However, Sb is an element that controls the softened surface thickness and enables strength adjustment. Therefore, the Sb content is preferably 0.001% or more.
[0042] [Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less] When the Ca, Mg, and REM contents are each 0.0100% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the initiation points of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Ca, Mg, and REM are contained, their contents are preferably 0.0100% or less. The contents of Ca, Mg, and REM are more preferably 0.0050% or less. There are no particular lower limits for the contents of Ca, Mg, and REM. However, Ca, Mg, and REM are elements that spheroidize the shape of nitrides and sulfides and improve the ultimate deformability of the steel sheet. Therefore, the contents of Ca, Mg, and REM are preferably 0.0005% or more.
[0043] [Zr: 0.100% or less, Te: 0.100% or less] When the Zr and Te contents are each 0.100% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Zr and Te are contained, their contents are preferably 0.100% or less. The Zr and Te contents are more preferably 0.080% or less. There are no particular lower limits for the Zr and Te contents. However, Zr and Te are elements that spheroidize the shape of nitrides and sulfides and improve the ultimate deformability of the steel sheet. Therefore, the Zr and Te contents are preferably 0.001% or more.
[0044] [Hf: 0.10% or less] If the Hf content is 0.10% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Hf is contained, its content is set to 0.10% or less. The Hf content is more preferably set to 0.08% or less. There is no particular lower limit for the Hf content. However, Hf is an element that spheroidizes the shape of nitrides and sulfides and improves the ultimate deformability of the steel sheet. Therefore, the Hf content is preferably set to 0.01% or more.
[0045] [Bi: 0.200% or less] If the Bi content is 0.200% or less, large amounts of coarse precipitates and inclusions are not formed, and they do not become the starting point of delayed fracture. Therefore, the shear angle range is not reduced. Therefore, when Bi is contained, its content is set to 0.200% or less. The Bi content is more preferably set to 0.100% or less. There is no particular lower limit for the Bi content. However, Bi is an element that reduces segregation. Therefore, the Bi content is preferably set to 0.001% or more.
[0046] The elements other than those mentioned above are Fe and unavoidable impurities. Examples of the unavoidable impurities include Zn, Pb, As, Ge, Sr, and Cs. These unavoidable impurities are allowed to be contained in a total amount of 0.100% or less.
[0047] Next, the structure of a steel sheet according to one embodiment of the present invention will be described. The structure of a steel sheet according to one embodiment of the present invention is a structure in which: an area fraction of tempered martensite: 83% or more; an area fraction of retained austenite: less than 3%; a total area fraction of ferrite and bainitic ferrite: 5% or more and less than 15%; and the occupancy rate of prior austenite grain boundaries by ferrite and bainitic ferrite is 20% or more. The reasons for each limitation will be described below. The area fraction of each phase is the area ratio that each phase occupies with respect to the entire structure.
[0048] [Area Fraction of Tempered Martensite: 83% or More] In a steel sheet according to one embodiment of the present invention, it is extremely important to have an area fraction of tempered martensite of 83% or more. That is, by using tempered martensite as the main phase, and particularly by setting its area fraction to 83% or more, it becomes possible to achieve a TS of 1180 MPa or more. Therefore, the area fraction of tempered martensite is set to 83% or more. The area fraction of tempered martensite is preferably 85% or more, more preferably 87% or more. There is no particular upper limit for the area fraction of tempered martensite. The area fraction of tempered martensite is, for example, preferably less than 95%, more preferably 94% or less, and even more preferably 93% or less.
[0049] [Area Fraction of Retained Austenite: Less than 3%] In a steel sheet according to one embodiment of the present invention, it is extremely important that the area fraction of retained austenite is less than 3%. That is, if the area fraction of retained austenite is 3% or more, it becomes difficult to achieve an excellent shear angle wide range. One of the causes of the deterioration of the shear angle wide range is that retained austenite undergoes stress-induced martensite transformation during shearing, becoming high-hardness martensite, which becomes the origin of fracture. Therefore, the area fraction of retained austenite is less than 3%. The area fraction of retained austenite is preferably 1% or less. Note that there is no particular lower limit for the area fraction of retained austenite. The area fraction of retained austenite may be 0%.
[0050] [Total Area Fraction of Ferrite and Bainitic Ferrite: 5% or More and Less than 15%] In a steel sheet according to one embodiment of the present invention, it is extremely important that the total area fraction of ferrite and bainitic ferrite is 5% or more and less than 15%. That is, if the total area fraction of ferrite and bainitic ferrite is 15% or more, it becomes difficult to achieve a TS of 1180 MPa or more. On the other hand, if the total area fraction of ferrite and bainitic ferrite is less than 5%, it becomes difficult to achieve excellent dimensional accuracy. Therefore, the total area fraction of ferrite and bainitic ferrite is set to 5% or more and less than 15%. The total area fraction of ferrite and bainitic ferrite is preferably 6% or more, more preferably 7% or more. Furthermore, the total area fraction of ferrite and bainitic ferrite is preferably 14% or less, more preferably 13% or less. Note that ferrite and bainitic ferrite may be contained alone, or both may be contained.
[0051] The area fraction of the remaining structure other than the above is preferably 5% or less. Examples of the remaining structure include pearlite, fresh martensite, and acicular ferrite. These remaining structures may be contained as long as they are 5% or less and do not affect the properties. The area fraction of the remaining structure may be 0%.
[0052] Here, the area fraction of tempered martensite and the total area fraction of ferrite and bainitic ferrite are measured, for example, as follows. A sample is cut out from a steel sheet so that the observation surface is a thickness cross section (L cross section) parallel to the rolling direction of the steel sheet. The observation surface of the sample is then polished. The observation surface of the sample is then corroded with 1 vol. % nital to reveal the structure. Ten fields of view are then observed at a 1 / 4 thickness position (a position corresponding to 1 / 4 of the thickness in the depth direction from the steel sheet surface) using an SEM at a magnification of 2000x. In the observed images, the tempered martensite has fine irregularities within the structure and contains carbides within the structure. Furthermore, the ferrite and bainitic ferrite have recesses and flat interiors, and do not contain carbides within the structure. The areas of the tempered martensite, ferrite, and bainitic ferrite are then determined for each field of view. Next, the areas occupied by tempered martensite, and ferrite and bainitic ferrite are each divided by the area of the entire observation field, and the result is multiplied by 100. The average values are then taken as the area fraction of tempered martensite and the total area fraction of ferrite and bainitic ferrite, respectively. Note that the structure of a steel sheet is usually approximately symmetrical from top to bottom in the thickness direction. Therefore, any one of the surfaces (front and back surfaces) of the steel sheet may be used as the starting point of the thickness position (0 thickness position), such as a 1 / 4 position in the thickness direction or a position 100 μm deep from the steel sheet surface.
[0053] The area fraction of retained austenite is measured, for example, as follows. That is, a steel plate is mechanically ground to a depth of 1 / 4-0.1 mm of the plate thickness so that the observation position is a position 1 / 4 of the plate thickness of the steel plate, and then chemically polished for an additional 0.1 mm. Using the polished surface as the observation surface, an X-ray diffractometer is used to determine the ratio of the integrated intensity of the diffraction peaks of the {200}, {220}, and {311} planes of fcc iron (austenite) to the integrated intensity of the diffraction peaks of the {200}, {211}, and {220} planes of bcc iron. Next, the volume fraction of retained austenite is calculated from the ratio of the integrated intensities of each plane. Then, assuming that the retained austenite is three-dimensionally homogeneous, the volume fraction of retained austenite is taken as the area fraction of retained austenite.
[0054] Furthermore, the area fraction of the remaining structure is calculated by subtracting the area fraction of tempered martensite, the total area fraction of ferrite and bainitic ferrite, and the area fraction of retained austenite, all calculated as described above, from 100%: [Area fraction of remaining structure (%)] = 100 - [Area fraction of tempered martensite (%)] - [Total area fraction of ferrite and bainitic ferrite (%)] - [Area fraction of retained austenite (%)]
[0055] [Occupancy Ratio of Prior Austenite Grain Boundaries by Ferrite and Bainitic Ferrite (hereinafter also referred to as Prior γ Grain Boundary Occupancy Ratio): 20% or More] In a steel sheet according to one embodiment of the present invention, it is extremely important to have a prior γ grain boundary occupancy ratio of 20% or more in order to achieve excellent shear angle range. Prior austenite grain (hereinafter also referred to as prior γ grain) boundaries are the initiation sites of delayed fracture. Here, it is important that the prior γ grain boundaries are occupied by soft ferrite and bainitic ferrite, and in particular, that the prior γ grain boundary occupancy ratio be 20% or more. This minimizes the influence of the shear angle during shearing, making it possible to suppress the occurrence of delayed fracture and achieve excellent shear angle range. Therefore, the prior γ grain boundary occupancy ratio is set to 20% or more. The prior γ grain boundary occupancy ratio is preferably set to 22% or more, more preferably 24% or more. Note that there is no particular upper limit for the prior γ grain boundary occupancy ratio. The prior γ grain boundary occupancy ratio may be 100%.
[0056] Here, the prior γ grain boundary occupancy ratio is determined, for example, as follows (see FIG. 1 ). In one prior γ grain (hereinafter also referred to as the prior γ grain) confirmed in the observation image in the measurement of the area fraction of tempered martensite and the total area fraction of ferrite and bainitic ferrite, the total length of the prior γ grain (the perimeter of the prior γ grain, which is the sum of the solid line (prior austenite grain boundary not occupied by ferrite and bainitic ferrite) and the dotted line in FIG. 1 , hereinafter referred to as L T ), and the length of the interface between the prior γ grain and the ferrite and bainitic ferrite in contact with the prior γ grain (the total prior γ grain boundary length of the dotted line in Figure 1, hereinafter referred to as L F Then, the prior γ grain boundary occupancy rate of the prior γ grain is calculated using the following formula: Prior γ grain boundary occupancy rate (%) = (L F / L T ) × 100 This measurement is performed on 30 prior γ grains in order from the closest to the prior γ grain, and the average value of the prior γ grain boundary occupancy ratio measured for each prior γ grain is taken as the prior γ grain boundary occupancy ratio of the steel sheet to be measured.
[0057] Also, L T and L F is measured, for example, as follows. A sample is cut out from a steel plate so that the plate thickness cross section (L cross section) parallel to the rolling direction of the steel plate serves as the observation surface. The observation surface of the sample is then polished. The observation surface of the sample is then corroded with 1 vol. % nital to reveal the structure. Next, the structure is observed at a 1 / 4 position of the plate thickness of the steel plate (a position corresponding to 1 / 4 of the plate thickness in the depth direction from the surface of the steel plate) using an SEM at a magnification of 2000x. From the obtained structure image, the L cross section is extracted using the object function of Adobe Illustrator. T and L F Measure.
[0058] The mechanical properties of the steel plate according to one embodiment of the present invention are as described above.
[0059] Furthermore, the steel sheet according to one embodiment of the present invention may have a plating layer on its surface. The plating layer may be provided on only one surface of the steel sheet, or on both surfaces. The plating layer is not particularly limited. An example of the plating layer is a zinc plating layer containing Zn as a main component (Zn content of 50.0 mass% or more). Furthermore, examples of the zinc plating layer include a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, and an electrogalvanized layer. A steel sheet having a zinc plating layer can also be referred to as a galvanized steel sheet. Furthermore, the steel sheets having the above-mentioned hot-dip galvanized layer, galvannealed hot-dip galvanized layer, and electrogalvanized layer can also be referred to as a hot-dip galvanized steel sheet (GI), a galvannealed hot-dip galvanized steel sheet (GA), and an electrogalvanized steel sheet (EG), respectively.
[0060] Examples of plating layers other than zinc plating layers include aluminum plating layers and alloy plating layers, such as hot-dip zinc-aluminum-magnesium alloy plating layers and Zn—Ni electrolytic alloy plating layers.
[0061] In addition, the plating amount per side of the plating layer is not particularly limited, but is preferably 20 g / m 2 80g / m or more 2 It is preferable to do the following:
[0062] The thickness of the steel plate according to one embodiment of the present invention is not particularly limited, but is preferably 0.50 mm or more and 2.50 mm or less.
[0063] [2] Member Next, a member according to one embodiment of the present invention will be described. The member according to one embodiment of the present invention is a member made using (using as a raw material) the above-mentioned steel plate. For example, the raw material steel plate is subjected to at least one of forming and joining processes to form a member. Here, the above-mentioned steel plate has a TS of 1180 MPa or more, and is also excellent in dimensional accuracy and shear angle range. Therefore, the member according to one embodiment of the present invention is particularly suitable for application as a raw material for automobile parts, for example. This makes it possible to improve fuel efficiency by reducing the weight of the automobile body, and CO 2 This will make a significant contribution to reducing emissions.
[0064] [3] Method for Manufacturing Steel Sheet Next, a method for manufacturing a steel sheet according to one embodiment of the present invention will be described.
[0065] A method for manufacturing a steel plate according to one embodiment of the present invention includes: a preparation step of preparing a base steel plate having the above-described chemical composition; a heating step of heating the base steel plate under conditions of an average heating rate of 5.0°C / s or less in a temperature range of 700°C to 750°C, and a maximum attainable temperature T1 of 800°C or more and 900°C or less; a first cooling step of cooling the base steel plate under conditions of an average cooling rate of 0.10°C / s or more and 5.00°C / s or less in a temperature range from the maximum attainable temperature T1 to an intermediate holding temperature T2; and an intermediate holding step of holding the base steel plate under conditions of an intermediate holding temperature T2 of 600°C to 750°C, an intermediate holding time t2 of 1.0 second to 2000.0 seconds, and a tension applied to the base steel plate of 5 MPa or more. The method includes a second cooling step in which the steel sheet is cooled to a second cooling end temperature under the following conditions: an average cooling rate in the temperature range of 300°C to 100°C: 300°C / s or more; and a tempering step in which the steel sheet is tempered under the following conditions: a tempering temperature T3: 100°C to 400°C, and a tempering time t3: 10 seconds to 10,000 seconds. Note that, unless otherwise specified, the above temperatures refer to the surface temperatures of the steel sheet. Furthermore, unless otherwise specified, the average heating rate and average cooling rate also refer to the surface temperatures of the steel sheet.
[0066] Preparation step: First, a base steel sheet having the above-mentioned chemical composition is prepared. For example, the base steel sheet can be prepared by hot rolling a steel slab to obtain a hot-rolled steel sheet, optionally subjecting this hot-rolled steel sheet to pickling and heat treatment, and then cold rolling it to obtain a cold-rolled steel sheet. The conditions for these steps are not particularly limited, and may be in accordance with conventional methods.
[0067] For example, any known melting method such as a converter or an electric furnace is suitable for producing steel slabs (steel materials). In order to prevent macrosegregation, it is preferable to produce steel slabs by a continuous casting method.
[0068] Examples of hot rolling include a method of rolling a steel slab after heating, a method of directly rolling a steel slab after continuous casting without heating, and a method of rolling a steel slab after continuous casting after short-term heat treatment. The slab heating temperature, slab soaking time, and coiling temperature in hot rolling are also not particularly limited. The slab heating temperature is preferably 1100°C or higher. The slab heating temperature is preferably 1300°C or lower. The slab soaking time is preferably 30 minutes or longer. The slab soaking time is preferably 250 minutes or shorter. The finish rolling temperature is Ar 3 The temperature is preferably equal to or higher than the transformation point. The coiling temperature is preferably 350°C or higher. The coiling temperature is preferably 650°C or lower. 3 The transformation point is calculated using the following formula: Ar 3 Transformation point (°C) = 868 - 396 x [%C] + 24.6 x [%Si] - 68.1 x [%Mn] - 36.1 x [%Ni] - 20.7 x [%Cu] - 24.8 x [%Cr]. In the above formula, the [% element symbol] represents the content (mass%) of the element in the above composition.
[0069] Pickling can remove oxides from the surface of the hot-rolled steel sheet and is preferably performed to ensure good chemical conversion treatability and plating quality in the final steel sheet product. Pickling may be performed once or multiple times. The hot-rolled steel sheet after pickling may be subjected to a heat treatment.
[0070] The total reduction in cold rolling is preferably 30% or more. The total reduction in cold rolling is preferably 80% or less. The number of rolling passes and the reduction in each pass are not particularly limited, and a predetermined effect can be obtained.
[0071] Heating Step Next, the base steel plate prepared in the preparation step is heated to a maximum temperature T1 at an average heating rate of 5.0°C / s or less in a temperature range of 700°C to 750°C.
[0072] [Average heating rate in the temperature range of 700°C to 750°C: 5.0°C / s or less] After extensive research, the inventors have found that the average heating rate in the temperature range of 700°C to 750°C (hereinafter simply referred to as the average heating rate) affects the prior γ grain boundary occupancy rate. That is, by setting the average heating rate to 5.0°C / s or less, the dissolution of carbides is promoted. This refines the prior γ grains, contributing to an increase in the prior γ grain boundary occupancy rate. As a result, the shear angle range is improved. Therefore, the average heating rate is set to 5.0°C / s or less. The average heating rate is preferably 3.0°C / s or less. There is no particular upper limit to the average heating rate. For example, the average heating rate is preferably 0.1°C / s or more.
[0073] [Maximum reachable temperature T1: 800°C or higher and 900°C or lower] If the maximum reachable temperature T1 is lower than 800°C, the total area fraction of ferrite and bainitic ferrite will be 15% or higher, making it difficult to achieve a TS of 1180 MPa or higher. On the other hand, if the maximum reachable temperature T1 exceeds 900°C, the total area fraction of ferrite and bainitic ferrite will be less than 5%, making it difficult to achieve excellent dimensional accuracy of the part. Therefore, the maximum reachable temperature T1 is set to 800°C or higher and 900°C or lower. The maximum reachable temperature T1 is preferably 810°C or higher. The maximum reachable temperature T1 is preferably 890°C or lower.
[0074] After the maximum temperature T1 is reached, the process may immediately proceed to the cooling step described later, or the maximum temperature T1 may be maintained for a certain period of time, for example, 1.0 to 5.0 seconds, before proceeding to the cooling step described later.
[0075] First Cooling Step Next, the base steel sheet is cooled under the condition of an average cooling rate of 0.10°C / s or more and 5.00°C / s or less in the temperature range from the maximum temperature T1 to the intermediate holding temperature T2.
[0076] [Average Cooling Rate in the Temperature Range from Maximum Reach Temperature T1 to Intermediate Holding Temperature T2 (hereinafter also referred to as First Average Cooling Rate): 0.10°C / s or More and 5.00°C / s or Less] As a result of extensive research, the inventors have found that the first average cooling rate affects the prior γ grain boundary occupancy rate. That is, by setting the first average cooling rate to 5.00°C / s or less, ferrite nucleation from the prior γ grain boundaries is promoted, contributing to an increase in the prior γ grain boundary occupancy rate. As a result, the shear angle range is improved. On the other hand, if the first average cooling rate is less than 0.10°C / s, the total area fraction of ferrite and bainitic ferrite becomes 15% or more, making it difficult to achieve a TS of 1180 MPa or more. Therefore, the first average cooling rate is set to 0.10°C / s or more and 5.00°C / s or less. The first average cooling rate is preferably 0.20°C / s or more. The first average cooling rate is preferably 3.00°C / s or less.
[0077] The first cooling end temperature may be set to 600° C. or higher and 750° C. or lower. For example, the first cooling end temperature may be set to the intermediate holding temperature T2.
[0078] Intermediate holding step: Next, the base steel sheet is held under the following conditions: intermediate holding temperature T2: 600°C or higher and 750°C or lower, intermediate holding time t2: 1.0 second or higher and 2000.0 seconds or lower, tension applied to base steel sheet: 5 MPa or higher.
[0079] [Intermediate Holding Temperature T2: 600°C or Higher and 750°C or Lower] If the intermediate holding temperature T2 is lower than 600°C, the transformation of ferrite and bainitic ferrite from locations other than the prior γ grain boundaries may be accelerated. This makes it difficult to achieve a prior γ grain boundary occupancy rate of 20% or higher, and it also makes it difficult to achieve an excellent shear angle range. On the other hand, if the intermediate holding temperature T2 exceeds 750°C, the total area fraction of ferrite and bainitic ferrite becomes less than 5%, making it difficult to achieve excellent dimensional accuracy of the part. Therefore, the intermediate holding temperature T2 is set to 600°C or higher and 750°C or lower. The intermediate holding temperature T2 is preferably 610°C or higher. The intermediate holding temperature T2 is preferably 740°C or lower. The intermediate holding temperature here refers to the holding temperature during the intermediate holding step. Note that the intermediate holding temperature may be constant during holding. The intermediate holding temperature does not have to be constant as long as it is in the temperature range of 600° C. to 750° C. and the temperature fluctuation is within ±10° C. of the set temperature.
[0080] [Intermediate Holding Time t2: 1.0 Second or More and 2000.0 Seconds or Less] If the intermediate holding time t2 is less than 1.0 second (including the case where no intermediate holding is performed), the prior γ grain boundary occupancy rate will be less than 20%, making it impossible to achieve an excellent shear angle range. On the other hand, if the intermediate holding time t2 exceeds 2000.0 seconds, the total area fraction of ferrite and bainitic ferrite will be 15% or more, making it difficult to achieve a TS of 1180 MPa or more. Therefore, the intermediate holding time t2 is set to 1.0 second or more and 2000.0 seconds or less. The intermediate holding time t2 is preferably 10.0 seconds or more. The intermediate holding time t2 is preferably 1500.0 seconds or less. Note that the intermediate holding time t2 is the holding time at the intermediate holding temperature T2.
[0081] [Tension Applied to Base Steel Sheet: 5 MPa or More] After extensive research, the inventors discovered that applying tension to the base steel sheet during intermediate holding affects the prior γ grain boundary occupancy rate. By applying a tension to the base steel sheet (hereinafter also simply referred to as the applied tension) of 5 MPa or more, the nucleation of ferrite from the prior γ grain boundaries is promoted, contributing to an increase in the prior γ grain boundary occupancy rate. This makes it possible to achieve a prior γ grain boundary occupancy rate of 20% or more, thereby achieving an excellent shear angle range. Therefore, the applied tension is set to 5 MPa or more. The applied tension is preferably 10 MPa or more. The upper limit of the applied tension is not particularly specified. The applied tension is preferably, for example, 100 MPa or less.
[0082] Furthermore, the base steel sheet may be subjected to a plating treatment between the intermediate holding step and the second cooling step described below. The plating treatment will be described later.
[0083] Second Cooling Step Next, the base steel sheet is cooled to a second cooling end temperature under the following conditions: average cooling rate in the temperature range of 300°C to 100°C: 300°C / s or more.
[0084] [Average cooling rate in the temperature range of 300°C to 100°C (hereinafter also referred to as second average cooling rate): 300°C / s or more] If the second average cooling rate is less than 300°C / s, the area fraction of retained austenite will be 3% or more, making it difficult to achieve excellent shear angle broadness. Therefore, the second average cooling rate is set to 300°C / s or more. The second average cooling rate is preferably 800°C / s or more. There is no particular upper limit for the second average cooling rate. For example, the second average cooling rate is preferably 2000°C / s or less.
[0085] The second cooling end temperature may be, for example, less than 100° C. The second cooling end temperature may be, for example, about room temperature.
[0086] Tempering Step Next, the base steel sheet is tempered under the conditions of a tempering temperature T3 of 100°C or more and 400°C or less, and a tempering time t3 of 10 seconds or more and 10,000 seconds or less.
[0087] [Tempering Temperature T3: 100°C or More and 400°C or Less] Tempered martensite is produced by tempering martensite through a tempering process. Here, if the tempering temperature T3 is less than 100°C, the martensite is not sufficiently tempered, resulting in a structure mainly composed of as-quenched martensite. Such a structure mainly composed of as-quenched martensite does not provide an excellent shear angle range. On the other hand, if the tempering temperature T3 exceeds 400°C, the martensite is tempered excessively, making it difficult to achieve a TS of 1180 MPa or more. Therefore, the tempering temperature T3 is set to 100°C or more and 400°C or less. The tempering temperature T3 is preferably set to 150°C or more. The tempering temperature T3 is preferably set to 350°C or less. The tempering temperature here refers to the holding temperature in the tempering process. The tempering temperature may be constant during holding. The tempering temperature does not have to be constant while being held as long as it is in the temperature range of 100°C or higher and 400°C or lower and the temperature fluctuation is within ±10°C of the set temperature.
[0088] [Tempering time t3: 10 seconds or more and 10,000 seconds or less] As described above, tempered martensite is produced by tempering martensite through a tempering process. Here, if the tempering time t3 is less than 10 seconds, the martensite is not sufficiently tempered, resulting in a structure mainly composed of as-quenched martensite. Such a structure mainly composed of as-quenched martensite does not provide excellent shear angle range. On the other hand, if the tempering time t3 exceeds 10,000 seconds, the martensite is tempered excessively, making it difficult to achieve a TS of 1180 MPa or more. Therefore, the tempering time t3 is set to 10 seconds or more and 10,000 seconds or less. The tempering time t3 is preferably set to 50 seconds or more. The tempering time t3 is preferably set to 5,000 seconds or less. Note that the tempering time t3 here refers to the holding time at the tempering temperature T3.
[0089] The cooling after tempering is not particularly limited. For example, the cooling may be performed by any method according to a conventional method. The cooling end temperature after tempering may be, for example, about room temperature.
[0090] After the tempering step, the base steel sheet may be worked under conditions that result in an equivalent plastic strain of 0.10% to 5.00%. After the working step, the base steel sheet may be reheated under conditions of 100°C to 400°C.
[0091] Furthermore, after the tempering step, the base steel sheet may be subjected to a plating treatment, as will be described later.
[0092] Plating Process The base steel sheet may also be optionally subjected to a plating process. The plating process is not particularly limited. Examples of plating processes include galvanizing processes such as hot-dip galvanizing, galvannealed hot-dip galvanizing, and electrogalvanizing. Examples of plating processes other than galvanizing include aluminum plating and alloy plating. Examples of alloy plating processes include hot-dip zinc-aluminum-magnesium alloy plating and Zn-Ni electroalloy plating. All of the processing conditions may be conventional. As described above, the plating process is preferably performed between the intermediate holding step and the second cooling step or after the tempering step. For example, the hot-dip galvanizing process and the galvannealed hot-dip galvanizing process are preferably performed between the intermediate holding step and the second cooling step. The electrogalvanizing process and the Zn-Ni electroalloy plating process are preferably performed after the tempering step.
[0093] In the case of hot-dip galvanizing and galvannealed hot-dip galvanizing, from the viewpoint of productivity, it is preferable to carry out a series of processes such as the heating step and the plating step in a continuous galvanizing line (CGL). After hot-dip galvanizing, wiping can be performed to adjust the coating weight of the coating.
[0094] Furthermore, after the plating treatment step, the base steel sheet may be processed under conditions that result in an equivalent plastic strain of 0.10% to 5.00%. Furthermore, after the processing, the base steel sheet (plated steel sheet) may be reheated under conditions of 100°C to 400°C.
[0095] Conditions other than those described above are not particularly limited and may be performed according to conventional methods. According to the method for producing a steel sheet according to one embodiment of the present invention described above, a steel sheet having a TS of 1180 MPa or more and excellent dimensional accuracy and shear angle range can be obtained. The obtained steel sheet can be suitably used, for example, as a material for automobile parts. When the steel sheet is to be traded, it is usually cooled to room temperature before being traded.
[0096] [4] Manufacturing Method of Member Next, a manufacturing method of a member according to one embodiment of the present invention will be described. The manufacturing method of a member according to one embodiment of the present invention includes a step of subjecting the above-mentioned steel plate to at least one of forming and joining to form a member. Here, the forming method is not particularly limited, and for example, a general processing method such as press forming can be used. Furthermore, the joining method is also not particularly limited, and for example, general welding such as spot welding, laser welding, and arc welding, rivet joining, caulking joining, etc. can be used. Note that the forming conditions and joining conditions are not particularly limited, and may be in accordance with conventional methods.
[0097] A steel having the chemical composition shown in Table 1 (the balance being Fe and unavoidable impurities) was melted in a converter and cast into a steel slab by continuous casting. The steel slab was then heated. The steel slab was then hot-rolled to form a hot-rolled steel sheet. The hot-rolled steel sheet was then pickled. The hot-rolled steel sheet was then cold-rolled to form a cold-rolled steel sheet. A base steel sheet was thus prepared. The prepared base steel sheet was then subjected to a heating step, a first cooling step, an intermediate holding step, a second cooling step, and a tempering step under the conditions shown in Table 2, to obtain a steel sheet (thickness: 0.6 to 2.2 mm) as a final product. Some of the steel sheets (those with the type column in Table 2 as GI, GA, and EG) were also plated. Of these, those with the type column in Table 2 as GI and GA were plated between the intermediate holding step and the second cooling step. In addition, for those in the type column of Table 2 that are marked EG, plating was carried out after the tempering process. Conditions not specified were those according to conventional methods.
[0098] Using the steel sheets thus obtained, the area fraction of tempered martensite, the area fraction of retained austenite, the total area fraction of ferrite and bainitic ferrite, and the prior γ grain boundary occupancy ratio were determined in the manner described above. The results are shown in Table 3.
[0099] The evaluations were carried out in the following manner, and the results are shown in Table 3.
[0100] (Evaluation of TS) JIS No. 5 test pieces (gauge length: 50 mm, parallel portion width: 25 mm) were taken from the obtained steel sheets so that the direction perpendicular to the rolling direction of the steel sheets was the longitudinal direction of the test pieces. Next, using the taken test pieces, a tensile test was performed in accordance with JIS Z 2241:2022 to measure TS and YS. The crosshead speed was 1.67 × 10 -1 The condition was mm / sec. TS was evaluated according to the following criteria: Good (pass, excellent): TS is 1180 MPa or more; Poor (fail): TS is less than 1180 MPa.
[0101] (Evaluation of Dimensional Accuracy) From TS and YS measured in the above evaluation of TS, YR was calculated by the following formula: YR = 100 x YS / TS Then, dimensional accuracy was evaluated according to the following criteria: Good (pass, excellent): YR is 65% or more and 85% or less Poor (fail): YR is less than 65% or YR is more than 85%
[0102] (Evaluation of Shear Angle Range) The obtained steel sheets were sheared into 16 mm x 75 mm specimens with the longitudinal direction perpendicular to the rolling direction. The clearance during shearing was 15% in all cases. The shear angle during shearing was varied in 0.25° increments within the range of 0° to 2.0°. Next, a four-point bending test was performed in accordance with ASTM (G39-99), and a stress of 1000 MPa was applied to the bend apex of the test specimen. Next, with the stress applied, the test specimen was immersed in hydrochloric acid at 25°C and pH: 3 for 100 hours. After immersion, the presence or absence of cracks was visually confirmed for each test specimen. The shear angle range was then evaluated according to the following criteria. Excellent (pass, particularly excellent): The appropriate range of shear angle to prevent delayed fracture is 0° to 1.0° or more. Good (pass, excellent): The appropriate range of shear angle to prevent delayed fracture is 0° to 0.5° or more and less than 1.0°. Poor (fail): The appropriate range of shear angle to prevent delayed fracture is the range of shear angles in which no cracks are observed in the test specimens in the above test. For example, if no cracks are observed in any of the test specimens prepared with a shear angle of 0° to 0.75° during shearing, but cracks are observed in test specimens prepared with a shear angle of 1.00° or more during shearing, the appropriate range of shear angle to prevent delayed fracture is "0° to 0.75°," and the specimen is evaluated as "good (pass, excellent)." Furthermore, if no cracks were observed in any of the test pieces prepared with a shear angle of 0° to 0.25° during shearing, but cracks were observed in the test pieces prepared with a shear angle of 0.50° or more during shearing, the appropriate range of the shear angle for delayed fracture would be "0° to 0.25°," and the test piece would be evaluated as "poor (failed)."
[0103]
[0104]
[0105]
[0106] As shown in Table 3, all of the inventive examples passed the test for TS, dimensional accuracy, and shear angle range. Furthermore, all of the components obtained by forming or joining the steel sheets of the inventive examples had the desired shape without cracking. Furthermore, the components did not experience delayed fracture even when the shear angle of the shearing process was changed. Dimensional accuracy was also good. On the other hand, the comparative examples failed at least one of TS, dimensional accuracy, and shear angle range.
Claims
1. A steel plate having a composition, by mass%, of C: 0.030% or more and 0.500% or less, Si: 0.010% or more and 2.500% or less, Mn: 0.10% or more and 5.00% or less, P: 0.100% or less, S: 0.0200% or less, N: 0.0100% or less, O: 0.0100% or less, and Al: 1.000% or less, with the balance being Fe and unavoidable impurities; and a structure having an area fraction of tempered martensite: 83% or more, an area fraction of retained austenite: less than 3%, a total area fraction of ferrite and bainitic ferrite: 5% or more and less than 15%, and an occupancy rate of prior austenite grain boundaries by the ferrite and the bainitic ferrite: 20% or more.
2. The composition further includes, in mass%, Ti: 0.200% or less, Nb: 0.200% or less, V: 0.200% or less, Ta: 0.10% or less, W: 0.10% or less, B: 0.0100% or less, Cr: 1.00% or less, Mo: 1.00% or less, Ni: 1.00% or less, Co: 0.010% or less, Cu: 1.00% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ca: 0.0100% or less, Mg: 0.0100% or less, REM: 0.0100% or less, Zr: 0.100% or less, Te: 0.100% or less, Hf: 0.10% or less, and The steel sheet according to claim 1, further comprising at least one selected from the following: Bi: 0.200% or less.
3. The steel sheet according to claim 1, having a plating layer on the surface.
4. The steel sheet according to claim 2, having a plating layer on the surface.
5. A member made using the steel plate according to any one of claims 1 to 4.
6. A method for manufacturing a steel plate according to any one of claims 1 to 4, comprising: a preparation step of preparing a base steel plate having the chemical composition according to claim 1 or 2; a heating step of heating the base steel plate under the following conditions: an average heating rate in the temperature range of 700°C to 750°C: 5.0°C / s or less; a maximum attainable temperature T1: 800°C or more and 900°C or less; a first cooling step of cooling the base steel plate under the following conditions: an average cooling rate in the temperature range of the maximum attainable temperature T1 to intermediate holding temperature T2: 0.10°C / s or more and 5.00°C / s or less; an intermediate holding step of holding the base steel plate under the following conditions: an intermediate holding temperature T2: 600°C or more and 750°C or less; an intermediate holding time t2: 1.0 second or more and 2000.0 seconds or less; and a tension applied to the base steel plate: 5 MPa or more; and a second cooling step of cooling the base steel plate to a second cooling end temperature under the condition of an average cooling rate in a temperature range of 300°C to 100°C: 300°C / s or more; and a tempering step of tempering the base steel plate under the conditions of a tempering temperature T3 of 100°C or more and 400°C or less and a tempering time t3 of 10 seconds or more and 10,000 seconds or less.
7. The method for producing steel sheet according to claim 6, further comprising a plating step of plating the base steel sheet between the intermediate holding step and the second cooling step, or after the tempering step.
8. A method for manufacturing a component, comprising the step of subjecting the steel plate according to any one of claims 1 to 4 to at least one of forming and joining to form a component.
Citation Information
Patent Citations
Ultra-high-strength steel plate having excellent delayed fracture resistance at cut end thereof
WO2016129550A1
High strength cold-rolled steel sheet with excellent moldability and manufacturing method therefor
WO2017212885A1
Steel sheet
WO2020262652A1
High-strength steel sheet and manufacturing method therefor
WO2022259837A1
High-strength steel sheet and manufacturing method therefor
WO2022259838A1
Cited By
Zinc-plated steel sheet and member, and method for producing the same
JP7708344B1
Galvanized steel sheet and member, and method for producing same
WO2025225065A1