Film laminate
The introduction of an amorphous oxide layer between the fluororesin and metal copper layers in film laminates addresses adhesion and heat resistance issues, ensuring low transmission loss and stability for high-frequency applications.
Patent Information
- Application Number
- PCT/JP2023/042287
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-11-27
- Publication Date
- 2024-10-03
AI Technical Summary
Film laminates with fluororesin and metal copper layers face issues with adhesion stability, especially at high frequencies and temperatures, due to interface roughness and oxidation, leading to increased transmission loss and reduced heat resistance.
A film laminate with an amorphous oxide layer formed between the fluororesin film and the metal copper layer, using oxides like Ge, Si, Al, Ti, Ta, Cr, and In/Zn, which provides strong chemical bonding, barrier properties, and resistance to adhesion deterioration at high temperatures.
The amorphous oxide layer ensures excellent adhesion and barrier properties, maintaining low transmission loss and heat resistance, making the film laminate suitable for high-frequency signal transmission wiring boards.
Smart Images

Figure JP2023042287_03102024_PF_FP_ABST
Abstract
Description
Film laminate
[0001] The present invention relates to a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film. This application claims priority to Japanese Patent Application No. 2023-052692, filed on March 29, 2023, the contents of which are incorporated herein by reference.
[0002] Generally, a film laminate in which a metal copper layer is laminated on the surface of an insulating resin layer as a conductive layer or a heat transfer layer is used as a wiring substrate for electronic and electrical devices. Here, wiring substrates for high-frequency signal transmission devices such as antennas and radars in the GHz band or higher are required to have low transmission loss when used in the high-frequency range. Therefore, as shown in Patent Documents 1 and 2, for example, film laminates using fluororesin films have been provided. Fluororesins have a low dielectric constant and low dielectric loss, making them particularly suitable as resin films for constituting wiring substrates for high-frequency signal transmission.
[0003] However, since the surface of a fluororesin film is very chemically stable, its adhesive strength with other materials tends to be low. Therefore, in Patent Document 1, protrusions are formed on the surface of the fluororesin, the metal foil is roughened, and the pressure lamination conditions are optimized to improve the adhesion between the copper film and the fluororesin through the anchor effect. In Patent Document 2, a metal thin film (nickel film or titanium film) is formed on the surface of the fluororesin by physical vapor deposition, and then copper plating is performed on this metal thin film to form a copper film, thereby improving the adhesion between the copper film and the fluororesin.
[0004] JP 2014-006668 A International Publication No. 2018 / 179904
[0005] However, in Patent Document 1, there is a problem that the interface between the fluororesin and the metal foil becomes rough, resulting in an increase in transmission loss.In addition, in Patent Document 2, when used in a high-temperature environment, the metal thin film formed on the surface of the fluororesin may oxidize, resulting in a decrease in adhesion, and the heat resistance is insufficient.
[0006] The present invention has been made in view of the above-mentioned circumstances, and aims to provide a film laminate that has particularly excellent adhesion between a fluororesin film and a metal copper layer, which has low transmission loss in the high frequency range, and that does not significantly decrease in adhesion even when used in a high-temperature environment, and is particularly suitable for wiring boards for high-frequency signal transmission.
[0007] In order to solve the above problems, a film laminate of Aspect 1 of the present invention is a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, and is characterized in that an amorphous oxide layer is formed between the fluororesin film and the metallic copper layer.
[0008] According to the film laminate of Aspect 1 of the present invention, an amorphous oxide layer is formed on the surface of the fluororesin film, and thus a chemical bond via O (oxygen) is formed at the outermost surface of the fluororesin, thereby achieving a strong bond between the fluororesin film and the amorphous oxide layer. Furthermore, since the amorphous oxide layer and the metallic copper layer have good bonding properties, the adhesion between the fluororesin film and the metallic copper layer is particularly excellent. Furthermore, since the amorphous oxide layer is chemically stable, reaction between the amorphous oxide layer and free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin is suppressed, thereby preventing a decrease in adhesion even when used in a high-temperature environment. Furthermore, since the amorphous oxide layer has no grain boundaries, it has excellent barrier properties, and therefore, even when used in a high-temperature environment, interdiffusion between the fluororesin and the metallic copper layer is suppressed, preventing a decrease in adhesion due to fluorination or oxidation of copper.
[0009] The film laminate of Aspect 2 of the present invention is characterized in that, in the film laminate of Aspect 1, the amorphous oxide layer has a thickness in the range of 10 nm to 100 nm. According to the film laminate of Aspect 2 of the present invention, the amorphous oxide layer has a thickness of 10 nm or more, thereby ensuring barrier properties and enabling accurate suppression of interdiffusion between the fluororesin and the metallic copper layer. Meanwhile, the amorphous oxide layer has a thickness of 100 nm or less, thereby enabling suppression of warpage of the film due to membrane stress.
[0010] The film laminate of Aspect 3 of the present invention is characterized in that, in the film laminate of Aspect 1 or Aspect 2, the oxide constituting the amorphous oxide layer contains one or more oxides selected from Ge, Si, Al, Ti, Ta, Zr, and Cr. According to the film laminate of Aspect 3 of the present invention, the oxide constituting the amorphous oxide layer contains one or more oxides selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, which makes the amorphous oxide layer more chemically stable and more effectively suppresses reactions between the amorphous oxide layer and free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin. Furthermore, sufficient barrier properties can be ensured, interdiffusion between the fluororesin and the metallic copper layer can be suppressed, and deterioration of adhesion due to fluorination or oxidation of copper can be effectively suppressed.
[0011] A film laminate of Aspect 4 of the present invention is characterized in that, in the film laminate of Aspect 1 or Aspect 2, the oxides constituting the amorphous oxide layer contain In and Zn. According to the film laminate of Aspect 4 of the present invention, the oxides constituting the amorphous oxide layer contain In and Zn, which makes the amorphous oxide layer even more chemically stable and makes it possible to further suppress reactions between the amorphous oxide layer and free F (fluorine) present on the surface of the fluororesin or adsorbed O (oxygen). Furthermore, sufficient barrier properties can be ensured, interdiffusion between the fluororesin and the metallic copper layer can be suppressed, and a decrease in adhesion due to fluorination or oxidation of copper can be effectively suppressed.
[0012] A film laminate of Aspect 5 of the present invention is the film laminate of any one of Aspects 1 to 4, characterized in that the thickness of the metallic copper layer is in the range of 2 μm to 20 μm. According to the film laminate of Aspect 5 of the present invention, since the thickness of the metallic copper layer is 2 μm or more, the influence of radiation loss can be suppressed and transmission loss can be reliably kept low. Meanwhile, since the thickness of the metallic copper layer is 20 μm or less, pattern formation by etching can be performed efficiently and accurately.
[0013] A film laminate of Aspect 6 of the present invention is characterized in that the electrical conductivity of the metallic copper layer is 80% IACS or more in the film laminate of any one of Aspects 1 to 5. According to the film laminate of Aspect 6 of the present invention, the electrical conductivity of the metallic copper layer is 80% IACS or more, and therefore the film laminate has particularly excellent transmission characteristics.
[0014] According to the present invention, it is possible to provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, which has excellent adhesion between a fluororesin film that has low transmission loss in the high-frequency range and a metal copper layer, and which does not significantly decrease in adhesion even when used in a high-temperature environment.
[0015] 1 is a schematic cross-sectional view of a film laminate according to an embodiment of the present invention; 2 is a flow chart showing an example of a method for producing a film laminate according to an embodiment of the present invention; 3 is a graph showing an example of an XRD measurement result in an example; 4 is a perspective view of a peel test in an example;
[0016] A film laminate according to one embodiment of the present invention will be described below: The film laminate according to one embodiment of the present invention is used as a wiring board for transmitting high-frequency signals.
[0017] As shown in FIG. 1 , the film laminate 10 of this embodiment includes a fluororesin film 11 and a metallic copper layer 12 laminated on the fluororesin film 11, and has a structure in which an amorphous oxide layer 13 is formed between the fluororesin film 11 and the metallic copper layer 12.
[0018] The fluororesin film 11 is made of a fluororesin such as PFA (perfluoroalkoxyalkane), PTFE (polytetrafluoroethylene), ETFE (ethylene-tetrafluoroethylene copolymer), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), or PCTFE (polychlorotrifluoroethylene). Fluororesins have low dielectric constants and low dielectric loss, making them particularly suitable as resin films for use in wiring substrates for high-frequency signal transmission. While there are no particular limitations on the thickness t1 of the fluororesin film 11, it is preferably within the range of 5 μm to 200 μm.
[0019] The metallic copper layer 12 is made of copper or a copper alloy having excellent electrical and thermal conductivity, and functions as a conductive layer or a heat transfer layer. Here, the metallic copper layer 12 preferably has a conductivity of 80% IACS or more, and more preferably 85% IACS or more.
[0020] Furthermore, the thickness t2 of the metallic copper layer 12 is preferably in the range of 2 μm or more and 20 μm or less. If the thickness t2 of the metallic copper layer 12 is 2 μm or more, the effect of radiation loss can be ignored without being equivalent to the skin effect. On the other hand, if the thickness t2 of the metallic copper layer 12 is 20 μm or less, etching can be performed efficiently and accurately when forming a circuit pattern on the metallic copper layer 12 by etching. The lower limit of the thickness t2 of the metallic copper layer 12 is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the thickness t2 of the metallic copper layer 12 is more preferably 18 μm or less, and even more preferably 15 μm or less.
[0021] An amorphous oxide layer 13 made of an amorphous oxide is formed between the fluororesin film 11 and the metallic copper layer 12. This amorphous oxide layer 13 firmly bonds the fluororesin film 11 and the amorphous oxide layer 13 through a chemical bond C-O-M (M is a component element contained in the amorphous oxide layer 13) mediated by O (oxygen). Furthermore, the amorphous oxide layer 13 is chemically stable, suppressing reaction between the amorphous oxide layer 13 and free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11. Furthermore, the amorphous oxide layer 13 has excellent barrier properties due to the absence of grain boundaries, thereby suppressing interdiffusion between the fluororesin film 11 and the metallic copper layer 12 and suppressing deterioration of adhesion due to fluorination or oxidation of copper.
[0022] Here, the oxide constituting the amorphous oxide layer 13 preferably contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr. When oxides of these metals are formed into a film by sputtering or the like, an amorphous oxide film is formed, which makes it possible to ensure sufficient barrier properties.
[0023] Alternatively, the oxide constituting the amorphous oxide layer 13 preferably contains In and Zn. When oxides of these metals are deposited by sputtering or the like, an amorphous oxide film is formed, making it possible to ensure sufficient barrier properties.
[0024] Furthermore, the thickness t3 of the amorphous oxide layer 13 is preferably in the range of 10 nm or more and 100 nm or less. If the thickness t3 of the amorphous oxide layer 13 is 10 nm or more, sufficient barrier properties can be ensured. On the other hand, if the thickness t3 of the amorphous oxide layer 13 is 100 nm or less, warping of the film due to membrane stress can be suppressed. The lower limit of the thickness t3 of the amorphous oxide layer 13 is more preferably 15 nm or more, and even more preferably 20 nm or more. The upper limit of the thickness t3 of the amorphous oxide layer 13 is more preferably 80 nm or less, and even more preferably 50 nm or less.
[0025] Next, a method for producing the film laminate 10 according to this embodiment will be described with reference to the flow chart of FIG.
[0026] (Fluororesin Film Preparing Step S01) First, prepare the fluororesin film 11. Note that, for the purpose of introducing functional groups into the surface of the fluororesin film 11, surface treatment such as plasma treatment may be performed.
[0027] (Amorphous oxide layer forming step S02) Next, the amorphous oxide layer 13 is formed to a predetermined thickness by sputtering on the surface of the fluororesin film 11. Note that an oxide target having a predetermined composition may be used as the sputtering target, or a metal target may be used to introduce oxygen for film formation.
[0028] (Seed layer formation step S03) Next, a copper layer is formed by sputtering on the amorphous oxide layer 13 as a seed layer for plating. The thickness of the seed layer (sputtered copper layer) is preferably in the range of 10 nm to 1000 nm. The seed layer is preferably formed continuously after the amorphous oxide layer 13 is formed without being exposed to the atmosphere.
[0029] (Copper plating layer forming step S04) Next, after forming a seed layer, a copper plating layer of a predetermined thickness is formed by electrolytic plating. The seed layer and the copper plating layer constitute the metal copper layer 12.
[0030] The film laminate 10 of this embodiment is manufactured through the above-mentioned steps. When the metallic copper layer 12 is formed on both sides of the fluororesin film 11, the amorphous oxide layer forming step S02 and the seed layer forming step S03 may be performed on one side of the fluororesin film 11, and then the amorphous oxide layer forming step S02 and the seed layer forming step S03 may be performed on the opposite side, followed by the copper plating layer forming step S04.
[0031] In the film laminate 10 of this embodiment configured as described above, the amorphous oxide layer 13 is formed on the surface of the fluororesin film 11, and thus a chemical bond via O (oxygen) is formed at the outermost surface of the fluororesin film 11, thereby firmly bonding the fluororesin film 11 and the amorphous oxide layer 13. Furthermore, the amorphous oxide layer 13 and the metallic copper layer 12 have good bonding properties, resulting in particularly excellent adhesion between the fluororesin film 11 and the metallic copper layer 12. Furthermore, the amorphous oxide layer 13 is chemically stable, suppressing reaction between the amorphous oxide layer 13 and free fluorine (F) or adsorbed oxygen (O) present on the surface of the fluororesin film 11, thereby preventing a decrease in adhesion even when used in a high-temperature environment. Furthermore, the amorphous oxide layer 13, which does not have grain boundaries, acts as a barrier layer, preventing interdiffusion between the fluororesin film 11 and the metallic copper layer 13 and preventing a decrease in adhesion due to fluorination or oxidation of copper, even when used in a high-temperature environment.
[0032] In the film laminate 10 of this embodiment, when the thickness t3 of the amorphous oxide layer 13 is in the range of 10 nm or more and 100 nm or less, the barrier properties can be ensured, the interdiffusion between the fluororesin and the metallic copper layer can be appropriately suppressed, and warping of the film due to membrane stress can be suppressed.
[0033] In the film laminate 10 of this embodiment, when the oxide constituting the amorphous oxide layer 13 contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, the amorphous oxide layer 13 is more chemically stable, and it becomes possible to further suppress the reaction between the free F (fluorine) present on the surface of the fluororesin and the adsorbed O (oxygen) and the amorphous oxide layer 13. In addition, an amorphous oxide film can be formed by sputtering, and the barrier properties of the amorphous oxide layer 13 can be sufficiently ensured.
[0034] When the film laminate 10 of this embodiment contains In and Zn, the amorphous oxide layer 13 is more chemically stable, and it becomes possible to further suppress the reaction between the free F (fluorine) present on the surface of the fluororesin and the adsorbed O (oxygen) and the amorphous oxide layer 13. In addition, an amorphous oxide film can be formed by sputtering, and the barrier properties of the amorphous oxide layer 13 can be sufficiently ensured.
[0035] In the film laminate 10 of this embodiment, when the thickness t2 of the metal copper layer 12 is in the range of 2 μm to 20 μm, the influence of radiation loss can be suppressed, the transmission loss can be reliably kept low, and pattern formation by etching can be performed efficiently and accurately. Furthermore, in the film laminate 10 of this embodiment, when the conductivity of the metal copper layer 13 is 80% IACS or more, the transmission characteristics are particularly excellent.
[0036] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical idea of the invention.
[0037] The results of confirmation experiments conducted to confirm the effectiveness of the present invention will be described below.
[0038] A PFA film (thickness: 50 μm) manufactured by AGC was prepared as the fluororesin film. An oxide layer shown in Table 1 was formed on the surface of this fluororesin film by sputtering. The oxide layer was formed under the following conditions. In Comparative Example 3, a metal Ti film was formed as the intermediate layer using a Ti target.
[0039] (Conditions for forming oxide layer) Target material: Si, Al, Ti, Ta, Zr, Cr, Ge, Zn, In, Sn, IZO (85 at% In-15 at% Zn composite oxide) (purity 99.9 mass% or more) Degree of vacuum at the start of film formation: 1.0 × 10 -4 Pa or less Sputtering gas: Mixture of high-purity argon and high-purity oxygen Sputtering gas pressure in chamber: 0.2 Pa DC power density: 7.5 W / cm 2 (Si, Al, Ti, Ta, Zr, Cr, Zn, In, Sn, IZO) AC power density: 10.0 W / cm 2 (Ge)
[0040] Next, a copper layer was formed to a thickness of 100 nm by sputtering as a seed layer for plating. The sputtering conditions were as follows. The seed layer was formed continuously after the intermediate layer was formed without being exposed to the atmosphere. (Seed layer formation conditions) Target material: Cu (purity 99.99 mass% or more) Degree of vacuum at the start of film formation: 1.0 × 10 -4 Sputtering gas: high-purity argon Sputtering gas pressure in chamber: 0.2 Pa DC power density: 7.5 W / cm 2
[0041] Next, a copper plating layer was formed on the seed layer by electroplating under the following conditions. The thickness of the metallic copper layer shown in Table 1 is the total thickness of the seed layer and the copper plating layer. (Electroplating Conditions) Pretreatment: Sulfuric acid washing Solution temperature: 25°C Anode: Phosphorous copper Stirring conditions: Air 12.5 L / min Plating conditions: 4 A, 45 min (time for a film thickness of 15 μm) Plating solution: CuSO 4 ・5H2 O 200g / L H 2 SO 4 54g / L 1molHCl 1.37mL / L
[0042] The film laminates produced as described above were evaluated for the crystallinity of the intermediate layer (oxide layer), the thickness of the intermediate layer, the thickness of the metallic copper layer, the conductivity of the metallic copper layer, the adhesive strength, and the heat resistance as follows. The evaluation results are shown in Table 1.
[0043] (Crystallization of Intermediate Layer) A single oxide film of 50 nm was formed on a fluororesin film, and the presence or absence of crystallinity of the intermediate layer (oxide layer) was determined by measuring it using the GI-XRD method (Rigaku Corporation, SmartLab). Cu Kα rays were used as incident X-rays, and measurements were performed at an X-ray incidence angle ω of 0.5° and a detection range of 2θ of 10 to 110°. An example of the XRD measurement results is shown in FIG. 3. As shown in FIG. 3, in Example 6, the pattern is similar to that of the fluororesin film (reference data), and no peaks indicating crystallinity are observed. On the other hand, in Comparative Example 1, peaks indicating crystallinity (see arrows in FIG. 3) are observed. For the other Examples and Comparative Examples, the presence or absence of peaks indicating crystallinity was similarly determined by XRD measurement to determine the presence or absence of peaks indicating crystallinity.
[0044] (Thickness of Intermediate Layer) The thickness of the intermediate layer is a target value based on the film formation rate. The film formation rate was calculated by measuring the film thickness after film formation on a dummy substrate for a certain period of time using a step measurement meter (Dektak-XT, manufactured by Bruker) and dividing the film thickness by the film formation time. The thickness of the intermediate layer was confirmed by observing the cross section of the film laminate with a TEM (transmission electron microscope: JEM-2010F, manufactured by JEOL Ltd.), and the result was a value equivalent to the target value based on the film formation rate.
[0045] (Thickness of Metallic Copper Layer) The thickness of the metallic copper layer (seed layer and copper plating layer) was confirmed by an eddy current method.
[0046] (Conductivity of metal copper layer) Conductivity of metal copper layer σ AThe resistivity (S / m) was measured by a four-probe method using a low resistivity meter (Loresta GP manufactured by Mitsubishi Chemical Corporation), and was converted to % IACS using the following formula: σ (% IACS) = σ A / (5.8 x 10 7 )
[0047] (Adhesion Strength) As shown in Figure 4, the intermediate layer and metallic copper layer formed on the fluororesin film were cut into 5 mm widths, and the adhesion strength of the film laminate was evaluated using a Tensilon universal testing machine (RTF-1310) manufactured by A&D Co., Ltd., under the conditions of a peel angle of 90 degrees and a peel speed of 50 mm / min. The adhesion strength of the film laminate was measured before and after the heat resistance test described below.
[0048] (Heat Resistance Test) As a heat resistance test, the film laminate was stored in a clean oven under the conditions of 150°C x 240 hours. After storage, the adhesion strength of the film laminate was measured as described above. Then, the rate of change in adhesion strength before and after the heat resistance test was calculated. (Rate of change) = (Adhesion strength after test - Adhesion strength before test) / Adhesion strength before test x 100 (%)
[0049]
[0050] In Comparative Example 1, a crystalline Zn oxide layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength significantly decreased after the heat resistance test. This is presumably due to interdiffusion between the fluororesin sheet and the metallic copper layer, resulting in fluorination and oxidation of the copper. In Comparative Example 2, a crystalline In—Sn oxide layer (ITO layer) was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength significantly decreased after the heat resistance test. This is presumably due to interdiffusion between the fluororesin sheet and the metallic copper layer, resulting in fluorination and oxidation of the copper.
[0051] In Comparative Example 3, a metallic Ti layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, but the adhesion strength significantly decreased after the heat resistance test. This is presumably because the metallic Ti layer, which was the intermediate layer, was fluorinated and oxidized. In Comparative Example 4, a metallic copper layer was formed directly on the fluororesin film without forming an intermediate layer, but the initial adhesion strength was low and the adhesion strength significantly decreased after the heat resistance test.
[0052] In contrast, in Examples 1 to 22, an amorphous oxide layer was formed as an intermediate layer between the fluororesin film and the metallic copper layer, and the initial adhesion was excellent. The adhesion strength did not decrease significantly even after the heat resistance test, and the heat resistance was also excellent.
[0053] From the above, it was confirmed that the examples provide a film laminate that is particularly suitable for wiring boards for high-frequency signal transmission, having excellent adhesion between the fluororesin film, which has low transmission loss in the high-frequency range, and the metal copper layer, and that does not significantly decrease adhesion even when used in a high-temperature environment.
Claims
1. A film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, characterized in that an amorphous oxide layer is formed between the fluororesin film and the metallic copper layer.
2. The film laminate according to claim 1, wherein the thickness of the amorphous oxide layer is within the range of 10 nm to 100 nm.
3. A film laminate according to claim 1 or 2, characterized in that the oxide constituting the amorphous oxide layer contains one or more elements selected from the group consisting of Ge, Si, Al, Ti, Ta, Zr and Cr.
4. The film laminate according to claim 1 or 2, characterized in that the oxide constituting the amorphous oxide layer contains In and Zn.
5. A film laminate according to claim 1 or 2, characterized in that the thickness of the metallic copper layer is within the range of 2 μm or more and 20 μm or less.
6. A film laminate according to claim 1 or 2, characterized in that the electrical conductivity of the metallic copper layer is 80% IACS or more.
Citation Information
Patent Citations
Printed wiring board and its manufacture
JP1997116256A
Manufacturing method for multilayer printed circuit board
JP2004363283A
Circuit device equipped with three-dimensional shaping circuit board
JP2008281570A
Flexible printed circuit board material and method for manufacturing flexible printed circuit board material
JP2010530612A
Anisotropy heat transfer body and production method thereof
JP2012016935A