Resin composition, resin coating material, insulated wire, wiring harness for automobile, and method for producing wiring harness for automobile

The resin composition for automotive wire harnesses, featuring an ethylene/α-olefin random copolymer and additives, addresses the challenges of flexibility, chemical resistance, and manufacturability by enhancing the properties of conventional resin coatings, ensuring efficient production and performance.

WO2024202765A1PCT designated stage expired Publication Date: 2024-10-03FURUKAWA ELECTRIC CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006555
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing resin compositions for insulated wires in automotive applications face challenges in achieving high flexibility, chemical resistance, and manufacturability while maintaining flame retardancy and heat resistance, with issues such as filler re-agglomeration causing clogging in extrusion processes.

Method used

A resin composition comprising an ethylene/α-olefin random copolymer as the base resin, blended with a wetting and dispersing agent, antioxidant, and crosslinking aid, which adjusts crystallinity and includes a softener, to enhance flexibility, chemical resistance, and manufacturability, and is crosslinked using an electron beam for improved properties.

Benefits of technology

The resin composition achieves excellent flexibility, chemical resistance, and manufacturability, preventing clogging in extrusion processes, and maintains the properties of conventional resin coating materials, resulting in a high-quality automotive wire harness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a resin composition containing the following components (A) to (D): (A) a base resin containing an ethylene-α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms; (B) a wetting and dispersing agent; (C) an antioxidant; and (D) a crosslinking aid; in which resin composition the crystallinity of the ethylene-α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms is 15-24%, and the component (B) content is 2-10 mass parts per 100 mass parts of the component (A) content.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, resin coating material, insulated wire, automotive wire harness, and method for manufacturing automotive wire harness

[0001] The present invention relates to a resin composition, a resin coating material, an insulated wire, an automotive wire harness, and a method for producing an automotive wire harness.

[0002] Flame-retardant insulated wires are widely used in various home appliances, office automation equipment, etc. Insulated wires used in automobiles and other applications are also required to have various properties, such as flame retardancy, heat resistance, flexibility, and mechanical properties. To date, resin compositions that can be used as conductor covering materials to realize insulated wires with flame retardancy, heat resistance, flexibility, and mechanical properties have been investigated and many reports have been published.

[0003] For example, Patent Document 1 describes an insulating resin composition that can form an insulating layer that has excellent flexibility, high tensile strength, excellent adhesion to an adhesive when an adhesive is used to waterproof a terminal, and stable pull-out force. This insulating resin composition includes a first copolymer that is a copolymer of an unsaturated hydrocarbon having 4 or more carbon atoms and ethylene, a copolymer of an unsaturated hydrocarbon having 4 or more carbon atoms and ethylene that is acid-modified and has a density of 0.88 g / cm. 3 and a third copolymer which is a copolymer of ethylene with an acrylic acid ester or the like, wherein the content ratio of the first to third copolymers is within a specific range, and the resin component contains 30 to 100 parts by mass of a flame retardant and 1 to 5 parts by mass of a cross-linking aid relative to 100 parts by mass of the resin component.

[0004] Patent Document 2 describes a resin composition having sufficient flexibility and heat resistance for use as a coating layer for an electric wire. This resin composition contains a resin component containing an ethylene-(meth)acrylic acid ester copolymer and at least one of an ethylene-propylene-diene terpolymer and an ethylene-acrylate rubber, and a flame retardant, and the resin component is crosslinked.

[0005] Patent Document 3 describes a heat-resistant resin composition that is applicable to cabtire cables and the like, because it has excellent high-temperature resistance, high flexibility and oil resistance, and the appearance of the resin after extrusion or the like is satisfactory. This heat-resistant resin composition contains specific amounts of each of components (A) to (E). Specifically, the density of component (A) before silane modification is 0.850 to 0.900 g / cm. 3 the total of components (A) to (D) contains 10 to 80 mass % of at least one of silane-modified polyethylene and silane-modified ethylene-α-olefin copolymer, the total of components (A) to (D) contains 3 to 60 mass % of component (B) polyolefin resin, the total of components (A) to (D) contains 10 to 50 mass % of component (C) at least one of styrene-based elastomer and ethylene-α-olefin copolymer rubber, the total of components (A) to (D) contains 5 to 60 mass % of component (D) paraffin-based oil, and the total of components (A) to (D) contains 0.005 to 0.5 mass parts of component (E) silanol condensation catalyst.

[0006] JP 2018-012817 A JP 2020-105319 A JP 2014-009238 A

[0007] In recent years, the development of environmentally friendly automobiles, particularly electric vehicles (EVs), has progressed rapidly around the world. In particular, the increasing diameter of electric wires in hybrid and electric vehicles (HEVs) requires higher currents, easier wiring management, and space-saving features. This has led to a growing demand for more flexible insulating coating materials. To provide flexibility to insulating coating materials, low-density polyethylene (LDPE) resins with densities of 0.910 to 0.930 have traditionally been used. However, it has proven difficult to achieve high flexibility with LDPE. While ethylene-based copolymers such as ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate copolymer (EMA), and ethylene-butyl acrylate copolymer (EBA) can improve flexibility by increasing the comonomer content, the increased polar component content can lead to a decrease in insulating properties. Furthermore, increased adhesion to metals can increase contact wear with metal dies during extrusion, potentially damaging the appearance and manufacturability of the resulting product. Furthermore, in order to further improve flame retardancy and heat resistance, fillers such as flame retardants and antioxidants are blended in large amounts, but fillers with small particle sizes tend to re-agglomerate, which can easily cause clogging of the screen mesh when manufacturing compounds using a feeder rudder or twin-screw extruder.

[0008] In view of the above circumstances, an object of the present invention is to provide a resin composition that, when used to form an insulating film (resin coating layer) for an insulated wire, can further improve the flexibility (flexibility) of the insulated wire, enhance chemical resistance (oil resistance), and further provide excellent compound manufacturability (less likely to clog a screen mesh) while fully maintaining the excellent properties (insulation, processability, flame retardancy, heat resistance, cold resistance, mechanical properties, etc.) of conventional resin coating materials. Another object of the present invention is to provide a resin coating material using the resin composition, an insulated wire having a layer of this resin coating material, an automotive wire harness including this insulated wire, and a method for manufacturing the same.

[0009] As a result of investigations aimed at solving the above-mentioned problems, the present inventors have found that, in a resin composition for an insulating coating material using an ethylene-α-olefin copolymer having an α-olefin component having 4 to 12 carbon atoms as a base resin, by adjusting the crystallinity of the copolymer within a specific range, incorporating a specific amount of a wetting and dispersing agent, and further incorporating an antioxidant and a cross-linking aid, the resulting resin composition has superior flexibility and chemical resistance while fully maintaining the excellent properties of conventional resin coating materials. Furthermore, the wetting and dispersing agent enhances the dispersibility of fillers, thereby suppressing clogging of screen meshes in feeder rudder or twin-screw extruders during compound production using the resin composition (i.e., excellent compound manufacturability). Based on these findings, the present inventors have conducted further investigations and have now completed the present invention.

[0010] That is, the above-mentioned problems have been solved by the following means. <1> A resin composition comprising the following components (A) to (D): (A) a base resin containing an ethylene / α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms, (B) a wetting and dispersing agent, (C) an antioxidant, and (D) a crosslinking aid, wherein the ethylene / α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms has a crystallinity of 15 to 24%, and the content of component (B) is 2 to 10 parts by mass per 100 parts by mass of component (A). <2> The resin composition according to <1> above, which contains component (E) a softener. <3> The resin composition according to <2> above, wherein component (E) is a chain hydrocarbon polymer and / or a hindered amine compound. <4> The resin composition according to any one of <1> to <3>, wherein the component (A) contains at least one of a styrene-based elastomer, an ethylene-propylene rubber, and an olefin-based block copolymer. <5> The resin composition according to any one of <1> to <4>, wherein the content of the component (C) is 10 to 30 parts by mass per 100 parts by mass of the component (A). <6> The resin composition according to any one of <1> to <5>, wherein the content of the component (D) is 0.5 to 6 parts by mass per 100 parts by mass of the component (A). <7> The resin composition according to any one of <1> to <6>, for forming a resin coating material for an insulated wire constituting an automotive wire harness. <8> A resin coating material obtained by crosslinking the resin composition according to any one of <1> to <7>. <9> An insulated wire, the insulating coating of which comprises the resin coating material according to <8>. <10> An automotive wire harness, comprising the insulated wire according to <9>. <11> A method for producing an automotive wire harness, comprising the steps of extrusion coating a conductor with the resin composition according to any one of <1> to <7> to provide a layer of the resin composition, and irradiating the layer of the resin composition with an electron beam of 80 to 250 kGy.

[0011] The resin composition of the present invention has excellent compound manufacturability, and when used to form an insulating coating (resin coating layer) for an insulated electric wire, it is possible to obtain an insulated electric wire that is excellent in flexibility and chemical resistance while fully maintaining the excellent properties of conventional resin coating materials. The automotive wire harness of the present invention has the above-mentioned resin coating material in the insulating coating of an insulated electric wire, and is excellent in flexibility and chemical resistance (oil resistance). The manufacturing method for an automotive wire harness of the present invention makes it possible to obtain an automotive wire harness that has the above-mentioned excellent properties and advantages.

[0012] [Resin Composition] The resin composition of the present invention contains a base resin (also referred to as component (A)) containing an ethylene-α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms, a wetting and dispersing agent (B) (also referred to as component (B)), an antioxidant (C) (also referred to as component (C)), and a crosslinking aid (D) (also referred to as component (D)). In the present invention, "comprising components (A) to (D)" is synonymous with "comprising a blend of components (A) to (D)." Furthermore, in the present invention, unless otherwise specified, the term "resin" is used to include an elastomer (i.e., a resin and / or an elastomer). Components (A) to (D) and the optional components described below may each be used alone or in combination of two or more. The components contained in the resin composition of the present invention are described below.

[0013] <(A) Base Resin> The resin composition of the present invention contains a base resin (hereinafter also simply referred to as "base resin") containing an ethylene-α-olefin random copolymer (hereinafter also simply referred to as "ethylene-α-olefin copolymer") in which the α-olefin component has 4 to 12 carbon atoms. From the viewpoint of further improving chemical resistance, the content of the ethylene-α-olefin copolymer in the base resin is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. Alternatively, the entire base resin may be an ethylene-α-olefin copolymer. The remainder of the base resin, excluding the ethylene-α-olefin copolymer, may contain other polymers, as described below.

[0014] ((A1) Ethylene / α-olefin random copolymer in which the α-olefin component has 4 to 12 carbon atoms) In the present invention, the α-olefin in component (A1) is not particularly limited as long as it has 4 to 12 carbon atoms, and examples include 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, and 1-dodecene. Component (A1) may contain a third component other than the ethylene component and the α-olefin component, as long as the effects of the present invention are not impaired.

[0015] The crystallinity of the component (A1) is 15 to 24%. From the viewpoint of improving chemical resistance, the crystallinity is preferably 16% or more, more preferably 17% or more, and even more preferably 18% or more. From the viewpoint of improving flexibility, the crystallinity is preferably 23% or less, more preferably 22% or less. In the resin composition of the present invention, the crystallinity of the component (A1) refers to the crystallinity of the component (A1) to be blended. In the present invention, the crystallinity refers to the crystallinity of the entire component (A1). In other words, when two or more ethylene-α-olefin copolymers are used as the component (A1), the crystallinity refers to the crystallinity of the entire two or more ethylene-α-olefin copolymers. The crystallinity of the entire component (A1) can be calculated based on the crystallinity of the blended ethylene-α-olefin copolymers and their blending amounts. For example, when an ethylene / α-olefin copolymer having a crystallinity of 10% and an ethylene / α-olefin copolymer having a crystallinity of 30% are mixed in a ratio of 7:3, the crystallinity of the entire component (A1) can be calculated as [10% × 0.7 + 30% × 0.3 = 16%].

[0016] Component (A1) is preferably a component consisting of a mixture of two or more copolymers. For example, it is preferable to mix an ethylene / α-olefin copolymer (component (A2)) having a crystallinity of 10% to 24% and an ethylene / α-olefin copolymer (component (A3)) having a crystallinity of more than 24% but less than 35%, and adjust the crystallinity of the resulting mixture of component (A1) to 15% to 24%. In this case, the components are mixed so that, relative to 100 parts by mass of the total amount of component (A1), the amounts of component (A2) and component (A3) are preferably 60 to 100 parts by mass, 0 to 40 parts by mass, more preferably 60 to 80 parts by mass, 20 to 40 parts by mass, and even more preferably 70 to 80 parts by mass, and 20 to 30 parts by mass, respectively.

[0017] The crystallinity of component (A1) can be determined by using a differential scanning calorimeter to measure the endothermic peak area (J) in a conventional manner, and then calculating the heat of fusion (J / g) from this endothermic peak area (J) and the sample amount (g). In this case, the crystallinity (%) can be calculated using the following formula (1): Crystallinity (%) = (heat of fusion / heat of dissolution of fully crystalline form) × 100 (Formula 1). The measurement conditions using the differential scanning calorimeter are a nitrogen gas atmosphere (nitrogen gas flow rate: 50 mL / min) and a heating and cooling rate of 10 °C / min. The "heat of fusion of fully crystalline form" can be a known value. For example, data from TA Instruments can be used. For resins whose "heat of fusion of fully crystalline form" is unknown, the heat of fusion of fully crystalline form of high-density polyethylene (293 J / g) is used as the heat of fusion of the fully crystalline form of the resin, and the crystallinity is calculated. The differential scanning calorimeter may be, for example, a DSC6200 (trade name) manufactured by Hitachi High-Tech Science Corp. When a commercially available product is used as component (A1), the crystallinity value listed in the catalog can be used as the crystallinity of component (A1).

[0018] The density of the component (A1) is 0.865 g / cm 3 ~0.880g / cm 3 It is also preferable that:

[0019] The component (A1) can be synthesized by a conventional method, or a commercially available product can be used, such as ENGAGE 7467 (trade name, ethylene-butene polyolefin elastomer, manufactured by Dow Chemical Company), ENGAGE 8150 (trade name, ethylene-octene polyolefin elastomer, manufactured by Dow Chemical Company), and ENGAGE 8452 (trade name, ethylene-octene polyolefin elastomer, manufactured by Dow Chemical Company).

[0020] (Other Polymers) The base resin may contain other polymers other than component (A1) as long as the effects of the present invention are not impaired. Examples of such other polymers include at least one of styrene-based elastomers, ethylene-propylene rubbers, and olefin-based block copolymers.

[0021] The styrene-based elastomer is a copolymer block of components derived from an aromatic vinyl compound and a conjugated diene compound, and / or a hydrogenated product of a block copolymer or random copolymer primarily composed of components derived from the above compounds. The aromatic vinyl compound may be, for example, one or more selected from styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, etc., with styrene being preferred. The conjugated diene compound may be, for example, one or more selected from butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc., with butadiene, isoprene, or a combination thereof being preferred. The styrene-based elastomer may be a binary or ternary copolymer composed of a polystyrene block and an elastomer block having a polyolefin structure. The styrene-based elastomer preferably contains 10 to 70% by mass of components derived from the aromatic vinyl compound. This content can be determined, for example, by measuring the UV absorption spectrum using a chloroform solution with an ultraviolet spectrophotometer. An example of a commercially available styrene elastomer is "Septon" (trade name, brand: 4033, type: SEEPS, styrene content: 30%, manufactured by Kuraray Co., Ltd.).

[0022] In the present invention and this specification, the ethylene-propylene rubber includes ethylene-propylene binary copolymers, ethylene-propylene-diene terpolymers, and the like, as well as olefin-based thermoplastic elastomers containing these as the primary components (e.g., polyolefins such as polypropylene and polyethylene serve as hard segments, and rubber components such as ethylene-propylene rubber serve as soft segments, with the hard and soft segments having a microphase-separated structure). Commercially available ethylene-propylene-diene copolymers include, for example, EP123 (trade name, ENB content: 4.5%, ethylene content: 58%, manufactured by ENEOS Materials Corporation). Furthermore, the olefin-based thermoplastic elastomer preferably has a hardness (durometer A) of 80 or less. Commercially available elastomers include, for example, Milastomer (registered trademark, product number: 4010NS, hardness (durometer A): 46, manufactured by Mitsui Chemicals, Inc.). The hardness (Durometer A) is determined by a method according to ISO 7619 2010.

[0023] The olefin-based block copolymer is a copolymer in which two types of polyolefins are alternately formed in blocks within one molecule. For example, an olefin-based block copolymer consisting of an amorphous ethylene-octene block (soft) having a high comonomer content and a low glass transition temperature and a crystallizable ethylene-octene block (hard) having a very low comonomer content and a high melting temperature can be used. The density of the olefin-based block copolymer is 0.89 g / cm. 3 It is preferable that the melting point is 130°C or less. Examples of commercially available products of such olefin-based block copolymers include INFUSE 9107 (trade name, olefin-based block copolymer (density 0.866 g / cm 3 ), melting point: 121°C, manufactured by The Dow Chemical Company).

[0024] The content of the other polymer in component (A) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more from the viewpoint of further improving flexibility, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less from the viewpoint of chemical resistance and crosslinkability.

[0025] <(B) Wetting and Dispersing Agent> The resin composition of the present invention contains (B) a wetting and dispersing agent. A wetting and dispersing agent is an additive that functions both as a wetting agent, acting as a surfactant to increase the wettability of dispersoids to the resin component, and as a wetting agent to prevent dispersoid aggregation through electrical repulsion, steric hindrance, and other mechanisms. The wetting function is typically performed by chains compatible with the resin component, while the function of preventing dispersoid aggregation is typically performed by adsorbent groups to the dispersoid. By incorporating a specific amount of a wetting and dispersing agent into the resin composition of the present invention, the dispersibility of the blended fillers (e.g., the flame retardant described below) can be improved, thereby improving the compound manufacturability of the resin composition. Wetting and dispersing agents are available in liquid or powder (or flake) form, with powder (or flake) forms being preferred from the standpoint of workability. Furthermore, those with a dropping point of 50°C or higher and a melting point of 100°C or lower are preferred. In the present invention, commercially available wetting and dispersing agents may be used as component (B). Examples of commercially available products include BYK-MAX D4221 and BYK-MAX P4102 (both trade names, manufactured by BYK Japan).

[0026] As described above, the resin composition of the present invention contains 2 to 10 parts by mass of component (B) per 100 parts by mass of component (A). From the viewpoint of suppressing mesh clogging and the occurrence of aggregated particles, and from the viewpoint of suppressing the occurrence of bloom and crosslinking inhibition, the resin composition preferably contains 3 to 9 parts by mass, more preferably 4 to 8 parts by mass, and even more preferably 5 to 7 parts by mass of component (B) per 100 parts by mass of component (A).

[0027] <(C) Antioxidant> The resin composition of the present invention contains an antioxidant (C). Examples of such component (C) include phenol compounds (phenolic antioxidants), imidazole compounds (imidazole antioxidants), and thioether compounds (thioether antioxidants), and one or more of these can be used. From the viewpoint of improving heat resistance, the resin composition of the present invention preferably contains 10 to 30 parts by mass, and more preferably 14 to 22 parts by mass, of component (C) (the total amount of antioxidants when the resin composition contains multiple antioxidants) per 100 parts by mass of component (A).

[0028] (Phenol-Based Antioxidant) Examples of the phenol-based antioxidant that can be used in the resin composition of the present invention include triethylene glycol-bis(3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate), 1,6-hexanediol-bis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), pentaerythritol-tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5,-di-t-butyl-4-hydroxybenzyl)benzene, Examples of antioxidants include tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate and isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. Among these, from the viewpoint of imparting high heat resistance to automotive wire harnesses, those having two or more 3,5-di-t-butyl-4-hydroxyphenyl groups or 3,5-di-t-butyl-4-hydroxybenzyl groups are preferred, and tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate and pentaerythritol-tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate) are particularly preferred. In the present invention, commercially available phenolic antioxidants may also be used. An example of a commercially available product is Irganox 1010 (trade name, manufactured by BASF).

[0029] When the resin composition of the present invention contains a phenolic antioxidant, from the viewpoint of improving heat resistance, the resin composition preferably contains 1 to 8 parts by mass, and more preferably 2 to 6 parts by mass, of the phenolic antioxidant per 100 parts by mass of the component (A).

[0030] (Imidazole-Based Antioxidant) Examples of imidazole-based antioxidants that can be used in the resin composition of the present invention include 2-sulfanylbenzimidazole, 2-sulfanylmethylbenzimidazole, 4-sulfanylmethylbenzimidazole, 5-sulfanylmethylbenzimidazole, and zinc salts thereof, with 2-sulfanylbenzimidazole and its zinc salt being preferred. Commercially available imidazole-based antioxidants may also be used in the present invention. Examples of commercially available products include Nocrac MBZ (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.).

[0031] When the resin composition of the present invention contains an imidazole-based antioxidant, from the viewpoint of improving heat resistance, the resin composition preferably contains 8 to 16 parts by mass, and more preferably 10 to 14 parts by mass, of the imidazole-based antioxidant per 100 parts by mass of component (A).

[0032] (Thioether-Based Antioxidant) Examples of the thioether-based antioxidant that can be used in the resin composition of the present invention include dilauryl 3,3′-thiodipropionate, dimyristyl 3,3′-thiodipropionate, distearyl 3,3′-thiodipropionate, 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-(dodecylthio)propionate] (also known as 2,2-bis[[3-(dodecylthio)-1-oxopropyloxy]methyl]-1,3-propanediyl bis[3-(dodecylthio)propionic acid]). Among these, 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-(dodecylthio)propionate] is preferred from the viewpoint of long-term thermal stability and improved resistance to extraction. A commercially available thioether antioxidant may also be used in the resin composition of the present invention. An example of a commercially available product is Adekastab AO-412S (trade name, manufactured by ADEKA Corporation).

[0033] When the resin composition of the present invention contains a thioether-based antioxidant, from the viewpoint of improving heat resistance, the thioether-based antioxidant is preferably contained in an amount of 0.5 to 4 parts by mass, and more preferably 1 to 3 parts by mass, per 100 parts by mass of the component (A).

[0034] <(D) Crosslinking Auxiliary Agent> The resin composition of the present invention contains a crosslinking auxiliary agent (D). Examples of component (D) include polyfunctional compounds, preferably compounds having two or more (preferably three or more, more preferably three to six) ethylenically unsaturated bonds (carbon-carbon double bonds) in the molecule. Specific examples of component (D) include (meth)acrylate compounds such as polypropylene glycol diacrylate and trimethylolpropane triacrylate, allyl compounds such as triallyl cyanurate, maleimide compounds, and divinyl compounds. In the present invention, a commercially available crosslinking auxiliary agent may be used as component (D). An example of a commercially available product is Ogmont T200 (trade name, manufactured by Shin-Nakamura Chemical Co., Ltd.). From the viewpoint of improving heat resistance and chemical resistance, the resin composition of the present invention preferably contains 0.5 to 6 parts by mass, more preferably 1 to 5 parts by mass, and even more preferably 2 to 4 parts by mass of component (D) per 100 parts by mass of component (A).

[0035] <Other Components> In addition to the above components (A) to (D), the resin composition of the present invention may contain other components such as the following softeners, flame retardants, processing aids, and additives, as long as the effects of the present invention are not impaired.

[0036] <(E) Softener> The resin composition of the present invention preferably contains a softener (E). As component (E) that can be used in the present invention, softeners that are generally used in insulating coating materials and are liquid at room temperature (25°C) and atmospheric pressure (0.1 MPa) can be used. Component (E) may be used alone or in combination of two or more. Examples of component (E) include naphthenic or aromatic process oils, linear hydrocarbon polymers, hindered amine compounds, phthalic acid derivatives such as dioctyl phthalate or dibutyl phthalate, white oil, and mineral oil. Of these, component (E) is preferably a linear hydrocarbon polymer and / or a hindered amine compound.

[0037] Examples of the linear hydrocarbon polymer include polybutene, polybutadiene, polyisoprene, and polyisoprene-butadiene copolymer. Of these, polybutene is preferred. The number average molecular weight of the linear hydrocarbon polymer is preferably 300 or more, and more preferably 900 or more. The number average molecular weight is preferably 10,000 or less, more preferably 5,000 or less, more preferably 4,000 or less, and even more preferably 3,500 or less. A preferred range for the number average molecular weight is 300 to 10,000, more preferably 300 to 5,000, even more preferably 900 to 4,000, and even more preferably 900 to 3,500.

[0038] The hindered amine compound is preferably an NOR (alkoxyimino group) type hindered amine compound having an N-alkoxyl group (>N-OR) structure, as opposed to an N-H type in which the imino group (>N-H) portion of the piperidine ring remains NH, or an N-methyl type in which H is replaced with a methyl group. Having such a structure can impart flame retardancy to the resin composition. Specific examples of NOR type hindered amine compounds include bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate.

[0039] In the present invention, a commercially available softener may be used as component (E). Examples of commercially available softeners include Polybutene HV-100 and Polybutene HV-1900 manufactured by ENEOS Corporation, and Adeka Stab FP-T80 manufactured by ADEKA Corporation.

[0040] When the resin composition of the present invention contains component (E), from the viewpoint of further improving chemical resistance and further improving flexibility, the resin composition preferably contains 9 parts by mass or more of component (E) per 100 parts by mass of component (A), more preferably 10 parts by mass or more, even more preferably 12 parts by mass or more, and even more preferably 14 parts by mass or more. Furthermore, from the viewpoint of improving chemical resistance, the resin composition preferably contains 21 parts by mass or less of component (E) per 100 parts by mass of component (A), more preferably 20 parts by mass or less, even more preferably 19 parts by mass or less, and even more preferably 18 parts by mass or less. The content of component (E) per 100 parts by mass of component (A) is preferably in the range of 9 to 21 parts by mass, more preferably 10 to 20 parts by mass, even more preferably 12 to 19 parts by mass, and even more preferably 14 to 18 parts by mass.

[0041] <Flame Retardant> The present invention can contain a flame retardant to the extent that the effects of the present invention are not impaired. Examples of such flame retardants include bromine-based flame retardants and antimony-based flame retardants. The present invention preferably contains at least one of a bromine-based flame retardant or an antimony-based flame retardant, and more preferably contains both a bromine-based flame retardant and an antimony-based flame retardant. Furthermore, the mixing ratio of the bromine-based flame retardant and the antimony-based flame retardant is preferably within a range such that the molar ratio of bromine to antimony is 2 to 5 times the molar amount of antimony contained in the resin composition. In other words, it is preferable to contain a bromine-based flame retardant that provides 2 to 5 times the molar amount of bromine contained in the antimony-based flame retardant. When the resin composition of the present invention contains a flame retardant, the total amount of the flame retardant is preferably 33 to 45 parts by mass per 100 parts by mass of component (A).

[0042] (Brominated Flame Retardant) The brominated flame retardant is preferably a bromine-containing compound. That is, the resin composition of the present invention preferably contains a bromine-containing compound as a flame retardant. Examples of brominated flame retardants that can be used include brominated N,N'-ethylenebisphthalimide or compounds derived therefrom (collectively referred to as "brominated N,N'-ethylenebisphthalimide compounds"), N,N'-bis(bromophenyl)terephthalamide or compounds derived therefrom (collectively referred to as "N,N'-bis(bromophenyl)terephthalamide compounds"), brominated bisphenol or compounds derived therefrom (collectively referred to as "brominated bisphenol compounds"), and 1,2-bis(bromophenyl)alkanes and other organic bromine-containing flame retardants. Among these, it is preferable to use, for example, brominated N,N'-ethylenebisphthalimide and / or 1,2-bis(pentabromophenyl)ethane. By using brominated N,N'-ethylenebisphthalimide and / or 1,2-bis(bromophenyl)alkane as a flame retardant, it is possible to form a resin coating material that hardly causes bleeding. The brominated flame retardant used in the resin composition of the present invention may be a commercially available brominated flame retardant. An example of a commercially available product is Cytex 8010 (trade name, manufactured by Albemarle).

[0043] When the resin composition of the present invention contains a brominated flame retardant, it preferably contains 15 to 35 parts by mass of the brominated flame retardant per 100 parts by mass of the component (A).

[0044] (Antimony-Based Flame Retardant) Examples of antimony-based flame retardants include antimony trioxide, antimony tetroxide, antimony pentoxide, and sodium antimonate. Antimony reacts with chlorine (a halogen), and the gas generated is thought to block oxygen, thereby promoting the formation of a carbonized layer and trapping free radicals (stopping the pyrolysis chain reaction). Of these, in the present invention, it is preferable to add antimony trioxide from the viewpoint of forming a more stable carbonized layer. Commercially available antimony trioxide may be used in the present invention. An example of a commercially available product is PATOX-C (trade name, manufactured by Nippon Seiko Co., Ltd.).

[0045] When the resin composition of the present invention contains an antimony-based flame retardant, it preferably contains 5 to 15 parts by mass of the antimony-based flame retardant per 100 parts by mass of the component (A).

[0046] (Other Flame Retardants) In addition to the bromine-based flame retardant and antimony-based flame retardant, the resin composition of the present invention may contain a flame retardant that can be commonly used in the insulating coating of an insulated electric wire. Examples of such flame retardants include metal hydroxides (hydroxide-based flame retardants) such as magnesium hydroxide and aluminum hydroxide. When the resin composition of the present invention contains a hydroxide-based flame retardant, the hydroxide-based flame retardant is preferably contained in an amount of 5 parts by mass or less, more preferably 3 parts by mass or less, per 100 parts by mass of the content of component (A).

[0047] <Processing Aid> The resin composition of the present invention preferably contains a processing aid to the extent that the effects of the present invention are not impaired. A preferred example of the processing aid is a metal soap (lubricant). Examples of metal soaps (lubricants) that can be used in the resin composition of the present invention include calcium stearate, zinc stearate, and magnesium stearate. Commercially available metal soaps may also be used in the present invention. An example of a commercially available product is Sinaka Red ZS-101 (trade name, manufactured by Shinagawa Chemical Industry Co., Ltd.).

[0048] When the resin composition of the present invention contains a metal soap, it preferably contains 0.5 to 2 parts by mass of the metal soap per 100 parts by mass of the component (A).

[0049] <Additives> The resin composition of the present invention can contain various additives, such as copper inhibitors, ultraviolet absorbers, dispersants (dispersants other than wetting dispersants), plasticizers, fillers, pigments, etc., as needed, within the range that does not impair the effects of the present invention. Examples of such additives include zinc compounds. Specific examples of zinc compounds include zinc sulfide and zinc oxide.

[0050] [Method of Manufacturing Resin Composition] The resin composition of the present invention can be obtained by blending the above-mentioned components (A) to (D) and, if necessary, the above-mentioned optional components, and melt-kneading them in a commonly used kneading device such as a batch kneader, a roll, a kneader, a Banbury mixer, or the like, or a twin-screw extruder.

[0051] [Automotive Wire Harness] The automotive wire harness of the present invention includes an insulated electric wire having a layer made of a resin coating material obtained by crosslinking the resin composition of the present invention on the surface of a conductor (including a conductor bundle and a fiber core). In the automotive wire harness of the present invention, the insulated electric wire may have an intermediate layer or a shielding layer between the conductor and the layer made of the resin coating material. Hereinafter, the automotive wire harness may also be simply referred to as a "wire harness."

[0052] [Method for manufacturing an automotive wire harness] The automotive wire harness of the present invention can be obtained by extrusion coating the resin composition of the present invention onto a conductor to form a layer of the resin composition, and then irradiating the layer of the resin composition with an electron beam of 80 to 250 kGy. This electron beam irradiation causes a crosslinking reaction in the layer of the resin composition, forming a resin coating material layer. The wire harness can be obtained by bundling the conductor and the insulated wire having the resin coating layer, and attaching a connector to the end.

[0053] The conductor may be a solid wire or a twisted wire, and may be bare, tin-plated, or enamel-coated. Metal materials for the conductor include annealed copper, copper alloys, and aluminum. The thickness of the resin coating layer formed around the conductor is not particularly limited, but is typically approximately 0.15 to 5 mm. The conductor diameter, conductor material, and coating layer thickness are not particularly limited and can be determined appropriately depending on the purpose and application. The crosslinking reaction by electron beam irradiation can be carried out using conventional methods and conditions, and is not limited. The electron beam irradiation conditions are preferably a dose of 50 to 450 kGy, more preferably 80 to 250 kGy, even more preferably 80 to 200 kGy, and particularly preferably 80 to 160 kGy. The acceleration voltage is preferably 300 to 5000 keV, more preferably 500 to 3000 keV. A multilayer structure may also be used, such as by providing an intermediate layer or shielding layer between the conductor and the coating layer, or between the coating layers.

[0054] The conditions for extrusion molding the resin composition of the present invention are not particularly limited as long as the resin composition of the present invention can be extruded, but the extrusion temperature (head) is preferably 100 to 230°C, more preferably 120 to 200°C, in order to reduce the load on the extruder (extrusion molding machine) and ensure shape retention. Other conditions for extrusion molding can be set appropriately depending on the purpose. The screw configuration of the extruder is not particularly limited, and a conventional full-flighted screw, double-flighted screw, tip double-flighted screw, Maddock screw, etc. can be used.

[0055] The present invention will be described in more detail based on the following examples and comparative examples, but the present invention is not limited to these.

[0056] [Examples 1 to 12 and Comparative Examples 1 to 5] The materials used to prepare the resin compositions of Examples 1 to 12 and Comparative Examples 1 to 5 are shown in Table 1 below. Details of the materials used are as follows.

[0057] <Materials used> (Component (A): Base resin) - Component (A1): Ethylene-α-olefin copolymer - ENGAGE 7467: Trade name, ethylene-butene polyolefin elastomer (crystallinity 12%, density 0.862 g / cm 3 ), ENGAGE 8150: Trade name, ethylene-octene polyolefin elastomer (crystallinity 16%, density 0.868 g / cm), manufactured by Dow Chemical Company 3 ), ENGAGE 8100: Trade name, manufactured by Dow Chemical Company, ethylene-octene polyolefin elastomer (crystallinity 18%, density 0.870 g / cm 3 ), ENGAGE 8452: Trade name, ethylene-octene polyolefin elastomer (crystallinity 20%, density 0.875 g / cm), manufactured by Dow Chemical Company 3 ), ENGAGE 7256: Trade name, ethylene-octene polyolefin elastomer (crystallinity 23%, density 0.885 g / cm), manufactured by Dow Chemical Company 3 ), ENGAGE 8003: Trade name, manufactured by Dow Chemical Company, ethylene-octene polyolefin elastomer (crystallinity 25%, density 0.885 g / cm 3 ), ENGAGE 8440: Trade name, ethylene-octene polyolefin elastomer (crystallinity 27%, density 0.897 g / cm), manufactured by Dow Chemical Company 3 ), ENGAGE 8480: Trade name, ethylene-octene polyolefin elastomer (crystallinity 33%, density 0.902 g / cm), manufactured by Dow Chemical Company 3 ), manufactured by Dow Chemical Company. Other polymers: Septon: trade name, brand name 4033, type SEEPS, styrene content 30%, manufactured by Kuraray Co., Ltd. EP123: trade name, ENB content 4.5%, ethylene content 58%, manufactured by ENEOS Materials Corporation. Milastomer: registered trademark, product number 4010NS, hardness (durometer A) 46, manufactured by Mitsui Chemicals, Inc. INFUSE 9107: trade name, olefin block copolymer (density 0.866 g / cm 3 ), melting point 121°C, manufactured by Dow Chemical Company

[0058] (Component (B): Wetting and dispersing agent) BYK-MAX D4221: Trade name, manufactured by BYK Japan

[0059] (Component (C): Antioxidant) Phenolic antioxidant: pentaerythritol-tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), phenolic antioxidant, Irganox 1010 (trade name), manufactured by BASF Imidazole antioxidant: zinc salt of 2-mercaptobenzimidazole, Nocrac MBZ (trade name), manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Thioether antioxidant: 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-(dodecylthio)propionate], Adekastab AO-412S (trade name), manufactured by ADEKA Corporation

[0060] (Component (D): Crosslinking aid) Multifunctional polymer: trimethylolpropane trimethacrylate, Ogmont T200 (trade name), manufactured by Shin-Nakamura Chemical Co., Ltd.

[0061] (Component (E): Softener) Polybutene HV-100: Trade name, polybutene (number average molecular weight: 980), manufactured by ENEOS Corporation Polybutene HV-1900: Trade name, polybutene (number average molecular weight: 2900), manufactured by ENEOS Corporation ADK STAB FP-T80: Trade name, bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate, manufactured by ADEKA Corporation

[0062] (Flame retardant) Brominated flame retardant: 1,2-bis(pentabromophenyl)ethane, Cytex 8010 (trade name), manufactured by Albemarle Antimony: antimony trioxide, PATOX-C (trade name), manufactured by Nippon Seiko Co., Ltd.

[0063] (Processing aid) Metal soap: zinc stearate, Sinaka Red ZS-101 (product name), manufactured by Shinagawa Kako Co., Ltd.

[0064] <Production of Resin Composition Pellets> According to the compositions shown in Table 1 below, the materials were melt-kneaded at 180°C using a 75-liter Banbury mixer, and the mixture (compound) was discharged and granulated through a screen mesh (mesh number: 200 mesh) of an extruder to obtain resin composition pellets.

[0065] [Performance Evaluation] The resin compositions (Examples 1 to 12 and Comparative Examples 1 to 5) produced as described above were subjected to the following performance evaluations.

[0066] <Evaluation of Compound Production> When producing the resin composition pellets, the presence or absence of replacement of the screen mesh due to clogging or the like was evaluated according to the following evaluation criteria. -Evaluation criteria- ⊚: Resin composition pellets could be produced without replacing the screen mesh even when 4 batches of 200 kg or more were produced. ◯: Screen mesh replacement was not necessary until 1 batch of 50 kg was produced, but the screen mesh was replaced by the time 4 batches of 200 kg were produced. ×: Screen mesh replacement was performed before 1 batch of 50 kg was produced.

[0067] <Flexibility (Bending Rigidity) Evaluation> Each of the obtained resin composition pellets was extrusion coated onto a copper conductor (19 strands / 26 strands / strand diameter 0.32 mm) using an extruder set at a temperature of 90 to 190°C. The formed resin composition layer was subjected to a cross-linking reaction by electron beam irradiation. 2An insulated wire (finished outer diameter approximately 12.0 mm) was obtained, having a 1.4 mm thick insulating coating around a copper conductor (≒40 sq). The electron beam crosslinking was performed at an acceleration voltage of 3000 keV and a dose of 160 kGy. Flexibility (bending rigidity) was measured according to the method specified in Japanese Industrial Standards JIS C6870-1-21:2018, Section 19, E17C. Each insulated wire (sample) was cut to a length of 400 mm, and a cable (insulated wire) bent 180 degrees was placed between parallel plates. The ends of the cable were fixed to the parallel plates, a load cell was placed on the plates, and the maximum load (N) was measured when the cable was bent to a bending distance of 100 mm. The obtained maximum load was evaluated based on the following evaluation criteria. The load cell's zero point was adjusted before attaching the sample, and the test was conducted at room temperature. -Evaluation criteria- ◎: Maximum load is less than 15N 〇: Maximum load is 15N or more but less than 20N ×: Maximum load is 20N or more

[0068] <Evaluation of Gasoline Swelling Resistance> Each resin composition pellet obtained was extruded at a temperature of 90 to 190°C to prepare a resin sheet having a thickness of 1.4 mm, which was then subjected to a crosslinking reaction by electron beam irradiation. Dumbbell pieces having a length of 15 mm and a width of 30 mm were punched out of the resin sheet and used as test pieces. These were immersed in gasoline at a temperature of 23±5°C for 20 hours, and the rate of change in the sheet thickness 30 minutes after removal was measured using the following formula (2), and the sheet was evaluated according to the following evaluation criteria: Rate of change (%) = {(Test piece thickness after immersion - Test piece thickness before immersion) / Test piece thickness before immersion} × 100 (Formula 2) Evaluation criteria: ◎: Rate of change less than 5% ◯: Rate of change 5% or more but less than 10% ×: Rate of change 10% or more

[0069] The results obtained are shown in Table 1. The amounts blended in the table are in parts by mass (mass ratio).

[0070]

[0071]

[0072] The content of each component in the table is in parts by mass. Blank spaces and "-" mean that the corresponding component is not included.

[0073] As is clear from Table 1, resin compositions (Comparative Examples 1 and 4) in which the crystallinity of component (A1) was outside the range specified in the present invention, and resin compositions (Comparative Examples 2 to 5) in which the content of component (B) was outside the range specified in the present invention were all inferior in at least one of the evaluations of flexibility, gasoline swelling resistance, and compound manufacturability. In contrast, resin compositions (Examples 1 to 12) that satisfied all of the specifications of the present invention were excellent in the evaluation of flexibility, the evaluation of gasoline swelling resistance, and the evaluation of compound manufacturability. Furthermore, these resin compositions had sufficient insulation, flame retardancy, durability, mechanical properties, etc. to be used as resin coating materials for insulated electric wires.

[0074] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.

[0075] This application claims priority based on Japanese Patent Application No. 2023-050983, filed on March 28, 2023, the contents of which are incorporated herein by reference as part of the present specification.

Claims

1. A resin composition comprising the following components (A) to (D): (A) a base resin containing an ethylene / α-olefin random copolymer having an α-olefin component with 4 to 12 carbon atoms; (B) a wetting and dispersing agent; (C) an antioxidant; and (D) a crosslinking aid; the ethylene / α-olefin random copolymer having 4 to 12 carbon atoms has a crystallinity of 15 to 24%, and the content of component (B) is 2 to 10 parts by mass per 100 parts by mass of component (A).

2. The resin composition according to claim 1, which contains component (E) a softening agent.

3. The resin composition according to claim 2, wherein the component (E) is a chain hydrocarbon polymer and / or a hindered amine compound.

4. The resin composition according to any one of claims 1 to 3, wherein the component (A) contains at least one of a styrene-based elastomer, an ethylene-propylene rubber, and an olefin-based block copolymer.

5. A resin composition according to any one of claims 1 to 4, wherein the content of said component (C) is 10 to 30 parts by mass per 100 parts by mass of the content of said component (A).

6. The resin composition according to any one of claims 1 to 5, wherein the content of said component (D) is 0.5 to 6 parts by mass per 100 parts by mass of the content of said component (A).

7. The resin composition according to any one of claims 1 to 6, which is used to form a resin coating material for an insulated electric wire that constitutes an automobile wiring harness.

8. A resin coating material obtained by crosslinking the resin composition according to any one of claims 1 to 7.

9. An insulated wire, the insulating coating of which comprises the resin coating material according to claim 8.

10. A wiring harness for an automobile, comprising the insulated wire according to claim 9.

11. A method for producing an automobile wire harness, comprising the steps of extrusion coating a conductor with the resin composition according to any one of claims 1 to 7 to provide a layer of the resin composition, and irradiating the layer of the resin composition with an electron beam of 80 to 250 kGy.

Citation Information

Patent Citations

  • Heat-resistant resin composition, and wiring material, cable and molded body including heat-resistant resin composition

    JP2014009238A

  • Insulative resin composition and insulated wire

    JP2018012817A

  • Resin composition, coated electric wire, and wire harness

    JP2020105319A

  • Transition piece, combustor, and gas turbine engine

    JP2023050983A

  • Thermoplastic elastomer composition and method for producing the same

    JP2004035618A