Thermoplastic polyester elastomer resin composition

The thermoplastic polyester elastomer resin composition, combining polyester-polycarbonate and olefin elastomers, addresses the shortcomings of conventional materials by enhancing acid, heat aging, and copper damage resistance, making it suitable for automotive cable coatings in electric vehicles.

WO2024202826A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO MC CORP

Patent Information

Application Number
PCT/JP2024/007088
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-02-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional polyester-polycarbonate type elastomers lack sufficient acid resistance, heat aging resistance, and copper damage resistance, making them unsuitable for use as materials for covering automotive cables, particularly in the context of electric vehicles where exposure to battery fluids and high temperatures is a concern.

Method used

A thermoplastic polyester elastomer resin composition is developed, combining a polyester-polycarbonate type thermoplastic polyester elastomer with an olefin elastomer that does not contain residual double bonds, along with an acid terminal blocking agent, to enhance acid resistance, heat aging resistance, and copper damage resistance.

Benefits of technology

The composition achieves excellent acid resistance, heat aging resistance, and copper damage resistance, making it suitable for use in automotive cable coatings, with improved flexibility and moldability, thus addressing the limitations of previous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present invention provides a thermoplastic polyester elastomer resin composition that has high acid resistance, heat aging resistance, copper damage resistance, and softness, and that is suitable for automotive components, particularly for an on-vehicle cable coating material. Provided is a resin composition comprising a thermoplastic polyester elastomer (A) and an olefin-based elastomer (B), wherein: (A) is obtained by bonding a hard segment and a soft segment; the hard segment comprises a polyester which has, as constituent components thereof, an aromatic dicarboxylic acid and an aliphatic or alicyclic diol; the soft segment contains aliphatic polycarbonate; (B) has an aromatic vinyl-based polymer block and a C3-20 alkene as monomer components and does not contain conjugated diene as a monomer component; the content of (A) in the thermoplastic polyester elastomer resin composition is 50-95 mass%; the content of (B) is 5-50 mass%; and the thermoplastic polyester elastomer resin composition contains 0-5 parts by mass of a carbodiimide compound or an epoxy compound as an acid terminal sealing agent (C), with respect to 100 parts by mass of the total of (A) and (B).
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic polyester elastomer resin composition

[0001] The present invention relates to a thermoplastic polyester elastomer resin composition useful as a coating material for automotive parts, particularly for in-vehicle cables, and particularly to a thermoplastic polyester elastomer resin composition excellent in acid resistance, heat aging resistance, copper damage resistance, and flexibility.

[0002] Thermoplastic polyester elastomers have been known as molding materials for automobile parts, which are obtained by bonding together a hard segment made of a crystalline polyester such as polybutylene terephthalate (PBT) or polybutylene naphthalate (PBN) and a soft segment made of a polyoxyalkylene glycol such as polytetramethylene glycol (PTMG) and / or a polyester such as polycaprolactone (PCL) or polybutylene adipate (PBA) (see Patent Documents 1 and 2).

[0003] However, polyester-polyether type elastomers using polyoxyalkylene glycols in the soft segment are known to have excellent water resistance and low-temperature properties but poor heat aging resistance, while polyester-polyester type elastomers using polyesters in the soft segment are known to have excellent heat aging resistance but poor water resistance and low-temperature properties.

[0004] To solve these problems, polyester-polycarbonate elastomers using polycarbonate in the soft segment have been proposed (see Patent Documents 3 to 8). These polyester-polycarbonate elastomers have excellent heat aging resistance and are therefore used in applications such as automobile engine peripheral components.

[0005] In the automotive industry, electric vehicles are expected to replace conventional gasoline-powered vehicles in the future. Due to their high heat aging resistance and flexibility, polyester-polycarbonate elastomers are expected to be used as next-generation in-vehicle cable coating materials for electric vehicles. To be used in this application, they must pass a battery fluid (sulfuric acid) drop test. However, conventional polyester-polycarbonate elastomers have not been able to pass this test.

[0006] Therefore, it has been proposed to improve acid resistance by blending inorganic fillers or olefin-based elastomers with polyester-polycarbonate elastomers (see Patent Documents 9 and 10). Although these methods can improve acid resistance to some extent, the heat aging resistance and copper damage resistance (heat aging resistance in contact with a copper plate) are insufficient, and there is still room for improvement before the materials can be put to practical use as coating materials for in-vehicle cables.

[0007] JP 10-017657 JP 2003-192778 JP 07-039480 JP 05-295049 JP 06-306202 JP 10-182782, JP 2001-206939, JP 2001-240663, JP 2022-150988, WO 2022 / 202629

[0008] The present invention has been made in view of the current state of the prior art, and an object of the present invention is to provide a thermoplastic polyester elastomer resin composition that combines high acid resistance, heat aging resistance, copper damage resistance, and flexibility, and is suitable for use as a coating material for automotive parts, particularly for in-vehicle cables.

[0009] As a result of extensive research to achieve the above object, the present inventors have found that by using an olefin elastomer having a specific structure that does not have any residual double bonds in the molecule as the olefin elastomer to be blended with a thermoplastic polyester-polycarbonate type elastomer, it is possible to sufficiently improve not only acid resistance but also heat aging resistance, copper damage resistance and flexibility, and have completed the present invention.

[0010] That is, the present invention has the following configurations (1) to (9): (1) A thermoplastic polyester elastomer resin composition containing a thermoplastic polyester elastomer (A) and an olefin-based elastomer (B), wherein the thermoplastic polyester elastomer (A) is formed by bonding hard segments and soft segments, the hard segments are made of a polyester having an aromatic dicarboxylic acid and an aliphatic or alicyclic diol as constituent components, the soft segments contain an aliphatic polycarbonate, and the olefin-based elastomer (B) is made of an aromatic vinyl polymer block and an alkene having 3 to 20 carbon atoms as monomer components, and a conjugated diene (2) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the olefin elastomer (B) is a copolymer of an aromatic vinyl polymer block and isobutene. (3) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the erosion depth of the thermoplastic polyester elastomer resin composition measured in accordance with an acid resistance test method is 1.2 mm or less. (4) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the elongation at break of the thermoplastic polyester elastomer resin composition measured in accordance with a heat aging resistance test method is 100% or more. (5) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the elongation at break of the thermoplastic polyester elastomer resin composition measured in accordance with a copper damage resistance test method is 100% or more.(6) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the thermoplastic polyester elastomer resin composition has a hardness of D25 to D55 as measured in accordance with the hardness testing method for thermoplastics specified in ASTM D 2240. (7) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the thermoplastic polyester elastomer (A) has a melting point of 150 to 225°C, and the melting point difference (Tm1 - Tm3) between the melting point (Tm1) of the thermoplastic polyester elastomer (A) measured at the first temperature decrease and the melting point (Tm3) of the thermoplastic polyester elastomer (A) measured at the third temperature decrease in a procedure using a differential scanning calorimeter, which involves heating the thermoplastic polyester elastomer (A) from room temperature to 300°C at a heating rate of 20°C / min, holding the thermoplastic polyester elastomer (A) at 300°C for 3 minutes, and then cooling the thermoplastic polyester elastomer (A) to room temperature at a heating rate of 100°C / min, is repeated three times, is 0 to 50°C. (8) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the thermoplastic polyester elastomer resin composition is for extrusion molding. (9) The thermoplastic polyester elastomer resin composition according to (1), characterized in that the thermoplastic polyester elastomer resin composition is for cable coating.

[0011] According to the present invention, a thermoplastic polyester elastomer resin composition having excellent acid resistance, heat aging resistance, copper damage resistance, and flexibility can be provided. Because the thermoplastic polyester elastomer resin composition of the present invention has the above-mentioned properties, it can be suitably used as a coating material for automotive parts, particularly for in-vehicle cable coatings.

[0012] The thermoplastic polyester elastomer resin composition of the present invention will be described in detail below. In this specification, the notation "A to B" means the upper and lower limits of a range (i.e., A or more and B or less). When no unit is specified for A and only a unit is specified for B, the unit for A and the unit for B are the same.

[0013] The thermoplastic polyester elastomer resin composition of the present invention contains a polyester-polycarbonate type thermoplastic polyester elastomer (A) and an olefin elastomer (B), and optionally also contains an acid end-capping agent (C). By using an olefin elastomer (B) with a specific structure that has no residual double bonds in the molecule, the thermoplastic polyester elastomer resin composition has excellent acid resistance, heat aging resistance, and copper damage resistance. Each of the components of the thermoplastic polyester elastomer resin composition of the present invention will be described below in order.

[0014] <Thermoplastic Polyester Elastomer (A)> The thermoplastic polyester elastomer (A) is formed by bonding hard segments and soft segments. The hard segments are composed of a polyester containing an aromatic dicarboxylic acid and an aliphatic or alicyclic diol as constituent components. The soft segments include an aliphatic polycarbonate. In this specification, the phrase "bonded" between a hard segment and a soft segment refers to both a state in which the hard segment and the soft segment are bonded together via a chain extender such as an isocyanate compound, and a state in which the constituent units of the hard segment and the soft segment are directly bonded together via an ester bond and / or a carbonate bond. Of these, it is preferable that the constituent units of the hard segment and the soft segment are directly bonded together via an ester bond and / or a carbonate bond.

[0015] (Hard Segment) As described above, the hard segment is composed of a polyester containing an aromatic dicarboxylic acid and an aliphatic or alicyclic diol as constituent components. A wide variety of conventionally known aromatic dicarboxylic acids can be used as the aromatic dicarboxylic acid constituting the polyester of the hard segment. Examples of the aromatic dicarboxylic acid include terephthalic acid and naphthalenedicarboxylic acid (2,6-naphthalenedicarboxylic acid is preferred among isomers). The content of these aromatic dicarboxylic acids is preferably 70 mol% or more, and more preferably 80 mol% or more, of the total dicarboxylic acids constituting the polyester of the hard segment. Other dicarboxylic acids include aromatic dicarboxylic acids such as diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and tetrahydrophthalic anhydride; and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. These dicarboxylic acids can be used in a range that does not significantly lower the melting point of the thermoplastic polyester elastomer (A). Specifically, the amount of these dicarboxylic acids is preferably 30 mol % or less, and more preferably 20 mol % or less, of the total dicarboxylic acids.

[0016] As the aliphatic or alicyclic diol constituting the polyester of the hard segment, a wide variety of conventionally known aliphatic or alicyclic diols can be used. As the aliphatic or alicyclic diol, alkylene glycols having 2 to 8 carbon atoms are preferred. Specific examples include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol. Of these, either ethylene glycol or 1,4-butanediol is preferred.

[0017] As the component constituting the polyester of the hard segment, a component comprising a constituent unit derived from butylene terephthalate (a constituent unit derived from terephthalic acid and 1,4-butanediol) or a constituent unit derived from butylene naphthalate (a constituent unit derived from 2,6-naphthalenedicarboxylic acid and 1,4-butanediol) is preferred from the viewpoints of physical properties, moldability, and cost performance.

[0018] The thermoplastic polyester elastomer (A) can be prepared by first preparing an aromatic polyester suitable as a polyester constituting the hard segment, and then copolymerizing it with the soft segment component described below. In this case, the aromatic polyester can be easily obtained according to a conventional polyester production method. The polyester constituting the hard segment preferably has a number average molecular weight of 10,000 to 40,000.

[0019] (Soft Segment) As described above, the soft segment contains an aliphatic polycarbonate. Therefore, the thermoplastic polyester elastomer (A) is a polyester-polycarbonate type elastomer. The aliphatic polycarbonate preferably contains structural units derived mainly from an aliphatic diol having 2 to 12 carbon atoms. Examples of these aliphatic diols include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,9-nonanediol, and 2-methyl-1,8-octanediol. In particular, from the viewpoint of imparting flexibility and low-temperature properties to the thermoplastic polyester elastomer (A), it is preferable that the aliphatic polycarbonate contains a structural unit derived from an aliphatic diol having 5 to 12 carbon atoms. These components may be used alone or in combination of two or more types as necessary, based on the examples described below.

[0020] The aliphatic polycarbonate diol used as a raw material for the aliphatic polycarbonate preferably has a low melting point (for example, 70°C or less) and a low glass transition temperature. For example, an aliphatic polycarbonate diol composed of structural units derived from 1,6-hexanediol is preferred because it has a low glass transition temperature of around -60°C and a melting point of around 50°C, resulting in good low-temperature properties. Furthermore, an aliphatic polycarbonate diol obtained by copolymerizing an appropriate amount of, for example, 3-methyl-1,5-pentanediol with the aliphatic polycarbonate diol has a slightly higher glass transition temperature than the aliphatic polycarbonate diol before copolymerization, but is preferred because it has a lower melting point or becomes amorphous and has good low-temperature properties. Furthermore, for example, an aliphatic polycarbonate diol made of 1,9-nonanediol and 2-methyl-1,8-octanediol is preferable because it has a melting point of about 30° C. and a glass transition temperature of about −70° C., which are sufficiently low, and therefore has particularly good low-temperature properties.

[0021] The aliphatic polycarbonate is not necessarily limited to being composed solely of a polycarbonate component, and may also contain small amounts of other glycols, dicarboxylic acids, ester compounds, or ether compounds. Examples of such copolymerization components include glycols such as dimer diol, hydrogenated dimer diol, and modified products thereof; dicarboxylic acids such as dimer acid and hydrogenated dimer acid; polyesters or oligoesters composed of aliphatic, aromatic, or alicyclic dicarboxylic acids and glycols; polyesters or oligoesters composed of ε-caprolactone; polyalkylene glycols or oligoalkylene glycols such as polytetramethylene glycol and polyoxyethylene glycol. Meanwhile, the soft segment is also preferably composed of an aliphatic polycarbonate.

[0022] The copolymerization component can be contained to an extent that does not substantially eliminate the effect of the aliphatic polycarbonate segment. In the thermoplastic polyester elastomer (A), the mass ratio of the hard segment to the soft segment (hard segment:soft segment) is preferably 30:70 to 95:5, more preferably 40:60 to 90:10, even more preferably 45:55 to 90:10, and most preferably 50:50 to 90:10.

[0023] Generally, in thermoplastic polyester elastomers, the higher the hard segment ratio, the better the acid resistance. On the other hand, the higher the hard segment ratio, the higher the hardness, which tends to impair flexibility and low-temperature properties. Therefore, in the thermoplastic polyester elastomer (A), the mass ratio of the hard segment to the soft segment is preferably within the above-mentioned range.

[0024] The thermoplastic polyester elastomer (A) can be produced by a known method, for example, by selecting an appropriate method from among a method comprising transesterifying a lower alcohol diester of a dicarboxylic acid, an excess amount of a low-molecular-weight glycol, and a soft segment component in the presence of a catalyst to obtain a reaction product, followed by polycondensation of the resulting reaction product, a method comprising esterifying a dicarboxylic acid, an excess amount of a glycol, and a soft segment component in the presence of a catalyst to obtain a reaction product, followed by polycondensation of the resulting reaction product, a method comprising preparing a hard segment polyester in advance, adding a soft segment component to the polyester, and randomizing the polyester through a transesterification reaction, a method comprising linking hard segments and soft segments with a chain linking agent, and a method comprising adding an ε-caprolactone monomer to a hard segment when poly(ε-caprolactone) is used for the soft segment.

[0025] The thermoplastic polyester elastomer (A) preferably has a melting point of 150 to 225°C, more preferably 190 to 220°C. If the melting point is below the lower limit, the thermoplastic polyester elastomer (A) may melt at high temperatures, limiting its use in high-temperature environments. If the melting point is above the upper limit, the molding temperature may be excessively high, which may lead to decomposition of the soft segment during molding, making it difficult to achieve the desired heat aging resistance.

[0026] The melting point (Tm) of the thermoplastic polyester elastomer (A) can be determined by the following method. That is, the thermoplastic polyester elastomer (A) is dried under reduced pressure at 50°C for 15 hours, and then measured using a differential scanning calorimeter DSC-50 (Shimadzu Corporation) at a temperature increase rate of 20°C / min from room temperature. The melting point (Tm) of the thermoplastic polyester elastomer (A) can be determined from the peak temperature of the endothermic heat generated by melting. A sample for measuring the melting point of the thermoplastic polyester elastomer (A) is prepared by weighing 10 mg into an aluminum pan (TA Instruments, product number 900793.901) and sealing it with an aluminum lid (TA Instruments, product number 900794.901). The melting point is measured under an argon atmosphere.

[0027] Furthermore, when a differential scanning calorimeter is used to perform three cycles of increasing the temperature from room temperature to 300°C at a rate of 20°C / min, holding at 300°C for three minutes, and then decreasing the temperature to room temperature at a rate of 100°C / min, the melting point (Tm1) of the thermoplastic polyester elastomer (A) measured at the time of the first temperature decrease and the melting point (Tm3) of the thermoplastic polyester elastomer (A) measured at the time of the third temperature decrease in the above operation, the melting point difference (Tm1-Tm3) is preferably 0 to 50°C. The melting point difference (Tm1-Tm3) is more preferably 0 to 40°C, and even more preferably 0 to 30°C.

[0028] The melting point difference is a measure of the ability of the thermoplastic polyester elastomer (A) to retain block properties. The smaller the melting point difference, the better the thermoplastic polyester elastomer (A) can be evaluated as having retained block properties. When the melting point difference of the thermoplastic polyester elastomer (A) is within the above range, molded articles with excellent quality uniformity can be obtained due to the excellent ability to retain block properties. When the melting point difference exceeds the above range, the ability to retain block properties deteriorates, and quality fluctuations during molding processing increase, which may deteriorate the quality uniformity and recyclability of molded articles.

[0029] Specifically, the melting point difference (Tm1 - Tm3) of the thermoplastic polyester elastomer (A) can be determined by the following method. First, 10 mg of the thermoplastic polyester elastomer (A) dried under reduced pressure at 50°C for 15 hours is weighed into an aluminum pan (manufactured by TA Instruments, product number 900793.901), and the pan is sealed with an aluminum lid (manufactured by TA Instruments, product number 900794.901) to prepare a measurement sample. Next, the aluminum pan containing the sealed measurement sample is heated from room temperature to 300°C at a heating rate of 20°C / min under a nitrogen atmosphere using a differential scanning calorimeter DSC-50 (manufactured by Shimadzu Corporation), and held at 300°C for 3 minutes. Thereafter, the aluminum pan is immersed in liquid nitrogen for rapid cooling, and the temperature is lowered to room temperature at a cooling rate of 100°C / min. After leaving it at room temperature for 30 minutes, the temperature is again raised from room temperature to 300° C. at a heating rate of 20° C. / min using a differential scanning calorimeter DSC-50 (manufactured by Shimadzu Corporation). This cycle is repeated three times, and the melting point (Tm1) of the measurement sample (thermoplastic polyester elastomer (A)) measured at the first time the temperature is lowered to room temperature and the melting point (Tm3) of the measurement sample (thermoplastic polyester elastomer (A)) measured at the third time the temperature is lowered to room temperature are measured, whereby the melting point difference (Tm1−Tm3) can be determined.

[0030] <Olefin-based elastomer (B)> The thermoplastic polyester elastomer resin composition of the present invention further contains an olefin-based elastomer (B) in addition to the thermoplastic polyester elastomer (A) described above. By containing the olefin-based elastomer (B), acid resistance of the non-polar resin can be imparted, and therefore the acid resistance of the thermoplastic polyester elastomer resin composition can be improved.

[0031] The olefin elastomer (B) has an aromatic vinyl polymer block (hard segment) and a rubber block (soft segment). The aromatic vinyl polymer block serves to form physical crosslinks and serve as crosslinking points, while the rubber block serves to impart elasticity.

[0032] The aromatic vinyl compound forming the aromatic vinyl polymer block (hard segment) is not particularly limited, and examples thereof include styrene, o-, m-, or p-methylstyrene, α-methylstyrene, β-methylstyrene, 2,6-dimethylstyrene, 2,4-dimethylstyrene, α-methyl-o-methylstyrene, α-methyl-m-methylstyrene, α-methyl-p-methylstyrene, β-methyl-o-methylstyrene, β-methyl-m-methylstyrene, β-methyl-p-methylstyrene, 2,4,6-trimethylstyrene, α-methyl-2,6-dimethylstyrene, α-methyl-2,4-dimethylstyrene, β-methyl-2,6-dimethylstyrene, β-methyl-2,4-dimethylstyrene, o-, m-, or p-chlorostyrene, 2 Examples of suitable chlorostyrenes include 2,4-dichlorostyrene, α-chloro-o-chlorostyrene, α-chloro-m-chlorostyrene, α-chloro-p-chlorostyrene, β-chloro-o-chlorostyrene, β-chloro-m-chlorostyrene, β-chloro-p-chlorostyrene, 2,4,6-trichlorostyrene, α-chloro-2,6-dichlorostyrene, α-chloro-2,4-dichlorostyrene, β-chloro-2,6-dichlorostyrene, β-chloro-2,4-dichlorostyrene, o-, m-, or p-t-butylstyrene, o-, m-, or p-methoxystyrene, o-, m-, or p-chloromethylstyrene, o-, m-, or p-bromomethylstyrene, styrene derivatives substituted with silyl groups, indene, and vinylnaphthalene. These may be used alone or in combination of two or more. Among these, styrene, α-methylstyrene, or a mixture thereof is preferred from the viewpoint of compatibility with the thermoplastic elastomer.

[0033] The rubber block (soft segment) must be an α-olefin that does not contain a conjugated diene as a monomer component, and the α-olefin must be an alkene having 3 to 20 carbon atoms. Specific examples of alkenes having 3 to 20 carbon atoms include propylene, isobutene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, Examples of the olefins include 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, and combinations thereof. These may be used alone or in combination of two or more. Among these, isobutene is preferred from the viewpoints of acid resistance, heat aging resistance, and copper damage resistance.

[0034] Specifically, as the olefin-based elastomer (B) composed of these aromatic vinyl polymer blocks and rubber blocks, styrene-isobutylene-styrene block copolymers (SIBS) are preferred from the viewpoints of heat aging resistance, copper damage resistance, and acid resistance. The styrene block content in these styrene-based elastomers is preferably 10% by mass or more from the viewpoint of extrusion moldability. The styrene block has a skeleton similar to the component consisting of an aromatic dicarboxylic acid and an aliphatic or alicyclic diol, which constitutes the hard segment of the thermoplastic polyester elastomer (A). Therefore, the greater the amount of styrene block, the better the compatibility with the thermoplastic polyester elastomer (A) and the better the extrusion moldability. Furthermore, from the viewpoint of flexibility, the upper limit of the styrene block content is preferably 60% by mass or less, and more preferably 40% by mass or less. Styrene-isobutylene-styrene block copolymers (SIBS) can be easily synthesized, for example, by referring to JP-A No. 2003-12887. Styrene-isobutylene-styrene block copolymers (SIBS) are also available as commercial products, such as "SIBSTAR 102T," "SIBSTAR 103T," and "SIBSTAR 062T" manufactured by Kaneka Corporation.

[0035] The olefinic elastomer (B) used in the present invention does not contain a conjugated diene as a monomer component and therefore does not have residual double bonds in the molecule. Generally, double bonds are a point of attack for oxygen, which accelerates heat aging, and are a factor in causing molecular weight reduction. Therefore, olefinic elastomers containing a conjugated diene as a monomer component, such as butylene-based olefinic elastomers, are hydrogenated to remove remaining double bonds in the segments and improve heat aging resistance. However, hydrogenation alone cannot completely remove double bonds, and some double bonds remain in the segments. Therefore, butylene-based olefinic elastomers such as those disclosed in Patent Documents 9 and 10 have a significant number of residual double bonds in the molecule. In contrast, the olefinic elastomer (B) used in the present invention does not contain a conjugated diene as a monomer component and inherently does not have residual double bonds in the molecule, as described above. Therefore, it is believed that the olefinic elastomer (B) not only has excellent acid resistance, but also excellent heat aging resistance and copper damage resistance (heat aging resistance when in contact with a copper plate).

[0036] The olefinic elastomer (B) may be either an unmodified olefinic elastomer or an acid-modified olefinic elastomer, but the unmodified olefinic elastomer is preferred because it can suppress reaction with the acid end-capping agent. When an acid-modified olefinic elastomer (B) is blended, a reaction between the acid end-capping agent and the acid-modified portion of the olefinic elastomer (B) or between the acid end-capping agent and the acid terminal of the thermoplastic polyester elastomer (A) may occur in a complex manner, which may cause an extreme increase in viscosity and gelation, and may result in a deterioration in the appearance of the extrusion-molded product.

[0037] From the viewpoint of improving acid resistance, it is more preferable that the olefinic elastomer (B) has a high melt flow rate (MFR) (low viscosity). Specifically, the MFR of the olefinic elastomer (B) is preferably 0.05 g / 10 min or more. If the MFR is below the lower limit, the olefinic elastomer (B) domains are less susceptible to shear during extrusion and are present as spheres in the matrix. As a result, the bypass effect obtained from the effective surface area and morphology of the olefinic elastomer (B), which exerts acid resistance, is reduced, which may lead to a deterioration in acid resistance. Furthermore, poor dispersibility and spherical domains may cause surface roughness during extrusion. The MFR of the olefinic elastomer (B) is more preferably 0.5 g / 10 min or more, and even more preferably 5 g / 10 min or more. The MFR of the olefinic elastomer (B) is preferably 15 g / 10 min or less. The MFR of the olefinic elastomer (B) is a value measured at a temperature of 230° C. and a load of 2.16 kg.

[0038] The thermoplastic polyester elastomer (A) and the olefin-based elastomer (B) in the thermoplastic polyester elastomer resin composition of the present invention are blended in a ratio of 50 to 95 mass% of the thermoplastic polyester elastomer (A) and 5 to 50 mass% of the olefin-based elastomer (B). That is, when the total of the thermoplastic polyester elastomer (A) and the olefin-based elastomer (B) is taken as 100 parts by mass, the mass ratio (A / B) of the thermoplastic polyester elastomer (A) to the olefin-based elastomer (B) is 95 / 5 to 50 / 50. The mass ratio (A / B) is preferably 90 / 10 to 50 / 50, more preferably 80 / 20 to 50 / 50, and even more preferably 70 / 30 to 50 / 50. If the amount of the olefinic elastomer (B) added is less than the above lower limit, acid resistance may be insufficient, whereas if the amount of the olefinic elastomer (B) added is more than the above upper limit, poor dispersion may occur, which may result in insufficient heat aging resistance, copper damage resistance, and extrusion moldability of the resin composition.

[0039] <Acid End-Capping Agent (C)> The thermoplastic polyester elastomer resin composition of the present invention may further contain an acid end-capping agent (C) if desired to improve hydrolysis resistance and flex fatigue resistance through chain extension. As the acid end-capping agent (C), any compound having a functional group (such as a carboxyl group, an acid anhydride group, an epoxy group, a hydroxyl group, a carbodiimide group, or an oxazoline group) capable of reacting with the terminal functional groups (carboxyl groups and / or hydroxyl groups) of the thermoplastic polyester elastomer (A) can be used. However, in view of changes in melt viscosity during melt retention and reactivity with the acid terminal functional groups of the thermoplastic polyester elastomer (A), it is preferred in the present invention to use an epoxy compound or a carbodiimide compound.

[0040] When the thermoplastic polyester elastomer resin composition of the present invention contains an acid end-capping agent (C), the content ratio thereof is up to 5 parts by mass, preferably up to 4 parts by mass, per 100 parts by mass of the total of the thermoplastic polyester elastomer (A) and the olefin-based elastomer (B). If the content ratio of the acid end-capping agent (C) exceeds the above upper limit, deterioration of flame retardancy and deterioration of mechanical properties due to foreign matter effects may occur. Note that when a high-molecular-weight thermoplastic polyester elastomer (A) that does not require chain extension or a thermoplastic polyester elastomer (A) with a sufficiently low terminal acid value is used as the thermoplastic polyester elastomer (A), the acid end-capping agent (C) may not be added.

[0041] <Other Components> The thermoplastic polyester elastomer resin composition of the present invention may contain various additives as needed, provided that the effects of the present invention are not impaired. Examples of such additives include resins other than thermoplastic polyester elastomers, thickeners, antioxidants, light stabilizers, coloring pigments, inorganic and organic fillers, stabilizers such as coupling agents, tackiness improvers, quenchers, and metal deactivators, and flame retardants. The amounts of the various additives added can be appropriately selected within a range that does not impair the effects of the present invention, and the amounts used in molding conventional thermoplastic resins can be used. Meanwhile, the thermoplastic polyester elastomer resin composition of the present invention preferably contains the thermoplastic polyester elastomer (A) and the olefin-based elastomer (B) in total at 75% by mass or more, more preferably at 80% by mass or more, and even more preferably at 90% by mass or more.

[0042] The composition and composition ratio of the thermoplastic polyester elastomer resin composition of the present invention can be determined, for example, by dissolving a sample in a solvent such as deuterated chloroform and measuring the composition. 1 It can be calculated from the proton integral ratio of H-NMR.

[0043] <Method for producing thermoplastic polyester elastomer resin composition> The thermoplastic polyester elastomer resin composition of the present invention can be obtained by applying a conventionally known method for producing this type of thermoplastic polyester elastomer resin composition, as long as the specific thermoplastic polyester elastomer (A) and the specific olefin-based elastomer (B) are blended in the above-mentioned ratio. For example, the thermoplastic polyester elastomer resin composition of the present invention can be obtained by charging the thermoplastic polyester elastomer (A), the olefin-based elastomer (B), and, if necessary, other components such as additives, into a co-rotating twin-screw extruder or the like, kneading them, and then pelletizing them.

[0044] <Characteristics of Thermoplastic Polyester Elastomer Resin Composition> The thermoplastic polyester elastomer resin composition of the present invention has excellent acid resistance. Specifically, the corrosion depth of the thermoplastic polyester elastomer resin composition measured in accordance with the acid resistance test method can be 1.2 mm or less. Hereinafter, a method for measuring the corrosion depth of the thermoplastic polyester elastomer resin composition using the acid resistance test method will be described.

[0045] First, a 3 mm thick plate-shaped molded article is obtained from the thermoplastic polyester elastomer resin composition. Next, 50 μL of a 37% by mass aqueous sulfuric acid solution is dropped onto the surface of the molded article, followed by heat treatment at 90°C for 8 hours. Furthermore, 50 μL of a 37% by mass aqueous sulfuric acid solution is dropped again onto the same location on the surface of the molded article, followed by heat treatment at 90°C for 16 hours. This operation constitutes one cycle, and a total of two cycles are performed. After that, the molded article is cut so as to include the area of ​​erosion caused by dropping the sulfuric acid aqueous solution, to obtain a cross section of the molded article. Finally, the depth of the erosion formed on the cross section of the molded article can be measured to determine the erosion depth of the thermoplastic polyester elastomer resin composition.

[0046] The thermoplastic polyester elastomer resin composition of the present invention can achieve a corrosion depth of 1.2 mm or less, further 0.9 mm or less, further 0.8 mm or less, and further 0.7 mm or less. Since the corrosion depth of the thermoplastic polyester elastomer resin composition of the present invention is equal to or less than the above upper limit, it has excellent acid resistance in the above-mentioned battery fluid (sulfuric acid) dropping test.

[0047] The thermoplastic polyester elastomer resin composition of the present invention has excellent heat aging resistance. Specifically, the thermoplastic polyester elastomer resin composition can have a tensile elongation of 100% or more as measured in accordance with a heat aging resistance test method.

[0048] The thermoplastic polyester elastomer resin composition of the present invention can achieve a tensile elongation of 100% or more, and even 200% or more. Since the tensile elongation of the thermoplastic polyester elastomer resin composition of the present invention is equal to or greater than the above-mentioned lower limit, it has excellent heat aging resistance in the above-mentioned heat aging resistance test.

[0049] The thermoplastic polyester elastomer resin composition of the present invention has excellent copper damage resistance. Specifically, the thermoplastic polyester elastomer resin composition can have a tensile elongation of 100% or more as measured in accordance with a copper damage resistance test method.

[0050] The thermoplastic polyester elastomer resin composition of the present invention can achieve a tensile elongation of 100% or more, and even 200% or more. Since the tensile elongation of the thermoplastic polyester elastomer resin composition of the present invention is equal to or greater than the lower limit, it has excellent copper damage resistance in the copper damage resistance test described above.

[0051] The thermoplastic polyester elastomer resin composition of the present invention has excellent flexibility, and the hardness of the thermoplastic polyester elastomer resin composition can be D25 to D55 as measured in accordance with the hardness testing method for thermoplastics specified in ASTM D 2240. In the present invention, the hardness of the thermoplastic polyester elastomer resin composition can be determined as follows in accordance with the hardness testing method for thermoplastics specified in ASTM D 2240.

[0052] First, a thermoplastic polyester elastomer resin composition is injected from an injection molding machine with a cylinder temperature set to 20°C above the melting point of the resin composition and a mold temperature set to 50°C to obtain an injection-molded product measuring 100 mm in length, 100 mm in width, and 2.0 mm in thickness. Next, a specified needle tip is dropped onto the injection-molded product, three of which are stacked in the thickness direction, in a 23°C environment, and the Shore D value at 15 seconds is read. The hardness of the thermoplastic polyester elastomer resin composition can be determined from the Shore D value at 15 seconds. The hardness refers to the so-called surface hardness.

[0053] The hardness of the thermoplastic polyester elastomer resin composition of the present invention is preferably D25 to D50, more preferably D25 to D45, and even more preferably D25 to D40. When the hardness is within the above range, the thermoplastic polyester elastomer resin composition of the present invention is particularly suitable for applications such as cable coating. When the hardness exceeds the above upper limit, the thermoplastic polyester elastomer resin composition may lack flexibility. On the other hand, when the hardness is below the above lower limit, the thermoplastic polyester elastomer resin composition may become excessively soft, making it impossible to ensure the strength of the molded product.

[0054] <Effects> As described above, the thermoplastic polyester elastomer resin composition of the present invention has excellent acid resistance, heat aging resistance, and copper damage resistance. Furthermore, it retains the inherent flexibility, moldability, chemical resistance, flex fatigue resistance, abrasion resistance, electrical properties, and other properties of thermoplastic polyester elastomers. Therefore, the thermoplastic polyester elastomer resin composition of the present invention can be used in a wide range of applications, including automotive parts, various parts for electrical appliances, hoses, tubes, and cable coating materials. Taking advantage of its excellent acid resistance, it is particularly suitable for use as a coating material for in-vehicle cables. The thermoplastic polyester elastomer resin composition of the present invention can be molded into various shapes by extrusion molding, injection molding, transfer molding, blow molding, and other methods.

[0055] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples. The measured values ​​described in the examples were measured by the following measurement methods.

[0056] <Hardness (Surface Hardness, Shore D)> The surface hardness of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example in an environment of 23°C was measured in accordance with the test method (Shore D) described in ASTM D 2240 as follows.

[0057] First, a thermoplastic polyester elastomer resin composition was injected from an injection molding machine with a cylinder temperature of 20°C above the melting point of the resin composition and a mold temperature of 50°C to obtain an injection-molded product measuring 100 mm in length, 100 mm in width, and 2.0 mm in thickness. Next, a predetermined needle tip was dropped onto the injection-molded product, three of which were stacked in the thickness direction, in an environment of 23°C, and the Shore D value at 15 seconds was read. The Shore D value at 15 seconds was taken as the hardness (surface hardness) of the resin composition. Note that surface hardness is an index of flexibility; the lower the surface hardness value, the better the flexibility.

[0058] <Acid Resistance (90° C. Dropping), That is, Measurement of Erosion Depth> In order to measure the erosion depth of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example, an acid resistance test was carried out as follows.

[0059] First, a 3 mm-thick flat molded article was obtained from the thermoplastic polyester elastomer resin composition. Next, 50 μL of a 37% by mass aqueous sulfuric acid solution was dropped onto the surface of the molded article, followed by heat treatment at 90°C for 8 hours. Furthermore, 50 μL of a 37% by mass aqueous sulfuric acid solution was dropped again onto the same location on the surface of the molded article, followed by heat treatment at 90°C for 16 hours. This operation constitutes one cycle, and a total of two cycles were performed. After that, the molded article was cut so as to include the erosion site caused by the dropping of the sulfuric acid aqueous solution, to obtain a cross section of the molded article. Finally, the depth (unit: mm) of the erosion formed on the cross section of the molded article was measured. If the erosion depth was a low value of 1.2 mm or less, the thermoplastic polyester elastomer resin composition could be evaluated as having excellent acid resistance.

[0060] <Heat Aging Resistance Test 1 (Measurement of Elongation at Break after Heat Treatment)> In order to evaluate the heat aging resistance of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example, the following elongation at break retention test was carried out.

[0061] (Preparation of Test Pieces) First, an injection-molded article having a length of 100 mm, a width of 100 mm, and a thickness of 2.0 mm was obtained by injecting a thermoplastic polyester elastomer resin composition from an injection molding machine with a cylinder temperature set to 20° C. higher than the melting point of the resin composition and a mold temperature set to 30° C. Next, a JIS No. 3 dumbbell shape was punched out of the injection-molded article along the flow direction to prepare a test piece.

[0062] (Dry heat treatment and measurement of elongation at break) The test piece was treated in a gear-type hot air dryer at 175°C for 240 hours. Thereafter, the absolute tensile elongation (elongation at break) of the test piece was measured in accordance with JIS K6251:2010.

[0063] <Heat Aging Resistance Test 2 (Checking for Cracks by Winding Test After Heat Treatment)> In order to evaluate the heat aging resistance of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example, a winding test was carried out after the following heat treatment to check for cracks.

[0064] (Preparation of Test Pieces) Test pieces (JIS No. 3 dumbbell shape) of the thermoplastic polyester elastomer compositions were prepared in the same manner as in the heat aging resistance test 1 above.

[0065] (Dry heat treatment, winding test) The test piece was treated in a gear-type hot air dryer at 175°C for 240 hours. After the test piece was sufficiently cooled, it was further cooled at -25°C for 5 hours or more, and while still cooled, it was wound around a mandrel in accordance with ASTM D 618, and the cross section of the test piece was observed for cracks. The observation results were evaluated according to the following criteria: A: No cracks were observed. B: Winding was possible, but slight cracks were observed. C: Winding was impossible, or numerous cracks were observed.

[0066] <Copper Damage Resistance Test 1 (Measurement of Elongation at Break after Heat Treatment)> In order to evaluate the copper damage resistance of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example, the following elongation at break test was carried out.

[0067] (Preparation of Test Pieces) First, an injection-molded article having a length of 100 mm, a width of 100 mm, and a thickness of 2.0 mm was obtained by injecting a thermoplastic polyester elastomer resin composition from an injection molding machine with a cylinder temperature set to 20° C. higher than the melting point of the resin composition and a mold temperature set to 30° C. Next, a JIS No. 3 dumbbell shape was punched out of the injection-molded article along the flow direction to prepare a test piece.

[0068] (Dry heat treatment and measurement of elongation at break) The above test specimen was placed on one side of a copper plate and treated in a gear-type hot air dryer at 175°C for 240 hours. Thereafter, the absolute tensile elongation (elongation at break) of the test specimen was measured in accordance with JIS K6251:2010.

[0069] <Copper Damage Resistance Test 2 (Checking for Cracks by Winding Test After Heat Treatment)> In order to evaluate the copper damage resistance of the thermoplastic polyester elastomer resin compositions of each Example and Comparative Example, a winding test was carried out after the following heat treatment to check for cracks.

[0070] (Preparation of Test Pieces) Test pieces (JIS No. 3 dumbbell shape) of the thermoplastic polyester elastomer compositions were prepared in the same manner as in the copper damage resistance test 1 above.

[0071] (Dry heat treatment, winding test) The above test piece was placed on one side of a copper plate and treated in a gear-type hot air dryer at 175°C for 240 hours. The test piece was then thoroughly cooled, and further cooled at -25°C for 5 hours or more. While still cooled, the test piece was wound around a mandrel in accordance with ASTM D 618, and the cross section of the test piece was observed for cracks. The observation results were evaluated according to the following criteria: A: No cracks were observed. B: Winding was possible, but slight cracks were observed. C: Winding was impossible, or numerous cracks were observed.

[0072] <Extrusion moldability> The pellets melt-kneaded in the twin-screw extruder were extruded again through a T-die in a single-screw extruder to produce a 0.2 mm thick sheet. The smoothness of the extrusion molded product was evaluated based on the sheet appearance using the following criteria: A: No roughness or foaming occurred, and the sheet appearance and surface smoothness were good. B: No sheet irregularities (melt fracture) or foaming occurred, but uniform roughness like embossing was present. C: Sheet irregularities (melt fracture) and foaming occurred, and the sheet appearance was poor.

[0073] <Melting Point (Tm) and Melting Point Difference (Tm1-Tm3)> The melting point (Tm) of the thermoplastic polyester elastomer (A) in each example and comparative example was determined by the following method. That is, the thermoplastic polyester elastomer (A) was dried under reduced pressure at 50°C for 15 hours and measured using a differential scanning calorimeter DSC-50 (Shimadzu Corporation) at a temperature increase rate of 20°C / min from room temperature, and the temperature at the peak of the endothermic heat due to melting was determined as the melting point (Tm) of the thermoplastic polyester elastomer (A). Here, a sample for measuring the melting point of the thermoplastic polyester elastomer (A) was prepared by weighing 10 mg into an aluminum pan (TA Instruments, product number 900793.901) and sealing it with an aluminum lid (TA Instruments, product number 900794.901). The melting point measurement was also performed under an argon atmosphere.

[0074] Furthermore, the melting point difference (Tm1-Tm3) of the thermoplastic polyester elastomer (A) was determined by the following method. First, 10 mg of the thermoplastic polyester elastomer (A) was dried under reduced pressure at 50°C for 15 hours and weighed into an aluminum pan (manufactured by TA Instruments, product number 900793.901). The pan was then sealed with an aluminum lid (manufactured by TA Instruments, product number 900794.901) to prepare a measurement sample. Next, the aluminum pan containing the sealed measurement sample was heated from room temperature to 300°C at a heating rate of 20°C / min under a nitrogen atmosphere using a differential scanning calorimeter DSC-50 (manufactured by Shimadzu Corporation), and held at 300°C for 3 minutes. Thereafter, the aluminum pan was immersed in liquid nitrogen for rapid cooling, and the temperature was lowered to room temperature at a cooling rate of 100°C / min. After leaving it at room temperature for 30 minutes, the temperature was again raised from room temperature to 300°C at a heating rate of 20°C / min using a differential scanning calorimeter DSC-50 (Shimadzu Corporation). This cycle was repeated three times, and the melting point difference (Tm1-Tm3) was calculated from the melting point (Tm1) measured when the temperature was lowered to room temperature the first time and the melting point (Tm3) measured when the temperature was lowered to room temperature the third time.

[0075] <Reduced Viscosity> 0.05 g of the resin was dissolved in 25 mL of a mixed solvent (phenol / tetrachloroethane=60 / 40 (mass ratio)), and the reduced viscosity was measured at 30° C. using an Ostwald viscometer.

[0076] <Terminal Acid Value> The terminal carboxyl group concentration (equivalent / 1×10) of the thermoplastic polyester elastomer (A) 6 g) was determined by dissolution titration in which 200 mg of a thoroughly dried sample (polyester elastomer) was dissolved in 10 mL of hot benzyl alcohol, the resulting solution was cooled, 10 mL of chloroform and phenol red were added, and the solution was titrated with a 1 / 25 N potassium alcohol solution (a solution of KOH in methanol) to determine the acid value (equivalent / 1 × 10 6 g) was calculated and used to calculate the terminal carboxyl group concentration (equivalents / 1×10 6 0.05 g of the resin was dissolved in 25 mL of a mixed solvent (phenol / tetrachloroethane=60 / 40 (mass ratio)), and the viscosity was measured at 30° C. using an Ostwald viscometer.

[0077] <Raw materials used in the examples and comparative examples> The following raw materials were used in the examples and comparative examples.

[0078] <Thermoplastic Polyester Elastomer (A)> (Thermoplastic Polyester Elastomer (A-1)) 100 parts by mass of an aliphatic polycarbonate diol (carbonate diol UH-CARB 200, molecular weight 2000, 1,6-hexanediol type, manufactured by Ube Industries, Ltd.) and 8.6 parts by mass of diphenyl carbonate were charged and reacted at a temperature of 205°C and 130 Pa. After 2 hours, the contents were cooled to obtain an aliphatic polycarbonate diol (number average molecular weight 10,000). 43 parts by mass of this aliphatic polycarbonate diol (PCD) and 57 parts by mass of polybutylene terephthalate (PBT) having a number average molecular weight of 30,000 were stirred at 230°C to 245°C under 130 Pa for 1 hour, and after confirming that the resin had become transparent, the contents were removed and cooled to obtain thermoplastic polyester elastomer (A-1). The melting point of this thermoplastic polyester elastomer (A-1) was 207°C, the melting point difference (Tm1-Tm3) was 25°C, the reduced viscosity was 1.21 dl / g, and the terminal acid value was 44 eq / ton. The composition and physical properties of the thermoplastic polyester elastomer (A-1) are shown in Table 1.

[0079] (Thermoplastic Polyester Elastomer (A-2)) 100 parts by mass of an aliphatic polycarbonate diol (carbonate diol UH-CARB 200 manufactured by Ube Industries, Ltd., molecular weight 2000, 1,6-hexanediol type) and 8.6 parts by mass of diphenyl carbonate were charged and reacted at a temperature of 205°C and 130 Pa. After 1 hour, the contents were cooled to obtain an aliphatic polycarbonate diol (number average molecular weight 5000). 43 parts by mass of this aliphatic polycarbonate diol (PCD) and 57 parts by mass of polybutylene terephthalate (PBT) having a number average molecular weight of 30,000 were stirred at 230°C to 245°C under 130 Pa for 1 hour, and after confirming that the resin had become transparent, the contents were removed. The removed pellets were heated at 170 to 180°C to carry out solid-state polycondensation, yielding a thermoplastic polyester elastomer (A-2). The melting point of this thermoplastic polyester elastomer (A-2) was 208°C, the melting point difference (Tm1 - Tm3) was 15°C, the reduced viscosity was 1.21 dl / g, and the terminal acid value was 7 eq / ton. The composition and physical properties of the thermoplastic polyester elastomer (A-2) are shown in Table 1.

[0080] (Thermoplastic Polyester Elastomer (A-3)) 100 parts by mass of an aliphatic polycarbonate diol (carbonate diol UH-CARB 200 manufactured by Ube Industries, Ltd., molecular weight 2000, 1,6-hexanediol type) and 8.6 parts by mass of diphenyl carbonate were charged and reacted at a temperature of 205°C and 130 Pa. After 2 hours, the contents were cooled to obtain an aliphatic polycarbonate diol (number average molecular weight 10,000). 30 parts by mass of this aliphatic polycarbonate diol (PCD) and 70 parts by mass of polybutylene terephthalate (PBT) having a number average molecular weight of 30,000 were stirred at 230°C to 245°C under 130 Pa for 1 hour, and after confirming that the resin had become transparent, the contents were removed and cooled to obtain thermoplastic polyester elastomer (A-3). The melting point of this thermoplastic polyester elastomer (A-3) was 212°C, the melting point difference (Tm1 - Tm3) was 18°C, the reduced viscosity was 1.20 dl / g, and the terminal acid value was 41 eq / ton. The composition and physical properties of the thermoplastic polyester elastomer (A-3) are shown in Table 1.

[0081] (Thermoplastic polyester elastomer (A-4)) Using the same method as above, a thermoplastic polyester elastomer (A-4) was obtained using terephthalic acid, 1,4-butanediol, and polyoxytetramethylene glycol (PTMG; number average molecular weight 1000) as constituent components, with a hard segment (polybutylene terephthalate) / soft segment (PTMG) ratio of 64 / 36 (mass %). The melting point of this thermoplastic polyester elastomer (A-4) was 203°C, the reduced viscosity was 1.75 dl / g, and the terminal acid value was 50 eq / ton. The composition and physical properties of the thermoplastic polyester elastomer (A-4) are shown in Table 1. Note that the thermoplastic polyester elastomer (A-4) is a polyether-type polyester elastomer for comparative examples, and does not contain an aliphatic polycarbonate as a soft segment.

[0082] (Polyester (A-5)) The following commercially available compound was prepared as polyester (A-5). Polybutylene terephthalate (PBT): 1100-211XG, manufactured by Changchun Group Co., Ltd. The MFR (235°C, 2.16 kg) of this PBT was 4 to 9 g / 10 min, melting point 223°C, reduced viscosity 1.23 to 1.30 dl / g, and terminal acid value 33 to 40 eq / ton. The composition and physical properties of polyester (A-5) are shown in Table 1.

[0083]

[0084] <Olefin-Based Elastomer (B)> The following commercially available compounds were prepared as the olefin-based elastomer (B): (B-1) Styrene-isobutylene-styrene block copolymer: Shibstar 102T, manufactured by Kaneka Corporation, styrene / isobutylene ratio = 15 / 85 (mass ratio), MFR (230°C, 2.16 kg) = 0.6 g / 10 min (B-2) Styrene-isobutylene-styrene block copolymer: Shibstar 103T, manufactured by Kaneka Corporation, styrene / isobutylene ratio = 30 / 70 (mass ratio), MFR (230°C, 2.16 kg) = 0.1 g / 10 min (B-3) Styrene-isobutylene-styrene block copolymer: Shibstar 062T, manufactured by Kaneka Corporation, styrene / isobutylene ratio = 23 / 77 (mass ratio), MFR (230°C, 2.16 kg) = 10 g / 10 min (B-4) Styrene-ethylene-butylene-styrene block copolymer: Tuftec H1052, manufactured by Asahi Kasei Corporation, styrene / ethylene-butylene ratio = 20 / 80 (mass ratio), MFR (230°C, 2.16 kg) = 13 g / 10 min. Note that (B-4) is an olefin-based elastomer for comparative examples containing a conjugated diene as a monomer component.

[0085] [Acid End-Capping Agent (C)] The following commercially available compounds were prepared as acid end-capping agents (C): (C-1) Alicyclic polycarbodiimide: Carbodilite HMV-15CA, manufactured by Nisshinbo Chemical Inc. (C-2) Bisphenol F-type diepoxy compound: Epicron 830, manufactured by DIC Corporation

[0086] <Preparation of Thermoplastic Polyester Elastomer Resin Compositions of Examples 1 to 10 and Comparative Examples 1 to 5> The above-mentioned thermoplastic polyester elastomer (A), olefin-based elastomer (B), and acid end-capping agent (C) were charged into a twin-screw extruder set at a cylinder temperature of 180 to 230°C in the combinations and ratios (parts by mass) shown in Table 2, and kneaded in the twin-screw extruder to obtain pellets of the thermoplastic polyester elastomer resin compositions of Examples 1 to 10 and Comparative Examples 1 to 5. The obtained pellets were used to perform the various evaluations described above. The results are shown in Table 2.

[0087]

[0088] <Discussion> Table 1 shows that the thermoplastic polyester elastomer resin compositions of Examples 1 to 10 all possess excellent flexibility (surface hardness), acid resistance, heat aging resistance, and copper damage resistance. Furthermore, a comparison of Examples 1 to 4 shows that flexibility and acid resistance improve as the amount of olefinic elastomer (B) added increases. A comparison of Examples 4 to 6 shows that Example 6, which uses a thermoplastic polyester elastomer (A-2) with a low terminal acid value, exhibits high heat aging resistance at the same level as Examples 4 and 5, which contain an acid terminal blocking agent (C), even without the addition of an acid terminal blocking agent (C). Furthermore, a comparison of Example 4 and Example 8 shows that no problems with heat aging resistance are observed, regardless of whether the acid terminal blocking agent (C) is an epoxy compound (Example 8) or a carbodiimide compound (Example 4). A comparison between Example 4 and Example 7 shows that increasing the hard segment content of the thermoplastic polyester elastomer (A) reduces flexibility, heat aging resistance, and the like, but further improves acid resistance. A comparison between Example 4 and Example 9 shows that in Example 9, the styrene content of the olefin elastomer (B-2) is high, which increases compatibility with the thermoplastic polyester elastomer (A) and improves extrusion moldability. A comparison between Example 4 and Example 10 shows that in Example 10, which uses an olefin elastomer (B-3) with a high MFR (low viscosity), heat aging resistance, copper damage resistance, and the like are reduced, but the domains are significantly affected by shear during extrusion, resulting in elongated rather than spherical domains, thereby improving acid resistance and extrusion moldability.

[0089] On the other hand, the thermoplastic polyester elastomer resin compositions of Comparative Examples 1 to 5 were inferior to those of the Examples in at least one of acid resistance, flexibility, heat aging resistance, copper damage resistance, and extrusion moldability. Specifically, Comparative Example 1, which did not contain the olefinic elastomer (B), was significantly inferior in flexibility and acid resistance. Comparative Example 2 was inferior in acid resistance and heat aging resistance because the soft segment of the thermoplastic polyester elastomer (A-4) was polyether. Comparative Example 3 contained an excessive amount of olefinic elastomer (B), resulting in poor dispersion and inferior heat aging resistance, copper damage resistance, and extrusion moldability. Comparative Example 4 was inferior in heat aging resistance and copper damage resistance because the olefinic elastomer (B-4) contained residual double bonds (unsaturated bonds). Comparative Example 5 was significantly inferior in flexibility, heat aging resistance, and copper damage resistance because a polyester resin (A-5) was used instead of the thermoplastic polyester elastomer (A).

[0090] The thermoplastic polyester elastomer resin composition of the present invention is excellent in acid resistance, heat aging resistance, copper damage resistance, and flexibility, and is therefore extremely useful as a coating material for automobile parts, particularly for in-vehicle cables.

Claims

1. A thermoplastic polyester elastomer resin composition containing a thermoplastic polyester elastomer (A) and an olefin-based elastomer (B), wherein the thermoplastic polyester elastomer (A) is formed by bonding hard segments and soft segments, the hard segments are made of a polyester having an aromatic dicarboxylic acid and an aliphatic or alicyclic diol as constituent components, the soft segments contain an aliphatic polycarbonate, and the olefin-based elastomer (B) is made of an aromatic vinyl polymer block and an alkene having 3 to 20 carbon atoms as monomer components, and a conjugated diene as monomer components. a content of the thermoplastic polyester elastomer (A) in the thermoplastic polyester elastomer resin composition being 50 to 95% by mass, a content of the olefin-based elastomer (B) in the thermoplastic polyester elastomer resin composition being 5 to 50% by mass, and the thermoplastic polyester elastomer resin composition further containing, as an acid end-blocking agent (C), 0 to 5 parts by mass of an epoxy compound or a carbodiimide compound per 100 parts by mass in total of the thermoplastic polyester elastomer (A) and the olefin-based elastomer (B).

2. The thermoplastic polyester elastomer resin composition according to claim 1, wherein the olefin elastomer (B) comprises a copolymer of an aromatic vinyl polymer block and isobutene.

3. The thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the corrosion depth of the thermoplastic polyester elastomer resin composition measured in accordance with an acid resistance test method is 1.2 mm or less.

4. A thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the elongation at break of the thermoplastic polyester elastomer resin composition measured in accordance with a heat aging resistance test method is 100% or more.

5. A thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the elongation at break of the thermoplastic polyester elastomer resin composition measured in accordance with the copper damage resistance test method is 100% or more.

6. The thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the hardness of the thermoplastic polyester elastomer resin composition measured in accordance with the hardness testing method for thermoplastics specified in ASTM D 2240 is D25 to D55.

7. The thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the thermoplastic polyester elastomer (A) has a melting point of 150 to 225°C, and the melting point difference (Tm1-Tm3) between the melting point (Tm1) of the thermoplastic polyester elastomer (A) measured at the first temperature drop in a differential scanning calorimeter-based operation in which the temperature is raised from room temperature to 300°C at a heating rate of 20°C / min, held at 300°C for 3 minutes, and then cooled to room temperature at a heating rate of 100°C / min, is repeated three times, and the melting point difference (Tm1-Tm3) between the melting point (Tm1) of the thermoplastic polyester elastomer (A) measured at the third temperature drop in the operation is 0 to 50°C.

8. The thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the thermoplastic polyester elastomer resin composition is for extrusion molding.

9. The thermoplastic polyester elastomer resin composition according to claim 1, characterized in that the thermoplastic polyester elastomer resin composition is for use in cable coating.

Citation Information

Patent Citations

  • Elastomer composition and molded article formed from the same

    JP2015164983A

  • Surface protective film

    JP2021014593A

  • Polyester elastomer resin composition and cable cover material comprising same

    WO2022202629A1

Cited By

  • Resin composition using biomass resource-derived polyester elastomer

    JP7913668B1