Etching method and etching device
A two-stage etching process using specific fluorine-containing gases addresses the challenge of selectively etching SiGe films on semiconductor wafers, reducing residue and surface roughness by controlling gas supply and pressure, enhancing etching selectivity and efficiency.
Patent Information
- Application Number
- PCT/JP2024/007682
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-03
AI Technical Summary
During the etching of silicon germanium films on semiconductor wafers, existing methods struggle to selectively etch the SiGe film without etching adjacent films, leading to residue and surface roughness issues.
The method involves a two-stage etching process using different fluorine-containing gases, where a first gas (e.g., F2) is supplied for an initial period, followed by a second gas (e.g., ClF3) for a shorter duration, under controlled pressure conditions to selectively etch the SiGe film while minimizing etching of adjacent Si films and semiconductor films.
This approach effectively reduces residue and surface roughness of the Si film, achieving high selectivity in etching the SiGe film while suppressing etching of adjacent Si and semiconductor films, thereby improving the etching process efficiency.
Smart Images

Figure JP2024007682_03102024_PF_FP_ABST
Abstract
Description
Etching method and etching apparatus
[0001] The present disclosure relates to an etching method and an etching apparatus.
[0002] In manufacturing a semiconductor device, a SiGe film formed on the surface of a semiconductor wafer (hereinafter referred to as a wafer) serving as a substrate may be etched. In Patent Document 1, a laminated film consisting of a Si film and a SiGe film is formed on a wafer, and when selectively etching the SiGe film of this laminated film, HF gas and ClF 3 Simultaneous gas supply is shown.
[0003] JP 2018-170380 A
[0004] The present disclosure provides a technique that, when etching a silicon germanium film, can reduce post-etching residues while suppressing etching of films adjacent to the silicon germanium film.
[0005] The etching method disclosed herein is a method for etching a silicon germanium film formed on a substrate, and includes: a first step of supplying a first etching gas, which is a fluorine-containing gas, to the substrate for a first period of time; and a second step of supplying, after the first step, a second etching gas, which is a fluorine-containing gas different from the first etching gas, to the substrate for a second period of time that is shorter than the first period of time.
[0006] The present disclosure makes it possible to reduce residues after etching a silicon germanium film while suppressing etching of films adjacent to the silicon germanium film.
[0007] FIG. 1 is a longitudinal sectional side view of a wafer subjected to an etching process according to an embodiment of the present disclosure. FIG. 2 is a chart showing a flow illustrating the etching process. FIG. 3 is a chart showing the timing of supply and shutdown of gas used in the etching process and changes in the pressure of a processing vessel. FIG. 4 is a longitudinal sectional side view of a wafer after the etching process. FIG. 5 is a longitudinal sectional side view of an apparatus according to an embodiment of the etching process. FIG. 6 is a graph showing the results of an evaluation test. FIG. 7 is an explanatory diagram showing images of chips on a substrate obtained in an evaluation test and various test results. FIG. 8 is a graph showing the results of an evaluation test. FIG. 9 is an explanatory diagram showing images of chips on a substrate obtained in an evaluation test and various test results. FIG. 10 is a longitudinal sectional side view of a substrate used in an evaluation test.
[0008] Before describing one embodiment of the etching method of the present disclosure, a film structure formed on a wafer W, which is a substrate to be etched, will be described. Fig. 1 is a longitudinal sectional front view of the film structure. In the figure, two mutually orthogonal directions in the surface direction of the wafer W are indicated as the X direction and the Y direction, and a direction in the thickness direction of the wafer W, which is orthogonal to both the X direction and the Y direction, is indicated as the Z direction. In the following description, it is assumed that the wafer W is placed horizontally, and the X direction will sometimes be referred to as the left-right direction, the Y direction as the front-rear direction, and the Z direction as the vertical direction.
[0009] A number of stacked layers 15 each composed of a Si (silicon) film 12, a SiGe (silicon germanium) film 13, and a porous film 14 are provided on an underlayer film 11 formed on a wafer W. The SiGe film 13 in the stacked layers 15 is the film to be etched. A plurality of stacked layers 15 are provided at intervals in the front-to-back and left-to-right directions, and are arranged in a matrix in plan view. The porous film 14 is, for example, an insulating film, and more specifically, a low-k film made of, for example, SiOC (carbon-doped silicon oxide), SiCOH, or SiOCN (a film composed of Si, oxygen, nitrogen, and carbon).
[0010] The structure of the stack 15 will now be described in further detail. Porous films 14 are formed adjacent to the left and right sides of the SiGe film 13. Therefore, the direction in which the SiGe film 13 and the Si film 12 are aligned intersects with the direction in which the SiGe film 13 and the porous film 14 are aligned. If the SiGe film 13 and the porous film 14 adjacent to it on the left and right are referred to as adjacent bodies, the stack 15 is formed by stacking multiple adjacent bodies and multiple Si films 12, with the adjacent bodies and the Si films 12 alternating in the vertical direction (Z direction). The upper end of the stack 15 is formed by the Si film 12, out of the adjacent bodies and the Si film 12. A semiconductor film 16 is provided between the stacks 15 aligned on the left and right, and the stack 15 and the semiconductor film 16 are adjacent to each other. The semiconductor film 16 is a film that forms the source or drain of a semiconductor product manufactured from the wafer W and is made of, for example, Si or SiGe.
[0011] An upper layer film 17 is provided on the stacked body 15 and the semiconductor film 16. A plurality of grooves 18 extending in the front-rear direction are formed in the upper layer film 17 at intervals from side to side, dividing the upper layer film 17 into left and right halves. Each groove 18 is positioned so as to overlap the SiGe film 13 in the vertical direction (Z direction). The lower side of the upper layer film 17 extends toward the space between the stacked bodies 15 arranged in the front-rear direction, thereby forming a recessed portion (not shown). A recessed portion 10 is formed, the sidewall of which is formed by the recessed portion and the Si film 12 and SiGe film 13 of the stacked body 15. This recessed portion 10 is connected to the groove 18. In other words, this recessed portion 10 is open between the upper layer films 17 in the left-right direction (X direction) and extends in the Z direction. Therefore, the Si film 12 and the SiGe film 13 are exposed on the surface of the wafer W as the sidewalls of the recessed portion 10 and are exposed to an etching gas supplied above the wafer W. The semiconductor film 16 is covered with the upper film 17 and is not exposed on the surface of the wafer W.
[0012] Although a detailed description of the structure is omitted, the upper layer 17 is made of silicon oxide (SiO 2The upper film 17 is resistant to an etching gas described later, and prevents the semiconductor film 16 from being etched from above by the etching gas.
[0013] The above-described film structure allows etching gas supplied above the wafer W to flow into the recess 10 through the groove 18 and etch the SiGe film 13 laterally. More specifically, the gas flowing into the recess 10 flows in the Y direction (the direction perpendicular to the plane of the drawing in FIG. 1 ) to etch the SiGe film 13 at each stage. The Si film 12 and the SiGe film 13 are adjacent to each other, but it is necessary to selectively etch the SiGe film 13 and minimize the roughness (surface roughness) of the Si film 12 after etching. Furthermore, it is also necessary to prevent any germanium (Ge) residues originating from the SiGe film 13 from remaining on the surface of the Si film 12 after etching.
[0014] Furthermore, the SiGe film 13 is adjacent to the semiconductor film 16 via the porous film 14, and even during etching of the SiGe film 13, the semiconductor film 16 is covered by the upper film 17 and the porous film 14 and is not exposed on the surface of the wafer W. However, during this etching, etching gas can pass through the holes in the porous film 14 and be supplied to the semiconductor film 16. It is also required to etch the SiGe film 13 in such a way that etching of the semiconductor film 16 is suppressed. The etching in this embodiment can meet these requirements.
[0015] The etching process of this embodiment will be specifically described below with reference to the flowchart of Fig. 2 and the timing chart of Fig. 3. This etching process is performed by supplying two types of fluorine-containing etching gases to a processing vessel in which a vacuum atmosphere is formed, with the wafer W described in Fig. 1 stored therein. The timing chart shows the timing of supplying and stopping the etching gases to and from the processing vessel, and the timing of changing the pressure in the processing vessel.
[0016] First, the wafer W described in FIG. 1 is loaded into a processing chamber. Then, the processing chamber is evacuated to form a vacuum atmosphere at a predetermined first pressure in the processing chamber. Then, a first etching gas, such as F 2 Fluorine gas is supplied into the processing chamber (time t1, step S1). This selectively etches the SiGe film 13 out of the Si film 12 and the SiGe film 13. When a preset first time elapses from time t1 and it becomes time t2, the fluorine gas is supplied into the processing chamber. 2 While the gas supply is stopped, a second etching gas, ClF 3 The supply of (chlorine trifluoride) gas into the processing vessel is started. Further, the exhaust flow rate in the processing vessel is adjusted to reduce the pressure in the processing vessel to a second pressure lower than the first pressure (step S2). 3 The gas removes the F remaining in the processing vessel. 2 Gas is purged from the process chamber, and the remaining portion of the SiGe film 13 is etched.
[0017] When a preset second time period has elapsed from time t2 and it becomes time t3, ClF 3 The supply of gas into the processing chamber is stopped. This second time (the time from time t2 to t3) is shorter than the first time (the time from time t1 to t2). FIG. 4 shows a longitudinal sectional front view of the wafer W after the etching process is completed. The supply of inert gas into the processing chamber prevents ClF 3 The gas is purged from the processing chamber, the etching process is completed, and the wafer W is unloaded from the processing chamber.
[0018] In this way, in the etching process of this embodiment, two-stage etching is performed by changing the type of gas. The reason for this is that when etching the SiGe film of a structure in which a Si film and a SiGe film are adjacent to each other, ClF 3 When gas is used, F 2 Compared with the case where ClF gas is used, adhesion of Ge residues to the Si film after etching and roughness of the Si film can be suppressed. 3The gas has a high etching ability for Si films, and Si films are easily etched. 3 When only gas is used, it is difficult to selectively etch the SiGe film.
[0019] Therefore, for the wafer W in FIG. 2 As will be shown in the evaluation test described later, 2 The Si film 12 is hardly etched by the gas. In other words, the SiGe film 13 can be etched with high selectivity relative to the Si film 12. 2 After the SiGe film 13 is mostly removed by the gas, ClF 3 The gas is supplied for a relatively short time, thereby suppressing etching of the Si film 12 and reducing the roughness of the Si film 12 and the amount of Ge residue adhering to the Si film 12.
[0020] By the way, ClF 3 As described above, the gas has a relatively high etching ability for Si films, but as will be shown in the evaluation test described later, it also has a relatively high etching ability for SiGe films. Therefore, although the semiconductor film 16 formed on the wafer W is made of Si or SiGe as described above, this ClF 3 However, the ClF gas in this embodiment has a high etching resistance. 3 Since the gas supply time is relatively short, the ClF 3 This prevents the gas from passing through the pores of the porous film 14 and being supplied to the semiconductor film 16. Therefore, etching of the semiconductor film 16 can also be prevented.
[0021] In addition, F 2 For the first pressure at the time t1 to t2 when the gas is supplied, ClF 3 The second pressure during the time period from t2 to t3 when the gas is supplied is low. 3 The gas is prevented from remaining in the processing chamber for a long time by maintaining the processing chamber at a relatively low pressure. Therefore, etching of the Si film 12 and the semiconductor film 16 is more reliably suppressed.2 The gas is kept at a relatively high pressure in the processing vessel, so that it remains in the processing vessel for a relatively long time and acts on the SiGe film 13. This prevents a decrease in the etching rate.
[0022] Next, an etching apparatus 2, which is an example of an etching apparatus capable of performing the etching process described with reference to Figures 2 and 3, will be described. Figure 5 is a longitudinal side view of the etching apparatus 2. In the figure, reference numeral 21 denotes the processing vessel described above, which constitutes the etching apparatus 2. In the figure, reference numeral 22 denotes a transfer port for the wafer W, which opens into the sidewall of the processing vessel 21 and is opened and closed by a gate valve 23. A stage 31 on which the wafer W is placed is provided within the processing vessel 21, and the stage 31 is provided with lift pins (not shown). The wafer W is transferred between the stage 31 and a substrate transfer mechanism located outside the processing vessel 21 via the lift pins.
[0023] A temperature adjustment unit 22 is embedded in the stage 31, and adjusts the temperature of the wafer W placed on the stage 31. This temperature adjustment unit 22 is configured as a flow path that forms part of a circulation path through which a temperature adjustment fluid, such as water, flows, and adjusts the temperature of the wafer W by heat exchange with the fluid. However, the temperature adjustment unit 22 is not limited to being a flow path for such a fluid, and may be configured as, for example, a heater for performing resistance heating.
[0024] One end of an exhaust pipe 24 opens into the processing vessel 21, and the other end of the exhaust pipe 24 is connected to an exhaust mechanism 26, which is, for example, a vacuum pump, via a valve 25, which is a pressure change mechanism. By adjusting the aperture of the valve 25, the exhaust flow rate in the processing vessel 21 is adjusted, and the pressure in the processing vessel 21 is set to a desired vacuum pressure. That is, as described above, switching between the first pressure and the second pressure can be performed by changing the aperture of the valve 25.
[0025] A shower plate 32 is provided at the upper side of the processing vessel 21, facing the stage 31. The shower plate 32 is connected to the downstream sides of gas supply paths 41 to 44, and the upstream sides of the gas supply paths 41 to 44 are connected to gas supply sources 51 to 54 via flow rate adjusters 40, respectively. Each flow rate adjuster 40 includes a valve and a mass flow controller. The supply of each gas to the downstream side from the gas supply sources 51 to 54 is stopped by opening and closing a valve included in the flow rate adjuster 40. The flow rate of each gas supplied to the downstream side is also adjusted by the flow rate adjuster 40. The gases supplied to the gas flow paths provided in the shower plate 32 are discharged downward from a number of discharge ports provided on the lower surface of the shower plate 32.
[0026] Gas supply sources 51, 52, 53, and 54 supply F 2 Gas, ClF 3 Gas, N 2 The N gas and Ar gas are supplied into the processing chamber 21 through the shower plate 32. The flow rate adjusting units 40 allow the supply of each gas independently. 2 The gas is used as a carrier gas during the etching process, and the etching gas (F 2 Gas and ClF 3 The Ar gas is supplied into the processing vessel 21 together with the etching gas through the shower plate 32. It is also supplied into the processing vessel after the supply of the etching gas has finished, and acts as a purge gas to purge the processing vessel. The Ar gas, which is an inert gas, is used to adjust the partial pressure of each etching gas, and is supplied into the processing vessel together with the etching gas. 2 A first gas supply unit is configured by a gas supply path 41 through which a gas flows, a flow rate adjusting unit 40 interposed in the gas supply path 41, and a shower plate 32. 3 A second gas supply unit is configured by a gas supply path 42 through which gas flows, a flow rate adjuster 40 interposed in the gas supply path 42, and the shower plate 32.
[0027] The etching apparatus 2 also includes a control unit 20, which is a computer, and the control unit 20 includes a program, a memory, and a CPU. The program contains instructions (steps) for processing the wafer W and transporting the wafer W as described above. The program is stored on a storage medium, such as a compact disc, a hard disk, a magneto-optical disc, or a DVD, and is installed in the control unit 20. The control unit 20 outputs control signals to each component of the etching apparatus 2 in accordance with the program, thereby controlling the operation of each component. Specifically, the operations of the etching apparatus 2 that are controlled in this manner include, for example, adjusting the temperature of the fluid supplied to the stage 31 (i.e., the processing temperature of the wafer W), supplying and stopping the gases from the shower plate 32, and adjusting the exhaust flow rate by the valve 25 (i.e., adjusting the pressure inside the processing chamber 21).
[0028] By adjusting the opening of the valve 25 of the etching device 2, the first pressure from time t1 to time t2 is set to, for example, 1.33 Pa (10 mTorr) to 133 Pa (1000 mTorr), and the second pressure from time t2 to time t3 is set to, for example, 0 Pa to 133 Pa. Also, the temperature adjustment unit 22 sets the temperature of the wafer W from time t1 to time t3 to, for example, -50°C to 150°C. The flow rates of the gases supplied into the processing chamber are set as follows: F 2 Gas: 1 to 500 sccm, ClF 3 Gas: 0.1 to 10 sccm, N 2 The gas is in the range of 50 to 1000 sccm, and the Ar gas is in the range of 10 to 1000 sccm.
[0029] Also, as mentioned above, F 2 Gas, ClF 3 Inert gas (N 2 The F gas and Ar gas are supplied into the processing chamber. 2 Gas, ClF 3 The relationship between the flow rate of the inert gas and the flow rate of the inert gas is, for example, ClF 3 Gas flow rate / inert gas flow rate F 2 The flow rate of gas / flow rate of inert gas is larger. 2 Gas, ClF 3When the gases are supplied to the wafer W, ClF 3 Gas is better than F 2 The flow rate of each gas may be adjusted so that the ClF ions are supplied to the Si film 12 and the semiconductor film 16 at a higher dilution rate with the inert gas than the ClF ions. 3 The etching action of the gas is more reliably suppressed.
[0030] F as the first etching gas 2 However, other fluorine-containing gases capable of selectively etching the SiGe film 13 relative to the Si film 12 may be used, such as F 2 Instead of gas, HF gas and F 2 Alternatively, a fluorine-containing gas having a relatively large etching effect on the SiGe film 13 may be used in combination with ClF 3 can be used as the second etching gas instead of the gas. For example, IF 7 (Iodine heptafluoride) gas and NF 3 Nitrogen trifluoride gas may be used as the second etching gas. Note that "containing fluorine" here means that fluorine is contained as a constituent component, not that fluorine is contained as an impurity.
[0031] In the processing example shown in the chart of FIG. 2 With the gas supply stopped, ClF 3 Gas is supplied and F 2 The gas is purged from the processing vessel 21 with ClF 3 It is done by gas, but F 2 From the time the gas supply is stopped, 3 There may be an interval until the gas supply is started. 2 The inert gas such as F 2 Gas may be purged. However, in order to shorten the processing time, as shown in FIG. 2 With the gas supply stopped, ClF 3 Gas is supplied and F 2 Gas purging with ClF 3 It is preferable to do this by gas.
[0032] As described above, the etching technique described in this embodiment suppresses the roughness of the Si film 12 adjacent to the SiGe film 13, and is therefore particularly effective when applied to a substrate in which the SiGe film 13 and the Si film 12 are adjacent to each other. However, since this etching technique can reduce the amount of Ge remaining after etching the SiGe film, it may also be used when etching the SiGe film 13 that is not adjacent to the Si film 12.
[0033] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive, and various omissions, substitutions, modifications, and combinations may be made in the above-described embodiments without departing from the scope and spirit of the appended claims.
[0034] [Evaluation Test 1] Each evaluation test performed in connection with the technology disclosed herein will be described. In Evaluation Test 1, multiple wafers W each having two chips fixed to their surfaces were prepared. Then, using the etching apparatus 2 described in the embodiment, processing was performed by changing the type of etching gas and the etching time for each wafer W. One of the two chips had a SiGe film stacked as an upper layer on top of a Si film as an underlayer. This SiGe film had a thickness of 50 nm and a Ge content of 25%. The other chip had a polysilicon film. After etching, the chips with the SiGe film were subjected to measurement of the amount of Ge using XPS (X-ray photoelectron spectroscopy), measurement of the root-mean-square roughness (RMS) using an AFM (atomic force microscope), image acquisition using a SEM (scanning electron microscope), and measurement of the etching amount of the SiGe film. The etching amount of the polysilicon film chips was also measured.
[0035] As an etching gas, F 2 Gas, ClF 3 Gas, F 2 Gas and ClF 3 The gases were supplied to the wafer W to perform etching. 2 Gas, ClF 3 Gas, F 2 Gas and ClF 3The tests using gases are referred to as evaluation tests 1-1, 1-2, and 1-3, respectively. 2 Gas, ClF 3 The gases were supplied simultaneously with the same supply start and end timings. In each of Evaluation Tests 1-1 to 1-3, the etching gas supply time (etching time) was changed for each wafer W. In performing the etching, the temperature of the wafer W, the pressure inside the processing vessel 21, and the flow rate of each gas supplied into the processing vessel were set to values within the ranges shown in the embodiment.
[0036] In describing the test results, the etching time set so that the etching depth of the SiGe film of the chip is 50 nm, the same as the thickness of the SiGe film (i.e., the SiGe film is just removed), is sometimes referred to as the time for performing JE (just etching). The time for further extending the etching time to etch the 50 nm SiGe film may sometimes be referred to as the time for performing OE (over etching). Specifically, assuming that the thicknesses of the SiGe film of the chip are 100 nm, 150 nm, 300 nm, and 550 nm, the time for the etching depth of the SiGe film to be equal to the thickness of the SiGe film is represented as the time for performing 100%, 200%, 500%, and 1000% OE, respectively. The time for each OE was calculated based on the relationship between the etching depth of a SiGe film of 50 nm or less and the etching time corresponding to this etching depth (see the graph in FIG. 6).
[0037] Figure 7 shows the SEM images, Ge detection amount, RMS, and polysilicon film etching amount obtained during the JE and OE processes for each of Evaluation Tests 1-1 to 1-3. As previously mentioned, the SEM images, Ge detection amount, and RMS were obtained from chips on which a SiGe film had been formed (i.e., chips whose surfaces were formed of Si after the SiGe film had been removed). Note that the Ge detection amount was actually obtained as a percentage value, and the RMS and polysilicon film etching amount were obtained as values in nm units. However, the values shown in the table were normalized by dividing these values by a predetermined coefficient. For the Ge detection amount, the larger the value in the figure, the greater the amount remaining on the Si film. For the RMS, the larger the value in the figure, the greater the roughness. For the polysilicon film etching amount, the larger the value in the figure, the greater the etching amount. For comparison, Figure 7 also shows an image of the surface of a chip on which a SiGe film had been formed before etching, and the normalized RMS in the lower right corner of the figure.
[0038] Figure 8 shows the ClF 3 9 shows a graph showing the relationship between the etching time by gas and the etching amount of the SiGe film and the polysilicon film. 2 Gas and ClF 3 6 shows a graph showing the relationship between the etching time by gas and the etching amount of the SiGe film and the polysilicon film. As in Evaluation Test 1-1, the JE and OE times were determined from the correspondence between the etching amount of the SiGe film and the etching time, and Evaluation Tests 1-2 and 1-3 were carried out. The vertical axis of each graph shows the etching amount of each film, and the obtained value is divided by a predetermined coefficient to show a normalized value. Note that this predetermined coefficient is the same as the coefficient used to normalize and represent the etching amount of the polysilicon film in FIG. 6.
[0039] F 2The results of Evaluation Test 1-1 using gas will be explained. In Evaluation Test 1-1 shown in FIG. 7, the specific etching times for JE, OE100%, OE200%, OE500%, and OE1000% are 82 seconds, 145 seconds, 208 seconds, 397 seconds, and 712 seconds, respectively. As shown in FIG. 2 As the etching time by the gas increases, the etching amount of the SiGe film increases. On the other hand, as shown in FIG. 7, the etching amount of the polysilicon film is generally constant and relatively low for the etching times of JE and each OE. Therefore, as described in the embodiment, F 2 It can be seen that when etching a Si film and a SiGe film using the gas, the SiGe film can be etched with high selectivity.
[0040] However, the detected amount of Ge is relatively large. As the OE percentage increases, the detected amount of Ge decreases, but it was confirmed that Ge remains even at 1000% OE. Furthermore, it was confirmed that the RMS value decreases as the OE percentage increases, but when this percentage is low and in the case of JE, the value is relatively large (i.e., the roughness is relatively large).
[0041] Next, ClF 3 The results of Evaluation Test 1-2 using gas will now be described. The specific etching times for JE, OE100%, and OE200% in Evaluation Test 1-2 shown in FIG. 7 were 50 seconds, 115 seconds, and 179 seconds, respectively. The amount of Ge detected was relatively low for JE, while no Ge was detected for OE100% and OE200%. Regarding RMS, the RMS values for JE, OE100%, and OE200% were comparable to the RMS values before etching, and were lower than the RMS values for JE, OE100%, and OE200% in Evaluation Test 1-1. Furthermore, the RMS values for OE100% and OE200% were particularly low.
[0042] However, as shown in FIG. 3When using gas, as the etching time increases, not only the etching amount of the SiGe film but also the etching amount of the polysilicon film increases. The etching amount of each of the polysilicon films in JE, OE 100%, and OE 200% in Evaluation Test 1-2 was found to be greater than the etching amount of each of the polysilicon films in JE and each OE in Evaluation Test 1-1.
[0043] Next, F 2 Gas + ClF 3 The results of Evaluation Test 1-3 using gas will now be described. The specific etching times for JE, OE 100%, and OE 200% in Evaluation Test 1-3 shown in FIG. 7 were 24 seconds, 54 seconds, and 85 seconds, respectively. As with Test 1-2, the amount of Ge detected was relatively low for JE, and no Ge was detected for OE 100% and OE 200%. Furthermore, the RMS values were particularly low for OE 100% and OE 200%, and were comparable to the RMS values before etching.
[0044] However, as shown in FIG. 2 Gas + ClF 3 Even when using gas, as the etching time increases, not only the etching amount of the SiGe film but also the etching amount of the polysilicon film increases. The etching amount of each of the polysilicon films in JE, OE 100%, and OE 200% in Evaluation Test 1-3 was greater than the etching amount of each of the polysilicon films in JE and each OE in Evaluation Test 1-1.
[0045] As described above, the results of this evaluation test 1 show that ClF is an etching gas. 3 It has been confirmed that the use of F gas can reduce the amount of Ge remaining on the Si film after etching (amount of residue) and can also suppress the roughness of the Si film. 2 It was also shown that the etching amount of the Si film was relatively large compared to when gas was used.
[0046] [Evaluation Test 2] In Evaluation Test 2, a wafer W having the same configuration as Evaluation Test 1 was etched under the same conditions as those in Evaluation Test 1-1, where OE was 100%. 2 Etching was carried out using this F gas. 2 Following the gas etching, F 2 Gas and NH 3 By supplying the gas into the processing vessel, the F 2 Gas purging and etching were performed. The pressure in the processing chamber was F 2 Gas and NH 3 F than the pressure during the gas supply period 2 The pressure was lowered during the period when the gas was supplied alone (the period when the gas was purged). After this etching, as in Evaluation Test 1, SEM images, detected amounts of Ge, and RMS were obtained from the chips on which the SiGe film had been formed, and the etching amount was also obtained from the chips on which the polysilicon film had been formed. 2 Gas and NH 3 The gas supply time (purging time) was changed, and tests were conducted with the gas supply time set to 5 seconds, 10 seconds, and 20 seconds, which were designated as evaluation tests 2-1, 2-2, and 2-3, respectively.
[0047] [Evaluation Test 3] As evaluation test 3, F 2 Gas and NH 3 F among gases 2 The test was carried out under the same processing conditions as in Evaluation Test 2, except that there was no period in which etching was carried out by supplying gas alone. 2 Gas and NH 3 Etching was performed only during a period in which both gases were supplied to the wafer W simultaneously (a period corresponding to the purge in Evaluation Test 2). 2 Gas and NH 3 The gas supply times were set to 5 seconds, 10 seconds, and 20 seconds, respectively, as in Evaluation Test 2. The tests conducted with these time settings were designated Evaluation Tests 3-1, 3-2, and 3-3, respectively. In Evaluation Test 3, the etching amounts of the SiGe film and the polysilicon film were measured.
[0048] The results of evaluation tests 2 and 3 are shown in Figure 10. Each value in the table is normalized in the same way as in evaluation test 1. Looking at the results of evaluation test 2, the amount of Ge detected and RMS were relatively large in each of evaluation tests 2-1 to 2-3. In addition, between evaluation tests 2-1 to 2-3, F 2 Gas and NH 3 The longer the gas supply time, the greater the amount of etching of the polysilicon film. Looking at the results of evaluation test 3, there was no significant difference in the amount of etching of the SiGe film between evaluation tests 3-1 to 3-3, but the amount of etching of the polysilicon film increased as the etching time increased. Therefore, from the results of evaluation tests 2 and 3, F 2 Gas and NH 3 It can be seen that the polysilicon film is etched to a relatively large extent by the action of the gas.
[0049] [Evaluation Test 4] Evaluation Test 4 was performed using the results of Evaluation Test 2. 2 Gas and NH 3 Instead of purging with gas, ClF 3 The treatment was carried out under the same conditions as in Evaluation Test 2, except that gas was supplied to perform purging and the length of the purging period was different from the range of 5 to 20 seconds set in Evaluation Test 2. Therefore, in Evaluation Test 4, as in the embodiment, F 2 After supplying the gas, 3 The pressure in the processing chamber is also the same as in the embodiment. 2 The pressure during the gas supply period is higher than that of ClF 3 The pressure was reduced during the gas supply period. 3 The gas supply times were set to 5 seconds, 20 seconds, and 60 seconds, respectively, and the tests conducted with these time settings were designated as evaluation tests 4-1, 4-2, and 4-3, respectively.
[0050] [Evaluation Test 5] As evaluation test 5, F 2 The test was carried out under the same processing conditions as in Evaluation Test 4, except that the period during which etching was carried out by supplying gas was not provided. 3 Etching is performed using only ClF gas. 3The gas supply times were set to 5 seconds, 20 seconds, and 60 seconds, respectively, as in Evaluation Test 4, and the tests conducted with these time settings were designated Evaluation Tests 5-1, 5-2, and 5-3, respectively. In Evaluation Test 5, as in Evaluation Test 3, the etching amounts of the SiGe film and the polysilicon film were measured.
[0051] The results of Evaluation Tests 4 and 5 are shown in FIG. 11. Each value in the table is normalized in the same manner as in Evaluation Test 1. Looking at the results of Evaluation Test 4, the amount of Ge detected was kept low in each of Evaluation Tests 4-1 to 4-3, and was a lower value than the amount of Ge detected in any of Evaluation Tests 2-1 to 2-3. Furthermore, the RMS was also kept low in each of Evaluation Tests 4-1 to 4-3, and was a lower value than the RMS in any of Evaluation Tests 2-1 to 2-3. Furthermore, the amount of etching of the polysilicon film was relatively low in each of Evaluation Tests 4-1 to 4-3, and was comparable to the values in Evaluation Tests 2-1 to 2-3.
[0052] 1 by the method described in the embodiment, it is possible to selectively etch the SiGe film 13 out of the Si film 12 and the SiGe film 13, thereby suppressing the residue of Ge. It is also possible to suppress the roughness of the Si film 12 after etching.
[0053] In addition, looking at the results of Evaluation Test 5, similar to Evaluation Test 1, 3 It is shown that the etching amount of the SiGe film and the polysilicon film increases as the gas supply time increases. The etching amount of the polysilicon film is relatively large in Evaluation Test 5-2, but is relatively small in Evaluation Test 5-1. From these results, it can be seen that the ClF 3 The time period from time t2 to time t3 during which gas is supplied (second time period) is preferably shorter than 20 seconds, and more preferably 5 seconds or less.
[0054] [Evaluation Test 6] For Evaluation Test 6-1, a substrate having the film structure shown in FIG. 12 was prepared. This film structure included a stack 62 in which Si films 12 and SiGe films 13 were alternately stacked upward, with a SiN (silicon nitride) film 61 formed on the uppermost Si film 12. A low-k porous film 63 was formed to cover this stack 62 from the sides to the top, and the porous film 63 was exposed on the surface of the substrate. In other words, when the etching gas was supplied, the porous film 63 was exposed to the etching gas. After supplying the etching gas to the substrate on which each film was formed in this manner, the etching gas was supplied as described in FIGS. 2 and 3 of the embodiment, and the state of the SiGe film 13 was observed. Furthermore, for Evaluation Test 6-2, a substrate having a similar film structure except that the porous film 63 was not formed was supplied with the etching gas as described in FIGS. 2 and 3, and the state of the SiGe film 13 was observed.
[0055] In evaluation test 6-2, the SiGe film 13 was etched from the sides, but in evaluation test 6-1, no etching from the sides of the SiGe film 13 was observed. From these test results, it is expected that etching of the semiconductor film 16 adjacent to the porous film 14 will be suppressed when etching is performed on a wafer W having the film structure shown in Figures 1 and 2 as described with reference to Figures 2 and 3.
[0056] W wafer 13 SiGe film
Claims
1. A method for etching a silicon germanium film formed on a substrate, comprising: a first step of supplying a first etching gas, which is a fluorine-containing gas, to the substrate for a first period of time; and a second step of supplying, after the first step, a second etching gas, which is a fluorine-containing gas different in type from the first etching gas, to the substrate for a second period of time shorter than the first period of time.
2. The etching method according to claim 1, wherein the first step is a step of selectively etching the silicon germanium film of the silicon germanium film and the silicon film exposed on the surface of the substrate, and the second step is a step of etching the remaining portion of the silicon germanium film.
3. The etching method according to claim 2, wherein the second etching gas is chlorine trifluoride gas.
4. The etching method according to claim 3, wherein the substrate is provided with: a silicon-containing film; and a porous film interposed between the silicon-containing film and the silicon germanium film.
5. An etching method according to claim 1, wherein the first step and the second step are steps of supplying the first etching gas and the second etching gas, respectively, to the substrate stored in a processing vessel, and the method includes a step of setting the pressure in the processing vessel in the second step to a pressure lower than the pressure in the processing vessel in the first step.
6. An etching apparatus for etching a silicon germanium film formed on a substrate, comprising: a processing vessel for storing the substrate; a first gas supply unit for supplying a first etching gas, which is a fluorine-containing gas, into the processing vessel for a first period of time; and a second gas supply unit for supplying a second etching gas, which is a fluorine-containing gas different from the first etching gas, into the processing vessel for a second period of time that is shorter than the first period of time after the supply of the first etching gas.
Citation Information
Patent Citations
Substrate processing method and storage medium
JP2018170380A
Etching method
JP2019129313A
Silicon-containing film etching method, computer storage medium, and silicon-containing film etching apparatus
JP2019201102A
Etching method, etching apparatus, and storage medium
JP2020053448A
Etching method and etching apparatus
JP2022191045A