Nickel-containing steel sheet for low-temperature applications and tank for low-temperature applications in which said steel sheet is used
The low-temperature nickel-containing steel plate with a tailored chemical composition and DI value addresses the toughness challenge under high heat input welding, ensuring robust low-temperature performance and efficient LNG tank construction.
Patent Information
- Application Number
- PCT/JP2024/007773
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-03
AI Technical Summary
Existing low-temperature nickel-containing steel plates used in LNG tanks face challenges in maintaining sufficient low-temperature toughness when high heat input welding is applied, as conventional methods focus on low heat input welding, and there is a lack of studies on suppressing martensite formation and grain boundary embrittlement in the heat-affected zone.
A low-temperature nickel-containing steel plate with optimized chemical composition and DI value, controlling elements like C, Si, Mn, P, S, Al, N, Mo, Ni, Cu, and Cr within specific ranges to suppress martensite formation and grain boundary embrittlement, ensuring adequate low-temperature toughness even under high heat input welding conditions.
The optimized steel plate maintains sufficient low-temperature toughness for LNG tank applications, ensuring Charpy impact absorption energy values of 34 J or more at -196°C, preventing brittle fracture and enhancing welding efficiency by allowing high heat input welding.
Smart Images

Figure JP2024007773_03102024_PF_FP_ABST
Abstract
Description
Nickel-containing steel plate for low temperature use and low temperature tank using the same
[0001] The present disclosure relates to a nickel-containing steel plate for low temperature use and a low temperature tank using the same.
[0002] In recent years, deregulation of the energy industry has progressed in Japan, and carbon dioxide (CO 2 There has been a shift from coal and oil, which have high emission factors, to LNG, a clean energy source with a low emission factor. Demand for liquefied natural gas (LNG) is expanding due to intensified environmental protection activities worldwide. This has led to an increase in the construction of cryogenic tanks used at extremely low temperatures (-196°C), such as for marine LNG fuel tanks. Nickel-containing low-temperature steel plates, such as 9% Ni steel, have excellent toughness at extremely low temperatures, making them widely used as materials for transporting and storing liquefied low-temperature gases such as LNG. LNG tanks are designed and constructed with particular consideration for safety. Therefore, low-temperature toughness is important not only for the steel materials and welding materials used, but also for welded joints. Charpy impact absorption energy values are specified in various standards, including ASTM (American Society for Testing and Materials).
[0003] When constructing structures such as low-temperature tanks using such nickel-containing steel plates, welding is essential, and it is essential to ensure the low-temperature toughness of the welded joints (welds) produced by welding.
[0004] Patent Document 1 discloses that reducing Si and P is an effective method for improving the low-temperature toughness of a dual-phase intercritically reheated heat-affected zone (hereinafter sometimes referred to as "IC-HAZ"). Patent Document 1 also describes that refinement of martensite locally formed in the IC-HAZ contributes to improving low-temperature toughness.
[0005] Patent Document 2 discloses a method for improving the CTOD characteristics of the HAZ portion by reducing Si and adding Mo.
[0006] Patent Document 3 describes a method for producing 9% Ni steel in which the toughness of a welded joint is improved by reducing the Si content, and shows that the amount of MA in the HAZ heated to the two-phase region of ferrite and austenite is reduced by reducing the Si content.
[0007] Patent Document 4 discloses a method for improving the HAZ toughness of the toe portion by reducing Si, Al, and N. It also shows that the effect is due to the promotion of auto-tempering by reducing Si and Al, and the reduction of AlN inclusions.
[0008] Patent Document 5 discloses that a method for improving the toughness of a base metal and a welded joint is to control the contents of C, Si, Al, and Mo. It also shows that the effect is due to the refinement of the structure during tempering by the addition of Mo and the suppression of the formation of hardened phases.
[0009] Patent Document 6 discloses a method for producing 9% Ni steel that is excellent in toughness of the base metal and welded joints, in which Si is reduced and hot rolling is performed in two stages.
[0010] JP-A-61-238911 JP-A-4-371520 JP-A-7-126749 Patent No. 5126780 JP-A 2002-129280 JP-A 2013-142197
[0011] In the manufacture of low-temperature tanks for LNG and other clean energy sources, automated TIG welding (GTAW) and surface-assisted welding (SAW) are the mainstream welding methods for the tank side plate vertical joints and horizontal joints, which account for the majority of welds. However, GTAW is a less efficient welding method, and SAW also suffers from the problem of being performed with a maximum heat input of 50 kJ / cm or less to reduce the risk of brittle fracture from the weld heat-affected zone. For this reason, there is a growing demand for high-heat-input welding, with a welding heat input exceeding 50 kJ / cm, to improve construction efficiency and reduce welding costs. However, with high-heat-input welding, the impact of the weld on the heat-affected zone is greater than with conventional welding methods (low-heat-input welding), making it difficult to ensure sufficient low-temperature toughness. The nickel-containing steel plates disclosed in Patent Documents 1 to 6 have all been evaluated for low-heat-input welded joints with a welding heat input of 50 kJ / cm or less, and sufficient consideration has not been given to suppressing the formation of MA in the IC-HAZ, where toughness deteriorates most when nickel-containing steel plates for low-temperature use are welded with high heat input, and to grain boundary embrittlement due to P. Therefore, the steel plates described in Patent Documents 1 to 6 may not be able to ensure low-temperature toughness of the welded joint sufficient to suppress brittle fracture of the tank when high-heat-input welding is applied.
[0012] The present disclosure has been made in view of the above circumstances, and aims to provide a nickel-containing steel plate for low-temperature use that can ensure sufficient low-temperature toughness of a welded joint even when large heat input welding is applied, and a low-temperature tank using the steel plate.
[0013] Aspect 1 of the present invention is a steel sheet comprising: C: 0.01 to 0.12 mass%, Si: 0.01 to 0.18 mass%, Mn: 0.2 to 1.8 mass%, P: 0.0100 mass% or less (including 0 mass%), S: 0.0100 mass% or less (including 0 mass%), Al: 0.001 to 0.100 mass%, N: 0.0080 mass% or less (including 0 mass%), Mo: 0.01 to 0.10 mass%, Ni: 8.75 to 10.0 mass%, Cu: 0.70 mass% or less (including 0 mass%), and Cr: 0.20 mass% or less (including 0 mass%), with the balance being Fe and inevitable impurities; This nickel-containing steel sheet for low temperature use has a DI value expressed by the following formula (1) of 1.03 or more and 1.65 or less, and a value calculated using the following formula (2) of 7.06 or less: DI=1.16×√([C] / 10)×(0.7[Si]+1)×(3.33[Mn]+1)×(0.35[Cu]+1)×(0.36[Ni]+1)×(2.16[Cr]+1)×(3[Mo]+1)×(1.75[V]+1)×(200[B]+1) (1) where [ ] represents the content of the element shown in [ ] in mass %. 3 [C] x [Si] 2.3 +1.5 x 10 10 × [P] 3.5 / √(133[Mo]+1) (2) where [ ] represents the content of the element shown in [ ] expressed in mass %.
[0014] A second aspect of the present invention is a low-temperature tank using the nickel-containing steel plate for low-temperature use according to the first aspect.
[0015] According to one embodiment of the present invention, it is possible to provide a nickel-containing steel plate for low-temperature use that can ensure sufficient low-temperature toughness of a welded joint even when large heat input welding is applied, and according to another embodiment of the present invention, it is possible to provide a low-temperature tank (for example, a tank for storing low-temperature liquefied gas such as LNG, which is a clean energy source) in which a welded joint has sufficient low-temperature toughness.
[0016] 1 is a graph showing the relationship between DI value and base material strength (yield stress and tensile strength). 2 is a graph showing the relationship between the value of the first term of formula (2) and the MA area fraction. 3 is a graph showing the relationship between the value of formula (2) and the Charpy impact absorption energy value vE at -196°C. -196 10 is a graph showing the relationship between
[0017] The present inventors conducted extensive research to solve the above-mentioned problems. As a result, they discovered that a desired tensile strength can be obtained without impairing the low-temperature toughness of the base metal and joint by optimizing the ranges of the contents of individual elements and by setting the DI value defined by the formula (1) described below to an appropriate value, and that by setting the value defined by the formula (2) described below within a predetermined range, the formation of MA (martensite-austenite constituent, island martensite) and grain boundary embrittlement in the IC-HAZ during high heat input welding can be suppressed, thereby more reliably improving low-temperature toughness. These findings led to the present invention. Each requirement defined in the embodiments of the present invention will be described in detail below.
[0018] 1. Chemical Composition The nickel-containing steel sheet for low temperature use according to an embodiment of the present invention has the chemical composition described below.
[0019] 1-1. Content of Individual Elements [C: 0.01% by mass or more, 0.12% by mass or less] C is one of the elements that characterize the embodiments of the present invention. If its content exceeds 0.12% by mass, it promotes the formation of MA (island martensite) in the IC-HAZ during high heat input welding, degrading the low-temperature toughness of the joint. For this reason, the upper limit of the C content is set to 0.12% by mass. On the other hand, C is an element that increases the strength of steel, and a content of 0.01% by mass or more is necessary to ensure the desired strength. Therefore, the C content is set to the range of 0.01 to 0.12% by mass. The upper limit of the C content is preferably 0.10% by mass, more preferably 0.08% by mass.
[0020] [Si: 0.01% by mass or more, 0.18% by mass or less] Si is one of the elements that characterize the embodiments of the present invention. By setting the Si content to 0.18% by mass or less, the formation of MA in the welded joint is suppressed and the low-temperature toughness of the joint is improved. On the other hand, Si is an element necessary as a deoxidizer and for ensuring strength, and if the content is less than 0.01% by mass, these effects are insufficient. Therefore, the Si content is set to the range of 0.01 to 0.18% by mass. Note that the lower the Si content, the more the formation of MA in the IC-HAZ is suppressed, so the upper limit of the Si content is preferably 0.14% by mass.
[0021] [Mn: 0.2% by mass or more, 1.8% by mass or less] Mn is an element necessary for improving the hardenability of steel and ensuring strength, but if its content is less than 0.2% by mass, this effect is insufficient, and if it exceeds 1.8% by mass, toughness deteriorates. Therefore, the Mn content is set to the range of 0.2 to 1.8% by mass. The preferred range of Mn content is 0.3 to 1.2% by mass.
[0022] [P: 0.0100% by mass or less (including 0% by mass)] P is one of the elements that characterize the embodiments of the present invention. It is inevitably present in steel as an impurity and segregates at grain boundaries, degrading the low-temperature toughness of the base metal and welded joints. Therefore, the upper limit is set to 0.0100% by mass. To improve the low-temperature toughness of the welded joints, the lower the P content, the more desirable it is.
[0023] In this specification, "including 0% by mass" means that the content in accordance with the embodiment is not intentionally added, for example, includes the case where the content is at the level of unavoidable impurities (it does not exclude the case where the element is intentionally added as long as it is within a predetermined range). On the other hand, in this specification, "not including 0% by mass" means that the element is intentionally added.
[0024] [S: 0.0100% by mass or less (including 0% by mass)] S is an element present in steel as an inevitable impurity. If the S content is too high, elongated MnS becomes the starting point for brittle fracture, degrading the toughness of the base material and the welded joint. Therefore, the upper limit of the S content is set to 0.0100% by mass. Note that, in order to improve the toughness of the joint, the lower the S content, the better.
[0025] [Al: 0.001% by mass or more, 0.100% by mass or less] Al is a deoxidizer and an element effective in suppressing grain coarsening and ensuring toughness, but if its content is less than 0.001% by mass, sufficient effects cannot be obtained. On the other hand, if its content exceeds 0.100% by mass, brittle fracture occurs originating from alumina inclusions, thereby deteriorating toughness. Therefore, the Al content is set to the range of 0.001 to 0.100% by mass.
[0026] [N: 0.0080 mass% or less (including 0 mass%)] N is an impurity that deteriorates the toughness of the base metal and the welded joint through the formation of precipitates such as AlN, so the upper limit is set to 0.0080 mass%. Note that, in order to improve the toughness of the joint, the lower the N content, the better.
[0027] [Ni: 8.75% by mass or more, 10.0% by mass or less] Ni is a basic element added to ensure toughness at cryogenic temperatures (low-temperature toughness), and in the present embodiment, the Ni content is set to 8.75% by mass or more. The higher the Ni content, the better the low-temperature toughness. However, if the Ni content exceeds 10.0% by mass, the effect of improving properties relative to the increase in alloy cost becomes small. Therefore, the Ni content is set to the range of 8.75 to 10.0% by mass. From the viewpoints of ensuring low-temperature toughness and suppressing alloy cost, a more preferable Ni content range is 8.95 to 9.85% by mass.
[0028] [Mo: 0.01% by mass or more, 0.10% by mass or less] Mo is one of the elements that characterize the embodiments of the present invention. By including 0.01% by mass or more of Mo, grain boundary embrittlement due to P during the cooling process after welding is suppressed, contributing to improved toughness. On the other hand, if the Mo content exceeds 0.10% by mass, the impact of toughness deterioration due to carbide formation becomes greater. Therefore, the Mo content is set to the range of 0.01 to 0.10% by mass. Note that within the range of 0.10% by mass or less, the effect of suppressing grain boundary embrittlement increases with increasing Mo content, so the lower limit of the Mo content is preferably 0.02% by mass, more preferably 0.03% by mass.
[0029] [Cu: 0.70% by mass or less (including 0% by mass)] Cu is an element contained in steel in trace amounts as an unavoidable impurity. Cu is usually contained at an impurity level of about 0.03% by mass or less. However, since adding a trace amount of Cu improves strength without impairing toughness, it may be intentionally added as needed. On the other hand, a Cu content exceeding 0.70% by mass deteriorates toughness. Therefore, when Cu is intentionally added, the Cu content is set to 0.70% by mass or less (excluding 0% by mass). In order to reliably obtain the above-mentioned strength improvement effect, the lower limit of the Cu content is preferably 0.05% by mass.
[0030] [Cr: 0.20% by mass or less (including 0% by mass)] Cr is an element contained in steel in trace amounts as an unavoidable impurity. Cr is usually contained at an impurity level of about 0.08% by mass or less. Cr may be intentionally added as needed to improve the hardenability and strength of steel. On the other hand, if the content exceeds 0.20% by mass, toughness is deteriorated. Therefore, when Cr is intentionally added, the Cr content is set to 0.20% by mass or less (excluding 0% by mass). To reliably obtain the above-mentioned effects, the lower limit of the Cr content is preferably 0.10% by mass.
[0031] [Balance] In one preferred embodiment of the present invention, the balance is iron and inevitable impurities. The inevitable impurities include elements (e.g., As, Sb, Nb, O, H, etc.) that are introduced depending on the conditions of raw materials, materials, manufacturing facilities, etc. It should be noted that, for example, P and S are elements whose content is usually the lower the better and therefore are inevitable impurities, but their composition ranges are separately specified as described above. For this reason, in this specification, the "unavoidable impurities" that make up the balance are a concept that excludes elements whose composition ranges are separately specified.
[0032] 1-2. DI Value The nickel-containing steel sheet for low temperature use according to an embodiment of the present invention has a DI value, expressed by the following formula (1), of 1.03 or more and 1.65 or less: DI=1.16×√([C] / 10)×(0.7[Si]+1)×(3.33[Mn]+1)×(0.35[Cu]+1)×(0.36[Ni]+1)×(2.16[Cr]+1)×(3[Mo]+1)×(1.75[V]+1)×(200[B]+1) (1) where [ ] represents the content of the element shown within, expressed in mass%. That is, for example, [C] means the content of C, expressed in mass%.
[0033] In order to use nickel-containing steel plates such as 9% Ni steel plates as materials for LNG tanks, the yield stress must be 590 MPa or more and the tensile strength must be 680 MPa or more. However, there is a trade-off between the toughness and strength of a material, and if the strength is excessively high, the toughness of the base material and welded joints will be impaired. Therefore, the upper limit of the tensile strength (TS) should be 830 MPa or less, more preferably 800 MPa or less.
[0034] The DI value defined by the above formula (1) is a general parameter that represents the hardenability of a steel material, and the higher the DI value, the greater the dislocation density introduced into the material during quenching. Therefore, by controlling the DI value, it is possible to control the strength of a nickel-containing steel sheet for low-temperature use manufactured by quenching-tempering, quenching-intermediate heat treatment-tempering, or direct quenching-tempering, which are manufacturing methods commonly applied to nickel-containing steel sheets for low-temperature use. If the DI value is in the range of 1.03 to 1.65, it is possible to keep the strength within the above range without impairing the toughness of the base metal and the welded joint.
[0035] 1-3. Value of Formula (2) In the nickel-containing steel sheet for low temperature use according to the embodiment of the present invention, the value calculated using Formula (2) (sometimes referred to as the "value of Formula (2)") is 7.06 or less. 3 [C] x [Si] 2.3 +1.5 x 10 10 × [P] 3.5 / √(133[Mo]+1) (2) where [ ] represents the content of the element shown in [ ] in mass %. For example, [P] means the content of P in mass %.
[0036] As a result of the inventors' investigations, the following became clear: When high heat input welding is applied to nickel-containing steel plates for low-temperature use, the cooling rate of the HAZ decreases as the welding heat input increases. Therefore, in the IC-HAZ, which is heated to a two-phase ferrite-austenite state, the amount of upper bainite, which is formed at relatively high temperatures from the grain boundaries of austenite formed by partial reverse transformation, increases. As a result, the concentration of C in untransformed austenite is promoted, and the formation of MA, a hard phase, becomes significant. This causes brittle fracture to occur starting from the MA, significantly deteriorating the Charpy impact absorption energy of the IC-HAZ.
[0037] As mentioned above, C promotes the formation of MA by concentrating in the untransformed austenite phase. Also, Si increases MA by suppressing the cementitization of the untransformed austenite phase, so reducing C and Si is effective in reducing MA in the IC-HAZ. Furthermore, as a result of investigating the influence of components on the amount of MA formed, it was found that the amount of MA in the IC-HAZ is C × Si 2.3 Therefore, the first term of the formula (2) "5.0 × 10 3 [C] x [Si] 2.3 " indicates the ease of formation of MA in the IC-HAZ.
[0038] It is also known that P reduces toughness by causing grain boundary embrittlement in nickel-containing steel for low temperature use. Mo has a repulsive interaction with P on the prior austenite grain boundaries, and therefore has the effect of expelling P from the grain boundaries. As a result of the inventors' investigations, it has become clear that the addition of a small amount of Mo can significantly suppress grain boundary embrittlement caused by P, and the degree of grain boundary embrittlement is determined by the content ratio of P to Mo. Therefore, the second term of formula (2), "1.5 x 10 10 × [P] 3.5 / √(133[Mo]+1)) indicates the degree of grain boundary embrittlement due to P.
[0039] By setting the value of formula (2) to 7.06 or less, the formation of MA and intergranular embrittlement in the IC-HAZ during high heat input welding are suppressed, and as shown in the experimental results of the examples described later (particularly the quadratic approximation curve in Figure 3, which will be described in detail later), the Charpy impact absorption energy value vE of the IC-HAZ of the welded joint at -196°C is -196 The Charpy impact absorption energy value vE is 34J or more, which suppresses brittle fracture even in applications where toughness at cryogenic temperatures is required, such as LNG tanks, and ensures excellent toughness of the welded joint. -196 The fact that the Charpy impact absorption energy is 34J or more means that the standard value (average 34J or more) for the L-direction Charpy impact absorption energy value of 9% Ni steel (joint) specified in the ASTM standards (ASTM A553 / A553M:2022 and ASTM A844 / A844M:2022) is satisfied.
[0040] 2. Manufacturing method In manufacturing the nickel-containing steel sheet for low temperature use according to the embodiment of the present invention, a well-known manufacturing method that is applied to the manufacture of ordinary nickel-containing steel sheets for low temperature use can be used as long as the above-mentioned chemical composition is satisfied and the DI value shown in formula (1) and the value of formula (2) are within the above-mentioned appropriate ranges. For example, a steel billet such as a slab that satisfies the above requirements is hot-rolled to form a hot-rolled steel sheet of a predetermined thickness, and then the hot-rolled steel sheet is subjected to Ac 3 After heating to a temperature range above the temperature point and quenching, 1 This can be obtained by tempering in a temperature range below the quenching point. 1 Ac above points 3 Alternatively, the hot-rolled steel sheet may be directly quenched online after hot rolling, and then subjected to Ac 1 Alternatively, the steel may be produced by tempering at a temperature below the annealing point.
[0041] By using the nickel-containing steel plates for low-temperature use according to the embodiments of the present invention obtained in this manner and welding them together, a low-temperature tank (for example, a tank for storing low-temperature liquefied gas such as LNG, which is a clean energy source) according to the embodiments of the present invention can be obtained. In particular, by using the nickel-containing steel plates for low-temperature use according to the embodiments of the present invention, the welded joint has excellent low-temperature toughness even when welding is performed by a large heat input welding method, and therefore a low-temperature tank having sufficient low-temperature toughness can be obtained.
[0042] Note that high heat input welding refers to a welding method in which the welding heat input exceeds 50 kJ / cm, as described in, for example, Table M4.2, Note (6) on page 16 of the "2021 Rules for Steel Ships, Part M" published by Nippon Kaiji Kyokai (ClassNK).
[0043] 1. Sample Preparation Continuously cast slabs or vacuum melted slabs produced by converter-continuous casting and having the chemical compositions shown in Table 1 were heated to 1000°C or higher and 1200°C or lower, and then hot-rolled to the thicknesses shown in Table 2, followed by air-cooling to room temperature to obtain hot-rolled samples. Table 1 shows the DI values calculated using formula (1) for each sample, the first term of formula (2) "5.0 × 10 3 [C] x [Si]2.3 " (the "first term of formula (2)" column in Table 1), the second term of formula (2) "1.5 × 10 10 × [P] 3.5 / √(133[Mo]+1)" (the "second term of formula (2)" column in Table 1) and the value of formula (2) are also listed.
[0044] Next, the obtained hot-rolled sample was heated to 780°C, water-quenched, and tempered at 590°C to obtain a steel plate sample. Details of the manufacturing conditions for the steel plate sample are shown in Table 2. A sample for thermal cycle testing was obtained by cutting out a 12 mm × 33 mm × 55 mm piece from the t / 4 position of the obtained steel plate sample (a position located at a distance of 1 / 4 of the plate thickness t from the surface (main surface) of the steel plate toward the center) so that the plate thickness direction was 12 mm and the rolling direction was parallel to the 55 mm direction. In addition, a bar-shaped test piece was taken from the t / 4 position of the steel plate sample in a direction perpendicular to the rolling direction, and this was used as a sample for tensile testing.
[0045]
[0046] 2. Sample Evaluation (Low-Temperature Toughness Evaluation) The above-described thermal cycle test sample was heated to 950°C at a heating rate of 50°C / sec by high-frequency heating and held for 10 seconds. It was then cooled from 950°C to 900°C in 6 seconds, from 900°C to 800°C in 80 seconds, from 800°C to 500°C in 240 seconds, and from 500°C to 50°C in 765 seconds, thereby providing a simulated thermal history of the IC-HAZ portion of a welded joint in a single-pass weld with a heat input of approximately 380 kJ / cm. Subsequently, V-notch Charpy standard test samples in accordance with Japanese Industrial Standard JIS 2242:2018 were prepared from each thermal cycle test sample. Then, using the V-notch Charpy standard test sample, a Charpy impact test was performed at -196°C, and the Charpy impact absorption energy value vE -196 The impact test was carried out three times for one type of sample (one sample number). -196 The measurement results are shown in the "each" column of Table 2, and the average values are shown in the "ave." column of Table 2.
[0047] (MA area fraction) The amount of MA in the thermal cycle test sample after the above-mentioned simulated thermal history was measured. The simulated thermal history was applied to the thermal cycle test sample, and the sample was subjected to wet polishing and then to REPELLER corrosion at a position excluding the end 3 mm. A 155 μm × 202 μm region was observed under an optical microscope at a magnification of 400 times to identify MA from the contrast, and the MA area fraction was calculated. The results are shown in Table 2.
[0048] (Tensile test) Using the above-mentioned bar-shaped test pieces, the yield stress and tensile strength were measured by a tensile test in accordance with JIS Z2241: 2022. The measurement results are shown in Table 2 as "base material strength" (strength of the material before applying a simulated thermal history to the IC-HAZ portion of the welded joint).
[0049] Figure 1 shows the relationship between the DI value and the base material strength (yield stress and tensile strength), Figure 2 shows the relationship between the value of the first term of formula (2) and the MA area fraction, and Figure 3 shows the relationship between the value of formula (2) and the Charpy impact absorption energy value vE at -196°C. -196 (average value of three samples) The dotted line in Figure 3 is a quadratic approximation curve.
[0050] (Quality Judgment) The base material strength is a yield stress of 590 MPa or more, a tensile strength of 680 MPa or more and 830 MPa or less, and a Charpy impact absorption energy value vE at -196°C. -196 For the average value of 34 J or more and vE of all three samples -196 A sample having a value of 27J or more was judged to be "good," and a sample not satisfying any one of the criteria was judged to be "poor." The results of the pass / fail judgment are shown in Table 2.
[0051]
[0052] As can be seen from Tables 1 and 2, Samples No. 1 to 8, which have chemical compositions specified in the embodiments of the present invention and have DI values and formula (2) values within the specified ranges, have sufficient strength and low-temperature toughness. In other words, they have the strength required for structural materials to be used in low-temperature tanks for LNG and the like, and can ensure sufficient low-temperature toughness for low-temperature tanks even when subjected to thermal history in the IC-HAZ, which is prone to toughness degradation during high-heat-input welding. Therefore, they can be said to contribute to improving welding efficiency through the application of high-heat-input welding.
[0053] On the other hand, Sample No. 9 has an excess of Si and an insufficient amount of Mo, and the value of formula (2) is outside the specified range. Therefore, when subjected to a thermal history of high heat input welding, the formation of MA is significant, and the influence of grain boundary embrittlement due to P is significant, making it impossible to ensure sufficient low-temperature toughness when high heat input welding is applied. Furthermore, Sample No. 10 has a small Mo to P content ratio, so the value of formula (2) is outside the specified range. Therefore, the influence of grain boundary embrittlement due to P is significant, making it impossible to ensure sufficient low-temperature toughness when high heat input welding is applied.
[0054] This application claims priority from Japanese Patent Application No. 2023-055986, filed March 30, 2023. Japanese Patent Application No. 2023-055986 is incorporated herein by reference.
Claims
1. C: 0.01 to 0.12 mass%, Si: 0.01 to 0.18 mass%, Mn: 0.2 to 1.8 mass%, P: 0.0100 mass% or less (including 0 mass%), S: 0.0100 mass% or less (including 0 mass%), Al: 0.001 to 0.100 mass%, N: 0.0080 mass% or less (including 0 mass%), Mo: 0.01 to 0.10 mass%, Ni: 8.75 to 10.0 mass%, Cu: 0.70 mass% or less (including 0 mass%), and Cr: 0.20 mass% or less (including 0 mass%), with the remainder being Fe and unavoidable impurities; A nickel-containing steel sheet for low temperature use, in which the DI value represented by the following formula (1) is 1.03 or more and 1.65 or less, and the value calculated using the following formula (2) is 7.06 or less: DI = 1.16 x √([C] / 10) x (0.7[Si] + 1) x (3.33[Mn] + 1) x (0.35[Cu] + 1) x (0.36[Ni] + 1) x (2.16[Cr] + 1) x (3[Mo] + 1) x (1.75[V] + 1) x (200[B] + 1) ... (1) where [ ] is the content, expressed in mass%, of the element shown therein. 5.0 x 10 3 [C] x [Si] 2.3 +1.5 x 10 10 × [P] 3.5 / √(133[Mo]+1) (2) where [ ] is the content, expressed as mass %, of the element shown therein.
2. A low-temperature tank using the nickel-containing steel plate for low-temperature use according to claim 1.
Citation Information
Patent Citations
Manufacture of steel for low temperature superior in toughness of weld heat affected zone
JP1986238911A
Production of thick 9% ni steel having excellent CTOD characteristic of base material and weld heat-affected zone
JP1992371520A
Production of 9%Ni steel excellent in toughness in weld zone
JP1995126749A
Ni ALLOY STEEL FOR LOW TEMPERATURE AND ITS PRODUCTION METHOD
JP2002129280A
Ni-ADDED STEEL PLATE HAVING EXCELLENT TOUGHNESS SUCH THAT CHARPY TEST VALUES OF BOTH OF BASE MATERIAL AND WELDING JOINT AT -196 C ARE EACH 100 J OR MORE AND EXCELLENT PRODUCTIVITY, AND METHOD FOR MANUFACTURING THE SAME
JP2013142197A