Metal carbide-coated carbon material
By employing a tantalum carbide-coated carbon material with controlled chlorine concentration and roughness, the issue of crystal polymorphism in semiconductor crystal growth is mitigated, enhancing yield and product life through improved adhesion and reduced polymorphism occurrence.
Patent Information
- Application Number
- PCT/JP2024/008309
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
The yield of semiconductor single crystals is hindered by crystal polymorphism during growth, particularly when using metal carbide-coated carbon materials, where existing methods do not adequately suppress this issue.
A metal carbide-coated carbon material with a tantalum carbide coating film having a chlorine concentration of 25,000 ppm/μm or less, a thickness of 10 μm to 100 μm, and an arithmetic mean roughness of 0.1 μm to 9.5 μm, applied to a carbon base material with a linear thermal expansion coefficient between 3.5×10⁻⁶ /℃ and 8.2×10⁻⁶ /℃, is used to suppress crystal polymorphism.
This approach significantly improves the yield of semiconductor single crystals by reducing crystal polymorphism and extends the product life of the coated carbon material by ensuring strong adhesion and preventing peeling of the carbide coating.
Smart Images

Figure JP2024008309_03102024_PF_FP_ABST
Abstract
Description
Metal carbide coated carbon material
[0001] The present invention relates to a metal carbide-coated carbon material in which the surface of a carbon substrate is coated with a metal carbide coating film.
[0002] Carbides such as tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide have high melting points and excellent chemical stability, strength, toughness, and corrosion resistance. Therefore, coating a carbon substrate with a carbide can improve the properties of the carbon substrate, such as heat resistance, chemical stability, strength, toughness, and corrosion resistance. Carbide-coated carbon materials, in which a carbide film is coated on the surface of a carbon substrate, particularly tantalum carbide-coated carbon materials, are used as components of semiconductor single crystal manufacturing equipment for Si (silicon), SiC (silicon carbide), GaN (gallium nitride), and the like.
[0003] The sublimation recrystallization method (modified Lely process) is a widely known method for producing bulk SiC single crystals. In this method, a crucible is filled with SiC raw material, and a SiC seed crystal is placed on top of it. A cylindrical guide member is also installed around the SiC seed crystal. Sublimation gas generated by heating the SiC raw material rises along the inner wall of the guide member, and a SiC single crystal grows on the SiC seed crystal.
[0004] Furthermore, SiC single crystal substrates used in semiconductor devices and the like are manufactured by epitaxially growing a SiC single crystal on a SiC substrate made of a bulk single crystal. Known methods for epitaxially growing a SiC single crystal include liquid phase epitaxy (LPE), vapor phase epitaxy (VPE), and chemical vapor deposition (CVD). Typically, the method for epitaxially growing a SiC single crystal is the CVD method. In the CVD epitaxial growth method, a SiC substrate is placed on a susceptor in an apparatus and a source gas is supplied at a high temperature of 1500°C or higher to grow the SiC single crystal.
[0005] In such a method for producing a SiC single crystal, in order to obtain a crystal of higher quality, Patent Document 1 discloses a method using a crucible whose inner surface of a graphite base is coated with tantalum carbide, and Patent Document 2 discloses a method using a guide member whose inner wall is coated with tantalum carbide.
[0006] JP 2019-99453 A JP 2019-108611 A
[0007] It is known that SiC single crystals grown using a metal carbide-coated carbon material as a crucible or guide member have improved crystal growth yields compared to those grown using uncoated carbon material. However, even when using a metal carbide-coated carbon material, further yield improvements are required. The main causes of yield reduction include point defects, extended defects (dislocations, stacking faults), and crystal polymorphism (polytype). Among these, the present invention attempts to improve the yield of semiconductor single crystals by focusing on suppressing crystal polymorphism.
[0008] Therefore, an object of the present invention is to suppress the crystal polymorphism of semiconductor single crystals and improve the yield by using a metal carbide-coated carbon material.
[0009] As a result of extensive research, the present inventors discovered that by setting the chlorine concentration in the metal carbide coating film of a metal carbide-coated carbon material to 25,000 ppm μm or less, it is possible to suppress the polymorphism of semiconductor single crystals and improve the yield of semiconductor single crystals, and thus completed the present invention. The gist of the present invention is as follows: [1] A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film coating at least a portion of the carbon substrate, wherein the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide, and the chlorine concentration in the metal carbide coating film is 25,000 ppm μm or less. [2] The metal carbide-coated carbon material according to [1] above, wherein the metal carbide coating film has a thickness of 10 μm or more and 100 μm or less. [3] The metal carbide-coated carbon material according to [1] or [2] above, wherein the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less. [4] The metal carbide-coated carbon material according to any one of [1] to [3] above, wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less. [5] The linear thermal expansion coefficient of the carbon substrate is 3.5 × 10 -6 / ℃ or more, 8.2 x 10 -6 / °C or less. [6] The metal carbide-coated carbon material according to any one of [1] to [5] above, wherein the metal carbide constituting at least the surface of the metal carbide coating film is tantalum carbide. [7] The metal carbide-coated carbon material according to any one of [1] to [6] above, wherein the metal carbide constituting the metal carbide coating film is tantalum carbide.
[0010] According to the present invention, the occurrence of crystal polymorphism during crystal growth and epitaxial growth of semiconductor single crystals can be suppressed, thereby improving the yield of semiconductor single crystals.
[0011] Fig. 1 is a schematic diagram of an external heating type low pressure CVD apparatus according to the present embodiment; Fig. 2 is a schematic diagram of a low pressure heating furnace for semiconductor single crystal growth according to the present embodiment; Fig. 3 is a schematic diagram of a semiconductor single crystal epitaxial growth apparatus according to the present embodiment; Fig. 4 is a result of GDMS analysis of the tantalum carbide coated carbon material of Example 1; Fig. 5 is a result of cross-sectional SEM observation of the tantalum carbide coated carbon material of Example 1; Fig. 6 is a result of surface SEM observation of the tantalum carbide coated carbon material of Example 1; Fig. 7 is a diagram for explaining a method for measuring the adhesion strength of a tantalum carbide coating film.
[0012] The metal carbide-coated carbon material of the present invention will be described using a tantalum carbide-coated carbon material as an example.
[0013] [Tantalum carbide-coated carbon material] A tantalum carbide-coated carbon material according to one embodiment of the present invention comprises a carbon substrate containing carbon as a main component and a tantalum carbide coating film that coats at least a portion of the carbon substrate, and the chlorine concentration in the tantalum carbide coating film is 25,000 ppm μm or less.
[0014] (Carbon substrate) The carbon substrate in the tantalum carbide-coated carbon material of one embodiment of the present invention is a substrate containing carbon as a main component. The carbon substrate may further contain chlorine. Examples of materials for the carbon substrate include isotropic graphite, extruded graphite, pyrolytic graphite, and carbon fiber-reinforced carbon composite materials (C / C composites). The shape and properties of the carbon substrate are not particularly limited, and a carbon substrate processed into any shape depending on the application can be used.
[0015] <Arithmetic surface roughness Ra> The arithmetic mean roughness Ra of the surface of the carbon substrate affects semiconductor single crystal growth and epitaxial growth. The larger the arithmetic mean roughness Ra of the surface of the carbon substrate, the greater the peel strength between the carbon substrate and the tantalum carbide coating film. Therefore, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 0.1 μm or more. On the other hand, if the arithmetic mean roughness Ra of the surface of the carbon substrate is too large, the specific surface area of the carbon substrate increases, making the tantalum carbide coating film more likely to crack or peel. As a result, when a tantalum carbide-coated carbon material is used as a member for semiconductor single crystal growth or epitaxial growth, the product life of the member may be shortened. Therefore, from the viewpoint of the product life of the tantalum carbide-coated carbon material, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 10.0 μm or less.
[0016] Considering the occurrence rate of cracks and peeling of the tantalum carbide coating film, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 0.1 μm or more and 10.0 μm or less, more preferably 2.0 μm or more and 6.0 μm or less.By making the arithmetic mean roughness Ra of the surface of the carbon substrate within the above range, the peel strength between the carbon substrate and the tantalum carbide coating film can be made 10 MPa or more, and the product life of the component when the tantalum carbide-coated carbon material is used as a component for semiconductor single crystal growth and epitaxial growth can be extended.The arithmetic mean roughness Ra of the surface of the carbon substrate is a value measured based on JIS B 0633:2001 (ISO 4288:1996).
[0017] <Linear thermal expansion coefficient> The linear thermal expansion coefficient of the carbon substrate is preferably 3.5×10 -6 / ℃ or more, 8.2 x 10 -6 / °C or less. The linear thermal expansion coefficient of the carbon substrate is 3.5 × 10 -6 / ℃ or more, 8.2 x 10 -6 / °C or less, the occurrence of microcracks in the tantalum carbide coating film can be further suppressed. From this viewpoint, the linear thermal expansion coefficient of the carbon substrate is more preferably 5.0 × 10 -6 ~7.5 x 10 -6 / °C. The linear thermal expansion coefficient of the tantalum carbide coating is approximately 6.3 × 10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate can be measured in accordance with JIS R 1618.
[0018] (Tantalum carbide coating film) The tantalum carbide coating film is mainly composed of tantalum carbide, and the chlorine concentration in the tantalum carbide coating film is 25,000 ppm μm or less. The tantalum carbide coating film may cover a part of the carbon substrate, or may cover the entire carbon substrate. In addition, the chlorine concentration in this specification is based on mass.
[0019] <Chlorine concentration> In one embodiment of the present invention, the tantalum carbide coating film of the tantalum carbide-coated carbon material has a chlorine concentration of 25,000 ppm μm or less. If the chlorine concentration in the tantalum carbide coating film is greater than 25,000 ppm μm, crystal polymorphism occurs in the semiconductor single crystal during crystal growth and epitaxial growth of the semiconductor single crystal, resulting in a decrease in the yield of the semiconductor single crystal. From this viewpoint, the chlorine concentration in the tantalum carbide coating film is preferably 10,000 ppm μm or less, more preferably 5,000 ppm μm or less, even more preferably 4,000 ppm μm or less, even more preferably 3,000 ppm μm or less, even more preferably 1,000 ppm μm or less, even more preferably 300 ppm μm or less, even more preferably 200 ppm μm or less, even more preferably 150 ppm μm or less, even more preferably 100 ppm μm or less, even more preferably 50 ppm μm or less, and particularly preferably 30 ppm μm or less.In addition, the lower limit of the range of the chlorine concentration in the tantalum carbide coating film is not particularly limited, but is usually 0.1 ppm μm or more, or 1 ppm μm.In addition, the chlorine concentration in the tantalum carbide coating film can be measured by the method described in the Examples below.
[0020] <Explanation of the Mechanism of Decreasing the Crystal Polymorph Occurrence Rate Due to a Decrease in the Chlorine Concentration in a Tantalum Carbide Coating Film> Next, the mechanism of decreasing the crystal polymorph occurrence rate due to a decrease in the chlorine concentration in a tantalum carbide coating film will be described, but this description does not limit the present invention in any way. Semiconductor single crystals are grown and epitaxially grown in high-temperature environments. The tantalum carbide-coated carbon material used as a component is also exposed to high-temperature environments. Therefore, chlorine components contained in the tantalum carbide coating film either detach from the tantalum carbide coating film by themselves due to heat, or react with impurity atoms contained in the tantalum carbide coating film and the carbon substrate to form halides, which then detach from the tantalum carbon coating film. When the source gas in the single crystal growth environment is highly supersaturated, chlorine components or halides adhere or adsorb to the facets of the growing semiconductor single crystal. When a crystal nucleus is formed starting from the adhesion or adsorption point, the orientation of the nucleus is randomly selected. Therefore, it is believed that the probability of generating a crystal polymorph with a crystal plane different from the crystal plane growing from the step increases.
[0021] <Method for Measuring Chlorine Concentration in Tantalum Carbide Coating Film> The chlorine concentration in the tantalum carbide coating film can be measured, for example, by glow discharge mass spectrometry (GDMS) using a glow discharge mass spectrometer (product name "VG9000") manufactured by VG Elemental under the following measurement conditions. (Measurement conditions) ・Discharge Gas: Ar (7N) ・Insulator: Ceramic ・Secondary Electrode: In Orifice ・Cell: Flat Cell Assembly・Nomakization: 1kV, 1.6mA ・Ion Current: Ta ~1.2×E-11 A ・Detectors: Faraday cup: 160msec ・Daly-multiplier: 500msec
[0022] The measurement data are values obtained by correcting the ion beam ratio (IBR) with the relative sensitivity factor (RSF). The RSF used here is a standard value incorporated into the software. The RSF varies depending on the measurement conditions and the shape of the discharge cell, but the value corrected using the RSF built into the software (RSF corrected value) is considered to be closer to the mass concentration than the IBR. As an example of measurement data, the results of Example 1 described below are shown in Figure 4. The vertical axis represents concentration (weight ppm), and the horizontal axis represents depth (μm). The depth is calculated based on the actual measured value of the crater depth after analysis, assuming that the sputtering rate during analysis was constant. Note that, since unevenness of several μm exists at the crater bottom after analysis, it is thought that there is an error of approximately 10% in the depth resolution.
[0023] The definition of "in the metal carbide coating film" is the interface between the tantalum carbide coating film and the carbon substrate where the carbon concentration fluctuates in the GDMS analysis within a range that can be correlated with the actual film thickness measured by cross-sectional observation using a scanning electron microscope (SEM) or the like. For example, in Example 1 described below, the film thickness was determined to be 30 μm by cross-sectional observation using an SEM, and the measurement data shown in Figure 4 shows an increase in carbon concentration near 30 μm. Therefore, for example, in the measurement data shown in Figure 4, the region from a depth of 0 μm to a depth of 30 μm, where the carbon concentration increases rapidly, is defined as "in the metal carbide coating film."
[0024] The chlorine concentration is calculated as the integral value of the chlorine concentration in the range "in the metal carbide coating film." For example, in the measurement data shown in FIG. 4, the integral value of the chlorine concentration from a depth of 0 μm to a depth of 30 μm is defined as the "chlorine concentration." In the measurement data shown in FIG. 4, the chlorine concentration value is 27.5 ppm μm.
[0025] <Other Atoms> The tantalum carbide coating film contains tantalum carbide as the main component and chlorine at a concentration of 25,000 ppm μm or less, but may contain trace amounts of atoms other than carbon, tantalum, and chlorine as long as the effects of the present invention are not impaired. For example, the tantalum carbide coating film may contain impurity elements or doping elements other than carbon, tantalum, and chlorine at a concentration of 10,000 ppm μm or less.
[0026] <Method for producing tantalum carbide-coated carbon material> A tantalum carbide-coated carbon material according to one embodiment of the present invention can be produced by forming a tantalum carbide layer on the surface of a carbon substrate. The tantalum carbide coating can be formed on the surface of the carbon substrate by, for example, chemical vapor deposition (CVD), sintering, or carbonization. Among these, CVD is preferred as a method for forming a tantalum carbide coating because it can form a uniform and dense tantalum carbide coating.
[0027] Furthermore, CVD methods include thermal CVD, photo-assisted CVD, and plasma CVD, and for example, thermal CVD can be used to form a tantalum carbide layer. Thermal CVD has advantages such as a relatively simple apparatus configuration and no damage to the carbon substrate caused by plasma. For example, an externally heated reduced-pressure CVD apparatus 10 as shown in FIG. 1 can be used to form a tantalum carbide coating film using thermal CVD. In the externally heated reduced-pressure CVD apparatus 10, a carbon substrate 14 is supported by a support means 15 in a reaction chamber 12 equipped with a heater 13, a raw material supply unit 16, an exhaust unit 17, etc.
[0028] A method for producing a tantalum carbide-coated carbon material according to one embodiment of the present invention will be described with reference to Figure 1. First, a carbon substrate 14 is placed in a reaction chamber 12 of an externally heated low-pressure CVD apparatus 10. The carbon substrate 14 is supported by a support means 15 having three supporting portions each having a pointed tip.
[0029] Next, the reaction chamber 12 is heated. For example, the reaction chamber 12 is heated under conditions of an atmospheric pressure of 10 to 1000 Pa and a temperature of 800 to 2200°C.
[0030] Next, a tantalum carbide coating film is formed on the surface of the carbon substrate 14. Methane (CH 4 ) and hydrogen (H 2 ) gas and tantalum pentachloride (TaCl 5) and a tantalum carbide gas such as tantalum halide are supplied to the reaction chamber 12. The tantalum halide gas can be generated, for example, by heating and vaporizing the tantalum halide or by reacting tantalum metal with a halogen gas. The source gas supplied from the source supply unit 16 is then subjected to a thermal CVD reaction at a high temperature and reduced pressure of 800 to 2200°C and 1 to 1000 Pa, to form a tantalum carbide coating film on the carbon substrate 14.
[0031] <Method for controlling chlorine concentration in tantalum carbide coating film> When supplying the raw material gas, hydrogen (H 2 By supplying the tantalum halide gas, the reaction of chlorine desorption from the tantalum halide gas is promoted, and as a result, the chlorine concentration in the tantalum carbide layer can be reduced to 25,000 ppm μm or less. In addition, it is preferable that the molar ratio of tantalum atoms contained in the tantalum halide gas and hydrogen atoms contained in the hydrogen gas in the source gas satisfies the following formula: tantalum atoms (Ta):hydrogen atoms (H)=1:x (4≦x<16). Note that when the value of x is 16 or more, the desorption of chlorine from the tantalum halide gas is promoted, but the Ta 2 A tantalum carbide coating film is formed that contains an excess amount of Ta, rather than a 1:1 Ta:C molar ratio like C or Ta metal. Here, the molar ratio of tantalum atoms contained in the tantalum halide gas and hydrogen atoms contained in the hydrogen gas in the source gas can be calculated from the standard volumetric flow rates of the tantalum halide gas and hydrogen gas, respectively. For example, when tantalum pentachloride is used as the tantalum halide gas, 1 mole of tantalum halide gas contains 1 mole of tantalum atoms. On the other hand, 1 mole of hydrogen gas contains 2 moles of hydrogen atoms.
[0032] The tantalum carbide-coated carbon material according to one embodiment of the present invention is an example of a metal carbide-coated carbon material according to the present invention, and the metal carbide-coated carbon material according to the present invention is not limited to the tantalum carbide-coated carbon material according to one embodiment of the present invention. In the metal carbide-coated carbon material according to the present invention, the metal carbide constituting the metal carbide coating film coating the carbon substrate is not limited to tantalum carbide. For example, carbides such as niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide can be used as the metal carbide constituting the metal carbide coating film coating the carbon substrate. Furthermore, a combination of two or more metal carbides selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide may also be used as the metal carbide constituting the metal carbide coating film coating the carbon substrate. Among tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide, tantalum carbide is preferred because it has the highest melting point and is also excellent in chemical stability, strength, and corrosion resistance.
[0033] When tantalum carbide is used for the metal carbide coating film, the entire metal carbide coating film does not need to be made of tantalum carbide, but it is sufficient that at least the surface of the metal carbide coating film is made of tantalum carbide.
[0034] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to these examples.
[0035] The metal carbide-coated carbon materials of Examples 1 to 21 and Comparative Example 1 were produced as follows. (Example 1) First, as shown in Figures 2 and 3, isotropic graphite was processed into a bottomed cylindrical shape (crucible 21), a truncated conical cylindrical shape (guide member 22), a disk shape (susceptor 31), and a cylindrical shape (inner wall member 38), which were used as carbon substrates (see reference numeral 14 in Figure 1). The arithmetic mean roughness Ra of the surface of the carbon substrate 14 was 6.0 µm, and the linear thermal expansion coefficient of the carbon substrate 14 was 7.0 × 10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate was measured using a thermomechanical analyzer (TMA7300) manufactured by Yamato Scientific Co., Ltd., and the thermal expansion coefficient was measured in the temperature range of 200°C to 1200°C.
[0036] Next, the carbon substrate 14 was placed in the reaction chamber 12 of the externally heated reduced pressure CVD apparatus 10 shown in Fig. 1. The carbon substrate 14 was supported by a support means 15 having three supporting portions each having a pointed tip. At this time, the tips of the supporting portions were in contact with the outer surface of the truncated conical carbon substrate 14, the outer surface of the carbon substrate 14 of the bottomed cylindrical carbon substrate 14, the lower surface of the disk-shaped carbon substrate 14, and the outer surface of the cylindrical carbon substrate 14.
[0037] Next, methane (CH 4 ) gas at 0.25 SLM, argon (Ar) gas at 1.0 SLM, hydrogen (H 2 Tantalum pentachloride (TaCl) was vaporized by heating the gas at 0.125 SLM and 220°C. 5 ) was supplied at 0.25 SLM, and the source gas was reacted in the reaction chamber 12 under conditions of an atmospheric pressure of 100 Pa and a temperature of 1250° C., to form a tantalum carbide coating film on the entire surface of the carbon substrate 14.
[0038] The carbon substrate 14 coated with the tantalum carbide coating film was removed from the reaction chamber 12, and a crucible 21 (see FIG. 2), guide member 22 (see FIG. 2), susceptor 31 (see FIG. 3), and inner wall member 38 (see FIG. 3) made of tantalum carbide-coated carbon material were completed. From cross-sectional observation of the tantalum carbide coating film using a scanning electron microscope (SEM), the film thickness was calculated to be 30 μm. SEM photographs of the cross section of the tantalum carbide coating film in the tantalum carbide-coated carbon material of Example 1 are shown in FIGS. 5 and 6 . Furthermore, the arithmetic mean roughness Ra of the tantalum carbide coating film surface was measured using a surface roughness measuring instrument (manufactured by Mitutoyo Corporation, product name "Surftest SJ-210"). As a result, the arithmetic mean roughness Ra of the tantalum carbide coating film surface was 5.5 μm.
[0039] Furthermore, the chlorine concentration in the tantalum carbide coating film was measured by glow discharge mass spectrometry (GDMS) described in this specification. The measurement data is shown in Figure 4. As a result, it was found that the chlorine concentration in the tantalum carbide coating film was 27.5 ppm μm.
[0040] The adhesion strength of the tantalum carbide coating film was measured and found to be 19.6 MPa. The adhesion strength of the tantalum carbide coating film was measured by the following method. The adhesion strength of the tantalum carbide coating film was measured, for example, using a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus"), by adhering the tantalum carbide coating film 41 and a pin 46 with adhesive 45, pressing down with a pressing jig 44, and pulling the pin 46, as shown in Fig. 7, to measure the stress when the tantalum carbide coating film 41 peeled off. Five measurements were performed, and the calculated average value of the five measurements was taken as the adhesion strength of the tantalum carbide coating film.
[0041] The fabricated crucible 21 and guide member 22 were placed in a reduced-pressure heating furnace 20 as shown in Figure 2, and a SiC single crystal was grown by sublimation recrystallization. A SiC raw material 25 was placed in the crucible 21, and a SiC seed crystal 24 with a diameter of 2 inches was placed above it. Argon gas was introduced into the reduced-pressure heating furnace 20 at a flow rate of 10 to 30 SLM, and the SiC raw material 25 was sublimated under conditions of a pressure of 500 to 1000 Pa and a temperature of 2000 to 2500°C, thereby growing a 5 mm-thick SiC single crystal on the SiC seed crystal 24.
[0042] The production of SiC single crystals was repeated multiple times to check the number of times the crucible 21 and the guide member 22 had been repeatedly used. As a result, after 24 uses, peeling of the tantalum carbide coating film on the crucible 21 was confirmed, making it necessary to replace the crucible 21 with a new member.
[0043] The fabricated susceptor 31 and inner wall member 38 were placed in a CVD apparatus 30 as shown in Figure 3, and a SiC single crystal was epitaxially grown by CVD. A SiC single crystal substrate 34, which had been processed from a bulk single crystal into a substrate shape, was placed on the susceptor 31. Monosilane (SiH 4 ) gas at 30 sccm, propane (C 3 H 8 The gas was flowed in at 70 sccm under a pressure of 45 Torr at a temperature of 1550° C., and a SiC single crystal was epitaxially grown on the SiC single crystal substrate.
[0044] The production of SiC single crystals was repeated multiple times to confirm the number of times that the susceptor 31 and the inner wall member 38 could be repeatedly used. As a result, peeling of the tantalum carbide coating film was confirmed after 96 uses, and it became necessary to replace the members with new ones.
[0045] Furthermore, when the polymorph occurrence rates of the obtained single crystals were examined, the polymorph occurrence rates of the SiC single crystals produced by the sublimation recrystallization method and the epitaxial growth method were both 0%. The polymorph occurrence rates were measured as follows. The grown SiC single crystals were irradiated with ultraviolet (UV) light, and their appearance was examined. If even the slightest crystal disorder was observed, it was deemed that polymorphism had occurred.
[0046] (Example 2) Hydrogen (H 2 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the gas flow rate was changed from 0.125 SLM to 0.2 SLM. The results are shown in Table 2.
[0047] (Example 3) Hydrogen (H 2 The flow rate of the tantalum pentachloride (TaCl) gas was changed from 0.125 SLM to 0.15 SLM. 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas mixture 11 was changed from 0.25 SLM to 0.3 SLM. The results are shown in Table 2.
[0048] (Example 4) Hydrogen (H 2 The flow rate of the tantalum pentachloride (TaCl) gas was changed from 0.125 SLM to 0.2 SLM. 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas mixture 11 was changed from 0.25 SLM to 0.4 SLM. The results are shown in Table 2.
[0049] (Example 5) Hydrogen (H 2 The flow rate of the tantalum pentachloride (TaCl) gas was changed from 0.125 SLM to 0.25 SLM. 5The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas mixture 11 was changed from 0.25 SLM to 0.5 SLM. The results are shown in Table 2.
[0050] (Example 6) Hydrogen (H 2 The flow rate of the tantalum pentachloride (TaCl) gas was changed from 0.125 SLM to 0.15 SLM. 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas containing oxygen was changed from 0.25 SLM to 0.3 SLM, and the film formation time was shortened to change the film thickness from 30 μm to 10 μm. The results are shown in Table 2.
[0051] (Example 7) Hydrogen (H 2 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the gas flow rate was changed from 0.125 SLM to 0.15 SLM and the film thickness was changed from 30 μm to 50 μm by extending the film formation time. The results are shown in Table 2.
[0052] Example 8 A crucible 12, a guide member 19, a susceptor 31, and an inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was changed from 6.0 μm to 0.1 μm. The results are shown in Table 2.
[0053] Example 9 A crucible 12, a guide member 19, a susceptor 31, and an inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was changed from 6.0 μm to 10 μm. The results are shown in Table 2.
[0054] (Example 10) The thermal expansion coefficient of the carbon substrate 14 was set to 7.0 × 10 -6 / °C to 3.5 x 10 -6 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the temperature was changed to / °C. The results are shown in Table 2.
[0055] (Example 11) The thermal expansion coefficient of the carbon substrate 14 was set to 7.0 × 10 -6 / °C to 8.2 x 10 -6 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the temperature was changed to / °C. The results are shown in Table 2.
[0056] Example 12 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to niobium pentachloride (NbCl 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the above-mentioned components were changed to those shown in Table 2.
[0057] Example 13 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to hafnium tetrachloride (HfCl 4 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the above-mentioned components were changed to those shown in Table 2.
[0058] Example 14 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to zirconium tetrachloride (ZrCl 4 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the above-mentioned components were changed to those shown in Table 2.
[0059] Example 15 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to tungsten pentachloride (WCl 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the above-mentioned components were changed to those shown in Table 2.
[0060] Example 16 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to tantalum pentachloride (TaCl 5 ) and niobium pentachloride (NbCl 5 ) mixed gas (TaCl 5 : NbCl 5 Except for changing the ratio of the melting point of the crucible 12 to the melting point of the guide member 19, the susceptor 31, and the inner wall member 38 ..., the crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were fabricated and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0061] Example 17 Without changing the flow rate of the metal chloride gas (0.25 SLM), the metal chloride gas was changed to tantalum pentachloride (TaCl 5 ) to tantalum pentachloride (TaCl 5 ) and tungsten pentachloride (WCl 5 ) mixed gas (TaCl 5 : WCl 5 Except for changing the ratio of the melting point of the crucible 12 to the melting point of the guide member 19, the susceptor 31, and the inner wall member 38 ..., the crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were fabricated and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0062] Example 18 A crucible 12, a guide member 19, a susceptor 31, and an inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the film formation time was shortened and the film thickness was changed from 30 μm to 2 μm. The results are shown in Table 2.
[0063] Example 19 A crucible 12, a guide member 19, a susceptor 31, and an inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was changed from 6.0 μm to 32 μm. The results are shown in Table 2.
[0064] Example 20 A crucible 12, a guide member 19, a susceptor 31, and an inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was changed from 6.0 μm to 0.05 μm. The results are shown in Table 2.
[0065] (Example 21) The thermal expansion coefficient of the carbon substrate 14 was set to 7.0 × 10-6 / °C to 1.9 x 10 -6 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the temperature was changed to / °C. The results are shown in Table 1.
[0066] (Comparative Example 1) Hydrogen (H 2 The flow rate of the tantalum pentachloride (TaCl) gas was changed from 0.125 SLM to 0 SLM. 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of the gas mixture 11 was changed from 0.25 SLM to 0.5 SLM. The results are shown in Table 2.
[0067] The production conditions for Examples 1 to 21 and Comparative Example 1 are shown in Table 1.
[0068] The evaluation results of Examples 1 to 21 and Comparative Example 1 are shown in Table 2.
[0069] Comparing the results of Examples 1 to 21 with the results of Comparative Example 1, it was found that by setting the chlorine concentration in the metal carbide coating film to 25,000 ppm μm or less, it is possible to suppress the crystal growth of the semiconductor single crystal and the occurrence of crystal polymorphism during epitaxial growth.
[0070] A comparison of the results of Examples 1 to 5 with the result of Comparative Example 1 shows that when the chlorine concentration in the tantalum carbide coating film is in the range of 25,000 ppm μm or less, the product life of the metal carbide-coated carbon material is long and the occurrence of polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal is suppressed. Note that, in the repeated use of the tantalum carbide-coated carbon material in Comparative Example 1, due to the occurrence of polymorphism, the use was discontinued before the tantalum carbide-coated carbon material became unusable due to peeling of the tantalum carbide coating film or the like.
[0071] Comparing the results of Examples 1, 6, and 7 with those of Example 18, it was found that when the thickness of the tantalum carbide coating film was 10 μm or more and 100 μm or less, the product life of the metal carbide-coated carbon material was long and the occurrence of polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal was suppressed. When the thickness of the tantalum carbide coating film was 10 μm or less, the occurrence of polymorphism during the crystal growth and epitaxial growth of the single crystal semiconductor was confirmed. Note that the repeated use of the tantalum carbide-coated carbon material in Example 18 was discontinued before the tantalum carbide-coated carbon material became unusable due to the occurrence of polymorphism, such as peeling of the tantalum carbide coating film. Furthermore, a thickness of the tantalum carbide coating film exceeding 100 μm is undesirable because it increases the film formation time and increases the film formation cost. Therefore, the thickness of the tantalum carbide coating film is preferably 10 μm or more and 100 μm or less.
[0072] Comparing the results of Examples 1, 8, and 9 with those of Examples 19 and 20, when the arithmetic mean roughness Ra of the surface of the metal carbide coating film was 0.1 μm or more and 9.5 μm or less, or when the arithmetic mean roughness Ra of the surface of the carbon substrate was 0.1 μm or more and 10.0 μm or less, the product life of the metal carbide-coated carbon material was long and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal was suppressed. When the arithmetic mean roughness Ra of the surface of the carbon substrate was greater than 10 μm, the product life of the metal carbide-coated carbon material was shortened, and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal was confirmed. When the arithmetic mean roughness Ra of the carbon substrate surface was less than 0.1 μm, the product life of the metal carbide-coated carbon material was shortened.
[0073] Comparing the results of Examples 1, 10, 11 and 21, it was found that the thermal expansion coefficient of the carbon substrate was 3.5 × 10 -6 / ℃ or more, 8.2 x 10 -6 When the thermal expansion coefficient of the carbon substrate is 3.5 × 10 / ° C. or less, the product life of the metal carbide-coated carbon material is long, and the occurrence of polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal is suppressed. -6When the temperature is lower than 100°C / °C, the product life of the metal carbide coated carbon material is shortened, and the occurrence of crystal polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal is confirmed.
[0074] Comparing the results of Example 1 and Examples 12 to 16, it was found that when the metal carbide-coated carbon material had at least a portion of the surface of a substrate primarily composed of carbon coated with a metal carbide coating film primarily composed of any one of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, tungsten carbide, or a combination of two or more of these metal carbides, and the chlorine concentration in the metal carbide coating film was 25,000 ppm μm or less, the metal carbide-coated carbon material had a long product life and suppressed the occurrence of crystal polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal.
[0075] REFERENCE SIGNS LIST 10 Externally heated low-pressure CVD apparatus 11 Top chamber 12 Reaction chamber 13 Heater 14 Carbon substrate 15 Support means 16 Raw material supply section 17 Exhaust section 20 Low-pressure heating furnace 21 Crucible 22 Guide member 23 Upper lid 24 SiC seed crystal 25 SiC raw material 30 Epitaxial growth apparatus 31 Susceptor 32 Reaction chamber 33 Heater 34 SiC single crystal substrate 35 Exhaust section 36 Raw material supply section 37 Top chamber 38 Inner wall member 41 Tantalum carbide coating film 42 Carbon substrate 44 Holding jig 45 Adhesive 46 Pin
Claims
1. A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film coating at least a portion of the carbon substrate, wherein the metal carbide constituting the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide, and the chlorine concentration in the metal carbide coating film is 25,000 ppm-μm or less.
2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide coating has a thickness of 10 μm or more and 100 μm or less.
3. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less.
4. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less.
5. The linear thermal expansion coefficient of the carbon substrate is 3.5×10 -6 / ℃ or more, 8.2 x 10 -6 The metal carbide-coated carbon material according to claim 1, wherein the temperature is 0.1 to 100° C.
6. The metal carbide coated carbon material according to claim 1, wherein the metal carbide constituting at least the surface of said metal carbide coating film is tantalum carbide.
7. The metal carbide coated carbon material according to claim 1, wherein the metal carbide constituting the metal carbide coating film is tantalum carbide.
Citation Information
Patent Citations
Tantalum carbide coating carbon material and method of manufacturing the same, and member for semiconductor single-crystal manufacturing apparatus
JP2019099453A
METHOD OF MANUFACTURING TaC COATING LAYER USING CVD AND PROPERTY OF TaC MANUFACTURED USING THE SAME
JP2019108611A