Antibacterial or antiviral film

The use of a polyester resin film with a specific refractive index profile and an antibacterial or antiviral layer with well-dispersed particles in antibacterial or antiviral films addresses the challenge of rainbow unevenness, maintaining optical stability and durability even after moist heat treatment.

WO2024203191A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/009206
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Antibacterial or antiviral films used in touch panels face challenges in suppressing rainbow unevenness over time, particularly after moist heat treatment, which affects their optical properties and durability.

Method used

A polyester resin film with a specific refractive index profile and an antibacterial or antiviral layer containing a binder, light scattering particles, and antibacterial or antiviral agent particles, which maintains well-dispersed particles and refractive index stability even after moist heat treatment, thereby suppressing rainbow unevenness.

Benefits of technology

The solution effectively prevents the occurrence of rainbow unevenness in antibacterial or antiviral films over a long period, ensuring consistent optical performance and durability even under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009206_03102024_PF_FP_ABST
    Figure JP2024009206_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This antibacterial or antiviral film has a substrate and an antibacterial or antiviral layer disposed on the substrate, wherein: the substrate is a polyester resin film that satisfies prescribed conditions; the antibacterial or antiviral layer contains a binder, light scattering particles, and antibacterial or antiviral agent particles; and the antibacterial or antiviral film satisfies prescribed conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Antibacterial or antiviral film

[0001] The present invention relates to antibacterial or antiviral films.

[0002] Protective films and / or shatterproof films are used on touch panels of liquid crystal displays, organic electroluminescence displays, and the like to protect the surface. Touch panels used in mobile devices such as game consoles and mobile phones are frequently used, which means they are prone to bacterial and viral adhesion. Furthermore, touch panel display devices such as those found in ticket vending machines at train stations, automated teller machines (ATMs) at banks, medical equipment in medical facilities, and ordering devices at restaurants are used by an unspecified number of people, so there is a high possibility that various bacteria and viruses will adhere to them in the usage environment. Therefore, in order to suppress the growth of bacteria and viruses and reduce the risk of disease infection, a technology has been proposed in which an antibacterial or antiviral film is applied to the surface of the touch panel.

[0003] Patent Document 1 describes a substrate with an antibacterial layer, which comprises a substrate having optical anisotropy and an antibacterial layer disposed on at least a portion of the surface of the substrate, wherein the antibacterial layer contains antibacterial agent particles having a specific average particle size and a binder, the thickness of the antibacterial layer is more than 5 μm and not more than 15 μm, and the tensile strength of the substrate is 200 MPa or more.

[0004] JP 2016-185686 A

[0005] In recent years, there has been a demand for further improvement in the rainbow prevention performance of antibacterial or antiviral films.

[0006] Therefore, an object of the present invention is to provide an antibacterial or antiviral film in which the occurrence of rainbow unevenness is suppressed for a long period of time.

[0007] The present invention provides the following: <1> An antibacterial or antiviral film having a substrate and an antibacterial or antiviral layer disposed on the substrate, wherein the substrate is a polyester resin film satisfying the condition of formula (1), the antibacterial or antiviral layer contains a binder, light-scattering particles, and antibacterial or antiviral agent particles, and the antibacterial or antiviral film satisfies the condition of formula (11): 0.153≦(nx+ny) / 2−nz<0.165 (1), in formula (1), nx represents the refractive index in the slow axis direction in the plane of the polyester resin film, ny represents the refractive index in the fast axis direction in the plane of the polyester resin film, and nz represents the refractive index in the thickness direction of the polyester resin film; |h1−h2|<3.0 (11) In formula (11), h2 is the average haze value in a wavelength range of 400 to 700 nm of the antiviral film after wet heat treatment for 720 hours under conditions of a temperature of 60°C and a relative humidity of 90%, and h1 is the average haze value in a wavelength range of 400 to 700 nm of the antiviral film before the wet heat treatment. <2> The antibacterial or antiviral film according to <1>, wherein the polyester resin film has a thickness of 20 to 60 μm. <3> The antibacterial or antiviral film according to <1> or <2>, wherein the polyester resin film has a carboxy group amount of 35 eq / ton or less. <4> The antibacterial or antiviral film according to any one of <1> to <3>, wherein the polyester resin film has a titanium element content of 5 to 15 ppm by mass. <5> The antibacterial or antiviral film according to any one of <1> to <4>, wherein the polyester resin film has a pre-peak temperature of 140 to 180°C.

[0008] According to the present invention, it is possible to provide an antibacterial or antiviral film in which the occurrence of rainbow unevenness is suppressed for a long period of time.

[0009] FIG. 1 is a cross-sectional view showing an example of an antibacterial or antiviral film.

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the upper and lower limits. In the numerical ranges described in stages in this specification, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this specification, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In this specification, when multiple substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. In this specification, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In this specification, a combination of two or more preferred aspects is a more preferred aspect.

[0012] <Antibacterial or Antiviral Film> The antibacterial or antiviral film of the present invention is an antibacterial or antiviral film having a substrate and an antibacterial or antiviral layer disposed on the substrate, wherein the substrate is a polyester resin film that satisfies the condition of formula (1), the antibacterial or antiviral layer includes a binder, light-scattering particles, and antibacterial or antiviral agent particles, and the antibacterial or antiviral film is characterized in that it satisfies the condition of formula (11).

[0013] Hereinafter, an "antibacterial or antiviral film" will also be referred to as an "antiviral film." An "antibacterial or antiviral layer" will also be referred to as an "antiviral layer." An "antibacterial or antiviral agent" will also be referred to as an "antiviral agent." An "antibacterial or antiviral agent particle" will also be referred to as an "antiviral agent particle."

[0014] The present inventors conducted extensive research into polyester resin films and found that polyester resin films that satisfy the conditions of formula (1) exhibit small rainbow unevenness. Further extensive research into antiviral films using this polyester resin film as a substrate revealed that the occurrence of rainbow unevenness in an antiviral film can be suppressed over a long period of time by using an antiviral layer containing a binder, light-scattering particles, and antiviral agent particles, and by the antiviral film satisfying the conditions of formula (11), thereby completing the present invention. The detailed reasons why such a configuration can suppress the occurrence of rainbow unevenness over a long period of time are unknown, but are presumed to be due to the following. The fact that the antiviral film satisfies the conditions of formula (11) means that the haze fluctuation is small even after moist heat treatment. Furthermore, the small haze fluctuation after moist heat treatment is presumed to be due to the fact that the light-scattering particles and antiviral agent particles in the antiviral layer are well dispersed, thereby suppressing fluctuations in the refractive index of the antiviral layer even after moist heat treatment. It is presumed that the antiviral film of the present invention has an antiviral layer in which the light-scattering particles and antiviral agent particles are well dispersed and the refractive index is less likely to fluctuate, and therefore an antiviral film in which the occurrence of iridescent unevenness is suppressed for a long period of time can be obtained.

[0015] The antiviral film of the present invention satisfies the condition of formula (11), preferably the condition of formula (11-1), and more preferably the condition of formula (11-2): |h1-h2|<3.0 (11) |h1-h2|<2.5 (11-1) |h1-h2|<2.0 (11-2)

[0016] In the above formula, h2 is the average haze value in the wavelength range of 400 to 700 nm of the antiviral film after wet heat treatment for 720 hours under conditions of a temperature of 60°C and a relative humidity of 90%, and h1 is the average haze value in the wavelength range of 400 to 700 nm of the antiviral film before wet heat treatment.

[0017] An antiviral film that satisfies the condition of formula (11) can be obtained by adjusting the thickness of the substrate or antiviral layer, the carboxyl value of the polyester resin film used as the substrate, the particle size of the light-scattering particles or antiviral agent particles used in the antiviral layer, etc. One example is a method of using a polyester resin film with a low carboxyl value as the substrate.

[0018] The configuration of the antiviral film of the present invention will be described below with reference to the drawings.

[0019] 1 is a cross-sectional view showing an example of the configuration of an antiviral film. The antiviral film 110 has a substrate 101 and an antiviral layer 102. The antiviral layer 102 contains antibacterial agent particles (not shown). In the antibacterial film 110, the surface of the substrate 101 and the antibacterial layer 102 are in direct contact with each other.

[0020] The antiviral film of the present invention is not limited to the configuration shown in Fig. 1 and may have other configurations. In the antiviral film shown in Fig. 1, the antiviral layer 102 is disposed on one surface of the substrate 101, but antiviral layers may be disposed on both surfaces of the substrate. In the antiviral film 110 shown in Fig. 1, the antiviral layer 102 is disposed over the entire surface of the substrate 101, but the antiviral layer may be disposed only on a portion of the substrate.

[0021] 1, an adhesive layer may be disposed on the surface of the substrate 101 opposite to the surface on which the antiviral layer 102 is disposed. In this case, a separator for protecting the adhesive layer may further be attached to the surface of the adhesive layer opposite to the surface on which the substrate 101 is disposed.

[0022] In the antiviral film 110 shown in FIG. 1 , a protective sheet for protecting the antiviral layer 102 may be disposed on the antiviral layer 102. When a protective sheet is disposed, the protective sheet is removed from the antiviral film when it is used.

[0023] In the antiviral film 110 shown in FIG. 1, the substrate 101 and the antiviral layer 102 are in direct contact with each other, but a primer layer may be included between the substrate and the antiviral layer.

[0024] Each component constituting the antiviral film will be described in detail below.

[0025] [Substrate] The antiviral film of the present invention has a substrate. The substrate is a polyester resin film that satisfies the conditions of formula (1). The value of "(nx + ny) / 2 - nz" (planar orientation coefficient) of the polyester resin film is an index of a physical property related to the orientation of polymer molecular chains that constitute the protective film. Because this can more effectively suppress the occurrence of iridescent unevenness, it is preferable for the polyester resin film to satisfy the conditions of formula (1-1), and more preferable for the film to satisfy the conditions of formula (1-2). When the polyester resin film is a film biaxially stretched in the width direction (TD) and the longitudinal direction (MD), a larger value of the planar orientation coefficient means that the polymer molecular chains are oriented perpendicular to the thickness direction of the polyester resin film.

[0026] 0.153≦(nx+ny) / 2-nz<0.165...(1) 0.155≦(nx+ny) / 2-nz<0.164...(1-1) 0.157≦(nx+ny) / 2-nz<0.163...(1-2)

[0027] In the above formula, nx represents the refractive index in the slow axis direction in the plane of the polyester resin film, ny represents the refractive index in the fast axis direction in the plane of the polyester resin film, and nz represents the refractive index in the thickness direction of the polyester resin film.

[0028] The nx, ny, and nz of a polyester resin film can be measured as follows. The orientation axis direction of the polyester resin film is determined using two polarizing plates, and a 4 cm × 2 cm rectangle is cut out so that the orientation axes are perpendicular to each other to prepare a measurement sample. The refractive indexes of the perpendicular biaxial directions (nx, ny) and the refractive index in the thickness direction (nz) of this sample are determined using an Abbe refractometer, and nx, ny, and nz are measured.

[0029] The value of "nx-ny" (in-plane birefringence) of the polyester resin film preferably satisfies the condition of formula (2), more preferably the condition of formula (2-1), and even more preferably the condition of formula (2-2), because this can more effectively suppress the occurrence of rainbow unevenness. 0<nx-ny≦0.020 (2) 0.001≦nx-ny≦0.015 (2-2) 0.002≦nx-ny≦0.012 (2-3)

[0030] In the above formula, nx represents the refractive index in the slow axis direction in the plane of the polyester resin film, and ny represents the refractive index in the fast axis direction in the plane of the polyester resin film.

[0031] Any 1m location on polyester resin film 2 The difference between the maximum and minimum values ​​of (nx-ny) in the formula (in-plane birefringence distribution) preferably satisfies the condition of formula (3), more preferably the condition of formula (3-1), and even more preferably the condition of formula (3-2), because this can more effectively suppress the occurrence of rainbow unevenness: 0<Δn≦0.014 (3) 0.001<Δn≦0.010 (3-1) 0.002<Δn≦0.008 (3-2)

[0032] In the above formula, Δn is the thickness of an arbitrary point of a polyester resin film in 1 m 2 where nx represents the refractive index in the slow axis direction in the plane of the polyester resin film, and ny represents the refractive index in the fast axis direction in the plane of the polyester resin film.

[0033] The Δn of the polyester resin film can be measured as follows: 2The film is sampled every 100 mm evenly in both the width and flow directions of the film. For example, for a film with a width of 2 m and a length of 0.5 m, 20 pieces are cut out in the width direction and 5 pieces in the flow direction, for a total of 100 film pieces. The film pieces are cut to the same size as the method described above for refractive index measurement (Abbe refractometer). The refractive index of each of the cut film pieces is measured using the same method as the refractive index measurement described above, and the value of nx - ny is derived. The difference between the maximum and minimum nx - ny values ​​of all the film pieces is defined as Δn.

[0034] The birefringence in the thickness direction, in-plane birefringence, and in-plane birefringence distribution of the polyester resin film can be adjusted by the type of polyester resin used in the polyester resin, the amounts of the polyester resin and additives, the addition of a retardation enhancer, the film thickness of the polyester resin, the stretching direction and stretching ratio of the polyester resin, etc. There are no particular limitations on the method for controlling the birefringence in the thickness direction, in-plane birefringence, and in-plane birefringence distribution of the polyester resin within the above-mentioned predetermined ranges, and this can be achieved, for example, by stretching or heat setting.

[0035] The amount of carboxy groups in the polyester resin film is preferably 35 eq / ton or less, more preferably 33 eq / ton or less, and even more preferably 30 eq / ton or less. The lower limit can be 0 eq / ton or more, 5 eq / ton or more, or even 10 eq / ton or more. When the amount of carboxy groups in the polyester resin film is 35 eq / ton or less, deterioration of the polyester resin film due to hydrolysis over time can be suppressed. Furthermore, fluctuations in haze in the wavelength range of 400 to 700 nm before and after moist heat treatment of the antiviral film can be further suppressed. This can suppress deformation and changes in orientation of the polyester resin film, allowing for excellent long-term suppression of iridescent unevenness.

[0036] The amount of carboxyl groups in a polyester resin film is determined by dissolving 0.1 g of a measurement sample in 10 ml of benzyl alcohol, adding chloroform to the mixed solution, adding a phenol red indicator dropwise to the mixed solution, titrating the resultant solution with a reference solution (0.01 N KOH-benzyl alcohol mixed solution), and then calculating the amount of carboxyl groups from the amount added.

[0037] The pre-peak temperature of the polyester resin film is preferably 140 to 200°C, more preferably 140 to 180°C, and even more preferably 150 to 180°C. When the pre-peak temperature of the polyester resin film is within the above range, the occurrence of rainbow unevenness in the antiviral film can be more effectively suppressed. Here, the pre-peak temperature of the polyester resin film refers to a minute endothermic peak that appears before the melting peak of the polyester resin film when the polyester resin film is subjected to differential scanning calorimetry. The pre-peak temperature of the polyester resin film generally corresponds to the highest attained film surface temperature (heat setting temperature) of the polyester resin film during heat setting in the transverse stretching process of the polyester resin film.

[0038] The heat shrinkage rate in both the MD and TD directions of the polyester resin film after standing at 80°C for 24 hours is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.3% or less. By setting the heat shrinkage rate to 1.0% or less, the occurrence of rainbow unevenness can be more effectively suppressed. Furthermore, when used in liquid crystal display devices and touch panels, shrinkage of the polyester resin film is suppressed, making display failure less likely to occur.

[0039] In this specification, the heat shrinkage rate in the MD direction of a polyester resin film after standing at 80°C for 24 hours (hereinafter also referred to as MD heat shrinkage rate) is defined as follows: Two reference lines are pre-marked on a sample piece M of polyester resin film cut to 30 mm in the TD direction and 120 mm in the MD direction, with a gap of 100 mm in the MD direction. The sample piece M is then left standing in a heating oven at 80°C for 24 hours under no tension, and the sample piece M is then cooled to room temperature, and the gap between the two reference lines is measured. The gap measured after the treatment is defined as A [mm]. The value [%] calculated using the pre-treatment gap of 100 mm and the post-treatment gap A mm using the formula "100 × (100 - A) / 100" is defined as the MD heat shrinkage rate of the sample piece M.

[0040] In this specification, the thermal shrinkage rate in the TD direction of a polyester resin film after standing at 80°C for 24 hours (hereinafter also referred to as TD thermal shrinkage rate) is defined as follows: Two reference lines are pre-marked on a sample piece M of polyester resin film cut to 30 mm in the MD direction and 120 mm in the TD direction, with a 100 mm gap in the TD direction. The sample piece M is then left standing in a heating oven at 80°C for 24 hours under no tension, and the sample piece M is then cooled to room temperature, and the gap between the two reference lines is measured. The gap measured after the treatment is defined as A [mm]. The TD thermal shrinkage rate of the sample piece M is calculated from the gap of 100 mm before the treatment and the gap A mm after the treatment using the formula "100 × (100 - A) / 100".

[0041] The density of the polyester resin film is 1.370 to 1.390 g / cm 3 is preferably 1.372 to 1.388 g / cm 3 More preferably, it is 1.374 to 1.386 g / m 3 When the density of the polyester resin film is within the above range, the film strength is good and the occurrence of rainbow unevenness is suppressed. The density can be measured in accordance with JIS K7112.

[0042] The crystallinity of the polyester resin film is preferably 5% or more, more preferably 20% or more, and even more preferably 30% or more.

[0043] From the viewpoint of transparency, it is preferable that the number of fine particles, foreign matter, and defects contained in the polyester resin film is small. The number of fine particles, foreign matter, and defects having a diameter of 1 μm or more in the polyester resin film is 50 / 10 mm. 2 Preferably, the number is 10 pieces / 10 mm or less. 2 More preferably, it is 3 pieces / 10 mm or less. 2 More preferably, the number is 0 / 10 mm or less. 2 It is particularly preferred that:

[0044] From the viewpoint of improving mechanical strength, the polyester resin film is preferably a polyester resin film that has been subjected to a stretching treatment, and more preferably a biaxially stretched polyester resin film. The stretching ratio is not particularly limited, but is preferably in the range of 1.5 times to 7 times. If the stretching ratio is less than 1.5 times, the mechanical strength may be insufficient, and if the stretching ratio is more than 7 times, the thickness may lack uniformity. The stretching ratio is more preferably in the range of 2 times to 5 times, and even more preferably in the range of 3 times to 4.5 times.

[0045] The arithmetic mean roughness Ra of the surface of the polyester resin film is preferably 0.005 to 0.02 μm, and more preferably 0.008 to 0.015 μm. The ratio (Rz / Ra) of the maximum height Rz to the arithmetic mean roughness Ra of the surface of the polyester resin film is preferably 5 to 50, and more preferably 10 to 30. The arithmetic mean roughness Ra and maximum height Rz of the surface of the polyester resin film can be measured in accordance with ISO 4287 by analyzing the shape of the polyester resin film surface using a laser microscope (for example, "VK-X1000" manufactured by KEYENCE Corporation).

[0046] The total light transmittance of the polyester resin film is preferably 90% or more, and more preferably 95% or more.

[0047] The titanium element content of the polyester resin film is preferably 5 to 15 ppm by mass, more preferably 7 to 12 ppm by mass. When the titanium element content is within this range, sufficient reactivity can be obtained during polymerization of the polyester resin, and the generation of foreign matter can be further suppressed. Furthermore, a polyester resin having high transmittance in the visible light wavelength range (e.g., a wavelength range of 400 to 700 nm) can be obtained.

[0048] The acetaldehyde content of the polyester resin film is preferably 50 ppm or less, more preferably 40 ppm or less, and even more preferably 30 ppm or less. Acetaldehyde easily undergoes a condensation reaction with itself, producing water as a by-product, which may accelerate the hydrolysis of the polyester. The lower limit of the acetaldehyde content is practically about 1 ppm. To keep the acetaldehyde content within the above range, methods can be adopted, such as maintaining a low oxygen concentration in each process, such as melt polymerization and solid-state polymerization, during the production of the polyester resin film, maintaining a low oxygen concentration during resin storage and drying, reducing the thermal history of the resin in the extruder, melt piping, die, etc. during the production of the polyester resin film, and preventing localized strong shear stress by using the screw configuration of the extruder during melting.

[0049] Examples of polyester resins constituting the polyester resin film include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polycyclohexanedimethylene terephthalate (PCT), etc., and polyethylene terephthalate or polyethylene naphthalate is preferred, and polyethylene terephthalate is more preferred.

[0050] Polyethylene terephthalate is a polyester having structural units derived from terephthalic acid as the dicarboxylic acid component and structural units derived from ethylene glycol as the diol component, and preferably 80 mol% or more of all repeating units are ethylene terephthalate. Polyethylene terephthalate may also contain structural units derived from other copolymerization components. Examples of other copolymerization components include dicarboxylic acid components such as isophthalic acid, p-β-oxyethoxybenzoic acid, 4,4'-dicarboxydiphenyl, 4,4'-dicarboxybenzophenone, bis(4-carboxyphenyl)ethane, adipic acid, sebacic acid, 5-sodium sulfoisophthalic acid, and 1,4-dicarboxycyclohexane, and diol components such as propylene glycol, butanediol, neopentyl glycol, diethylene glycol, cyclohexanediol, ethylene oxide adducts of bisphenol A, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. These dicarboxylic acid components and diol components may be used in combination of two or more types as needed. It is also possible to use an oxycarboxylic acid such as p-oxybenzoic acid in combination with the above carboxylic acid component or diol component. Dicarboxylic acid components or diol components containing an amide bond, a urethane bond, an ether bond, a carbonate bond, or the like can also be used as other copolymerization components. Polyethylene terephthalate can be produced by any production method, such as a so-called direct polymerization method in which terephthalic acid is directly reacted with ethylene glycol, and, if necessary, other dicarboxylic acids or other diols, or a so-called transesterification method in which a dimethyl ester of terephthalic acid is transesterified with ethylene glycol, and, if necessary, the dimethyl ester of other dicarboxylic acids or other diols.

[0051] The intrinsic viscosity IV of the polyester resin is preferably 0.58 to 0.80 dL / g, more preferably 0.60 to 0.76 dL / g, and even more preferably 0.62 to 0.68 dL / g. The intrinsic viscosity IV is determined by the combination of the solution viscosity (η) and the solvent viscosity (η 0 ) ratio η r (=η / η0 ; relative viscosity) minus 1 (η sp =η r -1) The value obtained by dividing by the concentration and extrapolating it to a state where the concentration is zero. The intrinsic viscosity (IV) is determined from the solution viscosity at 30°C in a mixed solvent of 1,1,2,2-tetrachloroethane / phenol (=2 / 3 [mass ratio]).

[0052] A catalyst is preferably used for the polymerization of polyester resins. Examples of catalysts include antimony-based catalysts and titanium-based catalysts, with titanium-based catalysts being preferred. Titanium-based catalysts have high polymerization activity and produce polyester resins with a lower amount of carboxyl groups than those produced using other catalysts, such as antimony-based catalysts, thereby suppressing the generation of catalyst-induced foreign matter and the production of by-products such as diethylene glycol units. Furthermore, the low generation of foreign matter results in high transmittance in the visible light wavelength range (e.g., wavelengths in the 400-700 nm range). Furthermore, thin films are less susceptible to breakage due to foreign matter when produced, resulting in films with high surface smoothness.

[0053] Examples of antimony catalysts include antimony trioxide, antimony pentoxide, antimony acetate, and antimony glycooxide. Examples of titanium catalysts include organic chelate titanium complexes with an organic acid as a ligand. Examples of organic acids include citric acid, lactic acid, trimellitic acid, and malic acid, with citric acid being preferred. In addition to organic chelate titanium complexes, titanium compounds such as oxides, hydroxides, alkoxide compounds, carboxylates, carbonates, oxalates, and halides containing titanium element can also be used as titanium catalysts. Examples of such titanium compounds include titanium alkoxides such as tetra-n-propyl titanate, tetra-i-propyl titanate, tetra-n-butyl titanate, tetra-n-butyl titanate tetramer, tetra-t-butyl titanate, tetracyclohexyl titanate, tetraphenyl titanate, and tetrabenzyl titanate; titanium oxides obtained by hydrolysis of titanium alkoxides; titanium-silicon or zirconium composite oxides obtained by hydrolysis of mixtures of titanium alkoxides and silicon alkoxides or zirconium alkoxides; titanium acetate, titanium oxalate, potassium titanium oxalate, sodium titanium oxalate, potassium titanate, sodium titanate, titanic acid-aluminum hydroxide mixtures, titanium chloride, titanium chloride-aluminum chloride mixtures, and titanium acetylacetonate.

[0054] The polyester resin can also be produced by, for example, the method described in paragraphs 0103 to 0109 of JP-A No. 2011-162777. The polyester resin film can also be produced by, for example, the method described in paragraphs 0053 to 0109 of JP-A No. 2015-184664.

[0055] The polyester resin film may contain known additives. Examples of such additives include ultraviolet absorbers, particles, lubricants, antiblocking agents, heat stabilizers, antioxidants, antistatic agents, light resistance agents, impact resistance modifiers, lubricants, dyes, pigments, etc. Examples of such additives include those described in paragraphs

[0043] to

[0052] of JP 2015-184664 A and paragraphs

[0057] and

[0058] of WO 2012 / 157662 A.

[0056] The thickness of the polyester resin film is preferably 20 to 60 μm. The lower limit is preferably 25 μm or more, more preferably 30 μm or more. The upper limit is preferably 55 μm or less, more preferably 50 μm or less. The thickness of the polyester resin film is determined by measuring the thickness at any 10 points on the polyester resin film with a micrometer, and calculating the arithmetic average of the measurement results.

[0057] An easy-adhesion layer (primer layer) may be formed on the surface of the polyester resin film on which the antiviral layer is disposed, in order to provide better handling properties. Examples of the easy-adhesion layer include a layer containing particles and a binder. The volume average particle diameter of the particles contained in the easy-adhesion layer is preferably 0.05 to 0.8 μm. The film thickness of the easy-adhesion layer is preferably 0.05 to 1.0 μm.

[0058] [Antiviral Layer (Antimicrobial or Antiviral Layer)] The antiviral film has an antiviral layer disposed on the above-described substrate. The antiviral layer contains at least a binder, light-scattering particles, and antibacterial or antiviral agent particles (hereinafter referred to as antiviral agent particles).

[0059] <Antiviral Agent Particles> The antiviral agent particles are not particularly limited, and any known particulate antibacterial or antiviral agent can be used. As the antiviral agent particles, those that exhibit a bactericidal effect against pathogenic bacteria such as Staphylococcus aureus and Escherichia coli are preferably used.

[0060] The shape of the antiviral agent particles is not particularly limited, and may be, for example, spherical, oval, rod-like, flat, needle-like, or irregular.

[0061] The antiviral particles preferably contain a metal. Metal ions are generated from the metal contained in the antiviral particles, and the metal ions act on microorganisms (hereinafter also referred to as bacteria), thereby exhibiting antibacterial and antiviral properties. Antiviral particles are preferred not only in terms of their antibacterial effect against pathogenic bacteria, but also in terms of their antibacterial properties against fungi such as mold and antiviral properties against viruses. Examples of viruses against which the antiviral particles are effective include influenza virus, SARS (severe acute respiratory syndrome) coronavirus (SARS-CoV), novel coronavirus (SARS-CoV-2), and feline calicivirus. Known methods can be used to evaluate antiviral activity. For example, measurements can be made using the method set forth in ISO 21702, with the test virus being replaced with a target virus such as influenza virus, SARS coronavirus, or novel coronavirus. The antiviral activity value or antibacterial activity value is preferably 2.0 or higher, and more preferably greater than 2.0.

[0062] Examples of the metal include silver, mercury, zinc, iron, lead, bismuth, titanium, tin, aluminum, and nickel. The form of the metal contained in the antiviral agent particles is not particularly limited, and examples include metal particles, metal ions, and metal salts (including metal complexes). Among these, copper, zinc, or silver is preferred as the metal because the virus layer has superior antibacterial and antiviral properties, and silver is more preferred because it is highly safe and has a broad antibacterial spectrum. Furthermore, metal salts are preferred as the metal. One type of antiviral agent particle may be used alone, or two or more types may be used in combination.

[0063] As the antiviral agent particles, silver-containing antiviral agent particles (hereinafter also referred to as "silver-based antiviral agent") are preferred because the antiviral layer has superior antibacterial and antiviral properties. That is, the metal is preferably silver. The silver-based antiviral agent is not particularly limited as long as it contains silver (silver atoms). The form of silver is also not particularly limited, and it may be contained in the form of, for example, metallic silver, silver ions, or silver salts (including silver complexes). For example, silver-based antiviral agents include silver particles that slowly release silver ions or inorganic antiviral agents containing silver (for example, silver and / or silver ions supported on a carrier). In this specification, silver complexes are included in the scope of silver salts.

[0064] Examples of silver salts include silver acetate, silver acetylacetonate, silver azide, silver acetylide, silver arsenate, silver benzoate, silver hydrogen fluoride, silver bromate, silver bromide, silver carbonate, silver chloride, silver chlorate, silver chromate, silver citrate, silver cyanate, silver cyanide, (cis,cis-1,5-cyclooctadiene)-1,1,1,5,5,5-hexafluoroacetylacetonate, silver diethyldithiocarbamate, silver fluoride (I), silver fluoride (II), silver 7,7-dimethyl-1,1,1,2,2,3,3-heptafluoro-4,6-octanedionate, silver hexafluoroantimonate, silver hexafluoroarsenate, silver hexafluorophosphate, silver iodate, and silver iodide. Examples of silver isothiocyanate include silver potassium cyanide, silver lactate, silver molybdate, silver nitrate, silver nitrite, silver (I) oxide, silver (II) oxide, silver oxalate, silver perchlorate, silver perfluorobutyrate, silver perfluoropropionate, silver permanganate, silver perrhenate, silver phosphate, silver picrate monohydrate, silver propionate, silver selenate, silver selenide, silver selenite, silver sulfadiazine, silver sulfate, silver sulfide, silver sulfite, silver telluride, silver tetrafluoroborate, silver tetraiodomucuriate, silver tetratungstate, silver thiocyanate, silver p-toluenesulfonate, silver trifluoromethanesulfonate, silver trifluoroacetate, and silver vanadate. Examples of silver complexes include histidine silver complex, methionine silver complex, cysteine ​​silver complex, aspartic acid silver complex, pyrrolidone carboxylic acid silver complex, oxotetrahydrofuran carboxylic acid silver complex, and imidazole silver complex.

[0065] As the silver-based antiviral agent, a silver-supported carrier containing a carrier and silver supported on the carrier is preferred in that it has superior antibacterial and antiviral properties.

[0066] The antiviral agent particles are preferably a metal-supported carrier containing a carrier and the above-mentioned metal supported on the carrier, and more preferably a silver-supported carrier. The type of carrier is not particularly limited, and known carriers can be used. Examples of carriers include zeolite-based antiviral agent carriers, calcium silicate-based antiviral agent carriers, zirconium phosphate-based antiviral agent carriers, calcium phosphate antiviral agent carriers, zinc oxide-based antiviral agent carriers, soluble glass-based antiviral agent carriers, silica gel-based antiviral agent carriers, activated carbon-based antiviral agent carriers, titanium oxide-based antiviral agent carriers, titania-based antiviral agent carriers, organometallic antiviral agent carriers, ion exchanger ceramic-based antiviral agent carriers, layered phosphate-quaternary ammonium salt-based antiviral agent carriers, and antiviral stainless steel carriers, but are not limited thereto. More specifically, examples of the carrier include zinc calcium phosphate, calcium phosphate, zirconium phosphate, aluminum phosphate, calcium silicate, activated carbon, activated alumina, silica gel, zeolite, hydroxyapatite, zirconium phosphate, titanium phosphate, potassium titanate, hydrous bismuth oxide, hydrous zirconium oxide, and hydrotalcite. Examples of zeolites include natural zeolites such as chabazite, mordenite, erionite, and clinoptilolite, and synthetic zeolites such as A-type zeolite, X-type zeolite, and Y-type zeolite. Furthermore, so-called ceramics are preferred as the carrier, as they provide superior effects of the present invention. Specifically, metal-supported ceramic particles are preferred as antiviral agent particles, and silver-supported ceramic particles are more preferred. The carrier may be crystalline or amorphous, but is preferably crystalline.

[0067] When the antiviral agent particles contain a metal, the content of the metal is not particularly limited, but is preferably 0.1 to 30 mass%, and more preferably 0.5 to 20 mass%, relative to the total mass of the antiviral agent particles (metal-supported carrier).

[0068] Examples of commercially available silver-based antiviral agents include silver zeolite-based antiviral agents such as "Zeomic" manufactured by Sinanen Zeomic Co., Ltd., "Silwell" manufactured by Fuji Silysia Chemical Ltd., and "Bactenon" manufactured by Japan Electronic Materials Co., Ltd.; silver-based antiviral agents in which silver is supported on inorganic ion exchanger ceramics, such as "Novalon" manufactured by Toagosei Co., Ltd. and "Atomi Ball" manufactured by Catalysts and Chemicals Industries Co., Ltd.; silver particles such as "Nanosilver" manufactured by Nippon Ion Co., Ltd.; and silver-supported ceramic particles (silver ceramic particles) in which silver is chemically bonded to ceramics, such as "Bactekiller" and "Bacterite" manufactured by Fuji Chemical Co., Ltd. and "Ionpure" manufactured by Ishizuka Glass Co., Ltd.

[0069] The average particle size of the antiviral agent particles is preferably 0.1 to 10 μm, more preferably 0.3 to 3 μm, in terms of achieving a good balance between ease of handling and transparency of the antiviral layer. Note that the average particle size of the antiviral agent particles is determined by measuring the 50% volume cumulative diameter (D50) three times using a laser diffraction / scattering particle size distribution analyzer manufactured by Horiba, Ltd., and using the arithmetic mean of the obtained measurements.

[0070] The content of the antiviral agent particles in the antiviral layer is not particularly limited, but in terms of better effects of the present invention, the content is preferably 0.1 to 20 mass %, more preferably 0.2 to 10 mass %, and even more preferably 1.0 to 7 mass %, relative to the total mass of the antiviral layer.

[0071] One type of antiviral particle may be used alone, or two or more types of antiviral particles may be used in combination. Furthermore, antiviral agents other than the antiviral particles may be used in combination with the antiviral particles. Examples of other antiviral agents include organic antibacterial or antiviral agents such as phenol ether derivatives, imidazole derivatives, sulfone derivatives, N-haloalkylthio compounds, anilide derivatives, pyrrole derivatives, quaternary ammonium salts, pyridine compounds, triazine compounds, benzoisothiazoline compounds, and isothiazolinone compounds. Organic antibacterial or antiviral agents also include natural antibacterial or antiviral agents. Examples of natural antibacterial or antiviral agents include chitosan, a basic polysaccharide obtained by hydrolyzing chitin contained in crab or shrimp shells.

[0072] <Binder> The antiviral layer contains a binder. There are no particular limitations on the binder, and known binders can be used. Examples of the binder include polyester resin, acrylic resin, methacrylic resin, resin composed of a methacrylic acid-maleic acid copolymer, polystyrene resin, fluororesin, polyimide resin, fluorinated polyimide resin, polyamide resin, polyamideimide resin, polyetherimide resin, cellulose acylate resin, polyurethane resin, polyether ether ketone resin, polycarbonate resin, alicyclic polyolefin resin, polyarylate resin, polyethersulfone resin, polysulfone resin, resin composed of a cycloolefin copolymer, fluorene ring-modified polycarbonate resin, alicyclic ring-modified polycarbonate resin, and fluorene ring-modified polyester resin.

[0073] The binder contained in the antiviral layer is preferably a polymer having a hydrophilic group (hereinafter also referred to as a "hydrophilic polymer"). When the antiviral layer contains a hydrophilic polymer, the antiviral layer exhibits greater hydrophilicity, has better antibacterial and antiviral properties, and can more easily remove contaminants adhering to the surface of the antiviral layer by washing with a washing liquid such as water.

[0074] The type of hydrophilic group is not particularly limited, and examples thereof include polyoxyalkylene groups (polyoxyethylene groups, polyoxypropylene groups, polyoxyalkylene groups in which oxyethylene groups and oxypropylene groups are block-bonded or random-bonded, etc.), amino groups, carboxy groups, alkali metal salts of carboxy groups, hydroxy groups, alkoxy groups, amide groups, carbamoyl groups, sulfonamide groups, sulfamoyl groups, sulfonic acid groups, and alkali metal salts of sulfonic acid groups. Among these, polyoxyalkylene groups are preferred because they provide better effects of the present invention. The main chain structure of the hydrophilic polymer is not particularly limited, and examples thereof include polyurethane, poly(meth)acrylate, polystyrene, polyester, polyamide, polyimide, and polyurea. Note that poly(meth)acrylate is a concept that includes both polyacrylate and polymethacrylate.

[0075] The hydrophilic polymer is preferably a polymer obtained by polymerizing a monomer having the above-mentioned hydrophilic group (hereinafter also referred to as "hydrophilic monomer"). The hydrophilic monomer refers to a compound (monomer and / or oligomer) having the above-mentioned hydrophilic group and a polymerizable group. The number of hydrophilic groups in the hydrophilic monomer is not particularly limited, but in order to make the antiviral layer more hydrophilic, one or more hydrophilic groups are preferred, one to six are more preferred, and one to three are even more preferred.

[0076] The type of polymerizable group in the hydrophilic monomer is not particularly limited, and examples thereof include radically polymerizable groups, cationically polymerizable groups, and anionically polymerizable groups. Examples of radically polymerizable groups include (meth)acryloyl groups, acrylamide groups, vinyl groups, styryl groups, and allyl groups. Examples of cationically polymerizable groups include vinyl ether groups, oxiranyl groups, and oxetanyl groups. Of these, (meth)acryloyl groups are preferred. The term "(meth)acryloyl group" encompasses both acryloyl groups and methacryloyl groups. The number of polymerizable groups in the hydrophilic monomer is not particularly limited, but is preferably 2 or more, more preferably 2 to 6, and even more preferably 2 to 3, in order to provide an antiviral layer with superior mechanical strength.

[0077] One preferred embodiment of the hydrophilic monomer is a compound represented by the following formula (A).

[0078]

[0079] In formula (A), R 1 represents a hydrogen atom or a substituent (monovalent substituent). The type of the substituent is not particularly limited, and examples thereof include known substituents, such as hydrocarbon groups which may have a hetero atom (e.g., alkyl groups and aryl groups), and the above-mentioned hydrophilic groups.

[0080] R 2 represents a polymerizable group, the definition of which is as described above.

[0081] L 1 represents a single bond or a divalent linking group. The type of the divalent linking group is not particularly limited, and examples thereof include -O-, -CO-, -NH-, -CO-NH-, -COO-, -O-COO-, an alkylene group, an arylene group, a heteroaryl group, and combinations thereof. 2 represents a polyoxyalkylene group. The polyoxyalkylene group means a group represented by the following formula (B).

[0082] Formula (B) *-(OR 3 ) m -* In formula (B), R 3 represents an alkylene group (for example, an ethylene group or a propylene group). m represents an integer of 2 or more, preferably 2 to 10, and more preferably 2 to 6. * represents a bonding position.

[0083] n represents an integer of 1 to 4.

[0084] The hydrophilic monomer having a hydrophilic group and a polymerizable group can be a commercially available product, such as "NK Ester A-GLY-9E" manufactured by Shin-Nakamura Chemical Co., Ltd., "Miramer M4004" manufactured by Toyo Chemicals Co., Ltd., or "Miramer M3150" manufactured by Toyo Chemicals Co., Ltd.

[0085] When producing a hydrophilic polymer, it is preferable to use a polyfunctional monomer having two or more polymerizable groups, as this will result in a superior mechanical strength of the antiviral layer. This is because polyfunctional monomers act as so-called crosslinking agents, forming a three-dimensional network structure that facilitates the movement of metal ions such as silver ions, making it possible to produce hydrophilic polymers that exhibit superior antibacterial and antiviral properties. From the above perspective, it is preferable to use two or more polyfunctional monomers. The polyfunctional monomer may or may not have a hydrophilic group. There is no particular restriction on the number of polymerizable groups contained in the polyfunctional monomer. From the perspective of superior mechanical strength of the antiviral layer and ease of handling, 2 to 10 polymerizable groups are preferred, and 2 to 6 are more preferred. Examples of polyfunctional monomers include trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, dipentaerythritol hexaacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate. Commercially available polyfunctional monomers (crosslinking agents) can be used. Examples of such commercially available products include "DPHA-76" (dipentaerythritol hexaacrylate) manufactured by Toshin Yushi Co., Ltd., "KAYARAD PET-30" (a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate) manufactured by Nippon Kayaku Co., Ltd., and "A-DPH" (dipentaerythritol hexaacrylate) manufactured by Shin-Nakamura Chemical Co., Ltd.

[0086] The hydrophilic polymer is preferably a copolymer composed of two or more different hydrophilic monomers. By using two or more hydrophilic monomers that differ in properties such as the number of functional groups and hydrophilicity, the strength, hydrophilicity, and / or optical properties of the antiviral layer can be controlled, thereby imparting properties to the antiviral layer according to the intended purpose. From the above perspective, the hydrophilic polymer is more preferably a copolymer composed of one or more compounds represented by formula (A) and one or more polyfunctional monomers, and even more preferably a copolymer composed of one or more compounds represented by formula (A) and two or more polyfunctional monomers. When the hydrophilic polymer is a copolymer of a compound represented by formula (A) and a polyfunctional monomer, the mixing ratio of the compound represented by formula (A) and the polyfunctional monomer is not particularly limited, but the ratio of the content (total content) of the compound represented by formula (A) to the content (total content) of the polyfunctional monomer is preferably 0.01 to 10, and more preferably 0.03 to 1, by mass.

[0087] A latex having the above-mentioned composition can also be used as the binder. Although various latexes can be used, acrylic latex is preferred because of its hydrophilicity and the ability to utilize aqueous coating. From the same viewpoint, it is also a preferred embodiment to use an aqueous polymer such as polyvinyl alcohol as the binder.

[0088] Alternatively, a siloxane resin, which is a polymer of a silicate-based compound, can be used as a hydrophilic binder. The silicate-based compound is a compound selected from the group consisting of a compound in which a hydrolyzable group is bonded to a silicon atom, a hydrolyzate thereof, and a hydrolyzed condensate thereof.

[0089] The binder content in the antiviral layer is not particularly limited, but is preferably 3 to 95% by mass, more preferably 5 to 90% by mass, and even more preferably 10 to 85% by mass, relative to the total mass of the antiviral layer.

[0090] <Light-diffusing particles> The antiviral layer contains light-diffusing particles. The light-diffusing particles are not particularly limited as long as they function as a so-called matting agent, and may be organic particles, inorganic particles, or organic-inorganic composite particles. Examples of organic particles include resin particles. More specifically, examples include silicone resin particles, acrylic resin particles such as polymethyl methacrylate (PMMA), nylon resin particles, styrene resin particles, polyethylene particles, urethane resin particles, and benzoguanamine particles. The organic particles may be particles having a hollow structure. Examples of inorganic particles include particles such as diamond, titanium oxide, zirconium oxide, lead oxide, lead carbonate, zinc oxide, zinc sulfide, antimony oxide, silicon oxide, and aluminum oxide. Titanium oxide and aluminum oxide are preferred from the viewpoint of the availability of particles with a suitable refractive index. As light-diffusing particles, silicone resin particles or acrylic resin particles are preferred, and acrylic resin particles are more preferred, because they can more effectively suppress rainbow unevenness.

[0091] Commercially available light diffusing particles include "MX-500," "MX-300," and "MX-80h3wT" manufactured by Soken Chemical & Engineering Co., Ltd., and "SSX-103" manufactured by Sekisui Chemical Co., Ltd.

[0092] The average particle size of the light diffusing particles is preferably 0.1 to 15 μm, more preferably 1.0 to 10 μm, and even more preferably 1.5 to 5 μm, because this allows rainbow unevenness to be more effectively suppressed.

[0093] The light-diffusing particles may be used alone or in combination of two or more types. The content of the light-diffusing particles is not particularly limited, but is preferably 1 to 15% by mass, more preferably 3 to 12% by mass, and even more preferably 6 to 8% by mass, of the total mass of the antiviral layer.

[0094] <Optional Components> The antiviral layer may contain optional components other than those described above, as long as the effects of the present invention are achieved. Examples of optional components include a dispersant, a surfactant, and a hydrophilicity-imparting agent.

[0095] (Dispersant) The antiviral layer may contain a dispersant. A dispersant is a compound that has the function of improving the dispersibility of antiviral agent particles. The dispersant is not particularly limited, and known dispersants can be used, but dispersants having an acidic group are preferred, and dispersants having both an acidic group and a basic group are more preferred. Examples of the acidic group include a carboxy group, a sulfonic acid group, and a phosphate group. Examples of the basic group include an amino group and an amide group.

[0096] Commercially available dispersants include, for example, DISPERBYK-102, DISPERBYK-106, DISPERBYK-108, DISPERBYK-110, DISPERBYK-111, DISPERBYK-140, DISPERBYK-142, DISPERBYK-9076, DISPERBYK-118 and DISPERBYK-180 (manufactured by BYK-Chemie Co., Ltd.), Solsperse 26000, Solsperse 36000, and Solsperse 41000 (manufactured by Lubrizol Co., Ltd.), and Ajisper PB821, Ajisper PB822, Ajisper PB824, and Ajisper PB881 (manufactured by Ajinomoto Fine-Techno Co., Ltd.). Among these, DISPERBYK-180 or AJISPER PB881, which have both an acidic group and a basic group, are preferred.

[0097] The dispersants may be used alone or in combination of two or more. When the antiviral layer contains a dispersant, the content of the dispersant is preferably 10 to 500% by mass relative to the total mass of the antiviral agent particles.

[0098] (Surfactant) The antiviral layer may contain a surfactant. The surfactant can adjust the water contact angle of the surface of the antiviral layer to a desired range. Furthermore, when the antiviral layer is formed by a coating method using the composition for forming an antiviral layer described below, a coating film with a more uniform thickness and / or a smoother surface is likely to be formed. The surfactant is not particularly limited, and known surfactants can be used. Examples of surfactants include nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants.

[0099] Examples of nonionic surfactants include ester types such as glycerin fatty acid esters, sorbitan fatty acid esters, and sucrose fatty acid esters, ether types such as polyoxyethylene alkyl ethers and polyoxyethylene polyoxypropylene glycols, ester-ether types such as fatty acid polyethylene glycols and fatty acid polyoxyethylene sorbitan, and alkanolamide types such as fatty acid alkanolamides. More specific nonionic surfactants include polyethylene glycol mono(meth)acrylate, polyethylene glycol monolauryl ether, polyethylene glycol monostearyl ether, polyethylene glycol monocetyl ether, polyethylene glycol monolauryl ester, and polyethylene glycol monostearyl ester.

[0100] Examples of ionic surfactants include anionic surfactants such as alkyl sulfates, alkyl benzene sulfonates, and alkyl phosphates; cationic surfactants such as alkyl trimethyl ammonium salts and dialkyl dimethyl ammonium salts; and amphoteric surfactants such as alkyl carboxy betaines.

[0101] As the surfactant, a fluorine-based surfactant can also be used, such as the compounds described in paragraphs 0082 to 0090 of JP-A-2014-119605.

[0102] The fluorine-based surfactant preferably contains a polymerizable group. Examples of surfactants containing a polymerizable group include X-71-1203E (manufactured by Shin-Etsu Chemical Co., Ltd.), Fluorosurf (registered trademark) FS-7072 (manufactured by Fluorotechnology Inc.), and Megafac (registered trademark) F-780-F, RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).

[0103] Since there are concerns about the environmental compatibility of compounds having a linear perfluoroalkyl group having seven or more carbon atoms, it is preferable to use alternative materials to perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS) as fluorosurfactants.

[0104] The surfactant may be used alone or in combination of two or more. When the antiviral layer contains a surfactant, the content of the surfactant is preferably 0.1 to 10% by mass relative to the total mass of the antiviral layer.

[0105] (Hydrophilicity Imparting Agent) The antiviral layer may contain a hydrophilicity imparting agent. The hydrophilicity imparting agent is a compound that has the function of reducing the water contact angle on the surface of the antiviral layer, and is intended to be a compound that is not included in the above-mentioned surfactants. The hydrophilicity imparting agent is not particularly limited as long as it is a compound that has the function of reducing the water contact angle on the surface of the antiviral layer, and examples thereof include ethyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate. One type of hydrophilicity imparting agent may be used alone, or two or more types may be used in combination. When the antiviral layer contains a hydrophilicity imparting agent, the content of the hydrophilicity imparting agent is preferably 0.1 to 30% by mass relative to the total mass of the antiviral layer.

[0106] Examples of optional components that the antiviral layer may contain other than those described above include a polymerization initiator, an ultraviolet absorber, a filler, an antioxidant, an antistatic agent, a flame retardant, an adhesion promoter, an antioxidant, an antifoaming agent, a leveling agent, a matting agent, a light stabilizer, a deodorizer, a dye, a fragrance, and a pigment, which will be described later.

[0107] <Physical Properties of Antiviral Layer> The thickness of the antiviral layer is not particularly limited, but from the viewpoints of film strength and suppression of curling, it is preferably 0.01 to 10 μm, more preferably 0.5 to 5 μm, and even more preferably 1 to 3 μm. The thickness of the antiviral layer is measured by embedding a sample piece having the antiviral layer in resin, cutting out a cross section with a microtome, and observing the cut-out cross section with a scanning electron microscope. The thickness of the antiviral layer is measured at any 10 positions on the antiviral layer using the method described above, and the arithmetic mean of the measured values ​​is used.

[0108] The water contact angle on the surface of the antiviral layer is preferably 20 degrees or more, more preferably 70 degrees or more, because stains such as sebum are less likely to adhere to the surface of the antiviral layer. While there is no particular upper limit, it is preferably 120 degrees or less, more preferably 110 degrees or less. In this specification, the water contact angle refers to a water contact angle measured by the following method. Using a contact angle meter (FAMMS DM-701, manufactured by Kyowa Interface Science Co., Ltd.), pure water (2 μL droplets) is dropped onto the surface of the antiviral layer, which is held horizontally. After the drop, the contact angles are measured at 10 points 20 seconds later, and the arithmetic mean value of the measurement results is taken as the water contact angle of the antiviral layer. The test is performed in accordance with the sessile drop method of JIS (Japanese Industrial Standards) R 3257:1999, at a room temperature of 20°C.

[0109] [Other Layers] The antiviral film may have layers other than the substrate and antiviral layer described above. Examples of layers other than the substrate and antiviral layer include a pressure-sensitive adhesive layer, a release film, the protective sheet described above, and the easy-adhesion layer (primer layer).

[0110] The antiviral film may have an adhesive layer. The adhesive layer is used to attach the antiviral film to the antiviral layer-forming surface of various devices. The adhesive layer may be any type that can attach the antiviral film to various antiviral layer-forming surfaces, and may be formed using a known adhesive. Examples of adhesives that can be used for the adhesive layer include (meth)acrylic adhesives, rubber-based adhesives, silicone-based adhesives, urethane-based adhesives, and polyester-based adhesives. The (meth)acrylic adhesive refers to an acrylic adhesive and / or a methacrylic adhesive. When the antiviral film has an adhesive layer, it is preferable that the antiviral layer is disposed on one surface of the substrate, and that the adhesive layer is disposed on the surface of the substrate opposite to the surface on which the antiviral layer is disposed. This ensures that when the antiviral film is attached to the antiviral layer-forming surface of a device, the antiviral layer is disposed closer to the exposed surface.

[0111] The thickness of the adhesive layer is not particularly limited, but is preferably 1 to 30 μm, and more preferably 2 to 20 μm. The adhesive strength of the adhesive layer is not particularly limited, but is preferably 2 to 20 cN / 25 mm. If the adhesive strength is 2 cN / 25 mm or more, peeling or the like is unlikely to occur when the antiviral film is attached to the surface of a touch panel or the like. On the other hand, if the adhesive strength is 20 cN / 25 mm or less, the antiviral film can be peeled off smoothly.

[0112] When the antiviral film has an adhesive layer, it preferably further has a release film. The release film is adhered to the adhesive layer to protect the adhesive layer until the antiviral film is used. Any release film can be used as long as it can protect the adhesive layer, and known release films can be used. Examples of release films include release agents such as silicone compounds, long-chain alkyl compounds, and polyvinyl alcohol carbamate. The thickness of the release film is not particularly limited, but is preferably 1 to 30 μm, and more preferably 2 to 20 μm.

[0113] [Method for Producing Antiviral Film] The method for producing an antiviral film is not particularly limited as long as it can produce an antiviral film having a substrate and an antiviral layer disposed on the substrate. Examples of methods for producing an antiviral film include a method of forming an antiviral layer on a substrate, a method of forming a substrate on an antiviral layer, a method of laminating a preformed antiviral layer and a preformed substrate, and a method of forming and adhering the antiviral layer and the substrate by coextrusion or the like. Among these, a method (coating method) of forming an antiviral film by applying an antiviral layer-forming composition to a predetermined position on a substrate to form a coating film and drying and / or curing the coating film is preferred, and a method including the steps of applying an antiviral layer-forming composition to a predetermined position on a substrate to form a coating film, heating and drying the coating film, and irradiating the coating film with ultraviolet light to cure the coating film to form an antiviral layer is more preferred.

[0114] The composition for forming an antiviral layer contains at least antiviral agent particles, a binder, and light-diffusing particles. When the binder is a polymer obtained by polymerizing a monomer, the composition for forming an antiviral layer may contain at least antiviral agent particles, a monomer (e.g., a hydrophilic monomer and a polyfunctional monomer), and light-diffusing particles. The composition for forming an antiviral layer will be described later.

[0115] The method for applying the antiviral layer-forming composition to the surface of the substrate is not particularly limited, and any known application method can be used. Examples of methods for applying the antiviral layer-forming composition to the surface of the substrate include a spray method, a wire bar coating method, an extrusion coating method, a direct gravure coating method, a reverse gravure coating method, an inkjet method, a die coating method, an electrostatic coating method, and a wipe method.

[0116] An antiviral layer is formed by drying and / or curing the coating film formed on the surface of the substrate by the above-mentioned coating method. Methods for removing the solvent from the coating film of the composition for forming an antiviral layer and drying it include, for example, heat treatment. The conditions for the heat treatment are not particularly limited, but the heating temperature is preferably 20 to 150°C, more preferably 20 to 60°C. The heating time is preferably 15 to 600 seconds.

[0117] The antiviral layer may be formed by curing the coated film of the monomer-containing composition for forming an antiviral layer through exposure treatment. The exposure treatment at this time is not particularly limited, but may be performed at a dose of 190 mJ / cm 2 It is preferable to cure the coating film by irradiating it with ultraviolet light in an amount equal to or greater than 600 mJ / cm. There is no particular upper limit to the amount of irradiation. 2 The following are preferred: In the case of ultraviolet irradiation, ultraviolet light emitted from light rays of an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a carbon arc, a xenon arc, a metal halide lamp, or the like can be used.

[0118] <Composition for forming an antiviral layer> The composition for forming an antiviral layer contains at least antiviral agent particles, a binder or monomer, and light diffusing particles. The composition for forming an antiviral layer may contain the optional components contained in the antiviral layer. The composition for forming an antiviral layer preferably contains a solvent. Furthermore, when the composition for forming an antiviral layer contains a monomer, it preferably further contains a polymerization initiator. When the composition for forming an antiviral layer contains a polymerization initiator, the antiviral layer containing the polymer has better mechanical strength. The components other than the solvent and the polymerization initiator, including their preferred embodiments, are as already explained.

[0119] The solvent contained in the composition for forming an antiviral layer is not particularly limited, and examples thereof include water and organic solvents. Among these, it is preferable that the solvent contains an organic solvent, since it is easier to make the thickness of the coating film more uniform. Examples of organic solvents include alcohol-based solvents, ester-based solvents, ketone-based solvents, and ether-based solvents. More specific examples of the organic solvent include methanol, ethanol, acetone, methyl ethyl ketone, cyclohexane, ethyl acetate, ethylene dichloride, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetylacetone, cyclohexanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether acetate, 3-methoxypropanol, methoxyethanol, methyl ethyl ether, methyl ... Examples of suitable organic solvents include alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate, n-propanol, isopropanol, n-butanol, 2-butanol, i-butanol, t-butanol, n-pentanol, t-amyl alcohol, n-hexanol, capryl alcohol, lauryl alcohol, myristyl alcohol, phenylethyl alcohol, ethylene glycol, ethylene glycol mono-n-butyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol mono-n-butyl ether, tetraethylene glycol mono-n-butyl ether, and dipropylene glycol monobutyl ether. The boiling point of the organic solvent is not particularly limited, but is preferably 70 to 160°C, more preferably 80 to 150°C. One solvent may be used alone, or two or more solvents may be used in combination. It is particularly preferred to use two or more solvents with different properties in combination, and it is more preferred to use three or more solvents with different properties in combination. Such properties include, for example, boiling point, chemical structure, and polarity.That is, it is preferable to use two or more solvents with different boiling points in combination as the solvent, and more preferably to use three or more solvents with different boiling points in combination. It is also preferable to use two or more solvents selected from the group consisting of alcohol-based solvents, ester-based solvents, ketone-based solvents, and ether-based solvents in combination. By using solvents with different properties in combination as described above and selecting a ratio that suits the type of raw material that becomes the solid content, the coating method, the drying method, and the like, it is possible to control the surface properties of the antiviral layer. The solid content of the antiviral layer-forming composition, i.e., the total content of components other than the solvent, is not particularly limited, but is preferably 1 to 50% by mass relative to the total mass of the antiviral layer-forming composition, in order to easily form a coating film with a more uniform thickness.

[0120] The polymerization initiator is not particularly limited, and known polymerization initiators can be used. Examples of the polymerization initiator include thermal polymerization initiators and photopolymerization initiators, with photopolymerization initiators being preferred due to their excellent reaction efficiency. Examples of the polymerization initiator include aromatic ketones such as benzophenone and phenylphosphine oxide; α-hydroxyalkylphenone compounds (IRGACURE (Omnirad) 184, 127, 2959, and DAROCUR 1173, manufactured by BASF); and phenylphosphine oxide compounds (monoacylphosphine oxide: IRGACURE (Omnirad) TPO manufactured by BASF, and bisacylphosphine oxide: IRGACURE (Omnirad) 819 manufactured by BASF). One type of polymerization initiator may be used alone, or two or more types may be used in combination. When the antiviral layer-forming composition contains a polymerization initiator, the content of the polymerization initiator is not particularly limited, but is preferably 0.1 to 15% by mass, and more preferably 1 to 6% by mass, relative to the content of the monomer.

[0121] The composition for forming an antiviral layer can be prepared by mixing the above components. The order of mixing the above components is not particularly limited, but when the composition for forming an antiviral layer contains a dispersant, the antiviral agent particles and the dispersant may be mixed first to prepare a dispersion in which the antiviral agent particles are dispersed.

[0122] [Uses of Antiviral Film] The antiviral film of the present invention can be used in a variety of applications. For example, by placing the antiviral film on the surface of various articles, antibacterial and antiviral properties can be imparted to the surface of the article. In particular, it is preferable to place the antiviral film of the present invention on the surface of the image display unit of a touch panel to produce a touch panel with the antiviral film. The antiviral film of the present invention can exhibit good antibacterial and antiviral properties and good rainbow unevenness suppression effect even in situations where the touch panel is frequently touched by fingers or the like when operating the touch panel.

[0123] The uses of the touch panel with an antiviral film are not particularly limited, and it can be used as an input device and an image display device in electronic devices such as personal computers, mobile phones, game machines, medical equipment, automated teller machines (ATMs), ordering devices, ticket vending machines, copiers, and car navigation systems.

[0124] The antiviral film of the present invention can also be used as a face guard or a partition board. The antiviral film of the present invention can also be used by being attached to a wall, window glass, or the like.

[0125] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below.

[0126] [Production of Polyester Resin Film] [Production Example 1] <Production Process of Polyester Resin Pellets (Material Polyester Resin)> A polyester resin was continuously produced using a continuous polymerization apparatus according to the following procedures (1) and (2).

[0127] (1) Esterification Reaction A mixing tank was charged with 4.7 tons of high-purity terephthalic acid and 1.8 tons of ethylene glycol as polyester resin precursors, and the mixture was mixed over 90 minutes to form a slurry. The resulting slurry was continuously supplied from the mixing tank to the first esterification reactor at a flow rate of 3,800 kg / h. Furthermore, an ethylene glycol solution of a citric acid chelate titanium complex (VERTEC AC-420, Johnson Matthey) in which citric acid was coordinated to Ti element was continuously supplied to the first esterification reactor, and the reaction was carried out at an internal temperature of 250°C with stirring for an average residence time of approximately 4.3 hours. The citric acid chelate titanium complex was continuously added so that the amount of Ti added was 9 ppm by mass, in elemental terms, relative to the total amount of polyester resin precursor. The acid value of the resulting reaction product (oligomer) was 500 eq / ton.

[0128] The reaction product obtained in the first esterification reactor was transferred to the second esterification reactor and reacted with stirring at an internal temperature of 250°C for an average residence time of 1.2 hours to obtain an oligomer having an acid value of 190 eq / ton. The interior of the second esterification reactor was partitioned into three zones, consisting of a first zone, a second zone, and a third zone, in the order in which the oligomers were supplied. An ethylene glycol solution of magnesium acetate was continuously supplied from the second zone so that the Mg addition amount was 75 ppm by mass, in elemental terms, relative to the total amount of oligomers, and subsequently an ethylene glycol solution of trimethyl phosphate was continuously supplied from the third zone so that the P addition amount was 60 ppm by mass, in elemental terms, relative to the total amount of oligomers.

[0129] (2) Polycondensation Reaction The esterification reaction product obtained above was continuously supplied to a first polycondensation reaction tank, and the mixture was stirred at a reaction temperature of 270°C and an internal pressure of 20 torr (2.67 x 10 -3 The intermediate polymer obtained in the first polycondensation reaction tank was transferred to a second polycondensation reaction tank, and the mixture was stirred at an internal temperature of 276°C and an internal pressure of 3.0 torr (3.99 x 10 -4The intermediate polymer obtained in the second polycondensation reaction tank was transferred to a third polycondensation reaction tank, and the reaction was continued under the conditions of an internal temperature of 278°C and an internal pressure of 1.0 torr (1.33 x 10 -4 The mixture was reacted (polycondensed) at a pressure of 1.5 MPa for a residence time of 1.5 hours, and a polyester resin (polyethylene terephthalate (PET) resin) was discharged as a product from the third polycondensation reaction tank. The resulting product was discharged into cold water in the form of a strand, and immediately cut to produce raw material polyester, which was polyester resin pellets (cross section: major axis approximately 4 mm, minor axis approximately 2 mm, length approximately 3 mm).

[0130] <Production Process of Polyester Resin Film> -Film Forming Process- The raw polyester obtained in the above process was dried to a moisture content of 100 ppm by mass or less and then charged into the hopper of a single-screw extruder with a diameter of 50 mm. The raw polyester was heated to 290°C to melt, and extruded through a die at a melt temperature of 280°C via a gear pump and a melt filter (leaf disc filter; NF2M-4C (manufactured by Nippon Seisen Co., Ltd.)). The molten resin extruded from the die was extruded onto a cooling cast drum set at a temperature of 25°C and adhered to the cooling cast drum using an electrostatic application method. The resin was peeled off using a peeling roll arranged opposite the cooling cast drum to obtain an unstretched polyester resin film.

[0131] The obtained unstretched polyester resin film had an intrinsic viscosity IV of 0.62 dL / g, a carboxyl group amount of 30 eq / ton, a refractive index in the longitudinal direction of 1.573, and a crystallinity of 0.2%.

[0132] The intrinsic viscosity IV was determined by dissolving an unstretched polyester resin film in a mixed solvent of 1,1,2,2-tetrachloroethane / phenol (=2 / 3 [mass ratio]) and measuring the solution viscosity at 25°C in the mixed solvent.

[0133] The refractive index of an unstretched polyester resin film was measured by the following method. Using two polarizing plates, the orientation axis direction of the unstretched polyester resin film was determined, and a 4 cm × 2 cm rectangle was cut out so that the orientation axes were perpendicular to each other to prepare a measurement sample. For this sample, the refractive indices of the orthogonal biaxial directions (nx, ny) and the refractive index in the thickness direction (nz) were determined using an Abbe refractometer (manufactured by Atago Co., Ltd., NAR-4T, measurement wavelength 589 nm).

[0134] The crystallinity of the unstretched polyester resin film was calculated by the following method. The crystallinity can be calculated from the density of the film. The density X (g / cm 3 ), density 1.335 g / cm at 0% crystallinity 3 , density at 100% crystallinity 1.501 g / cm 3 The crystallinity (%) was calculated using the following formula: Crystallinity = {Z x (X - Y)} / {X x (Z - Y)} x 100. The density was measured in accordance with JIS K7112.

[0135] - Longitudinal Stretching Step - The unstretched polyester resin film was passed between two pairs of nip rolls with different peripheral speeds and stretched in the longitudinal direction (conveyance direction) (longitudinal stretching) under the following longitudinal stretching conditions: <<Longitudinal Stretching Conditions>> Preheating temperature: 80°C Longitudinal stretching temperature: 90°C Longitudinal stretching ratio: 3.3 times

[0136] -Transverse Stretching Step- The longitudinally stretched polyester resin film was introduced into a tenter (transverse stretching machine) and preheated while the edges of the film were held with clips. The preheating temperature was 90°C. Next, the preheated unstretched polyester resin film was stretched in the width direction (transverse stretching) using the tenter under the following transverse stretching conditions. <<Transverse Stretching Conditions>> Transverse stretching temperature (average temperature during transverse stretching): 90°C Transverse stretching ratio: 3.3 times Film surface temperature at the start of transverse stretching: 95°C Film surface temperature at the end of transverse stretching: 150°C

[0137] The film surface temperature was measured using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, used with an emissivity of 0.95).

[0138] The polyester resin film after transverse stretching was cooled in an intermediate cooling section by blowing cold air from nozzles above and below the polyester resin film so that the minimum film surface temperature TMC of the polyester resin film was 85°C. The film surface temperature of the polyester resin film in the intermediate cooling section was measured using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95). The film surface temperature was measured at 10 points evenly spaced in the MD direction within the intermediate cooling section, and the minimum temperature was taken as the minimum film surface temperature TMC.

[0139] Next, hot air was blown onto the polyester resin film from above and below the film using a hot air blowing nozzle, and the polyester resin film was heat-set while controlling the film surface temperature within the following range: Maximum film surface temperature (heat-set temperature): 170°C; Heat-set time: 15 seconds.

[0140] The polyester resin film after heat setting was heated to the following temperatures by blowing hot air from a hot air blowing nozzle onto the polyester resin film from above and below, and the polyester resin film was relaxed. Heat relaxation temperature: maximum film surface temperature of the heat setting part -10°C (160°C in the case of Production Example 1) Heat relaxation rate: 15% in TD direction (film width direction), 5.5% in MD direction (film flow direction)

[0141] Next, the polyester resin film after the heat relaxation was cooled at a cooling temperature such that the film surface temperature of the polyester resin film became 40° C. The film surface temperature was measured using a radiation thermometer (manufactured by Hayashi Denko, model number: RT61-2, emissivity 0.95).

[0142] After cooling and releasing the film from the clips, both ends of the polyester resin film were trimmed by 30 cm. The trimmed film width was 2.0 m. After that, both ends were extruded (knurled) to a width of 10 mm, and the film was wound into a roll with a length of 10,000 m at a tension of 18 kg / m. In this way, a polyester resin film of Production Example 1 with a thickness of 40 μm was produced.

[0143] [Production Example 2] A polyester resin film was produced in the same manner as in Production Example 1, except that the longitudinal stretching ratio was changed to 3.4 times and the transverse stretching ratio was changed to 3.8 times.

[0144] [Production Example 3] A polyester resin film was produced in the same manner as in Production Example 1, except that the longitudinal stretching ratio was changed to 3.0 times and the transverse stretching ratio was changed to 3.0 times.

[0145] [Production Example 4] A polyester resin film was produced in the same manner as in Production Example 1, except that the thickness of the polyester resin film was changed to 19 µm.

[0146] [Production Example 5] A polyester resin film was produced in the same manner as in Production Example 1, except that the thickness of the film in Example 1 was changed to 63 µm.

[0147] [Production Example 6] [Production of Polyester Film] A polyester resin film was produced in the same manner as in Production Example 1, except that the melting temperature of the raw polyester was changed to 300°C to obtain an unstretched polyester resin film.

[0148] [Production Example 7] Polyester resin pellets (raw material polyester) were produced in the same manner as in Production Example 1, except that, during the synthesis of the polyester resin, an ethylene glycol solution of antimony trioxide was continuously supplied as a polymerization catalyst so that the Sb addition amount was 120 ppm by mass in elemental equivalent value, and an ethylene glycol solution of magnesium acetate and an ethylene glycol solution of trimethyl phosphate were continuously supplied to the second esterification reaction tank so that the Mg addition amount and P addition amount were 65 ppm by mass and 35 ppm by mass in elemental equivalent values, respectively. Using the obtained raw material polyester, a polyester resin film was produced in the same manner as in Production Example 1.

[0149] [Production Example 8] Polyester resin pellets (raw polyester) were produced in the same manner as in Production Example 1, except that in the synthesis of the polyester resin in Production Example 1, the amount of citric acid chelate titanium complex added was changed so that the amount of Ti added was 4.5 ppm by mass in terms of elemental value. Using the obtained raw polyester, a polyester resin film was produced in the same manner as in Production Example 1.

[0150] [Production Example 9] Polyester resin pellets (raw polyester) were produced in the same manner as in Production Example 1, except that in the synthesis of the polyester resin in Production Example 1, the amount of citric acid chelate titanium complex added was changed so that the amount of Ti added was 16 ppm by mass in terms of elemental value. Using the obtained raw polyester, a polyester resin film was produced in the same manner as in Production Example 1.

[0151] [Production Example 10] A polyester resin film was produced in the same manner as in Production Example 1, except that the transverse stretching ratio was changed to 3.8 times and the heat setting temperature after transverse stretching was changed to 150°C.

[0152] [Production Example 11] A polyester resin film was produced in the same manner as in Production Example 1, except that the longitudinal stretching ratio was changed to 3.2 times, the transverse stretching ratio was changed to 3.2 times, and the heat setting temperature after transverse stretching was changed to 190°C.

[0153] Comparative Production Example 1 A polyester resin film was produced in the same manner as in Production Example 7, except that the longitudinal stretching ratio was 3.4 times, the transverse stretching ratio was 4.0 times, the heat setting temperature was 230°C, and the thickness after stretching was 100 µm.

[0154] [Evaluation] <Plane Orientation Coefficient ((nx+ny) / 2-nz)> For the polyester resin film of each Production Example, nx (refractive index in the in-plane slow axis direction of the polyester resin film), ny (refractive index in the in-plane fast axis direction of the polyester resin film), and nz (refractive index in the thickness direction of the polyester resin film) were measured. Specifically, using two polarizing plates, the orientation axis direction of the polyester resin film was determined, and a 4 cm x 2 cm rectangle was cut out so that the orientation axis directions were perpendicular to each other to serve as a measurement sample. For this sample, the orthogonal biaxial refractive indices (nx, ny) and the thickness direction refractive index (nz) were determined using an Abbe refractometer (manufactured by Atago Co., Ltd., NAR-4T, measurement wavelength 589 nm). From these values, the value of "(nx+ny) / 2-nz" was calculated. The value of "(nx+ny) / 2-nz" for the polyester resin film is recorded in the "Plane Orientation Coefficient" column in the table below.

[0155] <Film Thickness> The thickness of the polyester resin film of each Production Example was determined as follows. Using a contact film thickness meter (manufactured by Anritsu Corporation), 50 samples were taken at equal intervals over 0.5 m in the longitudinal stretching direction (longitudinal direction) of the polyester resin film of each Production Example, and 50 samples were taken at equal intervals (divided into 50 equal parts in the width direction) across the entire width of the film in the film width direction (direction perpendicular to the longitudinal direction), and the thickness of these 100 samples was then measured. The average thickness of these 100 samples was determined and used as the thickness of the polyester resin film.

[0156] <Pre-peak temperature> The polyester resin film of each production example was subjected to differential scanning calorimetry from 30°C to 300°C at a temperature increase rate of 10°C / min, and a small endothermic peak appearing before the melting peak of the polyester resin film was measured to determine the pre-peak temperature of the polyester resin film.

[0157] <MD Heat Shrinkage Rate> The polyester resin film of each production example was cut at three points, the center in the width direction and both ends, to create three types of sample pieces M measuring 30 mm in the TD direction and 120 mm in the MD direction. Two reference lines were made on the three types of sample pieces M so that they were spaced 100 mm apart in the MD direction, and the pieces were left standing in a heating oven at 80°C under no tension for 24 hours. After this standing, the three types of sample pieces M were cooled to room temperature, and the distance between the two reference lines was measured. The average of these three values ​​was taken as A (unit: mm). The measured A and a value calculated from the formula "100 x (100 - A) / 100" were taken as the MD heat shrinkage rate.

[0158] The polyester resin film of each production example was cut at three points, the center in the width direction, and both ends, to create three types of sample pieces M measuring 30 mm in the MD direction and 120 mm in the TD direction. Two reference lines were made on the three types of sample pieces M so that they were 100 mm apart in the TD direction, and the pieces were left standing in a heating oven at 80°C under no tension for 24 hours. After this standing, the three types of sample pieces M were cooled to room temperature, and the distance between the two reference lines was measured, and the average of the three values ​​was taken as A (unit: mm). The measured A and a value calculated from the formula "100 x (100 - A) / 100" were taken as the MD heat shrinkage rate.

[0159] The catalysts used in each production example, the film-forming conditions, and the film properties are shown in the table below. Note that Ti1 in the "catalyst type" column is "citric acid chelate titanium complex," and Sb1 is "antimony trioxide." The numerical value in the "catalyst added amount" column is the amount of Ti added in elemental equivalent of citric acid chelate titanium complex relative to the total amount of polyester resin precursor when Ti1 is used as the catalyst, and is the amount of Sb added in elemental equivalent of antimony trioxide relative to the total amount of polyester resin precursor when Sb1 is used as the catalyst.

[0160]

[0161]

[0162] [Preparation of antiviral layer-forming compositions] The materials listed in the table below were mixed, and the resulting mixture was stirred to prepare antiviral layer-forming compositions (compositions A-1 and A-2). The solids concentration of compositions A-1 and A-2 was 26.0% by mass. The values ​​listed in the table below are in parts by mass.

[0163]

[0164] Details of the materials listed in the table above are as follows. Monomer 1: "DPHA-76" manufactured by Toshin Yushi Co., Ltd. (dipentaerythritol hexaacrylate, multifunctional monomer, solid content 76% by mass) Monomer 2: "KAYARAD PET-30" manufactured by Nippon Kayaku Co., Ltd. (mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate, multifunctional monomer) Monomer 3: "NK Ester A-GLY-9E" manufactured by Shin-Nakamura Chemical Co., Ltd. (ethylene oxide 9 mol modified glycerin triacrylate, hydrophilic monomer represented by the above-mentioned formula (A)) Antiviral agent particle 1: zirconium phosphate-based silver antibacterial agent (manufactured by Toagosei Co., Ltd., average particle size 1.0 μm, silver content 3.7% by mass, zirconium phosphate-based carrier) Light diffusion particle 1: "MX-300" manufactured by Soken Chemical & Engineering Co., Ltd. (acrylic resin particles, average particle size 3.0 μm) Light diffusing particles 2: "FS-101" manufactured by Nippon Paint Industrial Coatings (acrylic resin particles, average particle size 0.08 μm) Polymerization initiator 1: "Omnirad 184" manufactured by BASF Dispersant 1: "DISPERBYK-180" manufactured by BYK Surfactant 1: "X-71-1203E" manufactured by Shin-Etsu Chemical Co., Ltd. (urethane acrylate fluororesin composed of 2-isocyanate ethyl acrylate and ethylene glycol, solid content 20% by mass) Solvent 1: isopropyl alcohol Solvent 2: 1-methoxy-2-propyl acetate Solvent 3: 1-methoxy-2-propanol

[0165] [Production of Antiviral Film] [Example 1] An easy-adhesion layer containing a urethane resin and silica particles and having a thickness of 0.1 μm was formed on one side of the polyester resin film obtained in Production Example 1. Composition A-1 was applied to the surface of the polyester resin film on the easy-adhesion layer side to form a coating film. The coating film was then dried by heating at 60°C for 2 minutes, and then 290 mJ / cm 2 The coated film was cured by irradiating it with ultraviolet light at a dose of 1000 W / m² to form an antiviral layer. The thickness of the formed antiviral layer was 2.5 μm. The contents of the binder (hydrophilic polymer obtained by polymerizing the above-mentioned Monomer 1, Monomer 2, and Monomer 3), the antimicrobial particles, and the light diffusing particles in the antiviral layer were 76.5 mass %, 2.4 mass %, and 7.0 mass %, respectively, relative to the total mass of the antiviral layer.

[0166] Examples 2 to 11 Except for changing the type of polyester resin film to those shown in the table below, antiviral films were produced in the same manner as in Example 1. The contents of the binder (hydrophilic polymer obtained by polymerizing Monomer 1, Monomer 2, and Monomer 3), antimicrobial particles, and light-diffusing particles in the antiviral layer were 76.5% by mass, 2.4% by mass, and 7.0% by mass, respectively, relative to the total mass of the antiviral layer.

[0167] Comparative Examples 1 and 2 Antiviral films were produced in the same manner as in Example 1, except that the type of polyester resin film and the composition for forming the antiviral layer were changed to those shown in the table below.

[0168]

[0169] [Evaluation] <Evaluation of antiviral / antibacterial properties> (Anti-influenza virus property, anti-novel coronavirus property, and anti-Escherichia coli property) The antiviral / antibacterial properties of the antiviral film were measured by the following method: The antiviral film was cut into a 50 mm square, and the cut test piece was placed in a sterile petri dish to prepare a specimen.

[0170] (Evaluation of anti-influenza virus and anti-novel coronavirus properties) The number of viruses on the surface of the antibacterial layer of the prepared test piece was 1 × 107 ~5 x 10 7 0.4 ml of influenza virus fluid or novel coronavirus (SARS-CoV-2) fluid prepared to give PFU / ml was inoculated and cultured at 25°C. After 24 hours of culture, the antiviral activity value of each test piece was measured and the antiviral properties (anti-influenza virus activity and anti-novel coronavirus activity) were evaluated according to the following criteria. The antiviral activity values ​​for anti-influenza virus activity and anti-novel coronavirus activity were evaluated in accordance with the evaluation method described in ISO 21702.

[0171] -Evaluation criteria for anti-influenza virus activity- A: Antiviral activity value is 2.0 or more B: Antiviral activity value is less than 2.0

[0172] -Evaluation criteria for anti-coronavirus activity- A: Antiviral activity value is 2.0 or more B: Antiviral activity value is less than 2.0

[0173] (Evaluation of anti-E. coli activity) The number of bacteria on the surface of the antibacterial layer of the prepared test piece was 2.5 × 10 5 ~10 x 10 5 0.4 ml of Escherichia coli solution prepared to give a concentration of 100 cells / ml was inoculated onto the test specimens, and the specimens were cultured in an incubator at a temperature of 35°C and a relative humidity of 90%. The antibacterial activity of each test specimen was measured after 24 hours of culture, and the antibacterial activity was evaluated according to the following criteria. The antibacterial activity value for the anti-Escherichia coli activity was evaluated in accordance with the evaluation method described in JIS Z 2801.

[0174] - Evaluation criteria for anti-Escherichia coli activity A: Antibacterial activity value is 2.0 or more B: Antibacterial activity value is less than 2.0

[0175] <Evaluation of Optical Properties> The average haze (h1) in the wavelength range of 400 to 700 nm of the antiviral film immediately after production and the average haze (h2) in the wavelength range of 400 to 700 nm of the antiviral film after 720 hours of wet heat treatment at a temperature of 60°C and a relative humidity of 90% were measured. The haze of the antiviral film was measured using the following method. A spectrophotometer equipped with an integrating sphere unit ("VAP-7070" manufactured by JASCO Corporation) was used to measure the transmittance of light passing through the antiviral film. The antiviral film and the integrating sphere unit were positioned close to each other to measure the omnidirectional transmittance (τs) of the antiviral film, and the antiviral film and the integrating sphere unit were positioned apart to measure the rectilinear transmittance (τl) of the antiviral film. Each transmittance was measured every 5 nm in the measurement wavelength range of 400 to 700 nm. Furthermore, before measuring each transmittance, the spectrophotometer was calibrated by measuring the transmittance without the antiviral film installed. The haze (%) for each wavelength was calculated using the formula (τs-τl) x 100 / τs from the omnidirectional transmittance τs and rectilinear transmittance τl for each wavelength. The average haze value for wavelengths of 400 to 700 nm was calculated from the obtained haze for each wavelength. In addition, Δh (the degree of variation in the average haze value for the antiviral film in the wavelength range of 400 to 700 nm before and after moist heat treatment) was calculated using the following formula: Δh = |h1-h2|

[0176] <Iridescent unevenness> The rainbow unevenness (initial) of the antiviral film immediately after production and the rainbow unevenness (over time) of the antiviral film after wet heat treatment for 720 hours under conditions of a temperature of 60°C and a relative humidity of 90% were measured by the following method.

[0177] A polarizer was prepared according to paragraph 0225 of JP 2011-059488 A. The following cellulose acylate film was immersed in an alkaline aqueous solution and saponified according to paragraph 0275 of Japanese Patent No. 4,438,270. Next, a cellulose acylate film was prepared in the same manner as paragraphs 0199 to 0202 of Japanese Patent No. 4,731,143. The polarizer was sandwiched between each antiviral film and the saponified cellulose acylate, and an aqueous polyvinyl alcohol solution (a 5% aqueous solution of fully saponified polyvinyl alcohol) was applied between the polarizer / polyester and between the cellulose acylate / polarizer. These were then bonded together by pressure using nip rolls, and then dried at 70°C for 10 minutes to obtain a polarizing plate. Two pairs of the obtained polarizing plates were incorporated into a liquid crystal display device having a continuous light source (white LED) or a discontinuous light source (cold cathode tube) as a backlight, with the polyester film facing outward relative to the liquid crystal cell and the absorption axes of the polarizers arranged perpendicular to each other, and the light transmittance was adjusted to 50%. Light was incident on one side of the liquid crystal display device using a continuous light source (white LED) or a discontinuous light source (cold cathode tube), and the rainbow unevenness that occurred when visually observed from the opposite side through polarized sunglasses was evaluated according to the following criteria: A: No rainbow unevenness visible to the naked eye B: Rainbow unevenness visible to the naked eye C: Extremely large rainbow unevenness visible to the naked eye

[0178]

[0179] As shown in the table above, the antiviral films of the examples were able to suppress the occurrence of rainbow unevenness for a long period of time.

[0180] 101: Substrate 102: Antiviral layer 110: Antiviral film

Claims

1. An antibacterial or antiviral film having a substrate and an antibacterial or antiviral layer disposed on the substrate, wherein the substrate is a polyester resin film satisfying the condition of formula (1), the antibacterial or antiviral layer contains a binder, light scattering particles, and antibacterial or antiviral agent particles, and the antibacterial or antiviral film satisfies the condition of formula (11); 0.153≦(nx+ny) / 2−nz<0.165 ... (1) In formula (1), nx represents the refractive index in the slow axis direction in the polyester resin film plane, ny represents the refractive index in the fast axis direction in the polyester resin film plane, and nz represents the refractive index in the thickness direction of the polyester resin film; |h1−h2|<3.0 ... (11) In formula (11), h2 is the average haze value in the wavelength range of 400 to 700 nm of the antiviral film after wet heat treatment for 720 hours under conditions of a temperature of 60° C. and a relative humidity of 90%, and h1 is the average haze value in the wavelength range of 400 to 700 nm of the antiviral film before the wet heat treatment.

2. The antibacterial or antiviral film according to claim 1, wherein the thickness of the polyester resin film is 20 to 60 μm.

3. The antibacterial or antiviral film according to claim 1 or 2, wherein the amount of carboxy groups in the polyester resin film is 35 eq / ton or less.

4. The antibacterial or antiviral film according to claim 1 or 2, wherein the titanium element content of the polyester resin film is 5 to 15 ppm by mass.

5. The antibacterial or antiviral film according to claim 1 or 2, wherein the pre-peak temperature of the polyester resin film is 140 to 180°C.

Citation Information

Patent Citations

  • Polymerization method for polyester resin, polyester resin composition, and polyester film

    JP2011162777A

  • Anti-glare film, method for manufacturing the same, polarizing plate, and image display device

    JP2011197329A

  • Polyester resin film, method for producing polyester resin film, polarizing plate, image display device, hard coat film, sensor film for touch panels, glass scattering prevention film and touch panel

    JP2015184664A

  • Antibacterial film, touch panel, and method for producing antibacterial film

    WO2021256560A1

Cited By

  • Biaxially stretched polyester film for light diffusion film, and display device provided with same

    WO2025192678A1