Hydraulic composition, cured body, and method for producing hydraulic composition
A low-carbon hydraulic composition using calcined inorganic minerals like allophane or halloysite, with specific ratios and BET surface areas, addresses the limitations of kaolin-based compositions by achieving comparable compressive strength and reducing cement usage, enhancing reaction properties and fluidity.
Patent Information
- Application Number
- PCT/JP2024/009831
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to develop a low-carbon hydraulic composition that can achieve sufficient compressive strength without relying on kaolin, as its production is limited, and to find alternatives that can inhibit cement reaction while reducing the amount of cement used as an alkali stimulant.
A hydraulic composition is formulated using calcined inorganic minerals such as allophane or halloysite, with specific mass ratios of SiO2 to Al2O3 and BET specific surface areas, combined with an alkali stimulant, and optionally Portland cement, to create a paste that is cured with water, achieving compressive strength comparable to or exceeding that of kaolin-based compositions.
The solution provides a low-carbon hydraulic composition with sufficient compressive strength development, reducing the need for kaolin and minimizing cement usage, while maintaining good fluidity and reaction properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Hydraulic composition, cured product, and method for producing hydraulic composition
[0001] The present invention relates to a hydraulic composition, a hardened product, and a method for producing a hydraulic composition.
[0002] LC is a technology that uses inorganic minerals to increase their reactivity and replace them with cement admixtures such as blast furnace slag and fly ash. 3 Limestone Calcinated Clay Cement is known (for example, Non-Patent Document 1). This cement can be said to be a low-carbon cement, and the carbon dioxide emissions (CO ) associated with its production are lower than those of ordinary Portland cement. 2 ) can be reduced.
[0003] Karen Scrivener et al. : Calcined clay limestone cements (LC3), Cement and Concrete Research, Vol. 114, pp. 49-56 (2018)
[0004] Regarding the above technology, it has been shown that a material containing metakaolin, which is calcined kaolin as an inorganic mineral, can achieve good strength development. However, since kaolin is produced in limited regions and countries, the search for a material to replace kaolin has become an issue.
[0005] The present invention has been made in view of the above circumstances, and aims to provide a low-carbon hydraulic composition that is produced using an inorganic mineral other than kaolin and that exhibits sufficient compressive strength development. Another aim of the present invention is to provide a hardened product obtained from the hydraulic composition, and a method for producing the hydraulic composition.
[0006] The inventors focused on minerals such as allophane, which is usually said to inhibit the reaction of cement, as a material other than kaolin, and discovered that hydraulic compositions containing such minerals may have properties equivalent to or superior to those containing kaolin, and that the amount of cement to be blended as an alkali activator when preparing a hydraulic composition may be reduced, leading to the completion of the present invention.
[0007] One aspect of the present invention is as follows [1] to
[14] . [1] Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0, and the BET specific surface area is 30 to 180 m 2 [2] A hydraulic composition (first hydraulic composition) comprising a calcined inorganic mineral having a calcined inorganic mineral content of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator, and an alkaline activator content of 90 to 10 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator. 3+ / Fe 2+ ) is a calcined product of an inorganic mineral having a saturation temperature of 2.0 to 6.0, and Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 A hydraulic composition (second hydraulic composition) comprising 10 to 90 mass% of a calcined inorganic mineral having a saturation coefficient of 0.5 to 3.0 based on the total amount of the calcined inorganic mineral and the alkaline activator, and 90 to 10 mass% of an alkaline activator based on the total amount of the calcined inorganic mineral and the alkaline activator. [3] Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3A hydraulic composition (third hydraulic composition) comprising: a calcined inorganic mineral having a b value of 0.5 to 3.0 and a b value of 5.0 to 17.0 in the Lab color system, in an amount of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator; and an alkaline activator, in an amount of 90 to 10 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator. [4] The hydraulic composition according to any one of [1] to [3], wherein the hydraulic composition further comprises a carbonate, and the mass ratio of the carbonate to the mass of the calcined inorganic mineral (carbonate / calcined inorganic mineral) is 2.0 or less. [5] The hydraulic composition according to any one of [1] to [4], wherein the calcined inorganic mineral is a clay mineral calcined at 500 to 950°C. [6] The hydraulic composition according to any one of [1] to [5], wherein the alkaline activator includes Portland cement. [7] The hydraulic composition according to any one of [1] to [6], wherein the calcined inorganic mineral contains calcined allophane or calcined halloysite. [8] The hydraulic composition according to [7], wherein the calcined inorganic mineral contains 60 mass% or more of the calcined allophane or the calcined halloysite. [9] A hardened body obtained by hardening a paste containing the hydraulic composition according to any one of [1] to [8] and water.
[0008]
[10] Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0, and the BET specific surface area is 30 to 180 m 2 A method for producing a hydraulic composition (first method for producing a hydraulic composition), comprising a preparation step of mixing a calcined inorganic mineral having a calcined inorganic mineral content of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator with an alkaline activator, and preparing a hydraulic composition containing the calcined inorganic mineral in an amount of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator, and the alkaline activator in an amount of 90 to 10 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator.
[11] A method for producing a hydraulic composition (first method for producing a hydraulic composition), comprising a step of mixing a calcined inorganic mineral having a calcined inorganic mineral content of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator with an alkaline activator, and 3+ / Fe 2+ ) is a calcined product of an inorganic mineral having a saturation temperature of 2.0 to 6.0, and Al 2 O 3SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 A method for producing a hydraulic composition (second method for producing a hydraulic composition), comprising a preparation step of mixing a calcined inorganic mineral having a saturation index (SAR) of 0.5 to 3.0 with an alkaline activator to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline activator, and 90 to 10 mass% of the alkaline activator based on the total amount of the calcined inorganic mineral and the alkaline activator.
[12] 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 A method for producing a hydraulic composition (third method for producing a hydraulic composition), comprising a preparation step of mixing a calcined inorganic mineral having a b value of 0.5 to 3.0 in the Lab color system and a b value of 5.0 to 17.0 with an alkaline activator to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline activator, and 90 to 10 mass% of the alkaline activator based on the total amount of the calcined inorganic mineral and the alkaline activator.
[13] The method for producing a hydraulic composition according to any one of
[10] to
[12] , further comprising a calcination step, prior to the preparation step, of calcining the inorganic mineral at 500 to 950°C to obtain the calcined inorganic mineral.
[14] The method for producing a hydraulic composition according to
[13] , wherein the inorganic mineral is a clay mineral.
[0009] According to the present invention, it is possible to provide a low-carbon hydraulic composition that is produced using an inorganic mineral other than kaolin and that exhibits sufficient compressive strength development. Furthermore, according to the present invention, it is possible to provide a hardened body obtained from the hydraulic composition and a method for producing the hydraulic composition.
[0010] Preferred embodiments of the present disclosure are described in detail below. However, the present disclosure is not limited to the following embodiments. In the following description, when "X to Y" (X and Y are arbitrary numbers) is used, it means "X or more and Y or less" unless otherwise specified. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.
[0011] <Hydraulic Composition> The first hydraulic composition is Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0 or less, and the BET specific surface area is 30 to 180 m 2 The calcined inorganic mineral content is 10 to 90 mass %, and the alkaline irritant content is 90 to 10 mass %, based on the total amount of the calcined inorganic mineral and the alkaline irritant (100 mass %).
[0012] The second hydraulic composition has a mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ ) is a calcined product of an inorganic mineral having a saturation temperature of 2.0 to 6.0, and Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 The calcined inorganic mineral has a saturation index (SAR) of 0.5 to 3.0 or less, and an alkaline irritant. The calcined inorganic mineral content is 10 to 90 mass %, and the alkaline irritant content is 90 to 10 mass %, based on the total amount of the calcined inorganic mineral and the alkaline irritant (100 mass %).
[0013] The third hydraulic composition is Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO2 / Al 2 O 3 The calcined inorganic mineral has a b value of 0.5 to 3.0 and a b value of 5.0 to 17.0 in the Lab color system, and an alkaline irritant. The calcined inorganic mineral content is 10 to 90 mass%, and the alkaline irritant content is 90 to 10 mass%, based on the total amount of the calcined inorganic mineral and the alkaline irritant (100 mass%).
[0014] (Calinic inorganic mineral) Calcined inorganic mineral is obtained by calcining inorganic mineral at a predetermined temperature. Calcination increases the compressive strength of inorganic mineral, but calcination also reduces the SiO 2 and Al 2 O 3 Content, mass ratio SiO 2 / Al 2 O 3 This does not bring about any substantial changes to the
[0015] Mass ratio SiO 2 / Al 2 O 3 Examples of inorganic minerals (excluding kaolin) having a β-alkali content of 0.5 to 3.0 include allophane, halloysite, imogolite, illite, montmorillonite, and pyrophyllite. Among these, from the viewpoint of reactivity with the alkaline irritant, the inorganic mineral preferably contains allophane or halloysite, and more preferably contains allophane. In other words, the calcined inorganic mineral (excluding metakaolin) preferably contains calcined allophane or calcined halloysite, and more preferably contains calcined allophane.
[0016] From the viewpoint of easily achieving sufficient compressive strength, the content of calcined allophane or calcined halloysite in the calcined inorganic mineral (which can also be referred to as the content of allophane or halloysite in the inorganic mineral) is preferably 60% by mass or more, more preferably 80% by mass or more, and may even be 100% by mass (a calcined inorganic mineral consisting essentially of calcined allophane or calcined halloysite). The content of allophane in the inorganic mineral or the content of calcined allophane in the calcined inorganic mineral can be measured by an acid-alkali alternating dissolution method, and the content of halloysite in the inorganic mineral or the content of calcined halloysite in the calcined inorganic mineral can be measured by XRD Rietveld analysis.
[0017] The inorganic mineral may be a mineral produced by the weathering of volcanic ejecta, i.e., a mineral derived from volcanic ejecta. Examples of volcanic ejecta include volcanic ash, lapilli, pumice, and pyroclastic flow deposits. The inorganic mineral may also be a mineral produced by the weathering of igneous rock. Examples of igneous rock include granite. Generally, allophane is produced by the weathering of volcanic ejecta or igneous rock, halloysite is produced by further weathering of allophane, and kaolin is produced by further weathering of halloysite. Kaolin, allophane, and halloysite are all clay minerals.
[0018] Allophane is an amorphous inorganic mineral. Allophane generally has a particle size of 0.05 to 0.2 μm and a viscosity of 250 to 600 m. 2 Halloysite is a crystalline inorganic mineral. Halloysite generally has a particle size of 0.1 to 0.3 μm and a specific surface area of 40 to 100 m 2 / g BET specific surface area.
[0019] The above mass ratio SiO 2 / Al 2 O 3 When the mass ratio of SiO is in the above range, the reactivity between the calcined inorganic mineral and the alkali stimulant is easily improved. 2 / Al 2 O 3is 0.5 or more, preferably 0.6 or more, and more preferably 0.7 or more. 2 / Al 2 O 3 is 3.0 or less, preferably 2.5 or less, and more preferably 2.3 or less.
[0020] SiO in inorganic minerals 2 The content of Al in the inorganic mineral is preferably 30% by mass or more and 55% by mass or less from the viewpoint of reactivity with the alkaline irritant. 2 O 3 From the viewpoint of reactivity with the alkaline irritant, the content is preferably 20% by mass or more and 60% by mass or less.
[0021] In the first hydraulic composition, when the BET specific surface area is in the above range, the calcined inorganic mineral and the alkali activator react easily. From this viewpoint, the BET specific surface area is 30 m 2 / g or more, but 35m 2 / g or more, and 2 / g or more. The BET specific surface area is preferably 180 m 2 / g or less, but 160m 2 / g or less, and 2 The BET specific surface area is measured by a nitrogen gas adsorption method.
[0022] In the second hydraulic composition, the mass ratio of trivalent iron ions to divalent iron ions in the inorganic mineral, as measured by absorptiometry, is 3+ / Fe 2+ When the mass ratio of Fe to the calcined inorganic mineral is in the above range, the calcined product and the alkali activator react easily. 3+ / Fe 2+ is 2.0 or more. 3+ / Fe 2+ is 6.0 or less, preferably 5.7 or less, and more preferably 5.5 or less.
[0023] Iron (III) ion (Fe) in inorganic minerals determined by spectrophotometry 3+ From the viewpoint of the content of clay minerals contained in the inorganic minerals, the content of Fe can be 0.5% by mass or more, preferably 0.55% by mass or more, and more preferably 0.6% by mass or more. 3+ The content of can be 2.0% by mass or less, preferably 1.9% by mass or less, and more preferably 1.8% by mass or less, from the viewpoint that the content of clay minerals contained in inorganic minerals decreases as the amount of Fe compounds adsorbed on the clay mineral surface increases.
[0024] Divalent iron ion (Fe) in inorganic minerals measured by spectrophotometry 2+ From the viewpoint of the content of clay minerals contained in the inorganic minerals, the content of Fe can be 0.13% by mass or more, preferably 0.14% by mass or more, and more preferably 0.15% by mass or more. 2+ The content of can be 0.8% by mass or less, preferably 0.7% by mass or less, and more preferably 0.6% by mass or less, from the viewpoint that the content of clay minerals contained in inorganic minerals decreases as the amount of Fe compounds adsorbed on the clay mineral surface increases.
[0025] Mass ratio Fe 3+ / Fe 2+ is the amount of trivalent iron ion Fe based on the total amount of inorganic compounds measured by absorptiometry 3+ The amount (mass%) of divalent iron ions Fe 2+ It is calculated by dividing by the amount (mass%) of
[0026] In the third hydraulic composition, by focusing on the b value in the Lab color system, the mass ratio (SiO 2 / Al 2 O 3It is presumed that the degree of reactivity of the calcined inorganic mineral can be confirmed when the b value in the Lab color system is 0.5 to 3.0. When the b value is in the above range, the calcined inorganic mineral and the alkaline irritant react easily. From this viewpoint, the b value is 5.0 or more, preferably 5.5 or more, and more preferably 6.0 or more. From the same viewpoint, the b value can be 17.0 or less, preferably 16.0 or less, and more preferably 15.0 or less.
[0027] When the a-value in the Lab color system is 0.5 to 20.0, the amount of clay mineral contained in the inorganic mineral is sufficient, and calcination easily improves the reactivity with the alkaline irritant. From this viewpoint, the a-value is preferably 0.5 or more, and more preferably 1.0 or more. From the same viewpoint, the a-value is preferably 20.0 or less, and more preferably 15.0 or less.
[0028] When the L value in the Lab color system is 50.0 to 94.0, the amount of clay mineral contained in the inorganic mineral is sufficient, and calcination easily improves the reactivity with the alkaline irritant. From this viewpoint, the L value is preferably 50.0 or more, and more preferably 60.0 or more. From the same viewpoint, the L value is preferably 94.0 or less, and more preferably 90.0 or less.
[0029] The L, a, and b values in the Lab color system are calculated in the Hunter 1948 (Lab color system) color space.
[0030] Based on the total amount of the calcined inorganic mineral and the alkali activator, when the content of the calcined inorganic mineral is equal to or greater than the lower limit, good compressive strength can be obtained, and when the content is equal to or less than the upper limit, good fluidity can be maintained. From these viewpoints, the content is 10% by mass or more, preferably 20% by mass or more, and more preferably 30% by mass or more. Furthermore, the content is 90% by mass or less, preferably 80% by mass or less, and more preferably 70% by mass or less.
[0031] As described above, the calcined inorganic mineral is obtained by calcining an inorganic mineral at a predetermined temperature. The fact that the inorganic mineral is calcined can be explained as follows: 27 This can be confirmed by analyzing with Al-NMR. Specifically, in the calcined inorganic mineral, 27 When the sum of the peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al analyzed by Al-NMR is taken as 100%, the ratio of the peak area of at least one of tetracoordinated Al and pentacoordinated Al is 30 to 50%.
[0032] In calcined inorganic minerals, tetracoordinated Al and pentacoordinated Al have unstable frameworks, which are thought to contribute to increased reactivity with alkaline irritants. When the peak area ratio of at least one of tetracoordinated Al and pentacoordinated Al is 30% or more, the effect of this action can be fully enjoyed. On the other hand, if the ratio of tetracoordinated Al and pentacoordinated Al is too high, there is a risk that the reaction with alkaline irritants will proceed too rapidly. When the peak area ratio of at least one of tetracoordinated Al and pentacoordinated Al is 50% or less, such a phenomenon can be easily suppressed. From these perspectives, the peak area ratio of at least one of tetracoordinated Al and pentacoordinated Al is preferably 30 to 45%, more preferably 35 to 45%. From the perspective of easily achieving the above-mentioned effects, the peak area ratios of tetracoordinated Al and pentacoordinated Al may both be 30 to 50%, preferably 30 to 45%, more preferably 35 to 45%.
[0033] The sum of the peak areas of tetracoordinated Al and pentacoordinated Al is preferably 50% or more from the viewpoint of reactivity with alkaline irritants, and is preferably 90% or less from the viewpoint of reaction rate with alkaline irritants. From these viewpoints, the sum of the peak areas of tetracoordinated Al and pentacoordinated Al is more preferably 60 to 90%, and even more preferably 70 to 80%. From the above, the peak area of hexacoordinated Al is preferably 10 to 50%, more preferably 10 to 40%, and even more preferably 20 to 30%.
[0034] In order for the inorganic mineral to have the desired peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al, the inorganic mineral may be calcined at a predetermined temperature, more specifically, by calcining in accordance with the calcination step described below.
[0035] The ratio of the peak areas is measured as follows: 27 The chemical shift and coordination state of Al-NMR are analyzed using an NMR apparatus JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method is the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube is used. The analysis conditions are magnetic field strength: 18.79 T, frequency: 20 kHz, number of accumulations: 256, and pulse width: 90° (0.6 μs). 27 For the Al-NMR spectrum, the waveform of each peak is separated using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function. The integrated value of each separated peak is then used to calculate the area of each peak. 27 In the Al-NMR spectrum, peak P1 is observed in the chemical shift range of -10 ppm to 15 ppm, peak P2 in the chemical shift range of 50 ppm to 80 ppm, and peak P3 in the chemical shift range of 30 ppm to 40 ppm. Peak P1 corresponds to hexacoordinated Al, which originates from the inorganic mineral framework. Peaks P2 and P3 originate from tetracoordinated Al and pentacoordinated Al, respectively, which are thought to be generated by partial collapse of the inorganic mineral framework (e.g., decomposition and dehydroxylation of the hexacoordinated Al structure due to heat treatment at high temperature). From the obtained peak areas of P1 to P3, the sum of the area of P1 + P2 + P3 and the ratios of the areas of P2 and P3 based on this sum are calculated.
[0036] (Alkali stimulant) Examples of the alkali stimulant include Portland cement clinker, Portland cement, tricalcium silicate (3CaO.SiO 2 , C 3 S), slaked lime, etc.
[0037] The Portland cement clinker may be Portland cement clinker used to prepare various Portland cements specified in JIS R 5210:2003 "Portland Cement." Examples of the various Portland cements include ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, and low-heat Portland cement. The Portland cement clinker may be Portland cement clinker used to prepare ordinary Portland cement and high-early-strength Portland cement.
[0038] The mineral composition of Portland cement clinker can be calculated using the Bogue formula. The Bogue formula is a widely used formula for calculating the content of major minerals in Portland cement clinker from the content ratio of their chemical compositions. By using the Bogue formula shown below, the tricalcium silicate (3CaO.SiO 2 , C 3 S), dicalcium silicate (2CaO.SiO 2 , C 2 S), and tricalcium aluminate (3CaO·Al 2 O 3 , C 3 A). The "%" in the following formula means "% by mass." The chemical formula represents the content ratio (% by mass) of each compound indicated by the chemical analysis value according to JIS R 5204:2019 "Fluorescent X-ray analysis method for cement."
[0039] <Bogue style> C 3 S [%] = (4.07 x CaO [%]) - (7.60 x SiO 2 [%]) - (6.72 × Al 2 O 3 [%]) - (1.43 x Fe 2 O 3 [%]) - (2.85 x SO 3 [%]) C 2 S[%]=(2.87×SiO 2 [%]) - (0.754 × C 3 S [%]) C3 A[%]=(2.65×Al 2 O 3 [%]) - (1.69 x Fe 2 O 3 [%]) C 4 AF[%]=3.04×Fe 2 O 3 [%]
[0040] The Portland cement may be normal Portland cement, high early strength Portland cement, extra high early strength Portland cement, moderate heat Portland cement, low heat Portland cement, or sulfate resistant Portland cement.
[0041] When the content of the alkali stimulant is equal to or greater than the above lower limit based on the total amount of the calcined inorganic mineral and the alkali stimulant, good compressive strength can be obtained, and when the content is equal to or less than the above upper limit, CO 2 From these viewpoints, the content is 10% by mass or more, preferably 20% by mass or more, and more preferably 30% by mass or more. Also, the content is 90% by mass or less, preferably 80% by mass or less, and more preferably 70% by mass or less.
[0042] From the viewpoint of compressive strength, the total amount (content) of the calcined inorganic mineral and the alkaline activator in the hydraulic composition is preferably 75 mass % or more, more preferably 80 mass % or more, and more preferably 85 mass % or more, based on the total amount of the hydraulic composition, and may be 100 mass % (a hydraulic composition essentially consisting of the calcined inorganic mineral and the alkaline activator).
[0043] (Carbonate) The hydraulic composition may contain a carbonate. Examples of the carbonate include carbonates of alkaline earth metals, which are added to the hydraulic composition for the purpose of promoting the hydration reaction between the alkaline activator and the calcined inorganic mineral, and examples of the carbonate include calcium carbonate (limestone) and magnesium carbonate. Examples of the carbonate include sodium carbonate decahydrate (Na 2 CO 3 ・10H 2O), sodium carbonate (Na 2 CO 3 ), potassium carbonate (K 2 CO 3 ), sodium sesquicarbonate dihydrate (Na 3 H(CO 3 ) 2 NaHCO 3 ・2H 2 Carbonates of alkali metals such as HCl, HCl, and HCl (O) can also be used.
[0044] As the limestone, for example, commercially available limestone powder and powders containing calcium carbonate as a main component, such as kansui stone powder, can be used. The limestone preferably includes limestone that conforms to the minor mixing components described in JIS R 5210:2009 "Portland cement."
[0045] The content of carbonate in the hydraulic composition is 0% by mass or more, preferably more than 0% by mass, and may be 10% by mass or more, based on the total amount of the hydraulic composition, from the viewpoint of fluidity. On the other hand, from the viewpoint of compressive strength, it is preferably 25% by mass or less, and may be 20% by mass or less, or may be 15% by mass or less. Furthermore, from the viewpoint of compressive strength, the mass ratio of carbonate to the mass of calcined inorganic mineral (carbonate / calcined inorganic mineral) in the hydraulic composition is preferably 2.0 or less, more preferably 1.0 or less. Furthermore, the lower limit of this mass ratio is not particularly limited, but can be 0.
[0046] (Other Components) In addition to the calcined inorganic mineral, the alkali activator, and the carbonate, the hydraulic composition may contain inorganic fine powder, gypsum, etc. When the hydraulic composition contains these other components in addition to the carbonate, the total amount (content) of the carbonate and the other components can be 25% by mass or less, or may be 20% by mass or less, or may be 15% by mass or less, based on the total amount of the hydraulic composition.
[0047] The inorganic fine powder is added to the hydraulic composition for the purpose of improving the compressive strength. Examples of the inorganic fine powder include powdery materials such as silica stone and crushed stone. The content of the inorganic fine powder in the hydraulic composition is 0% by mass or more, preferably more than 0% by mass, based on the total amount of the hydraulic composition from the viewpoint of fluidity, while it is preferably 15% by mass or less from the viewpoint of compressive strength.
[0048] Gypsum is added to the hydraulic composition for the purpose of adjusting the hydration reaction rate. Examples of gypsum include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. The gypsum content in the hydraulic composition can be the same as the gypsum amount in general Portland cement, and is 0% by mass or more, preferably more than 0% by mass, based on the total amount of the hydraulic composition, while being 5% by mass or less is preferable from the viewpoint of easily maintaining a good hydration reaction rate.
[0049] <Hardened product> The hardened product is obtained by hardening a paste containing the hydraulic composition and water. The hardening conditions are not particularly limited. The hardened product can be prepared in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement."
[0050] The amount of water in the paste is preferably 35 parts by mass or more relative to 100 parts by mass of the total amount of the hydraulic composition from the viewpoint of fluidity, and is preferably 80 parts by mass or less from the viewpoint of easily making the pore structure of the hardened body dense. From these viewpoints, the amount of water is preferably 35 to 80 parts by mass, and more preferably 50 to 70 parts by mass.
[0051] <Method for producing hydraulic composition> The first method for producing a hydraulic composition is 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0, and the BET specific surface area is 30 to 180 m 2The method includes a preparation step of mixing a calcined inorganic mineral having a calcined inorganic mineral content of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator with an alkaline activator to prepare a hydraulic composition containing the calcined inorganic mineral in an amount of 10 to 90 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator, and the alkaline activator in an amount of 90 to 10 mass % based on the total amount of the calcined inorganic mineral and the alkaline activator.
[0052] The second method for producing a hydraulic composition is to determine the mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ ) is a calcined product of an inorganic mineral having a saturation temperature of 2.0 to 6.0, and Al 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 The method includes a preparation step of mixing a calcined inorganic mineral having a saturation coefficient of 0.5 to 3.0 with an alkaline activator to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline activator, and 90 to 10 mass% of the alkaline activator based on the total amount of the calcined inorganic mineral and the alkaline activator.
[0053] The third method for producing a hydraulic composition comprises: 2 O 3 SiO relative to the mass of 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0 and the b value in the Lab color system is 5.0 to 17.0, and mixing the calcined inorganic mineral with an alkali activator to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkali activator, and 90 to 10 mass% of the alkali activator based on the total amount of the calcined inorganic mineral and the alkali activator.
[0054] The method for producing a hydraulic composition may further include a calcination step of calcining an inorganic mineral at 500 to 950° C. to obtain a calcined inorganic mineral, prior to the preparation step. In this case, the inorganic mineral may be a clay mineral, as described above.
[0055] (Preparation Step) In the preparation step, the calcined inorganic mineral and the alkali activator are mixed. When mixing the two, carbonate and other components described above may also be mixed in. The blending amounts of each raw material are as described above.
[0056] In the preparation step, each raw material may be pulverized. When pulverization is performed, the order of mixing and pulverization is not particularly limited. That is, the raw materials may be mixed and then pulverized, or the raw materials may be pulverized individually and then mixed, or the raw materials may be mixed and pulverized simultaneously. The mixing may be performed using a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, or may be mixed and pulverized using a pulverizer such as a ball mill, a vertical roller mill, or a roller press, or each raw material may be pulverized individually and then mixed using a mixer such as a mechanical mixer.
[0057] (Calorination Step) The calcination temperature in the calcination step is preferably 500°C or higher from the viewpoint of increasing the compressive strength of the inorganic mineral, and is preferably 950°C or lower from the viewpoint of suppressing the formation of other minerals (for example, the formation of mullite in the case of allophane). From these viewpoints, the calcination temperature is more preferably 600 to 900°C. The calcination time is not particularly limited, but may be 0.5 to 5 hours, or may be 1 to 4 hours, from the viewpoint of the effect on the crystal structure.
[0058] The calcination process is 27 It can be said that this is a process of calcining an inorganic mineral so that the ratio of the peak area of at least one of tetracoordinated Al and pentacoordinated Al is 30 to 50% when the sum of the peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al analyzed by Al-NMR is 100%. If the area of peak P1 of hexacoordinated Al derived from the inorganic mineral skeleton is too large, sufficient compressive strength cannot be obtained. It can be said that the calcination process causes partial collapse of the inorganic mineral skeleton and produces peaks P2 and P3 derived from tetracoordinated Al and pentacoordinated Al, which contribute to improving compressive strength.
[0059] The present invention will be described in more detail by the following examples, but the present invention is not limited to these examples.
[0060] <Experiment 1: First Hydraulic Composition> [Raw Materials of Hydraulic Composition] (Inorganic Minerals) The types of inorganic mineral (clay mineral) samples used are shown in Table 1. When the inorganic mineral was metakaolin or halloysite, the inorganic mineral content was measured by Rietveld analysis using XRD, and when the inorganic mineral was allophane, the inorganic mineral content was measured by an acid-alkali alternating dissolution method.
[0061]
[0062] (Alkaline stimulant) Ordinary Portland cement (OPC, manufactured by UBE Mitsubishi Cement Co., Ltd.) was used as the alkaline stimulant.
[0063] (Carbonate) Calcium carbonate (Ube Material Industries, Ltd. (limestone fine powder, 325 mesh)) was used as the carbonate.
[0064] [Preparation of hydraulic compositions] Various inorganic minerals were calcined at 900°C for 1 hour to obtain calcined inorganic minerals. Next, the calcined inorganic minerals, alkaline activators, and, in some cases, carbonates were mixed according to the formulations shown in Table 4 to prepare hydraulic compositions.
[0065] (Measurement of Chemical Components) The chemical components of the calcined inorganic minerals were measured using an X-ray fluorescence analyzer (ZSX100e manufactured by Rigaku Corporation). The results are shown in Table 1.
[0066] (Method for measuring BET specific surface area) The amount of nitrogen gas adsorption was measured for calcined inorganic minerals that had been pretreated in a nitrogen gas atmosphere at 105°C for 1 hour using a BELSORPMINI manufactured by Microtrac-Bell. The specific surface area was calculated based on the results. The results are shown in Table 1.
[0067] (Calculation of peak area ratio) Nuclides of calcined inorganic minerals 27 The chemical shift and coordination state of Al-NMR were analyzed using an NMR spectrometer JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method was the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube was used. The analysis conditions were magnetic field strength: 18.79 T, frequency: 20 kHz, number of accumulations: 256, and pulse width: 90° (0.6 μs). 27For the Al-NMR spectrum, waveform separation of each peak was performed using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function. 27 In the Al-NMR spectrum, peak P1, which is in the chemical shift range of -10 ppm to 15 ppm, corresponds to hexacoordinated Al, peak P2, which is in the chemical shift range of 50 ppm to 80 ppm, corresponds to tetracoordinated Al, and peak P3, which is in the chemical shift range of 30 ppm to 40 ppm, corresponds to pentacoordinated Al. The integrated values of each separated peak were then used to calculate the area of each peak. From the obtained peak areas, the sum of the area of P1 + P2 + P3 and the percentage (%) of the areas of P1 to P3 based on this sum were calculated. The results are shown in Table 1.
[0068] [Preparation of hardened body] The prepared hydraulic composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water to prepare a hardened body in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until the ages of 7 and 28 days.
[0069] [Activity Index Measurement] The compressive strength of the above-mentioned hardened body was measured at ages of 7 and 28 days in accordance with the description of JIS R 5201:2015 "Physical Testing Methods for Cement." The activity index refers to the ratio of the compressive strength of the hardened body being measured to the compressive strength of a reference hardened body, expressed as a percentage. The reference hardened body was prepared by blending ordinary Portland cement with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement." The results are shown in Table 4.
[0070] <Experiment 2: Regarding the second hydraulic composition>
[0071] [Raw materials for hydraulic compositions] (Inorganic minerals) The types of inorganic mineral (clay mineral) samples used are shown in Table 2. When the inorganic mineral was metakaolin or halloysite, the inorganic mineral content was measured by Rietveld analysis using XRD, and when the inorganic mineral was allophane, the inorganic mineral content was measured by the acid-alkali alternating dissolution method. Fe in the inorganic mineral 2+ amount, Fe 3+Amount and their mass ratio Fe 3+ / Fe 2+ was measured and calculated by the phenanthroline absorptiometry method in accordance with JIS K0120:2016 "Factory wastewater testing method" using an ultraviolet-visible spectrophotometer (Hitachi High-Tech Science Corporation, product name: U-2900 type).
[0072]
[0073] (Alkaline stimulant) Ordinary Portland cement (OPC, manufactured by UBE Mitsubishi Cement Co., Ltd.) was used as the alkaline stimulant.
[0074] (Carbonate) Calcium carbonate (Ube Material Industries, Ltd. (limestone fine powder, 325 mesh)) was used as the carbonate.
[0075] [Preparation of hydraulic compositions] Various inorganic minerals were calcined at 900°C for 1 hour to obtain calcined inorganic minerals. Next, the calcined inorganic minerals, alkaline activators, and, in some cases, carbonates were mixed according to the formulations shown in Table 4 to prepare hydraulic compositions.
[0076] (Measurement of Chemical Components) The chemical components of the calcined inorganic minerals were measured using an X-ray fluorescence analyzer (ZSX100e manufactured by Rigaku Corporation). The results are shown in Table 2.
[0077] (Calculation of peak area ratio) Nuclides of calcined inorganic minerals 27 The chemical shift and coordination state of Al-NMR were analyzed using an NMR spectrometer JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method was the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube was used. The analysis conditions were magnetic field strength: 18.79 T, frequency: 20 kHz, number of accumulations: 256, and pulse width: 90° (0.6 μs). 27 For the Al-NMR spectrum, waveform separation of each peak was performed using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function. 27In the Al-NMR spectrum, peak P1, which is in the chemical shift range of -10 ppm to 15 ppm, corresponds to hexacoordinated Al, peak P2, which is in the chemical shift range of 50 ppm to 80 ppm, corresponds to tetracoordinated Al, and peak P3, which is in the chemical shift range of 30 ppm to 40 ppm, corresponds to pentacoordinated Al. The integrated values of each separated peak were then used to calculate the area of each peak. From the obtained peak areas, the sum of the area of P1 + P2 + P3 and the percentages (%) of the areas of P1 to P3 based on this sum were calculated. The results are shown in Table 2.
[0078] [Preparation of hardened body] The prepared hydraulic composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water to prepare a hardened body in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until the ages of 7 and 28 days.
[0079] [Activity Index Measurement] The compressive strength of the above-mentioned hardened body was measured at ages of 7 and 28 days in accordance with the description of JIS R 5201:2015 "Physical Testing Methods for Cement." The activity index refers to the ratio of the compressive strength of the hardened body being measured to the compressive strength of a reference hardened body, expressed as a percentage. The reference hardened body was prepared by blending ordinary Portland cement with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement." The results are shown in Table 4.
[0080] <Experiment 3: Third Hydraulic Composition> [Raw Materials of Hydraulic Composition] (Inorganic Minerals) The types of inorganic mineral (clay mineral) samples used are shown in Table 3. When the inorganic mineral was metakaolin or halloysite, the inorganic mineral content was measured by Rietveld analysis using XRD, and when the inorganic mineral was allophane, the inorganic mineral content was measured by an acid-alkali alternating dissolution method.
[0081]
[0082] (Alkaline stimulant) Ordinary Portland cement (OPC, manufactured by UBE Mitsubishi Cement Co., Ltd.) was used as the alkaline stimulant.
[0083] (Carbonate) Calcium carbonate (Ube Material Industries, Ltd. (limestone fine powder, 325 mesh)) was used as the carbonate.
[0084] [Preparation of hydraulic compositions] Various inorganic minerals were calcined at 900°C for 1 hour to obtain calcined inorganic minerals. Next, the calcined inorganic minerals, alkaline activators, and, in some cases, carbonates were mixed according to the formulations shown in Table 4 to prepare hydraulic compositions.
[0085] (Measurement of Chemical Components) The chemical components of the calcined inorganic minerals were measured using an X-ray fluorescence analyzer (ZSX100e manufactured by Rigaku Corporation). The results are shown in Table 3.
[0086] (Method for measuring each value in the Lab color system) Each value in the Lab color system of the calcined inorganic mineral was measured as follows. That is, using a spectrocolorimeter (SE7700, manufactured by Nippon Denshoku Industries Co., Ltd.), the L value, a value, and b value of the calcined inorganic mineral were measured three times according to the Hunter 1946 method, and the average values were calculated. The results are shown in Table 3.
[0087] (Calculation of peak area ratio) Nuclides of calcined inorganic minerals 27 The chemical shift and coordination state of Al-NMR were analyzed using an NMR spectrometer JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method was the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube was used. The analysis conditions were magnetic field strength: 18.79 T, frequency: 20 kHz, number of accumulations: 256, and pulse width: 90° (0.6 μs). 27 For the Al-NMR spectrum, waveform separation of each peak was performed using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function. 27 In the Al-NMR spectrum, peak P1, which is in the chemical shift range of -10 ppm to 15 ppm, corresponds to hexacoordinated Al, peak P2, which is in the chemical shift range of 50 ppm to 80 ppm, corresponds to tetracoordinated Al, and peak P3, which is in the chemical shift range of 30 ppm to 40 ppm, corresponds to pentacoordinated Al. The integrated values of each separated peak were then used to calculate the area of each peak. From the obtained peak areas, the sum of the area of P1 + P2 + P3 and the percentage (%) of the areas of P1 to P3 based on this sum were calculated. The results are shown in Table 3.
[0088] [Preparation of hardened body] The prepared hydraulic composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water to prepare a hardened body in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until the ages of 7 and 28 days.
[0089] [Activity Index Measurement] The compressive strength of the above-mentioned hardened body was measured at ages of 7 and 28 days in accordance with the description of JIS R 5201:2015 "Physical Testing Methods for Cement." The activity index refers to the ratio of the compressive strength of the hardened body being measured to the compressive strength of a reference hardened body, expressed as a percentage. The reference hardened body was prepared by blending ordinary Portland cement with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement." The results are shown in Table 4.
[0090]
Claims
1. Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0, and the BET specific surface area is 30 to 180 m 2 The hydraulic composition comprises 10 to 90 mass% of a calcined inorganic mineral having a molecular weight of 100 to 1000 / g based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of an alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.
2. The mass ratio of trivalent iron ions to divalent iron ions (Fe) measured by spectrophotometry 3+ / Fe 2+ ) is 2.0 to 6.0, and Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 The hydraulic composition comprises a calcined inorganic mineral having a sintering ratio of 0.5 to 3.0 in an amount of 10 to 90 mass% based on the total amount of the calcined inorganic mineral and the alkaline irritant, and an alkaline irritant in an amount of 90 to 10 mass% based on the total amount of the calcined inorganic mineral and the alkaline irritant.
3. Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 The hydraulic composition comprises 10 to 90 mass% of a calcined inorganic mineral having a b value of 0.5 to 3.0 and a b value of 5.0 to 17.0 in the Lab color system based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of an alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.
4. The hydraulic composition according to any one of claims 1 to 3, wherein the hydraulic composition further contains a carbonate, and the mass ratio of the carbonate to the mass of the calcined inorganic mineral (carbonate / calcined inorganic mineral) is 2.0 or less.
5. The hydraulic composition according to any one of claims 1 to 4, wherein the calcined inorganic mineral is a clay mineral calcined at 500 to 950°C.
6. The hydraulic composition according to any one of claims 1 to 5, wherein the alkaline activator includes Portland cement.
7. The hydraulic composition according to any one of claims 1 to 6, wherein the calcined inorganic mineral comprises calcined allophane or calcined halloysite.
8. The hydraulic composition according to claim 7, wherein the content of the calcined allophane or the calcined halloysite in the calcined inorganic mineral is 60 mass% or more.
9. A hardened body obtained by hardening a paste containing the hydraulic composition according to any one of claims 1 to 8 and water.
10. Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0, and the BET specific surface area is 30 to 180 m 2 The method for producing a hydraulic composition includes a preparation step of mixing a calcined inorganic mineral having a molecular weight of 10 to 90% by mass based on the total amount of the calcined inorganic mineral and the alkaline irritant, and preparing a hydraulic composition containing the calcined inorganic mineral in an amount of 10 to 90% by mass based on the total amount of the calcined inorganic mineral and the alkaline irritant, and the alkaline irritant in an amount of 90 to 10% by mass based on the total amount of the calcined inorganic mineral and the alkaline irritant.
11. The mass ratio of trivalent iron ions to divalent iron ions (Fe) measured by spectrophotometry 3+ / Fe 2+ ) is 2.0 to 6.0, and Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 The method for producing a hydraulic composition includes a preparation step of mixing a calcined inorganic mineral having a calcination ratio of 0.5 to 3.0 with an alkaline irritant to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of the alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.
12. Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 ) is 0.5 to 3.0 and the b value in the Lab color system is 5.0 to 17.0, and an alkaline irritant is mixed with the calcined inorganic mineral to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of the alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.
13. The method according to any one of claims 10 to 12, further comprising a calcination step, prior to the preparation step, of calcining the inorganic mineral at 500 to 950°C to obtain the calcined inorganic mineral.
14. The method according to claim 13, wherein the inorganic mineral is a clay mineral.
Citation Information
Patent Citations
Cement admixture and cement composition using the same
JP1991265549A
Admixture for cement and cement composition containing the same
JP2001302296A
Fire-proof composition
JP2003128450A
Hydraulic composition, cured product, and method for producing hydraulic composition