Steel sheet, member, and production methods for same
The patent addresses the formability and axial crushing challenges of high-strength steel plates by optimizing the composition and microstructure of steel plates with specific alloying elements and thermal treatments, achieving enhanced ductility and axial crushing properties for energy-absorbing applications in vehicles.
Patent Information
- Application Number
- PCT/JP2024/010115
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
High-strength steel plates with tensile strength of 980 MPa or more face challenges in formability due to decreased ductility and axial crushing properties, limiting their application in energy-absorbing members for vehicles where both stretch flangeability and axial crushing characteristics are essential for safety and weight reduction.
A steel plate composition with specific alloying elements and microstructural control through annealing and cooling processes to achieve a balance of tensile strength, ductility, and axial crushing properties, including a composition of C: 0.10-0.30%, Si: 0.5-2.0%, Mn: 1.5-3.0%, and controlled microstructural ratios of ferrite, tempered martensite, bainite, and retained austenite, along with a galvanized layer for enhanced properties.
The solution results in a steel plate with tensile strength of 980 MPa or more, exhibiting excellent ductility, stretch flangeability, and axial crushing properties, making it suitable for energy-absorbing applications in vehicles, contributing to reduced vehicle weight and improved fuel efficiency.
Smart Images

Figure JP2024010115_03102024_PF_FP_ABST
Abstract
Description
Steel plates, components, and their manufacturing methods
[0001] The present invention relates to high-strength steel plates and members with excellent formability that are used in various applications such as automobiles and home appliances and are particularly suitable for energy absorbing members, and to methods for manufacturing the same.
[0002] In recent years, due to the increasing need for lightweight automobile bodies, the application of high-strength steel sheets having a tensile strength (TS) of 980 MPa or more to automobile frame components and seat components has been promoted. However, when these high-strength steel sheets are formed by cold pressing, press cracking is likely to occur due to reduced ductility and stretch flangeability. For this reason, these high-strength steel sheets are required to have better formability than conventional steel sheets.
[0003] Furthermore, from the viewpoint of passenger safety, it is necessary to suppress deformation around the cabin during a collision, and therefore energy-absorbing components such as side members are required to absorb collision energy by deforming during a collision. However, high-strength steel plates with a tensile strength of 980 MPa or more have a problem in that, due to reduced axial crushing properties, fracture of the components is likely to occur at the points that have undergone primary processing by forming during a collision, making it difficult to stably exhibit collision energy absorption capacity.
[0004] From the above, in order to apply high strength steel sheets of 980 MPa or more to energy absorbing members of automobiles, they are required to have excellent axial crushing properties in addition to ductility and stretch flangeability.
[0005] In this context, for example, Patent Document 1 discloses the following in mass %: C: 0.15% or more and 0.30% or less, P: 0.040% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0060% or less, one or two of Si and Al: 0.70% or more and 2.50% or less in total, one or two of Mn and Cr: 1.50% or more and 3.50% or less in total. %, Mo: 0% or more and 1.00% or less, Ni: 0% or more and 1.00% or less, Cu: 0% or more and 1.00% or less, Nb: 0% or more and 0.30% or less, Ti: 0% or more and 0.30% or less, V: 0% or more and 0.30% or less, B: 0% or more and 0.0050% or less, Ca: 0% or more and 0.0400% or less, Mg: 0% or more and 0.0400% or less, and REM : 0% or more and 0.0400% or less, with the balance consisting of Fe and impurities, and the area ratio relative to the entire structure is as follows: one or two of ferrite and granular bainite: 10% or more and 50% or less in total, one or two of upper bainite and lower bainite: 10% or more and 50% or less in total, tempered martensite: more than 0% and 30% or less, retained austenite: 5% or more, and one or two or more of pearlite, cementite, and martensite: 0% or more and 10% or less in total, and by setting the area ratio of the ferrite to the total area ratio of the ferrite and the granular bainite to 25% or less, a steel sheet having a tensile strength of 980 MPa or more and excellent elongation and hole expandability can be obtained.
[0006] In Patent Document 2, the steel composition contains, in mass %, C: 0.07 to 0.20%, Si: 0.1 to 2.0%, Mn: 2.0 to 3.5%, P: 0.05% or less, S: 0.05% or less, and Sol. Al: 0.005 to 0.1%, with the balance being Fe and unavoidable impurities, and the steel structure has, in area ratios, ferrite: 60% or less, tempered martensite: 40% or more, and fresh martensite: 10% or less, and the void number density of the bent portion in a VDA bending test is 1500 voids / mm 2 It is disclosed that by satisfying the following conditions, a high-strength hot-dip galvanized steel sheet having a tensile strength of 980 MPa or more and excellent fracture resistance characteristics in the event of a collision can be obtained.
[0007] Patent Document 3 discloses a high-strength cold-rolled steel sheet containing, by mass%, C: 0.10 to 0.40%, Mn: 0.5 to 4.0%, Si: 0.005 to 2.5%, Al: 0.005 to 2.5%, Cr: 0 to 1.0%, with the balance being iron and inevitable impurities, with P: 0.05% or less, S: 0.02% or less, and N: 0.006% or less. The steel structure contains, in area ratio, 2 to 30% retained austenite, martensite is limited to 20% or less, the average grain size of cementite is 0.01 μm or more and 1 μm or less, and the cementite contains 30% or more and 100% or less cementite having an aspect ratio of 1 to 3. This discloses that a high-strength cold-rolled steel sheet having excellent strength, ductility, and hole expandability can be obtained.
[0008] Patent No. 6338038 Patent No. 6795122 Patent No. 4903915
[0009] However, although the techniques described in Patent Documents 1 and 3 provide high-strength steel sheets excellent in ductility and stretch flangeability, they do not take into consideration axial crushing properties.
[0010] Furthermore, Patent Document 2 discloses that high-strength steel sheets of 980 MPa or more have excellent fracture resistance properties during collision, but does not consider formability and is limited to steel sheets having a hot-dip galvanized layer.
[0011] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a steel plate, a member, and a method for manufacturing the same, which have a tensile strength (TS) of 980 MPa or more, high ductility and stretch flangeability, and excellent axial crushing properties.
[0012] In the present invention, the tensile strength is measured by a tensile test in accordance with JIS Z 2241 (2011).
[0013] In the present invention, high ductility refers to the following, with respect to the total elongation (T-El) measured in a tensile test in accordance with JIS Z 2241 (2011): (A) T-El is 14.0% or more when TS is in the range of 980 MPa or more and less than 1180 MPa; (B) T-El is 12.0% or more when TS is in the range of 1180 MPa or more and less than 1320 MPa; and (C) T-El is 10.0% or more when TS is 1320 MPa or more.
[0014] In the present invention, high stretch flangeability refers to a specimen having a size of 100 mm x 100 mm square, punched using a punching tool with a punch diameter of 10 mm and a die diameter of 10.3 mm (clearance 13%), and then the hole is expanded using a conical punch with an apex angle of 60 degrees, with the burrs generated during punching being on the outside, until a crack penetrating the plate thickness occurs. 0 : initial hole diameter (mm), d: hole diameter at crack occurrence (mm), hole expansion ratio λ (%) = {(d - d 0 ) / d 0}×100 is 45% or more.
[0015] In the present invention, the term "excellent axial crushing properties" refers to a steel sheet having a VDA bending angle α of 80° or more in VDA bending.
[0016] Here, the VDA bending test refers to a bending test (Verband der Automobilindustrie: VDA bending test) conforming to the VDA standard (VDA238-100) prescribed by the German Association of the Automotive Industry, and is a three-point plate bending test characterized by very closely spaced rolls and a sharp punch. The VDA bending test uses a 60 mm x 60 mm square test piece, the bending ridge direction is parallel to the rolling direction, the roll diameter D is 30 mm, and the distance L between the rolls is (plate thickness a 0The test is performed by supporting the specimen with a roll of 0.5 mm (×2) +0.5 mm and pressing a punch with a tip r of 0.4 mm from above at a stroke speed of 20 mm / min. The VDA bend angle α is the bend angle (° (more specifically, the unit is "° / mm", but hereinafter will be expressed as "°")) calculated using equations (1) to (5) from the stroke S (mm) at the maximum load in the bending test, and can be used as an index of axial crushing properties. The stroke S (mm) at the maximum load is the length (mm) traveled by the punch from the start of the test to the point at which the maximum load is obtained.
[0017] c (mm)=D / 2+r+a 0 ...(Formula 1)
[0018] p (mm) = D / 2 + L / 2 ... (Formula 2)
[0019]
[0020]
[0021]
[0022] The present inventors have conducted extensive research into steel sheets that are high in strength, excellent in ductility and stretch flangeability, and also excellent in axial crushing properties, and have reached the following conclusions: (1) After hot-rolling and cold-rolling a steel slab having a predetermined chemical composition, the annealing temperature: (A c3Annealing is performed in the austenite single-phase region of from (°C) -15°C to 900°C, and cooling is performed from the annealing temperature at a predetermined cooling rate to control the ferrite area ratio to 15% or less. (2) In cooling after the annealing, the cooling stop temperature is set to 200°C or higher and (martensitic transformation start temperature Ms point (°C) -30°C) or lower, thereby partially replacing austenite with martensite and / or bainite. The martensite and bainite thus produced enrich carbon in the surrounding untransformed austenite in the overaging treatment step after cooling is stopped, thereby ensuring a predetermined C concentration in the retained austenite and contributing to improved ductility. Furthermore, a retention treatment can be performed during cooling. By retaining the steel in a temperature range from 500°C to above the martensitic transformation start temperature Ms point and above 320°C for 10 seconds to 60 seconds, more bainite can be obtained, further improving ductility. (3) In the overaging treatment step after cooling is stopped, the steel sheet is heated to a heating temperature of 300°C or higher and 450°C or lower. Next, the steel sheet is cooled to a temperature 30°C or higher and 150°C or lower than the heating temperature at an average cooling rate of 0.5°C / s or higher, and further cooled to a temperature of 150°C or higher and 350°C or lower at an average cooling rate of 0.1°C / s or higher. Next, the steel sheet is held at a temperature range of 150°C or higher and 350°C or lower for 20 seconds or higher and 1000 seconds or lower. This minimizes the precipitation of carbides in tempered martensite present in the steel sheet surface, which serve as starting points for crack propagation during VDA bending, and improves axial crushing properties. In addition, the heat treatment step (a step of heating to 300 to 450°C after cooling is stopped, and then finally holding the temperature in the range of 150°C to 350°C for 20 seconds to 1000 seconds) promotes carbon distribution from the surrounding structure to the untransformed austenite region, thereby making it possible to further increase the carbon concentration of the retained austenite and improve ductility.
[0023] In this way, by appropriately controlling the temperature history, particularly during the cooling process after annealing and the overaging process, it is possible to simultaneously reduce the amount of carbides in the tempered martensite and increase the carbon concentration of the retained austenite, thereby enabling the production of a steel sheet that has a tensile strength TS of 980 MPa or more, as well as excellent ductility, stretch flangeability, and axial crush resistance.
[0024] The present invention has been made based on the above findings, and specifically provides the following: [1] In mass%, C: 0.10% or more and 0.30% or less, Si: 0.5% or more and 2.0% or less, Mn: 1.5% or more and 3.0% or less, P: 0.10% or less, S: 0.020% or less, sol. A steel sheet having a component composition containing Al: 1.00% or less, N: 0.015% or less, with the balance being Fe and unavoidable impurities, and having a steel structure containing, in area ratios, ferrite: 15% or less, tempered martensite: 30% to 80%, bainite: 10% to 40%, retained austenite: 5% or more, and fresh martensite: 10% or less, wherein an average C concentration in the retained austenite is 0.60 mass% or more, and the content of Fe element present as carbides in the tempered martensite is 0.20 mass% or less on average in a region within 100 μm from the steel sheet surface in the sheet thickness direction. [2] The steel sheet according to [1], wherein the chemical composition further contains, in mass%, at least one selected from the group consisting of Ti: 0.100% or less, Nb: 0.100% or less, V: 0.100% or less, B: 0.0050% or less, Cr: 1.000% or less, Cu: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Ta: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, and REM: 0.0050% or less. [3] The steel sheet according to [1] or [2], which has a zinc-plated layer on the surface of the steel sheet. [4] A member made using the steel sheet according to any one of [1] to [3]. [5] A steel slab having the component composition according to [1] or [2] is hot-rolled and cold-rolled, and then the resulting cold-rolled steel sheet is subjected to the following steps: (A c3After annealing at an annealing temperature of 200°C or higher and (Ms point (°C) - 15°C) or lower and 900°C or lower, cooling from the annealing temperature to a temperature T1 of 200°C or higher and (Ms point (°C) - 30°C) or lower at an average cooling rate CR1 of 3°C / s or higher and 100°C / s or lower, heating from the temperature T1 to a temperature T2 of 300°C or higher and 450°C or lower at an average heating rate of 2°C / s or higher, cooling from the temperature T2 to a temperature T3 of (T2 - 150°C) or higher and (T2 - 30°C) or lower at an average cooling rate CR2 of 0.5°C / s or higher, cooling from the temperature T3 to a temperature T4 of 150°C or higher and 350°C or lower and lower than the temperature T3 at an average cooling rate CR3 of 0.1°C / s or higher, holding in the temperature range of 150°C or higher and 350°C or lower and lower than the temperature T4 for 20 s or higher and 1000 s or lower, [6] A method for producing a steel sheet, comprising: cooling the steel slab having the chemical composition described in [1] or [2] above at an average cooling rate of CR4: 1°C / s or more to a temperature of 50°C or less. c3After annealing at an annealing temperature of not less than 900°C (temperature (°C) - 15°C), cooling from the annealing temperature to 500°C at an average cooling rate CR5 of not less than 5°C / s and not more than 100°C / s, retaining for not less than 10 seconds and not more than 60 seconds at an average cooling rate CR6 of not more than 10°C / s in a temperature range from 500°C to a residence stop temperature T5 of not less than Ms point (°C) and not less than 320°C, cooling from the residence stop temperature T5 to a temperature T1 of not less than 200°C and not more than (Ms point (°C) - 30°C) at an average cooling rate CR7 of not less than 3°C / s and not more than 100°C / s, heating from the temperature T1 to a temperature T2 of not less than 300°C and not more than 450°C at an average heating rate of not less than 2°C / s, [7] A method for producing a steel sheet according to [5] above, comprising cooling from the temperature T2 to a temperature T3 of (T2-150°C) or more and (T2-30°C) or less at an average cooling rate CR2 of 0.5°C / s or more, cooling from the temperature T3 to a temperature T4 of 150°C or more and 350°C or less and the temperature T3 or less at an average cooling rate CR3 of 0.1°C / s or more, holding the temperature in the temperature range of 150°C or more and 350°C or less and the temperature T4 or less for 20 seconds or more and 1000 seconds or less, and cooling to a temperature of 50°C or less at an average cooling rate CR4 of 1°C / s or more. [7] A method for producing a steel sheet according to [5] above, wherein the steel sheet is subjected to a hot-dip galvanizing treatment or a galvannealed hot-dip galvannealing treatment after cooling at the average cooling rate CR1 of 3°C / s or more and 100°C / s or less. [8] A method for producing a steel sheet according to the above [6], wherein the steel sheet is subjected to a hot-dip galvanizing treatment or a galvannealed hot-dip galvanizing treatment after cooling at the average cooling rate CR7: 3°C / s or more and 100°C / s or less. [9] A method for producing a steel sheet according to the above [5] or [6], wherein the steel sheet is subjected to an electrogalvanizing treatment after cooling at the average cooling rate CR4: 1°C / s or more.
[10] A method for producing a member, comprising a step of subjecting the steel sheet according to any one of the above [1] to [3] to at least one of forming and joining to produce a member.
[0025] According to the present invention, it is possible to obtain a steel sheet having a tensile strength (TS) of 980 MPa or more and excellent ductility, stretch flangeability, and axial crushing properties. The steel sheet of the present invention has excellent axial crushing properties, making it suitable for energy absorbing members. By applying the steel sheet obtained by the present invention to automotive parts, vehicle weight reduction can be achieved, and improvement in fuel efficiency is expected.
[0026] Fig. 1 is a photograph of the structure of an example of a steel sheet according to the present invention. Fig. 2 is a diagram for explaining a method for measuring the steel structure of a steel sheet according to the present invention. Fig. 3 is a diagram for explaining a method for manufacturing a steel sheet according to the present invention. Fig. 4 is a diagram for explaining a method for calculating a VDA bending angle.
[0027] The present invention will be specifically described below. The steel sheet of the present invention contains, in mass %, C: 0.10% to 0.30%, Si: 0.5% to 2.0%, Mn: 1.5% to 3.0%, P: 0.10% or less, S: 0.020% or less, sol. The steel sheet has a component composition containing Al: 1.00% or less, N: 0.015% or less, with the balance being Fe and unavoidable impurities, and has a steel structure containing, in area ratios, ferrite: 15% or less, tempered martensite: 30% to 80%, bainite: 10% to 40%, retained austenite: 5% or more, and fresh martensite: 10% or less, wherein the average C concentration in the retained austenite is 0.60 mass% or more, and the content of Fe element present as carbides in the tempered martensite in a region within 100 μm from the steel sheet surface in the sheet thickness direction is 0.20 mass% or less on average.
[0028] First, the chemical composition of the steel sheet of the present invention will be described. In the following description, the unit of "%" for the content of component elements means "mass %" unless otherwise specified.
[0029] [C: 0.10% or more and 0.30% or less] C is essential for ensuring the amount of tempered martensite and the amount of retained austenite stable at room temperature. Additionally, C is an element necessary for stabilizing the retained austenite by concentrating it in the retained austenite and improving ductility. If the C content is less than 0.10%, these effects cannot be fully achieved, making it difficult to ensure the strength and workability of the steel sheet. Therefore, the C content must be 0.10% or more, preferably 0.12% or more, and more preferably 0.15% or more. On the other hand, if the C content exceeds 0.30%, the amount of carbides in the tempered martensite increases, causing cracks to form from the carbides during bending deformation. This not only deteriorates the axial crushing properties, but also reduces ductility due to the excessive increase in strength. Therefore, the C content must be 0.30% or less, preferably 0.28% or less, and more preferably 0.25% or less.
[0030] [Si: 0.5% or more and 2.0% or less] Si is a useful element for suppressing the formation of carbides in martensite and bainite, promoting the formation of retained austenite, and improving the stability of the retained austenite. To achieve these effects, the Si content must be 0.5% or more, preferably 0.6% or more, and more preferably 0.7% or more. On the other hand, if the Si content exceeds 2.0%, excessive strength is obtained, resulting in reduced ductility and stretch flangeability. This may also raise concerns about increased rolling load during hot rolling, liquid metal embrittlement cracking when welded to a galvanized material, and deterioration of chemical conversion treatability. Therefore, the Si content is set to 2.0% or less, preferably 1.5% or less, and more preferably 1.0% or less.
[0031] [Mn: 1.5% or more and 3.0% or less] Mn is effective in ensuring a predetermined area fraction of tempered martensite and / or bainite to ensure strength. Furthermore, Mn is an important element for stabilizing retained austenite by lowering its Ms point, thereby increasing the area fraction of retained austenite and improving ductility. Therefore, the Mn content must be 1.5% or more, preferably 1.8% or more, and more preferably 2.0% or more. On the other hand, a Mn content exceeding 3.0% not only leads to excessively high strength but also significantly delays bainite transformation, resulting in reduced ductility. Furthermore, significant Mn segregation in the sheet thickness direction raises concerns about reduced material stability. Therefore, the Mn content is set to 3.0% or less, preferably 2.8% or less, and more preferably 2.5% or less.
[0032] [P: 0.10% or less] P is an element that strengthens steel, but a high P content deteriorates spot weldability. Therefore, the P content is set to 0.10% or less, preferably 0.02% or less. Note that P may not be contained, but from the viewpoint of manufacturing costs, the P content is preferably 0.001% or more.
[0033] [S: 0.020% or less] S has the effect of improving scale peeling during hot rolling and suppressing nitriding during annealing, but is an element that has a significant adverse effect on bendability, hole expandability, and spot weldability. In order to reduce these adverse effects, the S content is at least 0.020% or less. In the present invention, from the viewpoint of suppressing deterioration of bendability and hole expandability, the S content is preferably 0.0020% or less, and more preferably less than 0.0010%. Note that S may not be contained, but the S content is preferably 0.0001% or more from the viewpoint of production costs. The S content is more preferably 0.0005% or more.
[0034] [Sol. Al: 1.00% or Less] Al is an element effective in suppressing the formation of carbides and promoting the formation of retained austenite. It is also an element added as a deoxidizer in the steelmaking process. Therefore, although the lower limit of the sol. Al content is not particularly specified, it is preferably 0.005% or more, and more preferably 0.01% or more, in order to perform stable deoxidation. On the other hand, if the sol. Al content exceeds 1.00%, the number of inclusions in the steel sheet increases, deteriorating ductility. Therefore, the sol. Al content is set to 1.00% or less, preferably 0.50% or less. The sol. Al content is more preferably 0.25% or less, and even more preferably 0.10% or less.
[0035] [N: 0.015% or less] N is an element that forms nitrides such as BN, AlN, and TiN in steel, and reduces the hot ductility and surface quality of the steel. Furthermore, in steels containing B, N has the adverse effect of eliminating the effects of B through the formation of BN. If the N content exceeds 0.015%, the surface quality significantly deteriorates. Therefore, the N content is set to 0.015% or less, and preferably 0.010% or less. The N content is more preferably 0.005% or less, and even more preferably 0.002% or less. While N may not be contained, the N content is preferably 0.0001% or more, more preferably 0.001% or more, from the viewpoint of manufacturing costs.
[0036] The balance other than the above is Fe and unavoidable impurities. The steel sheet of the present invention preferably has a component composition containing the above basic components with the balance being iron (Fe) and unavoidable impurities.
[0037] The steel sheet of the present invention may contain the following optional elements in addition to the above-mentioned components.
[0038] [Ti: 0.100% or less, Nb: 0.100% or less, V: 0.100% or less] Ti, Nb, and V form fine precipitates during hot rolling or annealing, thereby increasing strength. To achieve this effect, Ti is preferably 0.010% or more, Nb is preferably 0.020% or more, and V is preferably 0.020% or more. On the other hand, if the contents of Ti, Nb, and V each exceed 0.100%, formability decreases. Therefore, when Ti, Nb, and V are added, their contents are preferably 0.100% or less, more preferably 0.080% or less, and even more preferably 0.050% or less.
[0039] [B: 0.0050% or less] B is an element that improves the hardenability of steel and has the advantage of facilitating the formation of a predetermined area ratio of tempered martensite and / or bainite. To achieve this effect, the B content is preferably 0.0005% or more, and more preferably 0.0010% or more. On the other hand, if the B content exceeds 0.0050%, not only does the effect saturate, but it also significantly reduces hot ductility and causes surface defects. Therefore, when B is added, the B content is preferably 0.0050% or less, more preferably 0.0040% or less, and even more preferably 0.0025% or less.
[0040] [Cr: 1.000% or less, Cu: 1.000% or less] Cr and Cu not only serve as solid solution strengthening elements, but also stabilize austenite and facilitate the formation of a composite microstructure during the cooling process during annealing. Therefore, Cr and Cu are not necessarily contained, but to obtain these effects, the Cr and Cu contents are preferably 0.005% or more, more preferably 0.008% or more, and even more preferably 0.010% or more. The Cr and Cu contents are preferably 0.020% or more. The Cr and Cu contents are more preferably 0.04% or more. On the other hand, if both the Cr content and the Cu content exceed 1.000%, the formability of the steel sheet decreases. Therefore, when Cr and Cu are added, their contents are preferably 1.000% or less, more preferably 0.800% or less, and even more preferably 0.400% or less. The Cr and Cu contents are each preferably 0.200% or less, and more preferably 0.100% or less.
[0041] [Sb: 0.200% or less, Sn: 0.200% or less] Sb and Sn are elements effective in suppressing decarburization in a region of several tens of micrometers in the surface layer of the steel sheet, which occurs due to nitriding and oxidation of the steel sheet surface. Suppressing such nitriding and oxidation prevents a decrease in the amount of martensite formed on the steel sheet surface, thereby ensuring the strength and material stability of the steel sheet. Therefore, although Sb and Sn are not necessarily added, if they are added, the Sb and Sn contents are preferably 0.002% or more, more preferably 0.004% or more, and even more preferably 0.006% or more. On the other hand, excessive content of either of these elements exceeding 0.200% leads to a decrease in toughness. Therefore, when Sb and Sn are added, the Sb and Sn contents are preferably 0.200% or less, more preferably 0.100% or less, and even more preferably 0.040% or less.
[0042] [Ta: 0.100% or less] Ta, like Ti and Nb, forms alloy carbides and alloy carbonitrides, contributing to increased strength. In addition, Ta partially dissolves in Nb carbides and Nb carbonitrides to form composite precipitates such as (Nb, Ta)(C, N), significantly suppressing precipitate coarsening and stabilizing the contribution of precipitation strengthening to improved strength of the steel sheet. To achieve this effect, Ta is preferably 0.005% or more. On the other hand, excessive Ta addition saturates the precipitate stabilization effect and increases alloy costs. Therefore, when Ta is added, the Ta content is preferably 0.100% or less, more preferably 0.080% or less, and even more preferably 0.050% or less.
[0043] [Ca: 0.0050% or less, Mg: 0.0050% or less, REM: 0.0050% or less] Ca, Mg, and REM are elements used for deoxidation, as well as elements effective in spheroidizing sulfides and improving the adverse effects of sulfides on local ductility and stretch flangeability. To achieve these effects, the Ca content is preferably 0.0001% or more, the Mg content is preferably 0.0001% or more, and the REM content is preferably 0.0001% or more. On the other hand, excessive Ca, Mg, and REM content exceeding 0.0050% increases inclusions and causes defects on the surface and inside. Therefore, the Ca, Mg, and REM contents are preferably each 0.0050% or less, more preferably 0.0025% or less, and even more preferably 0.0010% or less. The Ca content is more preferably 0.0008% or less. The Mg content is more preferably 0.0008% or less, and the REM content is more preferably 0.0008% or less.
[0044] In the present invention, REM refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM content in the present invention refers to the total content of one or more elements selected from the above-mentioned REM. The REM is not particularly limited, but is preferably La and / or Ce.
[0045] When the optional elements are contained in an amount less than the preferred lower limit, the amount of the optional elements contained in an amount less than the preferred lower limit does not impair the effects of the present invention.When the optional elements are contained in an amount less than the preferred lower limit, the optional elements are considered to be contained as inevitable impurities.
[0046] Next, the steel structure (microstructure) of the steel plate of the present invention will be described.
[0047] [Area Fraction of Ferrite: 15% or Less] Ferrite formed during annealing or cooling contributes to improving ductility, but a difference in hardness occurs between the ferrite and surrounding hard phases such as martensite, and cracks propagate from the interface between the ferrite and the hard phase during bending, resulting in a deterioration in stretch flangeability and axial crushing properties. Since an area fraction of ferrite of 15% or less does not impair the effects of the present invention, it is set to 15% or less. The area fraction of ferrite is preferably 10% or less, more preferably 5% or less. Furthermore, ferrite may be 0%.
[0048] [Area Fraction of Tempered Martensite: 30% or More and 80% or Less] To obtain predetermined strength and stretch flangeability, the area fraction of tempered martensite is set to 30% or more. Preferably, it is 40% or more, and more preferably, it is 50% or more. On the other hand, if the area fraction of tempered martensite exceeds 80%, excessive strength is obtained, resulting in a decrease in ductility. Therefore, the area fraction of tempered martensite is set to 80% or less, preferably, 75% or less, and more preferably, 70% or less.
[0049] [Bainite: 10% or More and 40% or Less] In the present invention, bainite is a general term for upper bainite and lower bainite. Here, upper bainite and lower bainite are defined as follows: Upper bainite is composed of lath-shaped bainitic ferrite and retained austenite and / or carbides present between the bainitic ferrite, and is characterized by the absence of regularly arranged fine carbides in the lath-shaped bainitic ferrite. Meanwhile, lower bainite, like upper bainite, is composed of lath-shaped bainitic ferrite and retained austenite and / or carbides present between the bainitic ferrite, but is characterized by the presence of regularly arranged fine carbides in the lath-shaped bainitic ferrite. In other words, upper bainite and lower bainite are distinguished by the presence or absence of regularly arranged fine carbides in the bainitic ferrite. Bainite, which forms during the cooling process after annealing and during the retention period during the cooling process, concentrates carbon in the surrounding untransformed austenite regions, allowing for the efficient production of more stable retained austenite. Therefore, the area fraction of bainite is set to 10% or more. However, because bainite is softer than tempered martensite, excessive formation of bainite leads to a decrease in strength and a decrease in stretch-flangeability due to an increase in the hardness difference with tempered martensite. Therefore, the area fraction of bainite is set to 40% or less, preferably 35% or less, and more preferably 30% or less. Since upper bainite concentrates more carbon in the surrounding untransformed austenite regions than lower bainite, upper bainite is advantageous from the perspective of efficiently obtaining retained austenite. Therefore, it is particularly preferable for the upper bainite content to be 10% or more, more preferably 15% or more. However, because upper bainite is softer than lower bainite, excessive formation of upper bainite is disadvantageous from the perspective of improving strength and stretch-flangeability. Therefore, the upper bainite content is preferably 30% or less, and more preferably 25% or less.
[0050] [Area Fraction of Retained Austenite: 5% or More] To ensure high ductility while obtaining the desired strength, the area fraction of retained austenite is set to 5% or more relative to the overall steel structure. The area fraction of retained austenite is preferably 7% or more, and more preferably 10% or more. This amount of retained austenite includes the retained austenite present between bainitic ferrite. The area fraction of retained austenite present between bainitic ferrite can be measured in the same manner as the area fractions of other retained austenite, using the measurement method described below. On the other hand, an excessive increase in the amount of retained austenite may result in reduced strength, reduced stretch flangeability, and deterioration of delayed fracture resistance. Therefore, although there is no upper limit for the area fraction of retained austenite, the area fraction of retained austenite is preferably 20% or less, and more preferably 15% or less.
[0051] [Area Fraction of Fresh Martensite: 10% or Less] Since this may result in a decrease in ductility and stretch flangeability, the area fraction of fresh martensite is set to 10% or less, preferably 8% or less, and more preferably 5% or less. Also, the area fraction of fresh martensite may be 0%.
[0052] [Average C concentration in retained austenite: 0.60 mass% or more] An increase in the C concentration in the retained austenite stabilizes the retained austenite, enabling improvement in ductility. Therefore, in order to obtain sufficient ductility while ensuring the desired strength, the average C concentration in the retained austenite is set to 0.60 mass% or more, preferably 0.80 mass% or more. Although there is no particular upper limit, if the average C concentration in the retained austenite increases excessively, the retained austenite may not transform during deformation, and the effect of improving ductility may not be sufficiently obtained. Therefore, the average C concentration in the retained austenite is preferably 2.0 mass% or less, more preferably 1.5 mass% or less.
[0053] [Fe element content present as carbides in tempered martensite in a region within 100 μm from the steel sheet surface in the sheet thickness direction: average 0.20 mass% or less] Carbides precipitated in tempered martensite serve as crack initiation sites during bending deformation, resulting in a decrease in axial crushing properties. In addition, carbide precipitation is a phenomenon that competes with carbon partitioning, and there is a concern that carbon consumption in carbide precipitation may inhibit carbon concentration in untransformed austenite. Therefore, the content of Fe element present as carbides in tempered martensite is preferably 0.20 mass% or less on average, more preferably 0.15 mass% or less. Note that no lower limit is particularly specified, but in the present invention, the Fe element content is substantially 0.001 mass% or more.
[0054] As described above, the steel structure of the present invention is a steel structure containing ferrite (including 0%), tempered martensite, bainite, retained austenite, and fresh martensite (including 0%). The steel structure of the present invention may be a steel structure consisting of ferrite (including 0%), tempered martensite, bainite, retained austenite, and fresh martensite (including 0%). Furthermore, the steel structure of the present invention may contain 5% or less of pearlite or cementite as phases other than those mentioned above, without impairing the effects of the present invention.
[0055] Next, a method for measuring the steel structure will be described.
[0056] The area ratio of the massive structure (martensite-austenite constituent: MA) consisting of ferrite, tempered martensite, fresh martensite, and / or retained austenite (described later) is measured by cutting a cross section of the steel sheet perpendicular to the surface and parallel to the rolling direction, mirror-polishing it, and then etching it with 3 vol% nital. The cross section is then observed at 1 / 4 of the thickness using a SEM at 5000x magnification, with a field of view of 20 μm × 20 μm, and 10 fields of view are observed. Figure 1 shows an example of an SEM photograph of the steel structure of a steel sheet. As shown in Figure 1, ferrite (see symbol F in Figure 1) is the region that appears blackest in the SEM image, with almost no carbides present inside and is relatively equiaxed. Tempered martensite (see symbol TM in Figure 1) is the region with a lath-like substructure and carbide precipitation present inside the SEM image. MA (fresh martensite and / or retained austenite) (see symbols FM and RA in FIG. 1) are massive regions that appear white under SEM, with no substructure visible inside.
[0057] In the present invention, bainite is defined as the sum of the area fractions of upper bainite and lower bainite. Upper bainite is determined by SEM observation, similar to the above-mentioned ferrite. Upper bainite is defined as a structure consisting of bainitic ferrite, which is the region that appears darkest on the SEM without the precipitation of regularly arranged fine carbides, and carbides or retained austenite, which appear white on the SEM (see symbol UB in Figure 1). When it is difficult to distinguish between ferrite and bainitic ferrite, the region of ferrite with an aspect ratio of ≦2.0 is defined as ferrite, and the region with an aspect ratio >2.0 is defined as bainitic ferrite. Figure 2 is a diagram illustrating a method for measuring the steel structure of the steel plate of the present invention. As shown in Figure 2, the aspect ratio can be calculated as a / b for both an elliptical shape (as shown in (1)) and a polygonal shape (as shown in (2)). Here, a refers to the length of the longest line segment formed by two points on the periphery of each phase region, and b refers to the length of the longest line segment formed by two points on the periphery of the region that is perpendicular to the line forming a. Furthermore, as shown in Figure 2 (3), when calculating the aspect ratio, if grains are in contact with each other, they are not considered as a single grain but are measured as two or more separate grains. Specifically, if grains are in contact with each other, as shown by the dashed line in Figure 2 (3), the grains are divided at positions where the area ratios of the individual grains are approximately equal, and the size of each grain is measured. Furthermore, in SEM observation, lower bainite (see symbol LB in Figure 1) and tempered martensite both exhibit a structure in which fine white carbides are precipitated in a gray matrix, making it difficult to distinguish between them. Therefore, lower bainite and tempered martensite are distinguished by observing the variant morphology of carbides using transmission electron microscopy (TEM). Note that the carbide morphology of lower bainite is a single variant that precipitates regularly in one direction within the substructure, whereas the carbides of tempered martensite are multi-variant with random precipitation directions within the substructure.The area fractions of the lower bainite and tempered martensite exhibiting these characteristics can be determined by observing 10 fields of view of a 1.5 μm square region using a TEM, calculating the area fractions of the constituent phases (lower bainite and tempered martensite) for the 10 fields of view of the obtained structural images using Adobe Photoshop, and averaging these values.
[0058] The area fraction of retained austenite and the average C concentration in the retained austenite are determined by grinding and polishing the steel sheet to a quarter position in the thickness direction and measuring the X-ray diffraction intensity. The volume fraction of retained austenite is calculated from the intensity ratio of the (200), (220), and (311) planes of austenite to the diffraction intensity of the (200) and (211) planes of ferrite using a Mo tube radiation source. The average C concentration in the retained austenite is calculated from the lattice constant A of austenite obtained from the peak angle of the (220) plane of austenite using a Co tube radiation source, and then calculated using the following formula (6). Note that Mn%, Si%, and Al% below represent the mass % content of each element (Mn, Si, Al) in the steel sheet.
[0059] Average C concentration in retained austenite (mass%) = A - {(0.3572 + 0.0012 × Mn% - 0.00157 × Si% + 0.0056 × Al%)} / 0.033 (Equation 6)
[0060] The area fraction of fresh martensite (Fresh Martensite: FM) is calculated by the following formula (7), and is the value obtained by subtracting the area fraction of retained austenite (RA) from the area fraction of MA (fresh martensite and / or retained austenite). Note that the "area fraction" of RA (retained austenite) in the present invention can be considered to be equal to the "volume fraction" of retained austenite calculated by XRD measurement.
[0061] FM (%) = MA (%) - RA (%) ... (Formula 7)
[0062] The average content of Fe element present as carbides in tempered martensite in a region within 100 μm from the steel sheet surface in the sheet thickness direction is determined by extraction residue analysis. A 10 mass% AA electrolyte (acetylacetone-1 mass% tetramethylammonium chloride-methanol) is used as the electrolyte, and the current density is 20 mA / cm 2 Electrolysis was performed under conditions of 0.1 μm / min, and the electrolysis time was 30 minutes, dissolving the steel sheet surface to a depth of 100 μm. The sample was then immersed in methanol and subjected to ultrasonic agitation to remove the residue (precipitates remaining after the electrolysis). The residue was then filtered using a 0.2 μm pore size filter, and the amount of Fe element in the collected residue was determined by ICP emission spectrometry and converted into a mass % of the steel sheet. The collected residue consisted entirely of precipitates present within a region within 100 μm from the steel sheet surface. In this case, the amount of carbides outside the tempered martensite (e.g., bainite and ferrite) was extremely small compared to the amount of carbides in the tempered martensite. Furthermore, the Fe element was assumed not to exist as an iron-based compound other than carbon. Therefore, the above measurement yielded the average content of Fe element present as carbides in the tempered martensite within a region within 100 μm from the steel sheet surface in the thickness direction.
[0063] The steel sheet of the present invention may have a zinc-plated layer on one or both sides of the steel sheet surface. The plated layer may be either a hot-dip plated layer or an electroplated layer.
[0064] The steel sheet of the present invention preferably has a thickness of 0.5 mm or more, and more preferably has a thickness of 2.0 mm or less.
[0065] Next, a method for manufacturing a steel sheet according to the present invention will be described. Hereinafter, a case in which a holding treatment under predetermined conditions is not performed as a subsequent treatment after an annealing treatment will be described as a first embodiment, and a case in which a holding treatment under predetermined conditions is performed as a subsequent treatment after an annealing treatment will be described as a second embodiment.
[0066] In the present invention, the temperature specified in each step refers to the surface temperature of the slab (steel slab) or steel plate.
[0067] FIG. 3 is a diagram for explaining the steel sheet manufacturing method of the present invention, and particularly shows the change in the surface temperature of a slab (steel slab) or a steel sheet over time. Details of each step, including the change in temperature over time, will be described below. FIG. 3(a) shows the change in the surface temperature of a slab (steel slab) or a steel sheet over time in the steel sheet manufacturing method of the first embodiment (when no holding treatment is performed). FIG. 3(b) shows the change in the surface temperature of a slab (steel slab) or a steel sheet over time in the steel sheet manufacturing method of the second embodiment (when holding treatment is performed).
[0068] <First embodiment> In a manufacturing method of a steel sheet according to a first embodiment of the present invention, as shown in FIG. 3(a), a steel slab having the above-described composition is hot-rolled and cold-rolled, and then the obtained cold-rolled steel sheet is subjected to (A c3 After annealing at an annealing temperature of 200°C or higher and (Ms point (°C) - 15°C) or lower and 900°C or lower, the steel sheet is cooled from the annealing temperature to a temperature T1 of 200°C or higher and (Ms point (°C) - 30°C) or lower at an average cooling rate CR1 of 3°C / s or higher and 100°C / s or lower, and heated from temperature T1 to a temperature T2 of 300°C or higher and 450°C or lower at an average heating rate of 2°C / s or higher, and then heated from temperature T2 to a temperature of (T2 - 150°C) or higher (T2 - 30°C). The material is cooled at an average cooling rate CR2 of 0.5°C / s or more through a temperature range from temperature T3 to a temperature T4 of 150°C or more and 350°C or less and temperature T3 or less, at an average cooling rate CR3 of 0.1°C / s or more, and is held in the temperature range of 150°C or more and 350°C or less and temperature T4 or less for 20 seconds or more and 1000 seconds or less, and then cooled to a temperature of 50°C or less at an average cooling rate CR4 of 1°C / s or more.
[0069] (Hot rolling step) Hot rolling may be carried out according to a conventional method. For example, a steel slab having the above-described predetermined component composition is heated to a slab heating temperature of 1100°C or higher, the soaking time is 20 minutes or more, and the finish rolling delivery temperature is Ar. 3 Hot rolling may be performed at a temperature equal to or higher than the transformation point, and coiling may be performed at a coiling temperature of 400°C or higher. The slab heating temperature may be 1300°C or lower. The soaking time may be 300 min or shorter. The finish rolling delivery temperature is Ar 3The coiling temperature may be set to transformation point + 200°C or less. The coiling temperature may be set to 720°C or less. The coiling temperature is preferably controlled from the viewpoint of suppressing thickness fluctuations and stably ensuring high strength. Specifically, the coiling temperature is preferably set to 430°C or more. The coiling temperature is preferably set to 530°C or less.
[0070] (Cold Rolling Process) The cold rolling may be performed at a rolling ratio (cumulative rolling ratio) of, for example, 30% or more. The rolling ratio may be 85% or less. From the viewpoint of stably ensuring high strength and reducing anisotropy, it is preferable to control the rolling ratio. Specifically, the rolling ratio is preferably 35% or more. When the rolling load is high, softening annealing can be performed at a temperature of 450°C or more and 730°C or less in a CAL (continuous annealing line) or BAF (box annealing furnace).
[0071] (Annealing step) After hot rolling and cold rolling a steel slab having a predetermined chemical composition, it is annealed under the following specified conditions. The annealing equipment is not particularly limited, but from the viewpoint of productivity and ensuring the desired heating rate and cooling rate, it is preferable to carry out the annealing in a continuous annealing line (CAL) or a continuous hot-dip galvanizing line (CGL).
[0072] [Annealing treatment step: Annealing temperature: (A c3 In order to secure a predetermined area ratio of tempered martensite and / or bainite and a predetermined area ratio of retained austenite, the annealing temperature is set to A c3 The annealing temperature (°C) is set to -15°C or higher and 900°C or lower. In order to make the ferrite content 15% or lower, it is preferable to adjust the annealing temperature so as to achieve austenite single phase region annealing. The annealing temperature is preferably adjusted to A c3 The annealing temperature is preferably A c3 The annealing temperature is set to 900°C or less (temperature (°C) + 15°C). On the other hand, if the annealing temperature exceeds 900°C, the austenite grain size becomes excessively large, and the diffusion distance of C atoms required to obtain retained austenite with a desired carbon concentration becomes long, resulting in a decrease in ductility. Therefore, the annealing temperature is set to 900°C or less. The annealing temperature is preferably 880°C or less. c3The temperature can be determined by measuring the volume change when a cylindrical test piece (diameter 3 mm × height 10 mm) is heated from room temperature (25°C) to the austenite single phase region using a Formaster testing machine.
[0073] [First Cooling Treatment Step: Cooling at an Average Cooling Rate CR1 of 3°C / s or More and 100°C / s or Less in the Range from the Annealing Temperature to a Temperature T1 of 200°C or More and (Martensitic Transformation Start Temperature Ms Point (°C) - 30°C) or Less] After the annealing treatment, rapid cooling is required to obtain a predetermined area ratio of tempered martensite and / or bainite. If the average cooling rate CR1 in the temperature range from the annealing temperature to a temperature T1 (cooling stop temperature T1) of 200°C or More and (Martensitic Transformation Start Temperature Ms Point (°C) - 30°C) or less is less than 3°C / s, ferrite is generated during the cooling process, which reduces strength, stretch flangeability, and axial crush resistance. Therefore, from the viewpoint of suppressing the generation of ferrite, the average cooling rate CR1 in the temperature range from the annealing temperature to a cooling stop temperature T1 of 200°C or More and (Ms Point (°C) - 30°C) or less is set to 3°C / s or more. The average cooling rate CR1 is preferably 5°C / s or more, more preferably 8°C / s or more. On the other hand, if the average cooling rate CR1 is too high, the sheet shape deteriorates, so the average cooling rate CR1 is set to 100°C / s or less. The average cooling rate CR1 is preferably 50°C / s or less.
[0074] Furthermore, in order to ensure a predetermined amount of retained austenite, the temperature T1 (cooling stop temperature T1) is set to 200°C or higher. The temperature T1 (cooling stop temperature T1) is preferably 220°C or higher, and more preferably 240°C or higher. If the cooling stop temperature T1 exceeds (Ms point (°C) - 30°C), a large amount of massive untransformed austenite remains, the amount of fresh martensite at the time of final cooling increases, and stretch flangeability deteriorates. Therefore, the cooling stop temperature T1 is set to (Ms point (°C) - 30°C) or lower. The cooling stop temperature T1 is preferably (Ms point (°C) - 35°C) or lower.
[0075] The martensitic transformation start temperature Ms point (°C) was measured using a Formaster tester. c3The volume change can be determined by using a cylindrical test piece similar to that used when measuring the temperature, holding it at a predetermined annealing temperature, and then quenching it with helium gas.
[0076] Here, the average cooling rate CR1 is "(annealing temperature (cooling start temperature) (°C) - (Ms point (°C) - 30°C) (cooling stop temperature (°C))) / (cooling time (seconds) from annealing temperature to (Ms point (°C) - 30°C))".
[0077] [Heat Treatment Step: Heating from Temperature T1 to Temperature T2 of 300°C or higher and 450°C or lower at an average heating rate of 2°C / s or higher] By heating in a short time from the above-mentioned temperature T1 (cooling stop temperature T1: 200°C or higher and (martensitic transformation start temperature Ms point (°C) - 30°C) or lower) to a temperature T2 of 300°C or higher and 450°C or lower, carbide precipitation is suppressed, and at the same time, carbon is concentrated from the surrounding structure into untransformed austenite, thereby ensuring high ductility. If the temperature T2 is less than 300°C, carbon is not sufficiently concentrated into untransformed austenite, and further, tempering of the martensite does not proceed sufficiently, resulting in an excessive increase in the strength of the tempered martensite, which is disadvantageous from the viewpoint of improving ductility and stretch flangeability. On the other hand, if the temperature T2 after heating exceeds 450°C, untransformed austenite decomposes and massive fresh martensite increases, resulting in reduced ductility and stretch flangeability, and excessive carbides precipitate, resulting in poor axial crushing properties. Therefore, the temperature T2 is set to 300°C or higher and 450°C or lower. The temperature T2 is preferably 330°C or higher, and more preferably 350°C or higher. The temperature T2 is preferably 420°C or lower, and more preferably 400°C or lower.
[0078] Furthermore, if the average heating rate from temperature T1 to temperature T2 (300°C or higher and 450°C or lower) is slow, the amount of carbide precipitation increases, deteriorating the axial crushing characteristics. Furthermore, as the amount of carbide increases, the amount of carbon concentrated in retained austenite decreases, leading to a decrease in ductility. Therefore, the average heating rate in the temperature range from temperature T1 (cooling stop temperature T1) to temperature T2 (300°C or higher and 450°C or lower) is set to 2°C / s or higher. From the viewpoint of suppressing carbide precipitation, the average heating rate is preferably 5°C / s or higher, and more preferably 10°C / s or higher. While there is no particular upper limit to the average heating rate, the average heating rate is preferably 50°C / s or lower, and more preferably 30°C / s or lower.
[0079] Here, the average heating rate is "temperature T2 (heating stop temperature) (°C) - temperature T1 (heating start temperature) (°C)) / (heating time from temperature T1 to temperature T2 (seconds))".
[0080] [Second cooling treatment step: cooling from temperature T2 to a temperature T3 of (T2-150°C) or more (T2-30°C) or less at an average cooling rate CR2 of 0.5°C / s or more] [Third cooling treatment step: cooling from temperature T3 to a temperature T4 of 150°C or more and 350°C or less and temperature T3 or less at an average cooling rate CR3 of 0.1°C / s or more] In the overaging treatment step after cooling is stopped (from the above-mentioned heat treatment step to the holding treatment step after the third cooling treatment step), fresh martensite is transformed into martensite by tempering, and this transformation causes carbide precipitation and carbon partitioning to untransformed austenite. Since the carbide precipitation rate tends to slow as the heating temperature after cooling is stopped decreases, by quickly cooling to a temperature range at a certain cooling rate or more that allows carbide precipitation to be suppressed, carbide precipitation can be suppressed and axial crush resistance can be improved. On the other hand, a decrease in the heating temperature after cooling is stopped may inhibit carbon enrichment in untransformed austenite and tempering of fresh martensite, potentially resulting in excessive strength increase and deterioration of ductility and stretch-flangeability. For these reasons, a second cooling treatment step under specific conditions is performed between the heat treatment step and the third cooling treatment step to simultaneously obtain excellent axial crushing properties, ductility, and stretch-flangeability by cooling to a predetermined temperature range to suppress carbide precipitation and promote carbon enrichment in untransformed austenite and tempering of fresh martensite. Specifically, to achieve the above-described effects, the temperature T3 (cooling stop temperature T3) in the second cooling treatment step is set to be equal to or higher than (T2-150°C) and equal to or lower than (T2-30°C). The temperature T3 is preferably equal to or higher than (T2-120°C), more preferably equal to or higher than (T2-100°C). The temperature T3 is preferably equal to or lower than (T2-50°C), more preferably equal to or lower than (T2-70°C).
[0081] The average cooling rate CR2 is set to 0.5° C. / s or more, preferably 0.6° C. / s or more, and more preferably 0.7° C. / s. Although there is no particular upper limit, a high average cooling rate tends to delay carbon partitioning to retained austenite and tempering of fresh martensite, resulting in a decrease in ductility and stretch flangeability. Therefore, the average cooling rate CR2 is preferably set to 5° C. / s or less.
[0082] Here, the average cooling rate CR2 is "(temperature T2 (°C) (cooling start temperature) - temperature T3 (°C) (cooling stop temperature)) / (cooling time (seconds) from temperature T2 to temperature T3)".
[0083] After cooling to a temperature T3 in the second cooling treatment, further cooling is performed as a third cooling treatment to suppress carbide precipitation while simultaneously promoting carbon distribution and improving the carbon concentration and amount of retained austenite. If the cooling temperature is lowered, the carbon distribution rate may decrease, raising concerns that carbon may not be sufficiently concentrated in the untransformed austenite. On the other hand, an increase in the cooling temperature or a decrease in the average cooling rate may lead to carbide precipitation during cooling, resulting in deterioration of axial crushing properties. Therefore, the temperature T4 is set to 150°C or higher and 350°C or lower. The temperature T4 is preferably 180°C or higher, more preferably 200°C or higher. The temperature T4 is also preferably 300°C or lower, more preferably 250°C or lower.
[0084] The average cooling rate CR3 is set to 0.1° C. / s or more, preferably 0.2° C. / s or more, and more preferably 0.3° C. / s or more. Although there is no particular upper limit, from the viewpoint of sufficiently promoting carbon distribution to untransformed austenite, the average cooling rate CR3 is preferably set to not more than the average cooling rate CR2 and not more than 1° C. / s.
[0085] Here, the average cooling rate CR3 is "(temperature T3 (°C) (cooling start temperature) - temperature T4 (°C) (cooling stop temperature)) / (cooling time (seconds) from temperature T3 to temperature T4)".
[0086] [Holding Treatment Step: Holding for 20 seconds or more and 1000 seconds or less in a temperature range of 150°C or more and 350°C or less and temperature T4 or less] The holding temperature is set to the above-mentioned temperature T4 or less. If the holding temperature is less than 150°C, the tempering of fresh martensite does not proceed sufficiently, resulting in an excessive increase in strength. Furthermore, the amount of carbon enrichment in untransformed austenite is reduced, which is disadvantageous from the viewpoint of improving ductility and stretch flangeability. On the other hand, if the holding temperature exceeds 350°C, the amount of carbide precipitation increases, resulting in inferior axial crushing properties. Furthermore, the carbide precipitation inhibits carbon enrichment in untransformed austenite, reducing retained austenite and resulting in inferior ductility. For these reasons, the holding temperature is set to 150°C or more and 350°C or less, and to temperature T4 or less. The holding temperature is preferably 180°C or more, more preferably 200°C or more. The holding temperature is preferably 300°C or less, more preferably 250°C or less.
[0087] Furthermore, by extending the holding time, the amount of carbon enriched in untransformed austenite can be increased, and the retained austenite can be stabilized, making it possible to improve ductility. On the other hand, by shortening the holding time, the amount of carbide precipitation tends to decrease, improving the axial crushing properties. For these reasons, the holding time is set to 20 seconds or more and 1,000 seconds or less. The holding time is preferably 100 seconds or more, and more preferably 200 seconds or more. The holding time is preferably 700 seconds or less, and more preferably 500 seconds or less.
[0088] Furthermore, after the first cooling treatment step (after cooling at an average cooling rate CR1 of 3°C / s or more and 100°C / s or less), i.e., before or after any of the steps from the heating treatment step from temperature T1 to temperature T2 described above to the holding treatment step of holding at 150°C or more and 350°C or less, or during any of the steps, a hot-dip galvanizing treatment or further alloying treatment can be performed to form a galvanized layer on the steel sheet surface. In this case, it is preferable to immerse the steel sheet in a galvanizing bath at 440°C or more and 500°C or less to perform the hot-dip galvanizing treatment, and then adjust the coating weight by gas wiping or the like. For the hot-dip galvanizing, a galvanizing bath containing 0.10% by mass or more and 0.22% by mass or less of Al is preferably used. Furthermore, a galvanizing alloying treatment can be performed after the hot-dip galvanizing treatment. When performing the galvanizing alloying treatment, it is preferable to perform it in a temperature range of 470°C or more and 590°C or less. Furthermore, heating up to this temperature range is acceptable because it does not impair the effects of the present invention.
[0089] [Fourth Cooling Treatment Step: Cooling at an Average Cooling Rate CR4 of 1°C / s or More to a Temperature of 50°C or Less] Thereafter, cooling is performed from the holding end temperature (150°C or more and 350°C or less, and temperature T4 or less) of the above-mentioned holding treatment step to a temperature of 50°C or less at an average cooling rate CR4 of 1°C / s or more to prevent softening due to excessive tempering and a decrease in ductility due to carbide precipitation. Skin-pass rolling can be performed on the steel sheet from the viewpoint of stabilizing press formability, such as adjusting the surface roughness and flattening the sheet shape, and from the viewpoint of increasing the yield strength. The skin-pass elongation is preferably 0.1% or more and 0.5% or less. The sheet shape can also be flattened using a leveler. The average cooling rate CR4 from the above-mentioned holding end temperature to a temperature of 50°C or less is 1°C / s or more, preferably 5°C / s or more. In the present invention, no upper limit is set for the average cooling rate CR4, but from the viewpoint of manufacturing and suppressing the transformation from retained austenite to fresh martensite, it is preferably 10° C. / s or less.
[0090] Here, the average cooling rate CR4 is "(temperature (cooling stop temperature) of 150°C or more and 350°C or less and temperature T4 (°C) or less (holding end temperature (cooling start temperature)) - 50°C or less)) / (cooling time (seconds) from holding end temperature to cooling stop temperature)".
[0091] From the viewpoint of improving stretch flangeability, it is also possible to perform a low-temperature heat treatment at 100 to 300°C for 30 seconds to 10 days after the above heat treatment or after skin-pass rolling. This treatment causes hydrogen that has entered the steel sheet during tempering or annealing of martensite formed during final cooling or skin-pass rolling to be released from the steel sheet. The low-temperature heat treatment can reduce hydrogen to less than 0.1 ppm by mass.
[0092] It is also possible to apply electroplating. That is, the steel sheet may be subjected to electrogalvanizing treatment after the fourth cooling treatment step (after cooling at an average cooling rate CR4 of 1°C / s or more). After the electroplating treatment, it is preferable to apply the above-mentioned low-temperature heat treatment from the viewpoint of reducing hydrogen in the steel.
[0093] Second Embodiment In a second embodiment of the manufacturing method for a steel sheet according to the present invention, as shown in FIG. 3( b ), a steel slab having the above-described component composition is hot-rolled and cold-rolled, and then the resulting cold-rolled steel sheet is subjected to a process of (A c3After annealing at an annealing temperature of (Ms point (°C) - 15°C) or higher and 900°C or lower, the steel sheet is cooled from the annealing temperature to 500°C at an average cooling rate CR5 of 5°C / s or higher and 100°C / s or lower (first cooling treatment before retention treatment), and then cooled from 500°C to a retention stop temperature T5 of (Ms point (°C) or higher and 320°C) or higher at an average cooling rate CR6 of 10°C / s or lower for 10 seconds or lower and 60 seconds or lower (retention treatment), and then cooled from the retention stop temperature T5 to a temperature T1 of (Ms point (°C) - 30°C) or higher at an average cooling rate CR7 of 3°C / s or higher and 100°C / s or lower (second cooling treatment after retention treatment). 1 cooling treatment), heating from temperature T1 to a temperature range of 300°C or higher to a temperature T2 of 300°C or higher to 450°C or lower at an average heating rate of 2°C / s or higher, cooling from temperature T2 to a temperature range of (T2-150°C) or higher to a temperature T3 of (T2-30°C) or lower at an average cooling rate CR2 of 0.5°C / s or higher, cooling from temperature T3 to a temperature range of 150°C or higher to 350°C or lower and temperature T3 or lower at an average cooling rate CR3 of 0.1°C / s or higher, holding in the temperature range of 150°C or higher to 350°C or lower and temperature T4 or lower for 20 seconds to 1000 seconds, and cooling to a temperature of 50°C or lower at an average cooling rate CR4 of 1°C / s or higher.
[0094] In the second embodiment, the hot rolling, cold rolling, and annealing treatments can be performed under the same conditions as in the first embodiment. Furthermore, in the second embodiment, the treatment in the first cooling treatment step in the first embodiment is a first cooling treatment before the retention treatment, a retention treatment, and a first cooling treatment after the retention treatment. Furthermore, in the second embodiment, the heating treatment, the second cooling treatment, the third cooling treatment, the holding treatment, and the fourth cooling treatment after the first cooling treatment after the retention treatment can be performed under the same conditions as the heating treatment, the second cooling treatment, the third cooling treatment, the holding treatment, and the fourth cooling treatment, respectively, in the first embodiment. Furthermore, in the second embodiment, the hot-dip galvanizing treatment can be performed under the same conditions as in the first embodiment, except that, whereas in the first embodiment, the hot-dip galvanizing treatment is performed after the first cooling treatment step (after cooling at an average cooling rate CR1: 3°C / s or more and 100°C / s or less), in the first embodiment, the hot-dip galvanizing treatment is performed after the first cooling treatment step after the retention treatment (after cooling at an average cooling rate CR7: 3°C / s or more and 100°C / s or less). In the second embodiment, other conditions, including the low-temperature heat treatment after the total heat treatment and the conditions for the electroplating treatment, can also be the same as those in the first embodiment. Hereinafter, in this embodiment, the first cooling treatment before the retention treatment, the retention treatment, and the first cooling treatment after the retention treatment will be mainly described.
[0095] [First cooling treatment step before residence treatment: cooling from the annealing temperature to 500°C at an average cooling rate CR5 of 5°C / s or more and 100°C / s or less] [Residence treatment: residence for 10 s or more and 60 s or less at an average cooling rate CR6 of 10°C / s or less in the temperature range from 500°C to a residence stop temperature T5 of not less than the Ms point (°C) and not less than 320°C] By performing residence treatment during cooling, a larger area fraction of bainite is obtained, carbon is concentrated from this bainite to untransformed austenite, and the retained austenite is stabilized, resulting in a steel sheet with better ductility. Therefore, from the viewpoint of improving ductility, it is desirable to perform residence treatment during cooling.
[0096] When a retention treatment is performed during cooling, the steel is first cooled from the annealing temperature to 500°C at an average cooling rate CR5 of 5°C / s or more and 100°C / s or less. If the average cooling rate CR5 is lower than 5°C / s, a large amount of ferrite is formed, resulting in a decrease in strength and a decrease in λ. The average cooling rate CR5 is preferably 8°C / s or more. On the other hand, if the average cooling rate CR5 is too high, the sheet shape deteriorates, so the average cooling rate CR5 is 100°C / s or less, preferably 50°C / s or less, and more preferably less than 30°C / s.
[0097] Here, the average cooling rate CR5 is "(annealing temperature (cooling start temperature) (°C) - 500°C (cooling stop temperature)) / cooling time from the annealing temperature to 500°C (seconds)".
[0098] Next, by holding the steel at a temperature range from 500°C to a temperature range from the martensitic transformation start temperature Ms point (°C) or higher to a holding stop temperature T5 of 320°C or higher at an average cooling rate of 10°C / s or lower for 10 seconds to 60 seconds, it is possible to form bainite, and adjacent retained austenite with a high carbon concentration can be formed. If the temperature range is below the Ms point (°C), martensite forms first, and the bainite transformation progresses excessively due to the swing back phenomenon, resulting in a decrease in strength and stretch flangeability. On the other hand, if the temperature range exceeds 500°C, the driving force for bainite transformation decreases, and the amount of bainite transformation decreases. In addition, if the temperature range is below 320°C, lower bainite is mainly formed. However, from the viewpoint of improving ductility and VDA bending properties, upper bainite without carbide precipitation is advantageous in terms of suppressing carbon-enriched carbides in untransformed γ and preventing deterioration of axial crushing properties due to carbide precipitation. Therefore, the retention stop temperature T5 is set to 320°C or higher. From the above, the temperature range is set to be equal to or higher than the Ms point (°C) and equal to or higher than 320°C and equal to or lower than 500°C. The temperature range is preferably 350°C or higher, and more preferably 380°C or higher. The temperature range is preferably 480°C or lower, and more preferably 460°C or lower.
[0099] If the average cooling rate CR6 exceeds 10°C / s, the amount of bainite transformation decreases. Therefore, the average cooling rate CR6 is set to 10°C / s or less. Furthermore, if the residence time is less than 10 seconds, the desired amount of bainite cannot be obtained, and if it exceeds 60 seconds, C concentration from bainite to massive untransformed austenite progresses, resulting in an increase in the amount of residual massive structure. Therefore, the residence time is set to 10 seconds or more and 60 seconds or less. From the viewpoint of ensuring bainite and retained austenite, a residence time of 20 seconds or more is preferable. Furthermore, from the viewpoint of improving stretch flangeability by reducing the mass of mass, a residence time of 50 seconds or less is preferable.
[0100] Here, the average cooling rate CR6 is "(500°C (retention start temperature) (°C) - (retention stop temperature (°C) above the Ms point (°C) and above 320°C)) / (retention time (seconds) from the retention start temperature to the retention stop temperature)."
[0101] [First Cooling Treatment Step After Dwell Treatment: Cooling in the Range from Dwell Stop Temperature T5 to Temperature T1, which is 200°C or higher and (Martensitic Transformation Start Temperature Ms Point (°C) - 30°C) or lower, at an Average Cooling Rate CR7 of 3°C / s or higher and 100°C / s or lower] After the above-mentioned dwell treatment, rapid cooling is required to obtain a predetermined area ratio of tempered martensite and / or bainite. If the average cooling rate CR7 in the temperature range from Dwell Stop Temperature T5 to Temperature T1, which is 200°C or higher and (Martensitic Transformation Start Temperature Ms Point (°C) - 30°C) or lower (Cooling Stop Temperature T1), is less than 3°C / s, ferrite is generated during the cooling process, which reduces strength, stretch flangeability, and axial crush resistance. Therefore, from the perspective of suppressing ferrite generation, the average cooling rate CR7 in the temperature range from Dwell Stop Temperature T5 to Cooling Stop Temperature T1, which is 200°C or higher and (Ms Point (°C) - 30°C) or lower, is set to 3°C / s or higher. The average cooling rate CR7 is preferably 5°C / s or more, more preferably 8°C / s or more. On the other hand, if the average cooling rate CR7 is too high, the sheet shape deteriorates, so the average cooling rate CR7 is set to 100°C / s or less. The average cooling rate CR7 is preferably 50°C / s or less.
[0102] Furthermore, in order to ensure a predetermined amount of retained austenite, the temperature T1 (cooling stop temperature T1) is set to 200°C or higher. The temperature T1 (cooling stop temperature T1) is preferably 220°C or higher, and more preferably 240°C or higher. If the cooling stop temperature T1 exceeds (Ms point (°C) - 30°C), a large amount of massive untransformed austenite remains, the amount of fresh martensite at the time of final cooling increases, and stretch flangeability deteriorates. Therefore, the cooling stop temperature T1 is set to (Ms point (°C) - 30°C) or lower. The cooling stop temperature T1 is preferably (Ms point (°C) - 35°C) or lower.
[0103] Here, the average cooling rate CR7 is "(retention stop temperature T5 (cooling start temperature) (°C) - (Ms point (°C) - 30°C) (cooling stop temperature (°C))) / (cooling time from retention stop temperature T5 to cooling stop temperature (seconds))".
[0104] Next, the member of the present invention and the method for manufacturing the same will be described.
[0105] The member of the present invention is obtained by subjecting the steel plate of the present invention to at least one of forming and joining. Also, the method for manufacturing the member of the present invention includes a step of subjecting the steel plate of the present invention to at least one of forming and joining to form the member.
[0106] The steel sheet of the present invention has a tensile strength of 980 MPa or more, and has high ductility, excellent stretch flange formability, and excellent axial crushing properties. Therefore, members obtained using the steel sheet of the present invention also have high strength and have higher ductility, excellent stretch flange formability, and excellent axial crushing properties than conventional high-strength members. Furthermore, the use of the member of the present invention enables weight reduction. Therefore, the member of the present invention can be suitably used, for example, for vehicle body frame parts. The member of the present invention also includes welded joints.
[0107] The forming process can be performed using a general processing method such as press working without any restrictions, and the joining process can be performed using general welding methods such as spot welding and arc welding, riveting, crimping, etc. without any restrictions.
[0108] Cold-rolled steel sheets with a thickness of 1.4 mm and having the chemical composition shown in Table 1 were treated under the annealing conditions shown in Tables 2 and 3 to produce steel sheets of the present invention and steel sheets of comparative examples. The cold-rolled steel sheets were obtained by hot-rolling (heating temperature: 1250°C, soaking time: 60 min, finish rolling delivery temperature: 1150°C, coiling temperature: 550°C) and cold-rolling (rolling reduction (cumulative reduction): 50%) a steel slab having the chemical composition shown in Table 1. Table 2 shows the conditions under which no dwell treatment was performed, and Table 3 shows the conditions under which dwell treatment was performed. Some of the steel sheets (cold-rolled steel sheets: CR) were subjected to hot-dip galvanizing treatment in any step from temperature T1 after heating until holding at 150°C or lower and 350°C or lower, to produce hot-dip galvanized steel sheets (GI). Here, the steel sheet was subjected to hot-dip galvanizing treatment by immersing it in a zinc plating bath at 440°C or higher and 500°C or lower, and then the coating weight was adjusted by gas wiping or the like. For the hot-dip galvanizing, a zinc plating bath containing an Al content of 0.10% or higher and 0.22% or lower was used. Furthermore, some of the hot-dip galvanized steel sheets were subjected to an alloying treatment after the hot-dip galvanizing treatment to obtain alloyed hot-dip galvanized steel sheets (GA). Here, the alloying treatment was performed in a temperature range of 460°C or higher and 590°C or lower. Furthermore, some of the steel sheets (cold-rolled steel sheets: CR) were subjected to electroplating to obtain electrogalvanized steel sheets (EG).
[0109]
[0110]
[0111]
[0112] The steel structure was measured by the method described above. The measurement results are shown in Tables 4 and 5. Table 4 shows the conditions without holding treatment, and Table 5 shows the conditions with holding treatment.
[0113] (Tensile strength, ductility) JIS No. 5 tensile test pieces and hole expansion test pieces were taken from the obtained steel sheets, and tensile tests (based on JIS Z2241 (2011)) were performed. The tensile strength TS and total elongation T-El are shown in Tables 4 and 5. A tensile strength of 980 MPa or more was judged to have excellent strength. Furthermore, a total elongation T-El of 14.0% or more for TS less than 1180 MPa, 12.0% or more for TS between 1180 MPa and 1320 MPa, and 10.0% or more for TS 1320 MPa or more was judged to have excellent ductility.
[0114] (Stretch flangeability) The stretch flangeability was evaluated by a hole expansion test in accordance with the provisions of the Japan Iron and Steel Federation standard JFST1001. That is, a sample of 100 mm × 100 mm square size was punched using a punching tool with a punch diameter of 10 mm and a die diameter of 10.3 mm (clearance 13%), and then a conical punch with an apex angle of 60 degrees was used to punch out the burrs generated during punching, until a crack penetrating the plate thickness occurred. In this case, 0 : initial hole diameter (mm), d: hole diameter at crack occurrence (mm), hole expansion ratio λ (%) = {(d - d 0 ) / d 0} × 100. The hole expanding ratio λ is shown in Tables 4 and 5. Steel sheets having a λ of 45% or more were judged to have excellent stretch flangeability.
[0115] (Axial Crush Property) Fig. 4 is a diagram for explaining a method for calculating the VDA bend angle. As shown in Fig. 4, to evaluate the axial crush property, the VDA bend angle α was evaluated by a bending test (Verband der Automobilindustrie: VDA bend test) in accordance with the VDA standard (VDA238-100) defined by the German Association of the Automotive Industry. The VDA bend test is a bending test (Verband der Automobilindustrie: VDA bend test) in accordance with the VDA standard (VDA238-100) defined by the German Association of the Automotive Industry, and is a three-point plate bending test characterized by very closely spaced rolls 10 and a sharp punch 11. In the VDA bending test, a test piece of 60 mm x 60 mm square was used, the bending ridge direction was parallel to the rolling direction, the roll diameter D was 30 mm, and the distance between the rolls L (not shown) was (plate thickness a 0 The specimen was supported by a roll of 0.5 mm thick (x2) and pressed from above with a punch having a tip r (radius of curvature) of 0.4 mm at a stroke speed of 20 mm / min (in the figure, reference numeral 11A indicates the punch before pressing, and reference numeral 11B indicates the punch after pressing). Note that in FIG. 4, for the sake of explanation, the test piece (steel plate X) can be illustrated symmetrically about the pressing axis. A , X B ), only one side of the roll 10 is shown in the figure. The VDA bending angle α is the bending angle (°) calculated using formulas (1) to (5) from the stroke S (mm) at the maximum load in the bending test, and can be used as an index of axial crushing properties. Steel plates with an α of 80° or more were determined to have excellent axial crushing properties.
[0116] c (mm)=D / 2+r+a 0 ...(Formula 1)
[0117] p (mm) = D / 2 + L / 2 ... (Formula 2)
[0118]
[0119]
[0120]
[0121]
[0122]
[0123] The examples of the present invention shown in Tables 4 and 5 are excellent in strength, ductility, stretch flangeability and axial crushing properties, whereas the comparative examples are inferior in any of these properties.
[0124] Furthermore, it was found that the steel sheets of the present invention were used to prepare components obtained by forming, joining, and further to prepare components by forming and joining, and that the steel sheets of the present invention have high strength, high ductility, excellent stretch flange formability, and excellent axial crushing properties, and therefore have high strength, high ductility, excellent stretch flange formability, and excellent axial crushing properties, similar to the steel sheets of the present invention.
[0125] The present invention makes it possible to produce steel sheets that are excellent in ductility, stretch flangeability, and axial crush resistance and are used for components of automobiles and home appliances, and are particularly suitable for energy absorbing components of automobiles, and can be preferably applied to the press forming of these components.
[0126] F Ferrite TM Tempered martensite UB Upper bainite LB Lower bainite FM Fresh martensite RA Retained austenite α VDA bending angle 10 Roll D Roll diameter 11 Punch 11A Punch before pressing 11B Punch after pressing S Stroke r Tip curvature radius X A Steel plate before pressing X B Steel plate after pressing a 0 Plate thickness
Claims
1. In mass percent, C: 0.10% or more and 0.30% or less, Si: 0.5% or more and 2.0% or less, Mn: 1.5% or more and 3.0% or less, P: 0.10% or less, S: 0.020% or less, sol. A steel sheet having a component composition containing Al: 1.00% or less, N: 0.015% or less, with the balance being Fe and unavoidable impurities, and having a steel structure containing, in area ratios, ferrite: 15% or less, tempered martensite: 30% to 80%, bainite: 10% to 40%, retained austenite: 5% or more, and fresh martensite: 10% or less, wherein an average C concentration in the retained austenite is 0.60 mass% or more, and the content of Fe element present as carbides in the tempered martensite is 0.20 mass% or less on average in a region within 100 μm from the steel sheet surface in the sheet thickness direction.
2. The steel plate according to claim 1, wherein the chemical composition further contains, in mass%, at least one selected from the following: Ti: 0.100% or less, Nb: 0.100% or less, V: 0.100% or less, B: 0.0050% or less, Cr: 1.000% or less, Cu: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Ta: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, REM: 0.0050% or less.
3. The steel sheet according to claim 1 or 2, which has a zinc-plated layer on the surface of the steel sheet.
4. A member made using the steel plate according to any one of claims 1 to 3.
5. A steel slab having the composition according to claim 1 or 2 is hot-rolled and cold-rolled, and then the resulting cold-rolled steel sheet is subjected to the following steps: (A c3 After performing annealing treatment at an annealing temperature of 200°C or more and (Ms point (°C) - 15°C) or less and 900°C or less, cooling from the annealing temperature to a temperature T1 of 200°C or more and (Ms point (°C) - 30°C) or less at an average cooling rate CR1 of 3°C / s or more and 100°C / s or less, heating from the temperature T1 to a temperature T2 of 300°C or more and 450°C or less at an average heating rate of 2°C / s or more, cooling from the temperature T2 to a temperature T3 of (T2 - 150°C) or more and (T2 - 30°C) or less at an average cooling rate CR2 of 0.5°C / s or more, cooling from the temperature T3 to a temperature T4 of 150°C or more and 350°C or less and the temperature T3 or less at an average cooling rate CR3 of 0.1°C / s or more, holding in the temperature range of 150°C or more and 350°C or less and the temperature T4 or less for 20 s or more and 1000 s or less, A method for manufacturing a steel plate, comprising cooling the steel plate to a temperature of 50°C or less at an average cooling rate of CR4: 1°C / s or more.
6. A steel slab having the composition according to claim 1 or 2 is hot-rolled and cold-rolled, and then the resulting cold-rolled steel sheet is subjected to the following steps: (A c3 annealing at an annealing temperature of not less than 900°C (temperature (°C) - 15°C), cooling at an average cooling rate CR5 of not less than 5°C / s and not more than 100°C / s in a temperature range from the annealing temperature to 500°C, retaining at an average cooling rate CR6 of not more than 10°C / s in a temperature range from 500°C to a residence stop temperature T5 of not less than Ms point (°C) and not less than 320°C for 10 s to 60 s, cooling at an average cooling rate CR7 of not less than 3°C / s and not more than 100°C / s in a temperature range from the residence stop temperature T5 to a temperature T1 of not less than 200°C and not more than (Ms point (°C) - 30°C), heating at an average heating rate of not less than 2°C / s in a temperature range from the temperature T1 to a temperature T2 of not less than 300°C and not more than 450°C, a temperature range from said temperature T2 to a temperature T3 of (T2-150°C) or more and (T2-30°C) or less, at an average cooling rate CR2: 0.5°C / s or more; a temperature range from said temperature T3 to a temperature T4 of 150°C or more and 350°C or less and said temperature T3 or less, at an average cooling rate CR3: 0.1°C / s or more; a temperature range of 150°C or more and 350°C or less and said temperature T4 or less, at least 20 s and at most 1000 s; and a temperature range of 50°C or less and at most 50°C ...
7. A method for producing a steel sheet according to claim 5, wherein the steel sheet is subjected to a hot-dip galvanizing treatment or a hot-dip galvannealing treatment after cooling at the average cooling rate CR1 of 3°C / s or more and 100°C / s or less.
8. A method for producing a steel sheet according to claim 6, wherein the steel sheet is subjected to a hot-dip galvanizing treatment or a hot-dip galvannealing treatment after cooling at an average cooling rate CR7 of 3°C / s or more and 100°C / s or less.
9. The method for producing steel sheet according to claim 5 or 6, wherein the steel sheet is subjected to an electrolytic galvanizing treatment after cooling at an average cooling rate CR4 of 1°C / s or more.
10. A method for manufacturing a component, comprising the step of subjecting the steel plate according to any one of claims 1 to 3 to at least one of forming and joining to form the component.
Citation Information
Patent Citations
High strength hot dip galvanized steel sheet and high strength hot dip alloyed galvanized steel sheet having excellent formability and hole expandability, method for producing high strength hot dip galvanized steel sheet and method for producing high strength hot dip alloyed galvanized steel sheet
JP2007211280A
High strength steel and manufacturing method
JP2017507241A
Method for producing high strength steel plate with improved ductility and formability and resulting steel plate
JP2019505691A
Steel sheet and manufacturing method therefor
WO2019186997A1
Steel sheet, member, method for producing said steel sheet, and method for producing said member
WO2022004817A1
Cited By
Steel plates, components, and methods for manufacturing them.
JP7948496B1
Steel sheet and manufacturing method therefor
WO2026135011A1
Steel sheet, member, and methods for manufacturing steel sheet and member
WO2026160042A1