Ultra-quick hardening mortar material for grout, and mortar-hardened body
The mortar material with cement, calcium aluminate, and gypsum, and adjusted expansion coefficients addresses the issue of excessive long-term expansion in conventional ultra-fast hardening mortars, ensuring structural stability and aesthetic integrity by controlling expansion rates and enhancing filling and strength properties.
Patent Information
- Application Number
- PCT/JP2024/011159
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional ultra-fast hardening mortar materials for grout lack long-term expansion control, leading to potential structural damage due to excessive expansion over time, which can impair the stability, waterproofness, and aesthetic appearance of structures.
A mortar material comprising cement, calcium aluminate, and gypsum, with an initial expansion coefficient adjusted within a predetermined range (0.005-0.5% at 3 days, 0.01-0.75% at 7 days, and 0.015-1.0% at 28 days), along with optional foaming and antifoaming agents, water reducers, and specific cement types to achieve a moderate long-term expansion rate.
The material ensures a controlled long-term expansion rate, preventing structural damage and maintaining adhesion and stability, while improving filling properties and strength development.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Ultra-fast hardening mortar material for grout, hardened mortar
[0001] The present invention relates to an ultra-rapid hardening mortar material for grout and a hardened mortar.
[0002] Grout is used for the construction of underground structures, the installation of bridge supports, the installation of various machinery, and for filling gaps in walls and pillars during earthquake reinforcement. In recent years, there has been an increasing demand for streamlined construction, and as a result, there is a demand for mortar materials that are ultra-fast hardening and have self-filling and self-leveling properties.
[0003] Mortar materials lose volume as the cement hydrates or dries, so when used as grout, there is a risk of cracking or a decrease in adhesion to existing structures.Cracking not only impairs the aesthetic appearance, but also has the risk of adversely affecting the stability, waterproofing, and watertightness of the structure.
[0004] Therefore, in order to compensate for the shrinkage of cement, suppress the occurrence of cracks, and maintain adhesion to the structure, for example, 3CaO·3Al 2 O 3 CaSO 4 (Auin), CaSO 4 In addition to calcium sulfoaluminate-based (aluminous-based expanding materials) whose main component is CaO, and lime-based (lime-based expanding materials) whose main component is free lime, expanding materials containing free lime, hydraulic material, and gypsum are also used.
[0005] Known examples of materials with excellent ultra-rapid hardening properties include ultra-rapid hardening cement compositions in which metal sulfates, fly ash, etc. are added to calcium aluminates or gypsum to ensure fluidity (Patent Documents 1 to 3). Also proposed are ultra-rapid hardening cements in which lithium carbonate is blended with calcium aluminates and gypsum (Patent Document 4), and mortars in which calcium aluminate, anhydrous gypsum, lithium carbonate, and slaked lime are blended with Portland cement (Patent Document 5).
[0006] JP 03-12350, JP 01-230455, JP 11-139859, JP 01-290543, JP 2005-75712
[0007] However, the above-mentioned conventional materials do not take into consideration long-term expansion, and there is a problem that after application as grout to a structure, the expansion becomes excessive over a long period of time, which may cause damage to the structure, etc. Therefore, there is a demand for a mortar material for grout that takes into consideration expansion performance from the initial stage to the long term.
[0008] SUMMARY OF THE INVENTION Accordingly, an object of the present invention is to provide an ultra-rapid hardening mortar material for grout that can maintain a suitable long-term expansion rate.
[0009] As a result of intensive research into solving the above-mentioned problems, the inventors have found that the above problems can be solved by an ultra-rapid-setting mortar material for grout, which contains cement, calcium aluminate, and gypsum and has an initial expansion coefficient adjusted to fall within a predetermined range, and have arrived at the present invention.
[0010] [1] An ultra-rapid hardening mortar material for grout, comprising cement, calcium aluminate, and gypsum, and having expansion coefficients of 0.005 to 0.5%, 0.01 to 0.75%, and 0.015 to 1.0% at ages of 3 days, 7 days, and 28 days, respectively. [2] The ultra-rapid hardening mortar material for grout according to [1] above, having an air content of 0 to 5% after mixing. [3] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having a flow value of 170 to 320 mm after mixing. [4] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing. [5] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having a flow value of 170 to 320 mm after mixing. [6] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing. [7] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing. [8] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing. [9] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing.
[10] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content of 0 to 5% after mixing.
[11] The ultra-rapid hardening mortar material for grout according to [1] or [2] above, having an air content 14 The ultra-rapid-setting mortar material for grout according to any one of [1] to [3] above, which has a funnel flow time of 6 to 10 seconds. [5] The ultra-rapid-setting mortar material for grout according to any one of [1] to [4] above, further comprising a foaming agent. [6] The ultra-rapid-setting mortar material for grout according to any one of [1] to [5] above, further comprising an antifoaming agent. [7] The ultra-rapid-setting mortar material for grout according to any one of [1] to [6] above, further comprising one or more water reducing agents selected from the group consisting of lignin-based water reducing agents, melamine-based water reducing agents, and naphthalene sulfone-based water reducing agents. [8] A hardened mortar obtained by using the ultra-rapid-setting mortar material for grout according to any one of [1] to [7] above.
[0011] According to the present invention, it is possible to provide an ultra-rapid hardening mortar material for grout that can maintain a suitable long-term expansion rate.
[0012] Hereinafter, one embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to this embodiment. In addition, "%" and "parts" in this specification are based on mass unless otherwise specified.
[0013] [Ultra-rapid-hardening mortar material for grout] The ultra-rapid-hardening mortar material for grout of the present invention contains cement, calcium aluminate, and gypsum, and has expansion coefficients of 0.005-0.5%, 0.01-0.75%, and 0.015-1.0% at ages of 3, 7, and 28 days, respectively. The expansion coefficients are preferably in the range of 3 days≦7 days≦28 days. The ultra-rapid-hardening mortar material for grout can be used as a grout by mixing with water, and by adjusting the initial expansion coefficient to fall within a predetermined range, the long-term expansion coefficient can be made appropriate. This prevents damage to structures and the like when used as a grout. Note that "long-term" refers to an age of at least 60 days or more. Further, the expansion coefficient in the present invention is measured according to the method specified in JIS A 6202:2017 "Expansive additive for concrete" Appendix A "Expansive additive mortar expansion test method".
[0014] The ultra-rapid hardening mortar material for grout has an expansion rate of 0.005 to 0.5% at 3 days old, preferably 0.01 to 0.4%, more preferably 0.05 to 0.3%, and even more preferably 0.1 to 0.2%. If the expansion rate at 3 days old is less than 0.005%, the long-term expansion rate may be insufficient, and if it exceeds 0.5%, the long-term expansion rate may be excessive.
[0015] The ultra-rapid hardening mortar material for grout has an expansion rate of 0.01 to 0.75% at 7 days, preferably 0.02 to 0.5%, more preferably 0.08 to 0.4%, and even more preferably 0.12 to 0.3%. If the expansion rate at 7 days is less than 0.01%, the long-term expansion rate may be insufficient, and if it exceeds 0.75%, the long-term expansion rate may be excessive.
[0016] The ultra-rapid hardening mortar material for grout has an expansion rate of 0.015 to 1.0% at 28 days, preferably 0.03 to 0.6%, more preferably 0.1 to 0.5%, and even more preferably 0.16 to 0.4%. If the expansion rate at 28 days is less than 0.015%, the long-term expansion rate may be insufficient, and if it exceeds 1.0%, the long-term expansion rate may be excessive.
[0017] The ultra-rapid hardening mortar material for grout has a ratio of the expansion rate at 3 days to the expansion rate at 7 days of preferably 1.00 to 1.55, more preferably 1.05 to 1.50, and even more preferably 1.08 to 1.40. When the ratio of the expansion rate at 3 days to the expansion rate at 7 days is within the above range, it is easy to maintain an appropriate long-term expansion rate.
[0018] The ultra-rapid hardening mortar material for grout has a ratio of the expansion rate at 7 days to the expansion rate at 28 days of preferably 1.15 to 1.60, more preferably 1.20 to 1.55, and even more preferably 1.30 to 1.50. When the ratio of the expansion rate at 7 days to the expansion rate at 28 days of is within the above range, it is easy to maintain an appropriate long-term expansion rate.
[0019] The ultra-rapid setting mortar material for grout preferably has an air content of 0 to 5% after mixing, more preferably 0 to 4%, and even more preferably 0 to 3%. When the air content after mixing is within the above range, strength development is improved. The air content in the present invention is measured in accordance with the method specified in JIS A 1116:2019 "Test method for unit volume mass of fresh concrete and test method for air content by mass (mass method)."
[0020] The ultra-rapid hardening mortar material for grout preferably has a flow value after mixing of 170 to 320 mm, more preferably 190 to 250 mm, and even more preferably 200 to 220 mm. When the flow value after mixing is within the above range, the filling property is improved. Note that the flow value in the present invention is measured using the method specified in JIS R 5201:2015 "Physical Testing Methods for Cement" without performing the 15 drop motions.
[0021] The ultra-fast hardening mortar material for grout is J after mixing. 14 The funnel flow time is preferably 6 to 10 seconds, more preferably 7 to 9 seconds, and even more preferably 7.5 to 8.5 seconds. 14 When the funnel flow time is within the above range, the filling property is improved. 14 The funnel flow time was measured in accordance with the method specified in the Japan Society of Civil Engineers standard JSCE-F 541-2013 "Test method for fluidity of filling mortar."
[0022] The cement contained in the ultra-rapid-hardening mortar material for grout according to this embodiment is not particularly limited, and examples include various Portland cements, such as normal, early-strength, extra-early-strength, low-heat, and medium-heat cements; various blended cements obtained by mixing these Portland cements with blast furnace slag, fly ash, or silica fume; environmentally friendly cements (ecocements) produced using raw materials such as municipal waste incineration ash or sewage sludge incineration ash; commercially available fine particle cements; and white cements. Various cements can also be finely powdered and used. Also, cements prepared by increasing or decreasing the content of components normally used in cements can be used. Furthermore, combinations of two or more of these cements can also be used.
[0023] In order to obtain appropriate fluidity and early strength, the cement should have a Blaine specific surface area value (hereinafter simply referred to as the "Blaine value") of 2,500 to 7,000 cm 2 / g, and 2,750 to 6,000 cm 2 / g, and more preferably 3,000 to 4,500 cm 2In the present invention, the Blaine specific surface area value is measured in accordance with JIS R 5201:2015 "Physical testing methods for cement."
[0024] The calcium aluminate contained in the ultra-fast hardening mortar material for grout according to this embodiment is a mixture of CaO and Al 2 O 3 It is a general term for compounds that have hydration activity and contain CaO and / or Al as the main components. 2 O 3 or a compound in which a part of the above is replaced with an alkali metal oxide, an alkaline earth metal oxide, silicon oxide, titanium oxide, iron oxide, an alkali metal halide, an alkaline earth metal halide, an alkali metal sulfate, an alkaline earth metal sulfate, or the like, or a compound in which CaO and Al 2 O 3 It is a substance in which these are dissolved in small amounts as a solid solution in a substance mainly composed of these, and calcium aluminate may be either crystalline or amorphous.
[0025] Specific examples of crystalline materials include CaO, C, and Al. 2 O 3 A, R 2 O(Na 2 O.K. 2 O, Li 2 O) is R, then C 3 A and C, which is a solid solution of alkali metals 14 R.A. 5 , C.A., C. 12 A 7 Or C 11 A 7 CaF 2 , C 4 A.Fe 2 O 3 , and C 3 A 3 CaSO 4 Among them, amorphous calcium aluminate is preferred because of its quick setting property. In the case of crystalline calcium aluminate, C 11 A 7 CaF 2 In the case of amorphous calcium aluminate, the vitrification rate is preferably 80% or more.
[0026] Calcium aluminate CaO / Al 2 O 3 The molar ratio is not particularly limited, but from the viewpoint of achieving appropriate fluidity retention and initial strength, the molar ratio is preferably 1.3 to 3.0, more preferably 1.4 to 2.5, even more preferably 1.5 to 2.0, and even more preferably 1.7 to 1.9.
[0027] Calcium aluminate can be obtained by combining CaO raw materials such as calcium carbonate and calcium hydroxide with Al raw materials such as bauxite. 2 O 3 Examples of the method include heat treating the raw materials in a rotary kiln, an electric furnace, etc. Specifically, the raw materials are mixed in a predetermined ratio, heated and melted in an electric furnace, etc., and then quenched by contacting with compressed air or water. By adjusting the ratio of the raw materials, the above CaO / Al 2 O 3 The molar ratio can be adjusted, and the vitrification rate can be adjusted by the temperature during heating and melting and the cooling method.
[0028] When calcium aluminate is obtained industrially, it may contain impurities. Specific examples of impurities include SiO 2 , Fe 2 O 3 , MgO, TiO 2 , MnO, Na 2 O.K. 2 O, Li 2 O, S, P 2 O 5 However, the presence of these impurities does not pose a problem as long as it does not substantially impair the object of the present invention. Specifically, it does not pose a problem as long as the total amount of these impurities is 10% or less.
[0029] It is preferable to use calcium aluminate with an ignition loss of 1% or more, as specified in JIS R 5202:2015 "Methods for Chemical Analysis of Cement," and it is more preferable to use calcium aluminate with an ignition loss of 2% or more. When the ignition loss of calcium aluminate is 1% or more, the occurrence of "collapse" is easily suppressed. There are no particular limitations on the method for achieving an ignition loss of 1% or more, and examples include a method of supplying water or moisture, a method of supplying carbon dioxide gas, etc.
[0030] The Blaine value of calcium aluminate is not particularly limited, but is usually 3,000 to 9,000 cm 2 / g is preferred, and 4,000 to 8,000 cm 2 / g is more preferred.
[0031] The content of calcium aluminate in the ultra-rapid hardening mortar material for grout is preferably 2 to 30 parts by mass, more preferably 5 to 20 parts by mass, and even more preferably 5 to 18 parts by mass, relative to 100 parts by mass of cement in the mortar material, from the viewpoint of adjusting the expansion coefficient at ages of 3 days, 7 days, and 28 days.
[0032] The gypsum contained in the ultra-rapid-hardening mortar material for grout according to this embodiment is a general term for gypsum anhydrite, gypsum hemihydrate, or gypsum dihydrate, and is not particularly limited. However, from the viewpoint of strength development, the use of gypsum anhydrite or gypsum hemihydrate is preferred, and the use of gypsum anhydrite is more preferred.
[0033] The Blaine value of gypsum is not particularly limited, but is usually 3,000 to 9,000 cm 2 / g is preferred, and 4,000 to 8,000 cm 2 / g is more preferred.
[0034] The content of gypsum in the ultra-rapid hardening mortar material for grout is preferably 3 to 40 parts by mass, more preferably 5 to 30 parts by mass, and even more preferably 7.5 to 28 parts by mass, relative to 100 parts by mass of cement in the mortar material, from the viewpoint of adjusting the expansion rate at ages of 3 days, 7 days, and 28 days.
[0035] The total content of calcium aluminate and gypsum relative to the cement content in the ultra-rapid hardening mortar material for grout is preferably 8 to 50%, more preferably 10 to 45%, and even more preferably 15 to 40%. When the total content of calcium aluminate and gypsum relative to the cement content is within the above range, it is easy to maintain an appropriate long-term expansion rate.
[0036] The ultra-rapid-hardening mortar material for grout preferably further contains a foaming agent. The foaming agent may be organic, inorganic, or a combination thereof. Organic foaming agents include oily substances such as vegetable oil and mineral oil, as well as nitrogen gas foaming agents that foam nitrogen gas under an alkaline atmosphere, such as azo compounds, nitroso compounds, and hydrazine derivatives. Inorganic foaming agents include percarbonates such as sodium percarbonate, potassium percarbonate, and ammonium percarbonate, permanganates such as potassium permanganate, peroxides such as hydrogen peroxide, and powders such as aluminum powder produced by atomization. Other foaming agents include flaky aluminum powder surface-treated with stearic acid.
[0037] The content of the foaming agent is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.45 parts by mass, and even more preferably 0.008 to 0.4 parts by mass, relative to 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout.
[0038] The ultra-rapid-hardening mortar material for grout preferably further contains an antifoaming agent. The type of antifoaming agent is not particularly limited as long as it does not significantly adversely affect the properties of the grout, and either liquid or powder form can be used. Examples of the antifoaming agent include polyether-based antifoaming agents, polyhydric alcohol-based antifoaming agents such as polyhydric alcohol esters and alkyl ethers, alkyl phosphate-based antifoaming agents, and silicone-based antifoaming agents.
[0039] The content of the antifoaming agent is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.45 parts by mass, and even more preferably 0.01 to 0.4 parts by mass, relative to 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout. By having the content of the antifoaming agent within the above range, strength development is improved.
[0040] The ultra-rapid-hardening mortar material for grout preferably further contains one or more water-reducing agents selected from the group consisting of lignin-based water-reducing agents, melamine-based water-reducing agents, and naphthalene sulfone-based water-reducing agents, and more preferably contains three types: lignin-based water-reducing agents, melamine-based water-reducing agents, and naphthalene sulfone-based water-reducing agents. Examples of lignin-based water-reducing agents include "Mighty 150" manufactured by Kao Corporation and "Plastocrete NC" manufactured by Sika Japan. Examples of melamine-based water-reducing agents include "Sikament FF24" manufactured by Sika Japan and "Master-Rehobuild 4000" manufactured by BASF Pozzolith. Examples of naphthalene sulfone-based water-reducing agents include "Mighty 100" manufactured by Kao Corporation, "Sanyo Revellon PHL" manufactured by Sanyo Chemical Industries, Ltd., and "Cellflow" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.
[0041] The content of the water reducing agent is preferably 0.05 to 2.0 parts by mass, more preferably 0.1 to 1.8 parts by mass, and even more preferably 0.15 to 1.0 parts by mass, in terms of solid content, relative to 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout. When the content of the water reducing agent is within the above range, the filling property is improved.
[0042] The total content of cement, calcium aluminate, gypsum, foaming agent, antifoaming agent, and water-reducing agent, excluding aggregate, in the ultra-rapid hardening mortar material for grout is preferably 90% or more, and more preferably 95% or more, which makes it easier to maintain a moderate long-term expansion rate.
[0043] The aggregate used in the present invention may be the same fine or coarse aggregate as that used in ordinary cement mortar or concrete, such as river sand, river gravel, mountain sand, mountain gravel, crushed stone, crushed sand, limestone aggregate, lime sand, silica sand, colored sand, artificial aggregate, blast furnace slag aggregate, sea sand, sea gravel, artificial lightweight aggregate, heavy weight aggregate, or a combination of these.
[0044] The content of the aggregate is preferably 40 to 250 parts by mass, more preferably 50 to 230 parts by mass, and even more preferably 60 to 200 parts by mass, per 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout. By having the content of the aggregate within the above range, strength development is improved and it is easy to maintain an appropriate long-term expansion rate.
[0045] In the present invention, the use of an alkali metal carbonate can enhance the fluidity-retaining effect and further improve strength development. Examples of alkali metal carbonates include sodium carbonate, potassium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, and lithium bicarbonate, and these can also be used in combination. In particular, the use of lithium carbonate is preferred from the viewpoint of strength development.
[0046] The content of the alkali metal carbonate is preferably 1 to 6 parts by mass, more preferably 2 to 5 parts by mass, in terms of solid content, relative to 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout. By having the content of the alkali metal carbonate within the above range, a constant handling time can be easily ensured and strength development can be improved.
[0047] The ultra-rapid hardening mortar material for grout of the present invention can contain a siliceous fine powder from the viewpoint of enhancing strength development. Examples of the siliceous fine powder include latent hydraulic substances such as ground granulated blast furnace slag, fly ash, and pozzolanic substances such as silica fume, among which silica fume is preferred. The type of silica fume is not limited, but from the viewpoint of fluidity, it is preferable to use ZrO as an impurity. 2It is more preferable to use silica fume containing 10% or less of the above-mentioned compound or acidic silica fume. Acidic silica fume is a silica fume that, when 1 g of silica fume is added to 100 cc of pure water and stirred, the supernatant liquid has an acidic pH of 5.0 or less.
[0048] The fineness of the silica fine powder is not particularly limited, but usually, the fine powder of granulated blast furnace slag and fly ash has a Blaine value of 3,000 to 9,000 cm 2 / g, and silica fume has a BET specific surface area of 20,000 to 300,000 cm 2 / g range.
[0049] The content of the siliceous fine powder is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 3 to 12 parts by mass, relative to 100 parts by mass of cement in the ultra-rapid hardening mortar material for grout. By having the content of the siliceous fine powder within the above range, strength development can be improved.
[0050] In the present invention, a setting retarder can also be used. As the setting retarder, a hydroxycarboxylic acid or a salt thereof is preferred, and as the hydroxycarboxylic acid, gluconic acid is more preferred, and as the salt, a sodium salt is more preferred.
[0051] The content of the set retarder is preferably 0.3 to 6 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of cement in the ultra rapid hardening mortar material for grout.
[0052] In the present invention, one or more of the following may be used to the extent that they do not adversely affect performance: gas foaming substances, water reducing agents, setting regulators, air-entraining agents, rust inhibitors, water repellents, antibacterial agents, colorants, antifreeze agents, admixtures such as fine limestone powder, slowly cooled blast furnace slag powder, sewage sludge incineration ash and its molten slag, municipal waste incineration ash and its molten slag, and pulp sludge incineration ash; thickeners; shrinkage reducing agents; polymers; clay minerals such as bentonite and sepiolite; and anion exchangers such as hydrotalcite.
[0053] In the ultra-rapid hardening mortar material for grout of the present invention, the method of mixing the materials is not particularly limited, and the materials may be mixed at the time of construction, or some or all of them may be mixed in advance. As the mixing device, any existing device such as a tilting mixer, omni mixer, Henschel mixer, V-type mixer, Plosser mixer, and Nauta mixer can be used.
[0054] [Hardened Mortar] The hardened mortar of the present invention contains the ultra-rapid-setting mortar material for grout of the present invention described above and water, and is obtained by kneading the ultra-rapid-setting mortar material for grout with water. The amount of water used for mixing in the present invention is not particularly limited, as it varies depending on the purpose and application of use and the content ratio of each material, but is preferably 10 to 70 parts by mass, more preferably 14 to 65 parts by mass, and even more preferably 16 to 60 parts by mass, per 100 parts by mass of cement material. By keeping the amount of water used for mixing within the above range, filling properties and strength development are improved.
[0055] Application methods using the ultra-rapid-setting mortar material for grout of the present invention include adding a predetermined amount of water, mixing, and pouring the mixture into the application area, filling the mixed grout using a pump, mixing the grout and then spraying it with compressed air, or applying it with a plastering trowel. The mixing method includes, but is not limited to, pouring the materials into a container such as a pail and mixing them with a hand mixer, mixing using a mixer, or hand mixing. The cement composition of the present invention hardens when mixed and filled into the application area. That is, a hardened product is obtained using the ultra-rapid-setting mortar material for grout of the present invention.
[0056] The present invention will be further explained below based on experimental examples, but the present invention is not limited to these.
[0057] Experimental Example 1: The materials shown below were mixed with 100 parts by mass of cement in the proportions shown in Table 1 to prepare an ultra-rapid-setting mortar material for grout. The aggregate and set modifier were mixed in amounts of 100 parts by mass and 1.5 parts by mass, respectively, per 100 parts by mass of cement, calcium aluminate, and gypsum combined. 18 parts by mass of water was added to 100 parts by mass of the prepared ultra-rapid-setting mortar material for grout, and the mixture was kneaded to prepare a grout, which was then subjected to various measurements. Furthermore, a hardened mortar was produced using the prepared grout, and its strength was measured.
[0058] (Materials used) Cement: Trial cement simulating ordinary Portland cement (mixed raw materials at the cement factory and various commercially available pure chemicals were used to adjust the chemical components), Blaine value 3,450 cm 2 / g. Calcium aluminate: vitrification rate 97%, CaO / Al 2 O 3 Molar ratio 1.7, loss on ignition 1.0%, main components CaO and Al 2 O 3 and 12CaO.7Al 2 O 3 , Blaine value 5,000 cm 2 / g. Gypsum: anhydrous gypsum, reagent. Aggregate: fine aggregate, lime sand 0.6 mm or less 50% and 0.6 to 1.2 mm 50% mixed. Density 2.52 g / cm 3 Antifoaming agent: A mixture of special nonionic surfactant and silica, commercially available. Foaming agent: Aluminum powder (surface treated), commercially available. Water reducer 1: Naphthalene sulfonic acid-based water reducer, commercially available. Setting adjuster: Sodium gluconate, reagent. Water: Tap water.
[0059] (Measurement items) Expansion rate: The expansion rate of the mixed grout was measured at ages of 3 days, 7 days, 28 days, and 60 days using a measurement method in accordance with the method specified in JIS A 6202:2017 "Expansive additives for concrete" Appendix A "Test method for expansion properties of expansive additives in mortar." The results are shown in Table 1. Air content: The mixed grout was measured using a method specified in JIS A 1116:2019 "Test method for unit volume mass of fresh concrete and test method for air content by mass (mass method)." The results are shown in Table 1. Flow value: The mixed grout was measured using a method specified in JIS R 5201:2015 "Physical test methods for cement" without performing 15 drop motions. The results are shown in Table 1. J 14 Funnel flow time: The mixed grout was measured in accordance with the method specified in the Japan Society of Civil Engineers standard JSCE-F 541-2013, "Test method for fluidity of filled mortar." The results are shown in Table 1. Expansion and shrinkage rate: The mixed grout was measured in accordance with the method specified in JSCE-F 542-2013, "Test method for bleeding rate and expansion rate of filled mortar." The results are shown in Table 1. Compressive strength: The compressive strength of the hardened mortar was measured at ages of 3 hours and 28 days in accordance with the method specified in JSCE-G 505-2018, "Test method for compressive strength of mortar or cement paste using cylindrical specimen." The results are shown in Table 1.
[0060]
[0061] Experimental Example 2 A grout was prepared and a hardened mortar was produced in the same manner as in Experimental Example 1, except that the following water-reducing agent was also used. The results are shown in Table 2.
[0062] (Materials used) Water reducing agent 2: Lignin-based water reducing agent, commercially available. Water reducing agent 3: Melamine-based water reducing agent, commercially available.
[0063] The ultra-rapid-hardening mortar material for grout of the present invention contains cement, calcium aluminate, and gypsum, and has an initial expansion rate within a predetermined range, thereby enabling a moderate long-term expansion rate. Therefore, the material can be widely used in the fields of civil engineering and construction, such as for fixing reinforcing steel bars in concrete structures used in water supply and sewage systems, agriculture and water supply systems, railways, electricity, roads, and construction.
Claims
1. An ultra-fast hardening mortar material for grout, comprising cement, calcium aluminate, and gypsum, and having expansion rates of 0.005-0.5%, 0.01-0.75%, and 0.015-1.0% at ages of 3, 7, and 28 days, respectively.
2. The ultra-fast hardening mortar material for grout according to claim 1, in which the air content after mixing is 0 to 5%.
3. The ultra-fast hardening mortar material for grout according to claim 1 or 2, which has a flow value after mixing of 170 to 320 mm.
4. J after mixing 14 The ultra-fast hardening mortar material for grout according to claim 1 or 2, wherein the funnel flow time is 6 to 10 seconds.
5. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising a foaming agent.
6. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising an antifoaming agent.
7. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising one or more water reducing agents selected from the group consisting of lignin-based water reducing agents, melamine-based water reducing agents, and naphthalene sulfone-based water reducing agents.
8. A hardened mortar obtained by using the ultra-fast hardening mortar material for grout according to claim 1 or 2.
Citation Information
Patent Citations
Nonshrinking mortar composition and quick-hardenable nonshrinking mortar composition
JP2001328856A
Ultra rapid hardening cement admixture, ultra rapid hardening cement composition, ultra rapid hardening grout mortar and mortar hardened body obtained by using the same
JP2005289656A
Supper quick-hardening high-fluidity cement composition and mortar or concrete using the same
JP2007145652A
Ultrarapid hardening cement composition, ultrarapid hardening mortar composition and ultrarapid hardening grout mortar
JP2007297250A
Rapid hardening type lightweight grout composition
JP2016113327A