Alumina-based composite oxide and method for producing alumina-based composite oxide
The alumina-based composite oxide with controlled element distribution addresses the issue of agglomeration and inactivity at high temperatures by supporting catalytic metal elements with high affinity, ensuring sustained catalytic activity and durability in exhaust gas purification systems.
Patent Information
- Application Number
- PCT/JP2024/011204
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional alumina-containing composite oxides with uniform element distribution become inactive and prone to agglomeration of catalytic metal elements at high temperatures, making it difficult to maintain catalytic activity over time.
An alumina-based composite oxide with controlled element distribution, specifically varying alumina and ceria/zirconia content across tertiary particles, supports catalytic metal elements with high affinity, preventing agglomeration and maintaining catalytic activity by using a method involving hydrated alumina suspension and ceria/zirconia precursors to control element distribution.
The alumina-based composite oxide effectively suppresses agglomeration and maintains catalytic activity of metal catalysts at high temperatures, enhancing the durability and performance of catalysts in exhaust gas purification systems.
Smart Images

Figure JP2024011204_03102024_PF_FP_ABST
Abstract
Description
Alumina-based composite oxide and method for producing alumina-based composite oxide
[0001] The present invention relates to an alumina-based composite oxide and a method for producing an alumina-based composite oxide.
[0002] As has been incorporated into recent exhaust gas regulation modes, the temperature of exhaust gas rises significantly when driving at high speeds and ultra-high speeds. As a result, the operating temperature of exhaust gas purification catalysts also rises significantly compared to conventional methods, making it difficult to prevent agglomeration of catalytic metal elements due to sintering.
[0003] Patent Document 1 discloses a composite metal oxide porous body useful as a catalyst support, which is a composite metal oxide porous body that is a mixture of first ultrafine particles containing alumina and second ultrafine particles containing zirconia, in which the first ultrafine particles and the second ultrafine particles are uniformly dispersed so as to satisfy the condition that, for all metal elements contained in the porous body at 0.1 mass % or more, the content (mass %) of the metal elements is measured at 100 measurement points in a microanalysis area of 20 nm square by energy dispersive X-ray spectroscopy using a scanning transmission electron microscope with a spherical aberration correction function, and the standard deviation of the content of each metal element obtained is 10 or less (see claim 1).
[0004] International Publication No. 2011 / 030875
[0005] Conventionally, in alumina-containing composite oxides for supporting catalytic metal elements, materials having a uniform element distribution have been used in order to suppress aggregation of the catalytic metal elements when exposed to high temperature regions for a long period of time, as exemplified in Patent Document 1.
[0006] However, the present inventors have found that if the element distribution in the alumina-containing composite oxide is extremely uniform, there is a possibility that the metal catalyst element will aggregate on elements of the alumina-containing composite oxide that are likely to become inactive when exposed to a high temperature range for a long period of time.
[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an alumina-containing composite oxide capable of further suppressing aggregation of catalytic metal elements when exposed to a high temperature range for a long period of time, and a method for producing the alumina-containing composite oxide capable of obtaining the alumina-containing composite oxide.
[0008] In order to solve the above-mentioned problems, the present inventors have conducted extensive research into alumina-containing composite oxides, and as a result have found that by appropriately controlling the element distribution of an alumina-containing composite oxide with high precision, it is possible to further suppress the aggregation of catalytic metal elements when exposed to a high temperature range for a long period of time, which has led to the completion of the present invention.
[0009] That is, the present invention provides the following: [1] An alumina-based composite oxide comprising alumina and ceria and / or zirconia, characterized in that, in point analysis of a total of 50 points using energy dispersive X-ray spectroscopy according to the following procedures a to c, all of the following (1) to (4) are satisfied: (1) at least one of the 50 measurement points has an alumina content of 50% by mass or more and 99% by mass or less, and an oxide content of elements other than alumina of 1% by mass or more and 50% by mass or less, (2) at least one of the 50 measurement points has an alumina content of 1% by mass or more and less than 50% by mass, and an oxide content of elements other than alumina of more than 50% by mass and 99% by mass or less, (3) the difference between the maximum and minimum alumina contents of the 50 measurement points is 20 to 95, and (4) the difference between the maximum and minimum contents of oxides of elements other than alumina of the 50 measurement points is 20 to 95. <Procedure> a: From particle images observed with a scanning electron microscope, select one particle image having a cross section of at least 4 μm in length and at least 4 μm in width. b: Perform composition analysis at 25 measurement points at 1 μm intervals within a range of 4 μm in length and 4 μm in width of the selected particle image. c: Select another particle image different from the one selected in procedure a, and perform the same composition analysis as in procedure b.
[0010] According to the above configuration, within particles having a cross section of at least 4 μm in length and at least 4 μm in width, the element distribution varies to satisfy the above conditions (1) to (4). That is, within the tertiary particles constituting the alumina-based composite oxide, there is a certain degree of variation in the element distribution. Therefore, when a metal catalyst element is supported on the alumina-based composite oxide, the metal catalyst element is preferentially supported on elements with high affinity. When the affinity with the support is high, aggregation of the metal catalyst elements is suppressed due to the anchoring effect, etc., even when exposed to high temperatures for a long period of time, and the metal catalyst maintains a more active state. Furthermore, elements with high affinity with the metal catalyst element often function as promoters. Therefore, preferential support of the metal catalyst element near the promoter is expected to improve catalytic activity. Additionally, because alumina and the additive metal element are present within the same tertiary particle, the alumina and the additive metal element act as diffusion barriers to each other when exposed to high temperatures for a long period of time, thereby suppressing catalyst degradation.
[0011] The present invention further provides the following: [2] The alumina-based composite oxide according to [1] above, which further satisfies all of the following (5) to (6) in the point analysis of the 50 points: (5) at least one measurement point out of the 50 points has an alumina content of 55% by mass or more and 99% by mass or less and an oxide content of elements other than alumina of 1% by mass or more and 45% by mass or less, and (6) at least one measurement point out of the 50 points has an alumina content of 1% by mass or more and 45% by mass or less and an oxide content of elements other than alumina of 55% by mass or more and 99% by mass or less.
[0012] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (4) but also the above (5) to (6), aggregation of the metal catalyst element is further suppressed.
[0013] The present invention further provides the following: [3] The alumina-based composite oxide according to [1] above, which further satisfies all of the following (7) to (8) in the point analysis of the 50 points: (7) there are 10 or more measurement points out of the 50 points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, and (8) there are 10 or more measurement points out of the 50 points where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and 99% by mass or less.
[0014] According to the invention [3], aggregation of the metal catalyst elements is further suppressed.
[0015] The present invention further provides the following: [4] The alumina-based composite oxide according to [2] above, which further satisfies all of the following (9) to (10) in the point analysis of the 50 points: (9) At least five of the 50 measurement points have an alumina content of 55% by mass or more and 99% by mass or less and an oxide content of elements other than alumina of 1% by mass or more and 45% by mass or less, and (10) At least five of the 50 measurement points have an alumina content of 1% by mass or more and 45% by mass or less and an oxide content of elements other than alumina of 55% by mass or more and 99% by mass or less.
[0016] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (4) but also the above (9) to (10), aggregation of the metal catalyst element is further suppressed.
[0017] The present invention further provides the following: [5] The alumina-based composite oxide according to any one of [1] to [4], wherein the alumina content is 15% by mass or more and 80% by mass or less in a composition analysis obtained by a fluorescent X-ray method.
[0018] When the alumina content is 15 mass % or more and 80 mass % or less in a composition analysis obtained by a fluorescent X-ray method, aggregation of a metal catalyst element is further suppressed when the metal catalyst element is supported on the alumina-based composite oxide.
[0019] In composition analysis using X-ray fluorescence spectroscopy, the content of each oxide contained in the entire alumina-based composite oxide is obtained, whereas in point analysis using energy dispersive X-ray spectroscopy ([1] and [2] above), the content of each oxide at a measurement point on the surface to be analyzed is obtained, rather than the content of the entire alumina-based composite oxide.
[0020] The present invention further provides the following: [6] The alumina-based composite oxide according to any one of [1] to [5], wherein the content of ceria and / or zirconia is 0.1 mass % or more and 85 mass % or less in a composition analysis obtained by a fluorescent X-ray spectrometry.
[0021] Since ceria and / or zirconia function as promoters, a ceria and / or zirconia content of 0.1% by mass or more is suitable for the catalyst support, and a ceria and / or zirconia content of 85% by mass or less can suppress thermal degradation.
[0022] The present invention further provides the following: [7] The alumina-based composite oxide according to any one of [1] to [6] above, which contains at least one oxide of a rare earth element (excluding cerium and promethium) as an oxide other than alumina, ceria, and zirconia.
[0023] When the catalyst contains one or more oxides of rare earth elements (excluding cerium and promethium), the crystalline phases of alumina, ceria, and zirconia are stabilized, and deterioration of the catalyst is further suppressed.
[0024] The present invention further provides the following: [8] A method for producing an alumina-based composite oxide according to any one of [1] to [7] above, comprising: Step 1 of adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; Step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3 of mixing the suspension A with the aqueous solution B-1 and / or suspension B-2 to obtain a precipitate of an aluminum-based composite precursor; and Step 4 of heat-treating the precipitate to obtain an alumina-based composite oxide.
[0025] While typical coprecipitation methods are effective for producing composite oxides with uniform elemental distribution, it is difficult to control the elemental distribution through anything other than the solubility product difference of the precipitates. On the other hand, in mixing methods that mix crystallized alumina with crystallized ceria and zirconia, the constituent elements of the individual tertiary particles remain the same as before mixing, resulting in an elemental distribution that makes it difficult to realize the properties of the composite of alumina, ceria, and zirconia. To address the above-mentioned problems, the invention of [8] above mixes hydrated alumina suspension A with aqueous solution B-1 and / or suspension B-2 of raw salts containing cerium and / or zirconium, thereby disposing ceria and zirconia precursors on the surface and / or interior of the hydrated alumina. This allows alumina secondary particles containing ceria and zirconia and secondary particles containing alumina to coexist within the tertiary particles of the alumina-based composite oxide. Additionally, controlling the aggregation of hydrated alumina and ceria and zirconia precursors allows the elemental distribution within the composite oxide tertiary particles to be controlled. By using such a production method, it is possible to obtain an alumina-based composite oxide having the above properties (1) to (4) of [1] above.
[0026] The present invention provides an alumina-containing composite oxide that can further suppress aggregation of catalytic metal elements when exposed to high temperatures for a long period of time, and a method for producing the alumina-containing composite oxide that can obtain the alumina-containing composite oxide.
[0027] 1 is a model diagram of tertiary particles of the alumina-based composite oxides of Examples 1 to 34. 2 is a model diagram of tertiary particles of the alumina-based composite oxides of Comparative Examples 1, 3 to 5, 7, 9, 12, and 13. 3 is a model diagram of tertiary particles of the alumina-based composite oxides of Comparative Examples 2, 6, 8, 10, and 14. 4 is a model diagram of tertiary particles of the alumina-based composite oxide of Comparative Example 11. 5 is an X-ray diffraction spectrum of the alumina-based composite oxide of Example 1.
[0028] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, the alumina-based composite oxide is a general one that contains 10 mass % or less of impurity metal compounds, including hafnium. In addition, in this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "substantially consist," and "consist only of."
[0029] The maximum and minimum values of the content of each component shown below are independently the preferred minimum and maximum values of the present invention, regardless of the content of other components.Furthermore, the maximum and minimum values of various parameters (measured values, etc.) shown below are independently the preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0030] [Alumina-Based Composite Oxide] The alumina-based composite oxide according to this embodiment contains alumina and ceria and / or zirconia, and is characterized in that, in point analysis of a total of 50 points using energy dispersive X-ray spectroscopy according to the following procedures a to c, all of the following (1) to (4) are satisfied: (1) at least one of the 50 measurement points has an alumina content of 50% by mass or more and 99% by mass or less, and an oxide content of elements other than alumina of 1% by mass or more and 50% by mass or less, (2) at least one of the 50 measurement points has an alumina content of 1% by mass or more and less than 50% by mass, and an oxide content of elements other than alumina of more than 50% by mass and 99% by mass or less, (3) the difference between the maximum and minimum alumina contents of the 50 measurement points is 20 to 95, and (4) the difference between the maximum and minimum contents of oxides of elements other than alumina of the 50 measurement points is 20 to 95. <Procedure> a: From particle images observed with a scanning electron microscope, select one particle image having a cross section of at least 4 μm in length and at least 4 μm in width. b: Perform composition analysis at 25 measurement points at 1 μm intervals within a range of 4 μm in length and 4 μm in width of the selected particle image. c: Select another particle image different from the one selected in procedure a, and perform the same composition analysis as in procedure b.
[0031] According to the alumina-based composite oxide, within particles having a cross section of 4 μm or more in length and 4 μm or more in width, the element distribution varies to satisfy the above conditions (1) to (4). That is, within the tertiary particles constituting the alumina-based composite oxide, there is a certain degree of variation in the element distribution. Therefore, when a metal catalyst element is supported on the alumina-based composite oxide, the metal catalyst element is preferentially supported on elements with high affinity. When the affinity with the support is high, aggregation of the metal catalyst elements is suppressed due to the anchoring effect, etc., even when exposed to high temperatures for a long period of time, and the metal catalyst maintains a more active state. Furthermore, elements with high affinity with the metal catalyst element often function as promoters. Therefore, preferential support of the metal catalyst element near the promoter is expected to improve catalytic activity. Additionally, because alumina and the added metal element are present within the same tertiary particle, they each act as a diffusion barrier when exposed to high temperatures for a long period of time, thereby suppressing catalyst degradation.
[0032] In this specification, tertiary particles refer to particles formed by agglomeration of secondary particles, and secondary particles refer to particles formed by agglomeration of crystallites (primary particles).
[0033] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (1), more preferably four or more, even more preferably seven or more, and particularly preferably ten or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (1), more preferably 46 or less, even more preferably 43 or less, and particularly preferably 40 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more and 48 or less measurement points that satisfy the above condition (1), more preferably four or more and 46 or less, even more preferably seven or more and 43 or less, and particularly preferably 10 or more and 40 or less measurement points.
[0034] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (2), more preferably four or more, even more preferably seven or more, and particularly preferably ten or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (2), more preferably 46 or less, even more preferably 43 or less, and particularly preferably 40 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more and 48 or less measurement points that satisfy the above condition (2), more preferably four or more and 46 or less, even more preferably seven or more and 43 or less, and particularly preferably 10 or more and 40 or less. The total of the measurement points that satisfy the above condition (1) and the measurement points that satisfy the above condition (2) is preferably 50. That is, it is preferable that all of the 50 measurement points satisfy either the above condition (1) or the above condition (2).
[0035] In particular, it is preferable that the alumina-based composite oxide further satisfies all of the following (7) to (8): (7) there are 10 or more measurement points out of 50 where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, and (8) there are 10 or more measurement points out of 50 where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and 99% by mass or less.
[0036] The difference between the maximum and minimum values of the alumina content at the 50 measurement points specified in (3) above is preferably 21 or more, more preferably 23 or more, and even more preferably 25 or more, from the viewpoint of suppressing aggregation of the metal catalyst element. The difference between the maximum and minimum values of the alumina content at the 50 measurement points specified in (3) above is preferably 94 or less, more preferably 92 or less, and even more preferably 90 or less, from the viewpoint of suppressing deterioration of the catalyst support (or suppressing aggregation of the metal catalyst element). The difference between the maximum and minimum values of the alumina content at the 50 measurement points specified in (3) above is preferably 21 or more and 94 or less, more preferably 23 or more and 92 or less, and even more preferably 25 or more and 90 or less, from the viewpoint of suppressing aggregation of the metal catalyst element.
[0037] The difference between the maximum and minimum values of the content ratio of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 21 or more, more preferably 23 or more, and even more preferably 25 or more, from the viewpoint of suppressing aggregation of the metal catalyst element. The difference between the maximum and minimum values of the content ratio of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 94 or less, more preferably 92 or less, and even more preferably 90 or less, from the viewpoint of suppressing deterioration of the catalyst support (or suppressing aggregation of the metal catalyst element). The difference between the maximum and minimum values of the content ratio of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 21 or more and 94 or less, more preferably 23 or more and 92 or less, and even more preferably 25 or more and 90 or less, from the viewpoint of suppressing aggregation of the metal catalyst element.
[0038] The alumina-based composite oxide preferably further satisfies all of the following (5) and (6): (5) there is at least one measurement point out of 50 where the alumina content is 55% by mass or more and 99% by mass or less and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, and (6) there is at least one measurement point out of 50 where the alumina content is 1% by mass or more and 45% by mass or less and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
[0039] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (4) but also the above (5) to (6), aggregation of the metal catalyst element is further suppressed.
[0040] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (5), more preferably three or more, and even more preferably five or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (5), more preferably 47 or less, and even more preferably 45 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more and 48 or less measurement points, more preferably three or more and 47 or less, and even more preferably five or more and 45 or less measurement points.
[0041] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (6), more preferably three or more, and even more preferably five or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (6), more preferably 47 or less, and even more preferably 45 or less measurement points. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more and 48 or less measurement points, more preferably three or more and 47 or less, and even more preferably five or more and 45 or less measurement points.
[0042] In particular, it is preferable that the alumina-based composite oxide further satisfies all of the following (9) to (10): (9) there are five or more measurement points out of 50 where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, and (10) there are five or more measurement points out of 50 where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
[0043] The alumina-based composite oxide preferably further satisfies all of the following (a) and (b): (a) there is at least one measurement point out of 50 where the alumina content is 60% by mass or more and 99% by mass or less and the content of oxides of elements other than alumina is 1% by mass or more and 40% by mass or less, and (b) there is at least one measurement point out of 50 where the alumina content is 1% by mass or more and 40% by mass or less and the content of oxides of elements other than alumina is 60% by mass or more and 99% by mass or less.
[0044] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (6) but also the above (a) to (b), aggregation of the metal catalyst element is further suppressed.
[0045] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (a), more preferably three or more, and even more preferably four or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (a), more preferably 47 or less, and even more preferably 46 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 2 to 48 measurement points that satisfy the above condition (a), more preferably three to 47, and even more preferably four to 46.
[0046] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be two or more measurement points that satisfy the above condition (b), more preferably three or more, and even more preferably four or more. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 48 or less measurement points that satisfy the above condition (b), more preferably 47 or less, and even more preferably 46 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there be 2 to 48 measurement points that satisfy the above condition (b), more preferably three to 47, and even more preferably four to 46.
[0047] The above (1) to (10) and (a) to (b) can be controlled by the production method. Specifically, they can be controlled by the following production method described below. The method for producing an alumina-based composite oxide includes: Step 1: adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; Step 2: preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3: mixing the suspension A with the aqueous solution B-1 and / or suspension B-2 to obtain a precipitate of an aluminum-based composite precursor; and Step 4: heat-treating the precipitate to obtain an alumina-based composite oxide.
[0048] <Particle diameter D 50 > Particle diameter D of the alumina-based composite oxide 50The particle diameter D is preferably 3.0 μm or more and 200 μm or less. 50 When the particle diameter D is 200 μm or less, no coarse particles remain when the powder is pulverized to a desired particle diameter. 50 When the diameter is 3.0 μm or more, it is possible to provide a variation in element distribution within the same tertiary particle.
[0049] The particle diameter D 50 The particle diameter D is more preferably 3.5 μm or more, and further preferably 4.0 μm or more. 50 The particle diameter D is more preferably 150 μm or less, and further preferably 120 μm or less. 50 refers to the value obtained by the method described in the Examples.
[0050] <Particle diameter D 90 > Particle diameter D of the alumina-based composite oxide 90 The particle diameter D is preferably 4.0 μm or more and 300 μm or less. 90 When the particle diameter D is 300 μm or less, no coarse particles remain when the powder is pulverized to a desired particle diameter. 90 When the diameter is 4.0 μm or more, it is possible to provide a variation in element distribution within the same tertiary particle.
[0051] The particle diameter D 90 The particle diameter D is more preferably 6.0 μm or more, and further preferably 8.0 μm or more. 90 The particle diameter D is more preferably 250 μm or less, and further preferably 220 μm or less. 90 refers to the value obtained by the method described in the Examples.
[0052] The particle diameter D 50 When measuring, not only tertiary particles but also non-aggregated secondary particles may be included, but the amount of non-aggregated secondary particles that may be contained in the alumina-based composite oxide is extremely small. 50 is the particle diameter D of the tertiary particles 50 It can be considered to represent the following.
[0053] The alumina-based composite oxide preferably has a pore volume of 0.10 mL / g or more and 1.0 mL / g or less across the entire range of pore diameter distribution (pore diameter of 3 nm or more and less than 200 nm) as determined by nitrogen adsorption / desorption. When the pore volume is 0.10 mL / g or more, the metal catalyst element is supported within the pores, making segregation of the unsupported metal catalyst element less likely to occur. When the pore volume is 1.0 mL / g or less, the secondary particles present within the same tertiary particle become densely aggregated, allowing the formation of tertiary particles with a variation in element distribution. The pore volume is more preferably 0.15 mL / g or more, even more preferably 0.20 mL / g or more. The pore volume is more preferably 0.90 mL / g or less, even more preferably 0.80 mL / g or less. The pore volume is more preferably 0.15 mL / g or more and 0.90 mL / g or less, even more preferably 0.20 mL / g or more and 0.80 mL / g or less. The pore volume is more preferably 0.15 mL / g or more and 0.90 mL / g or less, even more preferably 0.20 mL / g or more and 0.80 mL / g or less.
[0054] [Rh particle size after Rh loading and heat treatment] When the alumina content of the alumina-based composite oxide is 50% by mass or more and 80% by mass or less, the Rh particle size after loading Rh under the loading conditions below and performing heat treatment under the heat treatment conditions below is preferably 90 μm or less. When the alumina content of the alumina-based composite oxide is 30% by mass or more and less than 50% by mass, the Rh particle size after loading Rh under the loading conditions below and performing heat treatment under the heat treatment conditions below is preferably 95 μm or less. When the alumina content of the alumina-based composite oxide is 15% by mass or more and less than 30% by mass, the Rh particle size after loading Rh under the loading conditions below and performing heat treatment under the heat treatment conditions below is preferably 110 μm or less. When the Rh particle size after heat treatment is the above particle size or less, it can be said that aggregation of catalytic metal elements when exposed to a high temperature range for a long period of time is further suppressed. <Supporting conditions> Rh-supported powder is obtained by impregnating 2% by mass of 8% Rh nitrate solution, calculated as Rh, with respect to 100% by mass of alumina composite oxide, drying at 100° C., and then calcining for 5 hours at 500° C. <Heat treatment conditions> The obtained Rh-supported powder is heat-treated in air at 1200° C. for 12 hours to obtain a post-heat-treated sample.
[0055] When the alumina content is 50% by mass or more and 80% by mass or less, the Rh particle diameter is more preferably 85 μm or less, and even more preferably 80 μm or less. When the alumina content is 30% by mass or more and less than 50% by mass, the Rh particle diameter is more preferably 90 μm or less, and even more preferably 85 μm or less. When the alumina content is 15% by mass or more and less than 30% by mass, the Rh particle diameter is more preferably 105 μm or less, and even more preferably 100 μm or less. The smaller the Rh particle diameter, the better, but it is, for example, 20 μm or more, 30 μm or more, regardless of the alumina content.
[0056] The Rh particle diameter is a value obtained by the method described in the examples.
[0057] The alumina-based composite oxide contains alumina, and since the alumina-based composite oxide contains alumina, it can be suitably used as a catalyst support.
[0058] The alumina content is preferably 15% by mass or more and 80% by mass or less in composition analysis obtained by fluorescent X-ray spectroscopy. When the alumina content is 15% by mass or more and 80% by mass or less, thermal deterioration of the catalyst is suppressed, and therefore aggregation of the metal catalyst element when the metal catalyst element is supported on the alumina-based composite oxide is further suppressed.
[0059] The alumina content is more preferably 20% by mass or more, and even more preferably 25% by mass or more, and more preferably 75% by mass or less, and even more preferably 70% by mass or less.
[0060] The alumina-based composite oxide contains ceria and / or zirconia, and since the alumina-based composite oxide contains ceria and / or zirconia, it can be suitably used as a catalyst support.
[0061] The content of the ceria and / or zirconia is preferably 0.1% by mass or more and 85% by mass or less in composition analysis obtained by X-ray fluorescence spectroscopy. Since ceria and / or zirconia function as a promoter, a ceria and / or zirconia content of 0.1% by mass or more is suitable as a catalyst support. Furthermore, a ceria and / or zirconia content of 85% by mass or less can suppress thermal degradation.
[0062] When the alumina-based composite oxide contains ceria, the ceria content is preferably 1% by mass or more and 80% by mass or less, as determined by composition analysis using an X-ray fluorescence method. The ceria content is more preferably 3% by mass or more, and even more preferably 6% by mass or more. The ceria content is more preferably 75% by mass or less, and even more preferably 70% by mass or less.
[0063] When the alumina-based composite oxide contains zirconia, the zirconia content is preferably 1% by mass or more and 75% by mass or less, more preferably 5% by mass or more, and even more preferably 10% by mass or more, as determined by composition analysis using an X-ray fluorescence method. The zirconia content is more preferably 70% by mass or less, and even more preferably 65% by mass or less.
[0064] When the alumina-based composite oxide contains both ceria and zirconia, the total content of alumina, ceria, and zirconia is preferably 70% by mass or more and 98% by mass or less, when the total amount of the alumina-based composite oxide is taken as 100% by mass, as determined by composition analysis using an X-ray fluorescence method. By setting the total content of alumina, ceria, and zirconia to 70% by mass or more and 98% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0065] When both ceria and zirconia are contained, the total content of alumina, ceria, and zirconia is more preferably 75% by mass or more, and even more preferably 80% by mass or more, when the entire alumina-based composite oxide is taken as 100% by mass, as determined by composition analysis using an X-ray fluorescence method.When both ceria and zirconia are contained, the total content of alumina, ceria, and zirconia is more preferably 97% by mass or less, and even more preferably 96% by mass or less, when the entire alumina-based composite oxide is taken as 100% by mass.
[0066] When the alumina-based composite oxide contains ceria but not zirconia, the total content of alumina and ceria is preferably 70% by mass or more and 96% by mass or less, when the total amount of the alumina-based composite oxide is taken as 100% by mass, as determined by composition analysis using an X-ray fluorescence method. By setting the total content of alumina and ceria to 70% by mass or more and 96% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0067] When ceria is contained but zirconia is not contained, the total content of alumina and ceria is more preferably 75% by mass or more, and even more preferably 80% by mass or more, when the total alumina-based composite oxide is taken as 100% by mass. When ceria is contained but zirconia is not contained, the total content of alumina and ceria is more preferably 95% by mass or less, and even more preferably 94% by mass or less, when the total alumina-based composite oxide is taken as 100% by mass.
[0068] When the alumina-based composite oxide contains zirconia but not ceria, the total content of alumina and zirconia is preferably 70% by mass or more and 96% by mass or less, when the total amount of the alumina-based composite oxide is taken as 100% by mass, as determined by composition analysis using an X-ray fluorescence method. By setting the total content of alumina and zirconia to 70% by mass or more and 96% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0069] When zirconia is contained but ceria is not contained, the total content of alumina and zirconia is more preferably 75% by mass or more, and even more preferably 80% by mass or more, when the total amount of the alumina-based composite oxide is taken as 100% by mass. When zirconia is contained but ceria is not contained, the total content of alumina and zirconia is more preferably 95% by mass or less, and even more preferably 94% by mass or less, when the total amount of the alumina-based composite oxide is taken as 100% by mass.
[0070] The alumina-based composite oxide preferably contains one or more oxides of rare earth elements (excluding cerium and promethium) as oxides other than alumina, ceria, and zirconia. When an oxide of a rare earth element other than cerium and promethium is contained, aggregation of the metal catalyst element is further suppressed.
[0071] The alumina-based composite oxide preferably contains, among oxides of rare earth elements other than cerium and promethium, oxides of La, Nd, Pr, and Y. When the alumina-based composite oxide contains oxides of La, Nd, Pr, and Y, aggregation of the metal catalyst elements is further suppressed.
[0072] When an oxide of a rare earth element other than cerium and promethium is contained, the content of the oxide of a rare earth element other than cerium and promethium is preferably 2% by mass or more and 20% by mass or less when the entire alumina-based composite oxide is taken as 100% by mass in a composition analysis obtained by a fluorescent X-ray method. When the content of the oxide of a rare earth element other than cerium and promethium is 2% by mass or more and 20% by mass or less, aggregation of the metal catalyst element is further suppressed.
[0073] The content of the oxides of rare earth elements other than cerium and promethium is more preferably 3% by mass or more, and even more preferably 4% by mass or more, when the total mass of the alumina-based composite oxide is taken as 100% by mass, in a composition analysis obtained by X-ray fluorescence spectroscopy. The content of the oxides of rare earth elements other than cerium and promethium is more preferably 18% by mass or less, and even more preferably 16% by mass or less, when the total mass of the alumina-based composite oxide is taken as 100% by mass, in a composition analysis obtained by X-ray fluorescence spectroscopy.
[0074] The alumina-based composite oxide may contain one or more oxides selected from (A) an oxide of at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) a transition metal oxide (excluding oxides of rare earth elements), and (C) an alkaline earth metal oxide. These components (A) to (C) are also referred to as "other oxides" below.
[0075] Examples of the transition metal oxide include one or more oxides selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Nb, Mo, Ta, and W. Examples of the alkaline earth metal oxide include one or more oxides selected from the group consisting of Mg, Ca, Sr, and Ba.
[0076] When the alumina-based composite oxide contains the other oxides, the content of the other oxides is preferably 0.1% by mass or more and 30% by mass or less, based on 100% by mass of the entire alumina-based composite oxide. The content of the other oxides is more preferably 0.3% by mass or more and even more preferably 0.5% by mass or more, based on 100% by mass of the entire alumina-based composite oxide. The content of the other oxides is more preferably 25% by mass or less and even more preferably 20% by mass or less, based on 100% by mass of the entire alumina-based composite oxide.
[0077] Preferable composition ratios of the alumina composite oxide include the following combinations that do not exceed 100% by mass in total (combinations that total 100% by mass). (1) Alumina: 40% to 80% Zirconia: 1% to 30% Ceria: 1% to 30% Oxides of rare earth elements (excluding cerium and promethium): 1% to 15% Other oxides: 0% to 10% (2) Alumina: 20% to 60% Zirconia: 20% to 70% Ceria: 1% to 40% Oxides of rare earth elements (excluding cerium and promethium): 1% to 15% Other oxides: 0% to 10% (3) Alumina: 20% to 60% Zirconia: 20% to 75% Ceria: 0% to 30% Oxides of rare earth elements (excluding cerium and promethium): 1% to 15% Other oxides: 0% to 10% (4) Alumina ; 20% or more and 60% or less Zirconia; 0% or more and 20% or less Ceria; 20% or more and 70% or less Oxides of rare earth elements (excluding cerium and promethium); 5% or more and 20% or less Other oxides; 0% or more and 20% or less (5) Alumina; 20% or more and 60% or less Zirconia; 10% or more and 60% or less Ceria; 0% or more and 40% or less Oxides of rare earth elements (excluding cerium and promethium); 1% or more and 15% or less Other oxides; 1% or more and 20% or less
[0078] The use of the alumina composite oxide is not particularly limited, but it is suitable for use as a catalyst carrier, and particularly suitable for use as a catalyst carrier for an exhaust gas purification catalyst (exhaust gas purification catalyst carrier).
[0079] The metal catalytic element supported on the alumina-based composite oxide is not particularly limited, but preferable examples include Rh, Pt, Pd, Au, Ru, Ag, Ni, Co, Mn, Cu, and Fe. The metal catalytic element supported on the alumina-based composite oxide may overlap with an element contained in the alumina-based composite oxide. For example, when the alumina-based composite oxide contains Fe, Fe may be used as the metal catalytic element supported on the alumina-based composite oxide.
[0080] [Method for producing alumina-based composite oxide] An example of a method for producing an alumina-based composite oxide will be described below, although the method for producing an alumina-based composite oxide of the present invention is not limited to the following example.
[0081] The method for producing an alumina-based composite oxide according to this embodiment includes: Step 1: adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; Step 2: preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3: mixing the suspension A with the aqueous solution B-1 and / or suspension B-2 to obtain a precipitate of an aluminum-based composite precursor; and Step 4: heat-treating the precipitate to obtain an alumina-based composite oxide.
[0082] Hereinafter, each step of the method for producing an alumina-based composite oxide according to this embodiment will be described.
[0083] (1) Step 1 In step 1, sodium aluminate (NaAl(OH) 4 ) to obtain hydrated alumina suspension A.
[0084] The sodium aluminate may be in the form of a liquid or powder, but when a gas is used as the acid, it is preferable to use a liquid.
[0085] When a liquid sodium aluminate is used, the concentration of the sodium aluminate is preferably 1% by mass or more and 20% by mass or less in terms of aluminum oxide.
[0086] The temperature of the sodium aluminate is preferably 20°C or higher and 90°C or lower. The temperature of the sodium aluminate is more preferably 25°C or higher, and even more preferably 30°C or higher. The temperature of the sodium aluminate is more preferably 85°C or lower, and even more preferably 80°C or lower. By setting the temperature of the sodium aluminate within the above numerical range, it becomes easier to obtain an alumina-based composite oxide having an element distribution that satisfies the above (1) to (8). Specifically, the higher the temperature of the sodium aluminate, the greater the variation in element distribution tends to be within the range that satisfies the above (1) to (6).
[0087] The acid to be added to the sodium aluminate may be in the form of a gas or a liquid (solution). Specific examples of the acid include carbon dioxide, hydrochloric acid, nitric acid, sulfuric acid, and carboxylic acid. Among these, carbon dioxide gas is preferred from the viewpoint of containing fewer impurities.
[0088] When carbon dioxide gas is blown into the sodium aluminate, the flow rate of the carbon dioxide gas is 1.7 × 10 -7 m 3 / s or more 1.7×10 -5 m 3 / s or less, and 5.0 × 10 -7 m 3 / s or more 5.0×10 -6 m 3 When carbon dioxide gas is blown into the sodium aluminate, the blowing time is preferably from 6 hours to 48 hours, more preferably from 12 hours to 36 hours. By blowing carbon dioxide gas into the sodium aluminate under the above conditions, a suitable suspension A can be obtained.
[0089] (2) Step 2 In step 2, an aqueous solution B-1 of raw salt containing cerium and / or zirconium and / or a suspension B-2 of raw salt containing cerium and / or zirconium are prepared. In step 2, only the aqueous solution B-1 of raw salt containing cerium and / or zirconium may be prepared, only the suspension B-2 of raw salt containing cerium and / or zirconium may be prepared, or both the aqueous solution B-1 of raw salt containing cerium and / or zirconium and the suspension B-2 of raw salt containing cerium and / or zirconium may be prepared.
[0090] The aqueous solution B-1 can be obtained by mixing various raw material salts as described below.
[0091] The suspension B-2 is obtained by heat-treating the aqueous solution B-1. The heat treatment temperature is preferably 140°C or higher and 250°C or lower, and more preferably 160°C or higher and 200°C or lower. The heat treatment time is preferably 1 hour or higher and 10 hours or lower, and preferably 2 hours or higher and 5 hours or lower. When the suspension B-2 is used, the variation in element distribution tends to be greater compared to the case of the aqueous solution B-1, within the ranges satisfying the above (1) to (6).
[0092] When both the aqueous solution B-1 and the suspension B-2 are used, both the aqueous solution B-1 and the suspension B-2 may be prepared and mixed together.
[0093] Examples of raw material salts containing cerium include at least one of cerium nitrate, cerium chloride, cerium acetate, etc. Among these, cerium nitrate, which is a nitrate salt, is preferred.
[0094] The zirconium-containing raw material salt may be any salt capable of supplying zirconium ions, and examples thereof include at least one of zirconium oxynitrate, zirconium oxychloride, zirconium nitrate, etc. Among these, nitrate-based zirconium oxynitrate is preferred.
[0095] The aqueous solution B-1 and the suspension B-2 may contain a raw material salt containing a rare earth element (excluding cerium and promethium).
[0096] Examples of rare earth elements (excluding cerium and promethium) include at least one of Sc, Y, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Lu. Of these, Y, La, Nd, and Pr are preferred.
[0097] In addition to the above, the aqueous solution B-1 and the suspension B-2 may also contain one or more elements selected from (A) at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) transition metal elements (excluding rare earth elements and noble metal elements), and (C) alkaline earth metal elements.
[0098] The raw materials for rare earth elements, transition metal elements (excluding rare earth elements and noble metal elements), alkaline earth metals, In, Si, Sn, Bi, and P are not particularly limited as long as they are water-soluble. Examples include nitrates, sulfates, acetates, chlorides, and bromides, but nitrates are preferred as raw material salts because they can suppress the remaining impurities. The purity of these raw materials is preferably 95% or higher, and more preferably 98% or higher.
[0099] The solvent for preparing the aqueous solution B-1 may be appropriately selected depending on the type of raw material salt, etc., but it is usually desirable to use water (pure water, ion-exchanged water, etc.; the same applies hereinafter).
[0100] The metal salt concentration in the aqueous solution B-1 is preferably 1% or more and 15% or less in terms of oxide. By making it 1% or more, the concentration can be made somewhat high, and the treatment time can be made suitable. Furthermore, by making it 15% or less, an increase in viscosity during neutralization can be suppressed, and the compounding can be carried out suitably.
[0101] (3) Step 3 In step 3, the suspension A is mixed with the aqueous solution B-1 and / or the suspension B-2 to obtain a precipitate of an aluminum-based composite precursor.
[0102] Specifically, in step 3, first, suspension A obtained in step 1 is mixed with aqueous solution B-1 and / or suspension B-2 obtained in step 2, and an alkali is added to obtain a precursor precipitate of an alumina-based composite oxide. Although there are no particular limitations on the mixing, from the viewpoint of productivity such as filterability in the next step, it is preferable to add aqueous solution B-1 and / or suspension B-2 prepared in step 2 to suspension A prepared in step 1.
[0103] The alkali is not limited, and examples thereof include ammonium hydroxide, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, etc. Among these, sodium hydroxide is preferred from the viewpoint of industrial cost.
[0104] The amount of alkali to be added is not particularly limited as long as it can produce a precursor precipitate of an alumina-based composite oxide as a salt precipitate. The alkali is usually added so that the pH of the solution becomes 8.0 or more and 11.0 or less, preferably 9.0 or more and 10.0 or less.
[0105] Next, the resulting precipitate of aluminum-based composite precursor is recovered by solid-liquid separation, which may be performed according to a known method such as filtration, centrifugation, or decantation.
[0106] After recovery, it is preferable to wash the obtained alumina composite hydroxide with water as necessary to remove any adhering impurities.
[0107] The obtained alumina composite hydroxide may be further dried as needed. The drying method may be any known method, such as natural drying or heat drying. If necessary, the dried product may be subjected to pulverization, classification, or the like.
[0108] (4) Step 4 In step 4, the precipitate (recovered material) is heat-treated to obtain an alumina-based composite oxide.
[0109] The heat treatment temperature is not particularly limited, but is usually in the range of 500° C. to 1200° C. and 2 hours to 10 hours. The heat treatment atmosphere is not particularly limited, but may be in air or an oxidizing atmosphere.
[0110] The alumina-based composite oxide obtained by the heat treatment can be pulverized as needed. The pulverization method is not particularly limited, but can be a general pulverizer such as a planetary mill, ball mill, hammer mill, or jet mill.
[0111] In the above-described method for producing an alumina-based composite oxide, precursors of ceria and zirconia can be disposed on the surface and / or inside of the hydrated alumina by mixing hydrated alumina suspension A with aqueous solution B-1 and / or suspension B-2 of raw salts containing cerium and / or zirconium. This allows alumina secondary particles containing ceria and zirconia and secondary particles of alumina containing ceria and zirconia to coexist within the tertiary particles of the alumina-based composite oxide. Additionally, controlling the aggregation of the hydrated alumina and the precursors of ceria and zirconia makes it possible to control the element distribution within the tertiary particles of the composite oxide. This production method makes it possible to obtain an alumina-based composite oxide having the above properties (1) to (8).
[0112] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Note that the alumina-based composite oxides obtained in the examples and comparative examples contain 1 to 3 mass % of hafnium as an unavoidable impurity relative to zirconium (calculated using the following formula (X)). <Formula (X)> ([mass of hafnium] / ([mass of zirconium]+[mass of hafnium])×100(%)
[0113] The maximum and minimum values of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the content of other components. Also, the maximum and minimum values of the measured values shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0114] [Preparation of Alumina-Based Composite Oxide] (Example 1) Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 1.
[0115] Example 2 Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 2.
[0116] Example 3 Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the mixture at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). A composite metal salt suspension (Suspension B-2) was prepared by maintaining this aqueous solution B-1 in an autoclave at 180 ° C. for 2 hours. Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 3.
[0117] Example 4 Sodium aluminate (Asada Chemical Industry, #2019, 69 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / s for 24 hours while maintaining the temperature at 25°C. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 15 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 4.
[0118] Example 5 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 35°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 20 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% equivalent to the oxide, to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 5.
[0119] Example 6 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 20 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% equivalent to the oxide, to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 6.
[0120] Example 7 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 20 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% equivalent to the oxide, to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 7.
[0121] Example 8 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide, to prepare a nitrate aqueous solution (aqueous solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 8.
[0122] Example 9 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the suspension at a flow rate of 1 / s for 24 hours while maintaining the temperature at 50°C. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide, to prepare a nitrate aqueous solution (aqueous solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 9.
[0123] Example 10 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3 A hydrated alumina suspension (Suspension A) was prepared by maintaining the suspension at a flow rate of 1 / 2 s for 24 hours. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). A composite metal salt suspension (Suspension B-2) was prepared by maintaining this aqueous solution B-1 in an autoclave at 180°C for 2 hours. Suspension A and Suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 10.
[0124] Example 11 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / s for 24 hours while maintaining the temperature at 1 / s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 11.
[0125] Example 12 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3 A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / s for 24 hours while maintaining the temperature at 1 / s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain an alumina-based composite oxide according to Example 12.
[0126] Example 13 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3 A hydrated alumina suspension (Suspension A) was prepared by maintaining the suspension at a flow rate of 1 / 2 s for 24 hours. Diammonium cerium (IV) nitrate (Wako Pure Chemical Industries, special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). A composite metal salt suspension (Suspension B-2) was prepared by maintaining this aqueous solution B-1 in an autoclave at 180 °C for 2 hours. Suspension A and Suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 13.
[0127] Example 14 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 44 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 14.
[0128] Example 15 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by maintaining the flow rate at 1 / 200 rpm for 24 hours. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 44 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). A composite metal salt suspension (Suspension B-2) was prepared by maintaining this aqueous solution B-1 in an autoclave at 180 ° C. for 2 hours. Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 15.
[0129] Example 16 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3 A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1000 / s for 24 hours while maintaining the temperature at 1000 / s. Zirconium oxychloride octahydrate (Mitsuwa Chemical Co., Ltd., special grade reagent, 44 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were added to adjust the acid concentration to 0.67N and ZrO 2 The aqueous solution was heated in an autoclave reactor at a temperature of 120°C and a pressure of 2 x 10 5After adjusting the pH to 10 Pa, 650 g of a 5% aqueous sodium sulfate solution was added and held for another 15 minutes. The mixture was then allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. Next, cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to yttrium oxide) were added to the basic zirconium sulfate-containing slurry, and 25% aqueous sodium hydroxide solution was added until the pH reached 9 to prepare a composite metal salt suspension (Suspension B). Suspension A and Suspension B were mixed to obtain a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 16.
[0130] Example 17 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 60 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 17.
[0131] Example 18 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 60 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 18.
[0132] Example 19 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 19.
[0133] Example 20 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 20.
[0134] Example 21 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). A composite metal salt suspension (Suspension B-2) was prepared by maintaining this aqueous solution B-1 in an autoclave at 180 °C for 2 hours. Suspension A and Suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 21.
[0135] Example 22 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 70 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 22.
[0136] Example 23 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 70 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 23.
[0137] Example 24 Sodium aluminate (Asada Chemical Industry, #2019, 15 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 59 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 24.
[0138] Example 25 Sodium aluminate (Asada Chemical Industry, #2019, 15 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 70°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 59 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and Aqueous Solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Example 25.
[0139] Example 26 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide), and titanium (IV) tetrachloride (Wako Pure Chemical Industries, Ltd., 4.0 g in terms of titanium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide, to prepare a nitrate aqueous solution (Aqueous Solution B-1). Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 26.
[0140] Example 27 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide), and monoammonium phosphate (Wako Reagents, special reagent grade, 4.0 g in terms of phosphate) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 27.
[0141] Example 28 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide), and fumed silica AEROSIL (Nippon Aerosil Co., Ltd., 4.0 g in terms of silicon oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 28.
[0142] Example 29 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide), and ammonium metatungstate hydrate (Wako Reagents, Ltd., 4.0 g equivalent to tungsten oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 29.
[0143] Example 30 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide), and magnesium nitrate hexahydrate (Wako Reagents, special reagent grade, 4.0 g equivalent to magnesium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 30.
[0144] Example 31 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide), and calcium nitrate hexahydrate (Wako Reagents, special reagent grade, 4.0 g equivalent to calcium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 31.
[0145] Example 32 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide), and strontium nitrate hexahydrate (Wako Reagents, special reagent grade, 4.0 g equivalent to strontium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 32.
[0146] Example 33 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide), and barium nitrate hexahydrate (Wako Reagents, special reagent grade, 4.0 g in terms of barium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 33.
[0147] Example 34 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, and then heated to 50°C. Carbon dioxide gas was injected at 100 sccm (1.7 x 10) using a gas injection tube equipped with a filter plate. -6 m 3A hydrated alumina suspension (Suspension A) was prepared by blowing in the suspension at a flow rate of 1 / 2 s for 24 hours while maintaining the temperature at 1 / 2 s. A nitrate aqueous solution (Aqueous Solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 43 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide), and iron (III) nitrate nonahydrate (Wako Reagents, special reagent grade, 1.0 g in terms of iron oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. Suspension A and aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. The precursor precipitate was then recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours, thereby obtaining an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Example 34.
[0148] Comparative Example 1: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 78 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 8 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 8 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to prepare a nitrate aqueous solution at 3% oxide equivalent. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 1.
[0149] Comparative Example 2: A nitrate aqueous solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 8 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 8 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. This aqueous solution was then maintained in an autoclave at 180°C for 2 hours, and a 25% by weight aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in the atmosphere at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxides were mixed with alumina (AKP-G07, manufactured by Sumitomo Chemical Co., Ltd., 78 g in terms of aluminum oxide) and pulverized in a hammer mill to obtain the alumina composite oxide according to Comparative Example 2.
[0150] Comparative Example 3: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 69 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 15 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to prepare a nitrate aqueous solution at 3% oxide equivalent. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Comparative Example 3.
[0151] Comparative Example 4 Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 54 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 20 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to give an oxide equivalent of 3%, to prepare a nitrate aqueous solution. Next, 400 g of ammonium bicarbonate was dissolved in 7,600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The nitrate aqueous solution was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized using a hammer mill to obtain the alumina-based composite oxide of Comparative Example 4.
[0152] Comparative Example 5: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 42 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 3% in terms of oxide to prepare a nitrate aqueous solution. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain an alumina-based composite oxide according to Comparative Example 5.
[0153] Comparative Example 6: A nitrate aqueous solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 50 g equivalent to zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. This aqueous solution was maintained in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous solution of sodium hydroxide was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia-based composite oxide. The precipitate was then recovered and washed by solid-liquid separation. The solid was calcined in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia-based composite oxide. The ceria and zirconia composite oxide was mixed with alumina (Sumitomo Chemical, AKP-G07, 42 g in terms of aluminum oxide) and pulverized in a hammer mill to obtain an alumina composite oxide according to Comparative Example 6.
[0154] Comparative Example 7: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, special reagent grade, 42 g in terms of aluminum oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 3% in terms of oxide to prepare a nitrate aqueous solution. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain an alumina-based composite oxide according to Comparative Example 7.
[0155] Comparative Example 8: Diammonium cerium (IV) nitrate (Wako Pure Chemical Industries, special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) were dissolved in ion-exchanged water to a concentration of 5% in terms of oxide to prepare a nitrate aqueous solution. This aqueous solution was kept in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous solution of sodium hydroxide was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia-based composite oxide. The ceria and zirconia composite oxide was mixed with alumina (Sumitomo Chemical, AKP-G07, 42 g in terms of aluminum oxide) and pulverized in a hammer mill to obtain an alumina composite oxide according to Comparative Example 8.
[0156] Comparative Example 9: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 30 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 44 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to prepare a nitrate aqueous solution at 3% oxide equivalent. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in the air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Comparative Example 9.
[0157] Comparative Example 10 Zirconium oxychloride octahydrate (Mitsuwa Chemical Co., Ltd., special grade reagent, 44 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were added to adjust the acid concentration to 0.67N, ZrO 2 The aqueous solution was heated in an autoclave reactor at a temperature of 120°C and a pressure of 2 x 10 5After adjusting the pH to 10 Pa, 650 g of a 5% aqueous sodium sulfate solution was added and the mixture was maintained for another 15 minutes. The mixture was then allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. Next, cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g equivalent to yttrium oxide) were added to the basic zirconium sulfate-containing slurry, and a 25% aqueous sodium hydroxide solution was added until the pH reached 13 to obtain a precipitate. The precipitate was recovered and washed by solid-liquid separation. The solid was fired in an electric furnace at 900°C in air for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxide was mixed with alumina (Sumitomo Chemical, AKP-G07, 30 g in terms of aluminum oxide) and pulverized in a hammer mill to obtain an alumina composite oxide according to Comparative Example 10.
[0158] Comparative Example 11 Zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 44 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide) were dissolved in ion-exchanged water, and hydrogen peroxide solution was added in an amount 1.2 times the molar amount of cerium in the cerium nitrate and stirred to obtain a raw material solution. This aqueous solution was added with stirring to ammonia water in an amount 1.2 times the neutralization equivalent amount for the metal cations to obtain a precursor precipitate of a ceria-zirconia-based composite oxide. The precipitate was then centrifuged and thoroughly washed, then dried in air at 150°C for 7 hours and pre-calcined at 330°C for 5 hours to obtain a molded body. The molded body was pulverized in a grinder and calcined in air at 800°C for 5 hours to obtain a ceria-zirconia composite oxide. Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special grade reagent, 30 g in terms of aluminum oxide) was dissolved in ion-exchanged water. The ceria and zirconia composite oxide was suspended in the aluminum nitrate aqueous solution and stirred for 3 hours. The mixture was further heated with stirring to evaporate the water. The remaining solid was held in air at 110°C for 40 hours and then calcined at 800°C for 5 hours to obtain the alumina composite oxide of Comparative Example 11.
[0159] (Comparative Example 12) Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 60 g equivalent to zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g equivalent to cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to prepare a nitrate aqueous solution at 3% oxide equivalent. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide of Comparative Example 12.
[0160] Comparative Example 13: Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g equivalent to aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industry, special reagent grade, 70 g equivalent to zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) were dissolved in ion-exchanged water to a concentration of 3% equivalent to the oxide to prepare a nitrate aqueous solution. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% ammonium bicarbonate aqueous solution. The nitrate aqueous solution was then added to the ammonium bicarbonate aqueous solution to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in the atmosphere at 900° C. for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain an alumina-based composite oxide according to Comparative Example 13.
[0161] Comparative Example 14: A nitrate aqueous solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical Co., Ltd., special reagent grade, 70 g equivalent to zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to lanthanum oxide), neodymium(III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g equivalent to neodymium oxide), and yttrium(III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g equivalent to yttrium oxide) in ion-exchanged water to a concentration of 5% equivalent to the oxide. This aqueous solution was maintained in an autoclave at 180°C for 2 hours, and then a 25% by weight aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia-based composite oxide. The precipitate was then recovered and washed by solid-liquid separation. The solid was calcined in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia-based composite oxide. The ceria and zirconia-based composite oxide was mixed with alumina (Sumitomo Chemical, AKP-G07, 20 g in terms of aluminum oxide) and pulverized in a hammer mill to obtain an alumina-based composite oxide according to Comparative Example 14.
[0162] Comparative Example 15: In a stirred tank, 34.7 kg of deionized water and 8.31 wt % alumina (Al 2 O 3 10.95 kg of aluminum sulfate solution having a concentration of 26.9% by weight of La 2 O 3 Solution (A) was prepared by adding 1.43 kg of lanthanum nitrate solution having a concentration of 24.9 wt.% to 4.97 kg of 68 wt.% aqueous nitric acid solution. Solution (B) was prepared by adding 1.43 kg of lanthanum nitrate solution having a concentration of 24.9 wt.% to 4.97 kg of 68 wt.% aqueous nitric acid solution. 2 O 3 ) was a sodium aluminate solution having a pH of 5.0. 71 kg of deionized water was placed in a stirred reactor (250 rpm, four-blade spindle tilted at 45°). The reactor was then heated to a temperature of 65°C. This temperature was maintained throughout the reaction. 69% nitric acid solution was placed in the stirred reactor until a pH of 3 was reached. Solutions (A) and (B) were simultaneously introduced into the stirred reactor through inlet tubes near the stirring spindle. Solution (A) was introduced at a flow rate of 1.05 kg / min. Solution (B) was introduced at a flow rate capable of reaching a pH of 5 in 3 minutes. The flow rate of solution (A) remained constant at 1.05 kg / min, and the flow rate of solution (B) was adjusted to maintain the pH at 5.1 for 46 minutes. The introduction of solution (A) was stopped, and the addition of solution (B) continued until a pH of 10 was reached in 15 minutes. The reaction slurry was then poured onto a vacuum filter. At the end of the filtration, the cake was washed with deionized water at 60° C. After that, the cake was redispersed in deionized water to give a concentration of 8 wt.% of Al oxide (Al 2 O 3 -La 2 O 3 The suspension was spray dried to obtain a dried lanthanum-doped aluminum hydrate powder (Aluminum Hydrate 1).
[0163] In a vessel stirred with a 45° inclined four-blade spindle, 357 g of water, 114 g of zirconyl nitrate solution (21 g of zirconium oxide), 56 g of Ce IIIA precursor nitrate-based solution was prepared by adding nitrate solution (16.2 g in terms of cerium oxide), 4.4 g of lanthanum nitrate solution (1.2 g in terms of lanthanum oxide), and 16 g of yttrium nitrate solution (2.4 g in terms of yttrium oxide). 2.3 g of 69 wt. % nitric acid was then added to the resulting solution to obtain a precursor solution. While stirring, 64.5 wt. % alumina (18 g of Al 2 O 3 ) and 4.2 wt% La 2 O 3 28 g of aluminum hydrate 1 containing (1.17 g) was added. The precursor mixture was left stirring until a homogeneous dispersion was obtained. Next, 5.3 g of a 9.8 mol / L aqueous hydrogen peroxide solution was added. Stirring of the precursor mixture was continued. The precursor mixture was placed in a reactor containing 500 mL of a 2 mol / L ammonia solution and stirred (575 rpm) by a 45°-angled, four-blade spindle at ambient temperature for 60 minutes. At the end of the addition of the precursor mixture, the mixture was heated to a temperature of 95°C and maintained at this temperature for 30 minutes. The mixture was then cooled to a temperature below 40°C. 12 g of lauric acid was added to the cooled mixture while stirring at 650 rpm. Stirring was maintained for 30 minutes. The mixture was filtered under vacuum, and the cake was then washed with 720 g of an aqueous ammonia solution with a pH of 9. The resulting wet cake was then placed in a muffle furnace. The temperature of the furnace was increased at a rate of 4°C / min until it reached 950°C, and then this temperature was maintained for 4 hours. At the end of this firing in air, a mixed oxide was obtained. The recovered mixed oxide was then pulverized using a mortar. This was the alumina-based composite oxide according to Comparative Example 15.
[0164] Comparative Example 16: In a stirred tank, 34.7 kg of deionized water and 8.31 wt % alumina (Al 2 O 3 10.95 kg of aluminum sulfate solution having a concentration of 26.9% by weight of La 2 O 3Solution (A) was prepared by adding 1.43 kg of a lanthanum nitrate solution having a concentration of 1.0% by weight to 4.96 kg of a 68 wt. % aqueous nitric acid solution. Solution (B) was a sodium aluminate solution having an alumina concentration of 24.9 wt. %. 71 kg of deionized water was added to a stirred reactor (250 rpm, four-blade spindle tilted at 45°). The reactor was then heated to a temperature of 65°C. This temperature was maintained throughout the reaction. 69% nitric acid solution was added to the stirred reactor until a pH of 3 was reached. Solutions (A) and (B) were simultaneously added to the stirred reactor through inlet tubes near the stirring spindle. Solution (A) was added at a flow rate of 1.05 kg / min. Solution (B) was added at a flow rate capable of reaching a pH of 4.4 in 3 minutes. The flow rate of solution (A) remained constant at 1.05 kg / min, and the flow rate of solution (B) was adjusted to maintain the pH at a value of 4.4 for 46 minutes. The introduction of solution (A) was stopped, and the addition of solution (B) continued until a pH of 10 was reached in 15 minutes. The reaction slurry was then poured onto a vacuum filter. At the end of the filtration, the cake was washed with deionized water at 60°C. The cake was then redispersed in deionized water to obtain a solution of oxide (A) at a concentration of 8% by weight. l2 O 3 -La 2 O 3 The suspension was spray dried to obtain a dried lanthanum-doped aluminum hydrate powder (Aluminum Hydrate 2).
[0165] In a vessel stirred with a 45° inclined four-blade spindle, 357 g of water, 114 g of zirconyl nitrate solution (21 g of zirconium oxide), 56 g of Ce III A precursor nitrate-based solution was prepared by adding nitrate solution (16.2 g in terms of cerium oxide), 4.4 g of lanthanum nitrate solution (1.2 g in terms of lanthanum oxide), and 16 g of yttrium nitrate solution (2.4 g in terms of yttrium oxide). 2.3 g of 69 wt. % nitric acid was then added to the resulting solution to obtain the precursor solution. While stirring, 57.8 wt. % alumina (18 g of Al 2 O 3) and 3.8 wt% La 2 O 3 31.1 g of aluminum hydrate 2 containing (1.18 g) was added. The precursor mixture was left stirring until a homogeneous dispersion was obtained. Next, 5.3 g of a 9.8 mol / L aqueous hydrogen peroxide solution was added. Stirring of the precursor mixture was continued. 500 mL of a 2 mol / L ammonia solution was placed in a stirred reactor (600 rpm, four-blade spindle inclined at 45°). The precursor mixture was placed in the stirred reactor over a period of 60 minutes. This process was carried out at ambient temperature. At the end of the addition of the precursor mixture, the mixture was heated to a temperature of 95°C and maintained at this temperature for 30 minutes. The reaction medium was then cooled to a temperature below 40°C. 12 g of lauric acid was added to the cooled mixture while stirring at 500 rpm. Stirring was maintained for 30 minutes. The reaction medium was filtered under vacuum, and the cake was then washed with 1 L of aqueous ammonia (pH = 9). The resulting wet cake was then placed in a muffle furnace. The temperature of the furnace was increased at a rate of 4°C / min until it reached 950°C, and then this temperature was maintained for 4 hours. At the end of this firing in air, a mixed oxide was obtained. The recovered mixed oxide was then pulverized using a mortar. This was the alumina-based composite oxide of Comparative Example 16.
[0166] [Composition Measurement] The compositions (oxide equivalent) of the alumina composite oxides of the examples and comparative examples were analyzed using a wavelength dispersive X-ray fluorescence spectrometer ("ZSX Primus II" manufactured by Rigaku Corporation). The results are shown in Tables 1 to 6.
[0167] [Point Analysis Using Energy Dispersive X-ray Spectroscopy] Point analysis was performed on the alumina-based composite oxides of the Examples and Comparative Examples using energy dispersive X-ray spectroscopy. Specifically, first, the sample was embedded in resin and the surface was polished. Then, point analysis was performed at a total of 50 points using the following procedures a to c. <Procedure> a: From particle images observed with a scanning electron microscope (JEOL JSM-6700F), one particle image having a cross section of 4 μm or more in length and 4 μm or more in width was selected. b: Composition analysis was performed at 25 measurement points at 1 μm intervals within a range of 4 μm in length and 4 μm in width of the selected particle image. c: Another particle image different from the one selected in procedure a was selected, and the same composition analysis as in procedure b was performed.
[0168] The 50 measured points were classified as follows, and the scores for each point were tabulated. The results are shown in Tables 1 to 6. Note that some of the comparative examples had a core-shell structure. In these examples, the region extending from the edge of the particle toward the center of the particle by 1 μm or more in the particle image was regarded as the core portion (particle portion), and point analysis was performed. <Classification> - Number of measurement points where the alumina content is less than 1% by mass - Number of measurement points where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and 99% by mass or less - Number of measurement points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less - Number of measurement points where the alumina content is more than 99% by mass - Number of measurement points where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less - Number of measurement points where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less - Number of measurement points where the alumina content is 1% by mass or more and 40% by mass or less, and the content of oxides of elements other than alumina is 60% by mass or more and 99% by mass or less The number of measurement points where the alumina content is 60% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 40% by mass or less
[0169] The maximum and minimum values of the alumina content and the difference between the maximum and minimum values at the 50 measurement points are also shown in Tables 1 to 6. Furthermore, the maximum and minimum values of the content of oxides of elements other than alumina and the difference between the maximum and minimum values at the 50 measurement points are also shown in Tables 1 to 6.
[0170] [Measurement of pore volume] For the alumina-based composite oxides of the examples and comparative examples, a pore size distribution measuring device ("BELSOAP Mini II" manufactured by Microtrac-Bell) was used to obtain nitrogen adsorption / desorption isotherms, and then the pore size distribution was calculated from the desorption process using the BJH method. The measurement conditions were as follows. Then, the pore size was determined over the entire range of the pore diameter distribution (pore diameter of 3 nm or more and less than 200 nm). The results are shown in the table. <Measurement conditions> Measurement device: pore size distribution measuring device (BELSOAP Mini II manufactured by Microtrac-Bell) Measurement range: Pe / P0 = 0 to 1 Adsorption temperature: 77 K Number of measurement points: 10 points on the adsorption side, 25 points on the desorption side
[0171] [Measurement of Rh Particle Diameter (Catalyst Particle Diameter)] The alumina-based composite oxides of the Examples and Comparative Examples were impregnated with 2% by weight of 8% Rh nitric acid solution (manufactured by Tanaka Kikinzoku Kogyo Kogyo) in terms of Rh, dried at 100°C, and then calcined at 500°C for 5 hours to obtain Rh-supported powder. Subsequently, a heat treatment was performed in air at 1200°C for 12 hours to obtain a post-heat-treatment sample. 0.2 g of this sample was weighed into a cell, and the Rh particle diameter was measured by the CO pulse method using a BELCAT B manufactured by Microtrac-Bell. The results are shown in Tables 1 to 6. As can be seen from Tables 1 to 6, when the alumina-based composite oxides of the Examples were used, aggregation of Rh (catalytic metal element) was suppressed.
[0172] To facilitate understanding, model diagrams of the tertiary particles of the alumina-based composite oxides of the examples and the comparative examples are shown in Figures 1 to 4. As shown in Figure 1, the alumina-based composite oxides 1 of Examples 1 to 34 are in the form of tertiary particles and are composed of two types of secondary particles with different element distributions: secondary particles 2 with an alumina content of 50% by mass or more and 99% by mass or less (secondary particles 2 with an element oxide content other than alumina of 1% by mass or more and 50% by mass or less); and secondary particles 3 with an element oxide content other than alumina of more than 50% by mass and 99% by mass or less (secondary particles 3 with an alumina content of 1% by mass or more and less than 50% by mass). Therefore, aggregation of the catalytic metal elements is suppressed even when exposed to high temperatures for long periods of time.
[0173] 2 , the alumina-based composite oxides 4 of Comparative Examples 1, 3 to 5, 7, 9, 12, and 13 are in the form of tertiary particles, but are composed only of secondary particles 5 with little bias in element distribution. In other words, the alumina-based composite oxides 4 of Comparative Examples 1, 3 to 5, 7, 9, 12, and 13 have a small difference between the maximum and minimum alumina contents among the secondary particles. Therefore, when exposed to a high temperature range for a long period of time, the catalytic metal elements aggregate.
[0174] As shown in Figure 3, the alumina-based composite oxides 6 of Comparative Examples 2, 6, 8, 10, and 14 are in the form of tertiary particles, but are composed of secondary particles 7 and 8, which have significantly biased elemental distributions. The alumina-based composite oxides 4 of Comparative Examples 2, 6, 8, 10, and 14 have significantly large differences between the maximum and minimum alumina contents among the secondary particles. In other words, the alumina-based composite oxides 6 of Comparative Examples 2, 6, 8, 10, and 14 are tertiary particles that are mixtures of alumina particles and oxides of elements other than alumina, and have an elemental distribution that makes it difficult to exhibit the properties of a composite of alumina and oxides of elements other than alumina. Therefore, when exposed to high temperatures for a long period of time, the catalytic metal elements aggregate.
[0175] As shown in Fig. 4, the alumina-based composite oxide 9 of Comparative Example 11 is in the form of tertiary particles and is composed of secondary particles 10 that form the shell portion and secondary particles 11 that form the core portion. Secondary particles 10 and 11 are composed of secondary particles 7 and 8 that have a significantly large imbalance in element distribution. In other words, the alumina-based composite oxide 9 of Comparative Example 11 is a tertiary particle that is a mixture of alumina particles and an oxide of an element other than alumina, and has an element distribution that makes it difficult to exhibit the properties of a composite of alumina and an oxide of an element other than alumina. Therefore, when exposed to a high temperature range for a long period of time, the catalytic metal elements aggregate.
[0176] [Particle diameter D 50 , particle diameter D 90 Measurement of particle size distribution] 0.15 g of the alumina-based composite oxide of each of the Examples and Comparative Examples and 40 ml of a 0.2% aqueous solution of sodium hexametaphosphate were placed in a 50 ml beaker and dispersed for 2 minutes using an ultrasonic homogenizer "Sonifier S-450D" (Emerson Japan, Ltd.), and then the beaker was placed in an apparatus (laser diffraction particle size distribution analyzer ("LA-950" manufactured by Horiba, Ltd.)) and measured. The results are shown in Table 1.
[0177] [X-ray diffraction spectrum] An X-ray diffraction spectrum was obtained for the alumina-based composite oxide of Example 1 using an X-ray diffractometer (Ultima IV, manufactured by Rigaku). The measurement conditions were as follows. The results are shown in Figure 5. <Measurement conditions> Measurement device: X-ray diffractometer (Ultima IV, manufactured by Rigaku) Radiation source: CuKα radiation source Tube voltage: 50 kV Tube current: 30 mA Scanning rate: 2θ = 20 to 65°: 4° / min
[0178]
[0179]
[0180]
[0181]
[0182]
[0183]
Claims
1. An alumina-based composite oxide comprising alumina and ceria and / or zirconia, characterized in that in point analysis of a total of 50 points by the following procedures a to c using energy dispersive X-ray spectroscopy, all of the following (1) to (4) are satisfied: (1) there is at least one measurement point out of the 50 points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (2) there is at least one measurement point out of the 50 points where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and 99% by mass or less, (3) the difference between the maximum and minimum alumina content values of the 50 measurement points is 20 to 95, and (4) the difference between the maximum and minimum content values of oxides of elements other than alumina of the 50 measurement points is 20 to 95. <Procedure> a: Select one particle image having a cross section of 4 μm or more in length and 4 μm or more in width from particle images observed with a scanning electron microscope. b: Conduct composition analysis at 25 measurement points at 1 μm intervals within a range of 4 μm in length and 4 μm in width of the selected particle image. c: Select another particle image different from the one selected in procedure a, and conduct the same composition analysis as procedure b.
2. The alumina-based composite oxide according to claim 1, further characterized in that in the point analysis of the 50 points, all of the following (5) to (6) are satisfied: (5) there is at least one measurement point out of the 50 points where the alumina content is 55% by mass or more and 99% by mass or less and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, and (6) there is at least one measurement point out of the 50 points where the alumina content is 1% by mass or more and 45% by mass or less and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
3. The alumina-based composite oxide according to claim 1, further characterized in that in the point analysis of the 50 points, all of the following (7) to (8) are satisfied: (7) there are 10 or more measurement points out of the 50 points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, and (8) there are 10 or more measurement points out of the 50 points where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and 99% by mass or less.
4. The alumina-based composite oxide according to claim 2, further characterized in that in the point analysis of the 50 points, all of the following (9) to (10) are satisfied: (9) there are 5 or more measurement points out of the 50 points where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, and (10) there are 5 or more measurement points out of the 50 points where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
5. An alumina-based composite oxide according to any one of claims 1 to 4, characterized in that the alumina content is 15 mass % or more and 80 mass % or less in composition analysis obtained by fluorescent X-ray spectrometry.
6. An alumina-based composite oxide according to any one of claims 1 to 4, characterized in that the content of ceria and / or zirconia is 0.1 mass % or more and 85 mass % or less in composition analysis obtained by fluorescent X-ray spectrometry.
7. An alumina-based composite oxide according to any one of claims 1 to 4, characterized in that it contains at least one oxide of a rare earth element (excluding cerium and promethium) as an oxide other than alumina, ceria, and zirconia.
8. A method for producing an alumina-based composite oxide according to any one of claims 1 to 4, comprising: step 1 of adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; step 3 of mixing the suspension A with the aqueous solution B-1 and / or suspension B-2 to obtain a precipitate of an aluminum-based composite precursor; and step 4 of heat-treating the precipitate to obtain an alumina-based composite oxide.
Citation Information
Patent Citations
Composite metal oxide porous body, catalyst using same, and method for producing each
WO2011030875A1
Inorganic oxide, exhaust gas purification catalyst support and exhaust gas purification catalyst
JP2006036556A
Inorganic mixed oxide and exhaust gas purification catalyst using the same
JP2009107901A
Aging-resistant mixed oxides for automotive catalytic converters made from cerium, zirconium, aluminum, and lanthanum
JP2020514217A
Composition of aluminium oxide and cerium oxide with a particular porosity profile
WO2022248205A1