Method for producing α-sialon phosphor and method for producing light emitting device
The described method for manufacturing α-sialon phosphors with a high β-type silicon nitride content and subsequent reduction annealing in a hydrogen atmosphere addresses the inconsistent luminescent performance of LED packages by producing phosphors with improved light emitting characteristics, enhancing the luminescent performance and stability of LED packages.
Patent Information
- Application Number
- PCT/JP2024/011325
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
The luminescent performance of LED packages using α-type sialon phosphors does not improve as expected, even with phosphors having good luminescent properties, and conversely, phosphors with poor properties can sometimes exhibit better performance than expected, indicating a need for an effective manufacturing method to enhance light emission characteristics.
A method involving a mixture preparation step with silicon nitride, an aluminum source, and a europium source, followed by firing and reduction annealing in a hydrogen atmosphere, to produce α-sialon phosphors with more than 50% β-type silicon nitride, which are then combined with a curable resin material to form a wavelength conversion member for improved light emission in LED packages.
The method produces α-sialon phosphors with coarse particles and improved light emitting characteristics when used in LED packages, enhancing the overall luminescent performance and stability of the LED package.
Smart Images

Figure JP2024011325_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing α-sialon phosphor and method for manufacturing light-emitting device
[0001] The present invention relates to a method for producing an α-sialon phosphor and a method for producing a light-emitting device.
[0002] α-SiAlON phosphors have been actively studied as a material for forming a wavelength conversion member in an LED (Light Emitting Diode) package for converting blue light into light of a lower wavelength.
[0003] Patent Document 1 describes an α-sialon represented by a specific general formula. The oxygen content of this α-sialon is 1.2 mass% or less. The primary particles that make up this α-sialon are columnar. When this α-sialon is irradiated with ultraviolet light or visible light having a wavelength of 250 to 500 nm as an excitation source, it exhibits fluorescent properties with a peak in the wavelength range of 595 to 630 nm.
[0004] Patent Document 2 describes a phosphor that can provide a white LED having excellent luminous efficiency using a blue LED or an ultraviolet LED as a light source. This phosphor has the general formula: (M1) x (M2) y (Si, Al) 12 (O, N) 16 (wherein M1 is one or more elements selected from the group consisting of Li, Mg, Ca, Y and lanthanide elements (excluding La and Ce), and M2 is one or more elements selected from the group consisting of Ce, Pr, Eu, Tb, Yb and Er, and 0.3≦X+Y≦1.5 and 0<Y≦0.7) as the main component, and having a specific surface area of 0.2 to 0.5 m 2 / g of powder.
[0005] International Publication No. WO 2010 / 087348 International Publication No. WO 2007 / 129713
[0006] When constructing a wavelength conversion member in an LED package, an α-sialon phosphor is typically mixed with a curable resin material (encapsulant). Therefore, in addition to the performance of the α-sialon phosphor itself, it is preferable to obtain good light-emitting characteristics when the α-sialon phosphor is used together with a curable resin material to form a wavelength conversion member and then assembled into an LED package. Through preliminary studies, the present inventors have found that even if an α-sialon phosphor with good light-emitting characteristics (such as quantum yield) is used in powder evaluation, the light-emitting performance of the LED package may not be as improved as expected. Furthermore, based on this knowledge, even if an α-sialon phosphor with not very good light-emitting characteristics (such as quantum yield) is used in powder evaluation, the light-emitting performance of the LED package may be surprisingly good.
[0007] The present invention has been made in view of the above circumstances, and one of the objects of the present invention is to provide a method for producing an α-sialon phosphor that can be preferably used in the production of an LED package.
[0008] The present inventors have completed the invention provided below and solved the above problems.
[0009] 1. A method for producing an α-sialon phosphor, comprising: a mixture preparation step of preparing a mixture containing silicon nitride, an aluminum source, a calcium source, and a europium source; and a firing step of firing the mixture to obtain a fired product, wherein more than 50 mass% of the silicon nitride is β-type silicon nitride. 2. A method for producing an α-sialon phosphor according to 1., wherein the silicon nitride has an oxygen content of 0.5 mass% or less. 3. A method for producing an α-sialon phosphor according to 1. or 2., further comprising a reduction annealing step of heating the fired product in a reducing atmosphere to reduce it. 4. A method for producing an α-sialon phosphor according to 3., wherein the reduction annealing step is a step of heating the fired product in an atmosphere containing hydrogen gas. 5. 3. or 4. The method for producing an α-sialon phosphor according to claim 1, wherein the fired product contains lithium oxide (Li 2O) before carrying out the reduction annealing step. 6. A method for producing an α-sialon phosphor according to any one of 3. to 5., wherein the fired product is heated to 1300 to 1500°C in the reduction annealing step. 7. A method for producing an α-sialon phosphor according to any one of 1. to 6., wherein the mixture is fired at 1800°C or higher in the firing step. 8. A method for producing an α-sialon phosphor according to any one of 1. to 7., wherein the aluminum source contains aluminum nitride. 9. A method for producing an α-sialon phosphor according to any one of 1. to 8., wherein the calcium source contains calcium nitride. 10. A method for producing an α-sialon phosphor according to any one of 1. to 9. 11. A method for producing an α-sialon phosphor according to any one of items 1 to 10, wherein the europium source contains europium oxide. 12. A method for producing a light-emitting device, comprising combining a wavelength conversion member containing an α-sialon phosphor obtained by the method for producing an α-sialon phosphor according to any one of items 1 to 10, with a light-emitting element.
[0010] The α-sialon phosphor produced according to the present invention is used together with a curable resin material to form a wavelength conversion member, and an LED package produced using this wavelength conversion member exhibits good light-emitting properties.
[0011] 1 is a schematic cross-sectional view showing an example of the structure of a light-emitting device (specifically, an LED package).
[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar reference numerals, and descriptions thereof will be omitted where appropriate. To avoid complexity, when multiple identical components appear in the same drawing, only one of the components may be given a reference numeral, and not all of the components may be given a reference numeral. The drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to actual objects.
[0013] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."
[0014] <Method for manufacturing α-sialon phosphor> The method for manufacturing an α-sialon phosphor of this embodiment includes: a mixture preparation step of preparing a mixture containing silicon nitride, an aluminum source, a calcium source, and a europium source, and a firing step of firing the mixture to obtain a fired product. In the mixture preparation step, more than 50 mass %, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more, and particularly preferably 98 mass % or more of the silicon nitride (i.e., silicon nitride as a raw material) is β-type silicon nitride.
[0015] The silicon nitride to be used preferably has an oxygen content of 0.5% by mass or less. The oxygen content of the silicon nitride is more preferably 0.3% by mass or less, and even more preferably 0.2% by mass or less. The lower limit of this oxygen content is preferably zero (below the detection limit), but in reality it is 0.05% by mass or more.
[0016] Although the details are unclear, it is speculated that a manufacturing method using silicon nitride containing a large amount of β-type silicon nitride produces an α-SiAlON phosphor that is suitable for use in combination with other phosphors in terms of at least one of the following: the chemical composition of the phosphor, the morphology of the phosphor particles, and the surface condition of the phosphor particles. In particular, the inventors have found that the above-described manufacturing method tends to produce phosphor particles that are somewhat coarse and have a small aspect ratio. The fact that the particles are somewhat coarse and have a small aspect ratio may be related to improved light-emitting properties when packaged (when the phosphor particles are dispersed in an encapsulant). Incidentally, most conventional α-SiAlON phosphor particles are columnar and have a relatively large aspect ratio.
[0017] [Preparation of Silicon Nitride] Silicon nitride containing 50 mass% or more of β-type silicon nitride can be a commercially available product. Such silicon nitride may be a commercially available product. Alternatively, commercially available silicon nitride (the content of β-type silicon nitride is not limited) may be purchased and subjected to a heat treatment to increase the proportion of β-type silicon nitride.
[0018] As mentioned above, it is preferable to use silicon nitride with an oxygen content of 0.5 mass% or less. To use silicon nitride with such a low oxygen content, commercially available silicon nitride with a low oxygen content may be selected and used, or, as mentioned above, commercially available silicon nitride may be heated to increase the proportion of β-type silicon nitride while reducing the oxygen content. The heating conditions in this case may be, for example, in a nitrogen gas atmosphere at 1950 to 2050°C for 1 to 15 hours. Although the details are unknown, using silicon nitride with a low oxygen content makes it possible to obtain an α-sialon phosphor that is even more suitable for application to LED packages.
[0019] [Mixture Preparation Step] In the mixture preparation step, a mixture containing silicon nitride (more than 50 mass % of which is β-type silicon nitride), an aluminum source, a calcium source, and a europium source is prepared. Incidentally, the use of a calcium source means that the α-sialon phosphor obtained by the method for producing an α-sialon phosphor of this embodiment is a so-called calcium-α-sialon.
[0020] The aluminum source preferably contains aluminum nitride or aluminum oxide. The calcium source preferably contains calcium nitride, calcium oxide, or calcium carbonate. Examples of europium sources include oxides containing europium, hydroxides containing europium, nitrides containing europium, oxynitrides containing europium, and halides containing europium. These may be used alone or in combination of two or more. Among these, the europium source preferably contains europium oxide or europium nitride. Given that this embodiment is a method for producing an "α-sialon phosphor," the mixing ratio of each raw material may be appropriately determined based on the general formula of the α-sialon phosphor. The general formula is provided below for reference. Just to be clear, the composition of the α-sialon phosphor finally obtained is not limited to those corresponding to the general formula provided below.
[0021] The mixture preferably contains core particles of an α-sialon phosphor in addition to silicon nitride, an aluminum source, a calcium source, and a europium source. Core particles refer to pre-manufactured α-sialon phosphor particles. When core particles are used, their amount is, for example, 3 to 20 mass %, more preferably 5 to 15 mass %, of the total mixture. While the details are unclear, the use of core particles is thought to promote crystallization starting from the core particles in the subsequent firing process. This may make it easier to obtain larger particles or particles with a smaller aspect ratio. Perhaps as a result, it is possible to produce phosphor particles that exhibit particularly favorable light-emitting characteristics when used in an LED package.
[0022] The core particles can usually be obtained by undergoing steps similar to those of the phosphor powder manufacturing method of this embodiment. For example, they can be obtained by carrying out the following steps (1) and (2). However, when obtaining the core particles, it is not necessary to use silicon nitride powder rich in β-type silicon nitride as the raw material; silicon nitride powder rich in α-type silicon nitride may also be used. (1) Except for not using core particles, the [mixture preparation step], [firing step], and [pulverization step] described in this specification are carried out to obtain α-type SiAlON phosphor particles. (2) Using the α-type SiAlON phosphor particles obtained in step (1) above as temporary core particles, the [mixture preparation step], [firing step], and [pulverization step] described in this specification are carried out to obtain α-type SiAlON phosphor particles. These particles are used as core particles.
[0023] In order to increase the homogeneity of the core particles, the α-sialon phosphor particles obtained in (2) may be used as temporary core particles, and the step (2) may be further repeated one or several times to obtain core particles.
[0024] Methods for mixing the raw materials include dry mixing and wet mixing in an inert solvent that does not substantially react with the raw material components, followed by removal of the solvent. Mixing devices include V-type mixers, rocking mixers, ball mills, and vibration mills. When using raw materials that are unstable in the atmosphere, hydrolysis or oxidation of the raw materials can affect the properties of the synthesized product, so it is preferable to perform the process in a glove box with an inert atmosphere.
[0025] [Firing Step] In the firing step, the mixture obtained by mixing as described above is fired to obtain a fired product. The firing step is preferably carried out by placing the mixture in a container made of a material that is low in reactivity with the mixture and the phosphor to be synthesized, such as a boron nitride container. The firing step is preferably carried out in an inert gas atmosphere such as nitrogen gas. The pressure in the firing step is preferably set to approximately 0.5 to 1 MPa·G. In the firing step, the mixture obtained in the mixture preparation step is preferably fired at 1800°C or higher, more preferably 1800 to 2000°C, and even more preferably 1850 to 1950°C. The firing step time, specifically the time for heating the mixture at 1800°C or higher, is preferably 10 to 40 hours, more preferably 15 to 30 hours.
[0026] [Crushing Step] The method for producing an α-sialon phosphor according to this embodiment preferably includes a crushing step. In the crushing step, an appropriate external force is applied to the fired product (usually a mass) obtained in the firing step, to crush the fired product. Crushing can be preferably carried out using a jet mill. The crushing conditions can be, for example, 0.1 to 0.5 MPa.
[0027] [Reduction-annealing step] The method for producing an α-sialon phosphor of this embodiment preferably includes a reduction-annealing step, i.e., a step of annealing (heat treating) the fired product in a reducing atmosphere. In the reduction-annealing step, the fired product obtained in the firing step (preferably the fired product that has been subsequently pulverized) is heated in a reducing atmosphere.
[0028] The reductive annealing step is preferably a step of heating the fired product in an atmosphere containing hydrogen gas. More preferably, the reductive annealing step is a step of heating the fired product in an atmosphere containing 50 vol% or more of hydrogen gas. Even more preferably, the reductive annealing step is a step of heating the fired product in an atmosphere containing 80 vol% or more of hydrogen gas. Particularly preferably, the reductive annealing step is a step of heating the fired product in an atmosphere consisting essentially of hydrogen gas alone.
[0029] The reduction annealing step is preferably carried out by adding lithium oxide (Li 2Although the details are unclear, this method makes it possible to produce an α-sialon phosphor that is more suitable for application to LED packages. Although the details are unclear, one possibility is that lithium oxide (Li 2 It is speculated that lithium oxide (LiO) removes impurities that do not contribute to fluorescence. 2 O) is Eu 3+ EU 2+ It is possible that the performance of the α-sialon phosphor is improved by reducing it to
[0030] In the reduction annealing step, the fired product is preferably heated to 1300 to 1500°C, more preferably 1350 to 1450°C. The heating time (the time during which the fired product is heated to 1300 to 1500°C) is preferably 3 to 20 hours, more preferably 5 to 15 hours. The pressure is preferably 0.01 to 0.1 MPa·G, more preferably 0.01 to 0.05 MPa·G. The heating temperature, heating time, and pressure are determined appropriately from the viewpoint of sufficient reduction and saving energy costs.
[0031] [Acid Treatment Step] The method for producing an α-sialon phosphor according to this embodiment preferably includes an acid treatment step. Specifically, the phosphor after the reduction annealing step is preferably immersed in an acid aqueous solution and stirred appropriately. This may remove foreign matter on the phosphor surface or a different phase that does not contribute to fluorescence.
[0032] The acid aqueous solution may be an aqueous solution containing one or more acids selected from hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid, and is particularly preferably an aqueous solution containing a mixture of hydrofluoric acid and nitric acid.
[0033] The acid treatment can be carried out by stirring the phosphor in an aqueous acid solution for several minutes to several hours (for example, 10 minutes to 6 hours). A known stirrer or the like can be used for stirring. The temperature during stirring is, for example, 50 to 100°C, preferably 65 to 85°C (the liquid is maintained at this temperature). The stirring time is, for example, 1 minute to 2 hours, preferably about 10 minutes to 1 hour. The stirring speed is, for example, 300 to 600 rpm, preferably 400 to 500 rpm. After this treatment, it is desirable to perform filtration, washing with water, drying, etc. as appropriate.
[0034] [Elutriation Step] The method for producing an α-sialon phosphor according to this embodiment preferably includes an elutriation step. The elutriation step can remove ultrafine phosphor particles with poor luminous efficiency, thereby further improving the luminous properties of the final α-sialon phosphor. Specific methods for elutriation can be appropriately applied using known methods. The elutriation step preferably substantially removes fine phosphor particles with a particle size of 7 μm or less, and more preferably substantially removes fine phosphor particles with a particle size of 12 μm or less.
[0035] [Obtained Phosphor Particles: Composition, Particle Size Distribution, etc.] As described above, a particulate α-sialon phosphor (phosphor particles) can be obtained. The phosphor particles have, for example, a composition formula (Ca x , Eu y ) m/2 Si 12-(m+n) Al m+n O n N 16-n (m=2(x+y)), where m is preferably 3.0 to 4.0, x is preferably 1.2 to 1.7, y is preferably 0.04 to 0.10, and n is preferably 0 to 0.5.
[0036] It is preferable that the particle size distribution of the particulate α-sialon phosphor (phosphor particles) is appropriately adjusted, for example, by the degree of pulverization in the pulverization step and the specific conditions of the elutriation step.
[0037] The cumulative 50% diameter D50 (median diameter) of the obtained α-sialon phosphor is preferably 20 to 40 μm, more preferably 23 to 35 μm. The cumulative 90% diameter D90 of the obtained α-sialon phosphor is preferably 40 to 70 μm, more preferably 42 to 60 μm. The cumulative 10% diameter D10 of the obtained α-sialon phosphor is preferably 10 to 25 μm, more preferably 12 to 20 μm. In particular, from the viewpoint of reducing phosphors with extremely small particle sizes (fine powder) that tend to deteriorate luminous efficiency, it is preferable that D10 be within the above range.
[0038] Phosphor particles with too large a particle size tend to have poor fluorescent properties because excitation light cannot reach the interior of the particle. In this regard, the cumulative 97% diameter D97 of the resulting α-sialon phosphor is preferably 60 to 100 μm, more preferably 65 to 90 μm. Furthermore, the cumulative 100% diameter D100 of the resulting α-sialon phosphor is preferably 100 to 200 μm, more preferably 110 to 190 μm.
[0039] In relation to D10, the value of (D50-D10) / D50 is also a good indicator from the viewpoint that there is little phosphor with an extremely small particle size (fine powder). The value of (D50-D10) / D50 is preferably 0.40 to 0.50, and more preferably 0.43 to 0.49.
[0040] Furthermore, it is preferable that the particle size distribution of the resulting α-sialon phosphor powder is sharp. A sharp particle size distribution means that the phosphor particles in the phosphor powder are homogeneous, at least in terms of particle size. This is expected to lead to stable light emission and to reduced variation in light emission characteristics between product lots. The sharpness of the particle size distribution can be quantitatively measured using the index (D90-D10) / D50, which uses the above-mentioned D10, D50, and D90. The value of (D90-D10) / D50 is preferably 1.05 to 1.5, and more preferably 1.05 to 1.4.
[0041] <Method for manufacturing a light-emitting device> A light-emitting device (LED package) can be manufactured by combining a wavelength conversion member containing an α-sialon phosphor obtained by the above-mentioned manufacturing method with a light-emitting element. Here, the wavelength conversion member can be manufactured by a series of steps including, for example, a dispersion step in which the α-sialon phosphor is dispersed in a sealing material (resin material) to form a dispersion, and a curing step in which the dispersion is cured. Alternatively, the wavelength conversion member may be manufactured by mixing molten glass and an α-sialon phosphor to form a mixture and cooling the mixture.
[0042] The wavelength conversion member may or may not contain an α-sialon phosphor and a different phosphor (for example, red phosphors such as CASN and SCASN). If the desired light-emitting characteristics can be obtained using the α-sialon phosphor alone, there is no need to use a different phosphor.
[0043] The sealing material used to manufacture the wavelength conversion member is usually a thermosetting resin material, preferably a silicone-based thermosetting material. Silicone-based thermosetting materials are preferably used in terms of heat resistance and light transmittance after curing. When manufacturing the wavelength conversion member, the amount of phosphor / the amount of sealing material (resin material), i.e., the ratio of phosphor / sealant when manufacturing the wavelength conversion member, is adjusted by mass, preferably between 0.2 and 0.7, more preferably between 0.4 and 0.7. The same can be said for the amount of phosphor / the amount of glass when manufacturing a wavelength conversion member using molten glass.
[0044] 1 is a schematic cross-sectional view showing an example of the structure of a light emitting device. As shown in Fig. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite 40.
[0045] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. Mounting the light emitting element 120 on the heat sink 130 can improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.
[0046] The light-emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 to 500 nm, which corresponds to near-ultraviolet to blue light, can be used as the light-emitting element 120. One electrode (not shown) disposed on the upper surface of the light-emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light-emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.
[0047] A generally funnel-shaped recess whose diameter gradually increases from the bottom to the top is formed in the case 140. The light emitting element 120 is provided on the bottom of the recess. The wall of the recess surrounding the light emitting element 120 serves as a reflector.
[0048] The composite 40 is filled in the recess whose wall is formed by the case 140. The composite 40 is a wavelength conversion material that converts the excitation light emitted from the light emitting element 120 into light with a longer wavelength. The wavelength conversion material as described above is used as the composite 40. In FIG. 1 , the composite 40 is composed of phosphor particles 1 and a sealing material 30.
[0049] 1 illustrates a surface-mounted light-emitting device, but the light-emitting device is not limited to the surface-mounted type. The light-emitting device may be a bullet type, a COB (chip-on-board) type, a CSP (chip-scale package) type, or the like.
[0050] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.
[0051] The embodiments of the present invention will be described in detail based on examples and comparative examples. However, it should be noted that the present invention is not limited to the examples.
[0052] <Preparation of Raw Materials> The following raw materials were prepared.
[0053] Silicon nitride powder (main component: β-type): β-type silicon nitride powder purchased from H.C. STARK was heated at 2000°C for 3 hours at 0.85 MPa·G in a nitrogen atmosphere. β-type silicon nitride ratio: 99 mass%, oxygen content: 0.12 mass%. Silicon nitride powder (main component: α-type): E10 grade (α-type silicon nitride ratio: 98 mass%) manufactured by Ube Industries, Ltd. Aluminum nitride powder: E grade manufactured by Tokuyama Corporation Calcium nitride powder: High Purity Chemical Laboratory Co., Ltd. Europium oxide powder: Japan Yttrium Co., Ltd.
[0054] α-SiAlON core particles (for Examples): α-SiAlON particles produced as follows, D10 = 10.1 μm, D50 = 21.3 μm, D90 = 43.0 μm. (1) The [Mixture Preparation Step], [Firing Step], and [Crushing Step] in the <Production of α-SiAlON Phosphor> described below were carried out to obtain α-SiAlON particles (silicon nitride powder (main component: α-type) was used), except that α-SiAlON core particles were not used. (2) The [Mixture Preparation Step], [Firing Step], and [Crushing Step] in the <Production of α-SiAlON Phosphor> described below were carried out using the α-SiAlON particles obtained in (1) above as core particles to obtain α-SiAlON particles (silicon nitride powder (main component: β-type) was used). The α-SiAlON particles thus obtained were used as α-SiAlON core particles for Examples.
[0055] α-SiAlON core particles (for comparative examples): α-SiAlON particles produced as follows, D10 = 7.2 μm, D50 = 16.7 μm, D90 = 33.9 μm. (1) The [Mixture Preparation Step], [Firing Step], and [Crushing Step] in the <Production of α-SiAlON Phosphor> described below were carried out to obtain α-SiAlON particles (main component: α-type) except that α-SiAlON core particles were not used. (2) The [Mixture Preparation Step], [Firing Step], and [Crushing Step] in the <Production of α-SiAlON Phosphor> described below were carried out using the α-SiAlON particles obtained in (1) above as core particles to obtain α-SiAlON particles (main component: α-type)). The α-SiAlON particles thus obtained were used as α-SiAlON core particles for the comparative examples.
[0056] Lithium oxide (Li) used in the reduction annealing process 2 O): High Purity Chemical Laboratory Co., Ltd.
[0057] In the above, the α / β silicon nitride ratio in the silicon nitride powder was determined by obtaining an XRD diffraction pattern using an X-ray diffraction measuring device "D8" manufactured by Bruker, and then performing Rietveld analysis of the pattern using analysis software "TOPAS."
[0058] The amount of oxygen in the silicon nitride powder was measured using an EMGA-920 manufactured by HORIBA.
[0059] <Production of α-type Sialon phosphor> [Mixture preparation step] 138.22 g of the silicon nitride powder (main component: β-type in the examples, main component: α-type in the comparative examples), 46.92 g of aluminum nitride powder, 3.60 g of europium oxide powder, 27.26 g of calcium nitride powder, and 24.00 g of α-type Sialon core particles (above (for the examples) or (for the comparative examples)) were thoroughly mixed. This gave a mixture. (The mixing ratio of the above raw materials, calculated without including the core particles, is ideally (Ca x , Eu y ) m/2 Si 12-(m+n) Al m+n O n N 16-n(In the general formula of m = 2(x + y)), the ratios are m = 3.35, x = 1.62, ys = 0.06, and n = 0 (oxygen amount is not taken into consideration).) As a supplementary note, the mixture is common to Examples 1 to 3, and also to Comparative Examples 1 and 2, and also to Comparative Examples 3 and 4.
[0060] [Firing Step] Each of the resulting mixtures was placed in a boron nitride container (manufactured by Denka Co., Ltd.) and fired in a nitrogen gas atmosphere under the conditions shown in the table below.
[0061] [Pulverization Step] The fired product obtained in the firing step was pulverized using a jet mill under conditions of 0.30 MPa and 40 g / min.
[0062] [Reduction Annealing Step] The fired product after the pulverization step was annealed under the conditions of 1425°C, 8 hours, and 0.03 MPa G in an atmosphere consisting essentially of hydrogen gas. In some examples and comparative examples, Li was added to the fired product before annealing. 2 0.25% by mass of O was added and mixed well.
[0063] [Acid Treatment Step] The fired product that had undergone the reduction annealing step was placed in a mixed aqueous solution of hydrofluoric acid and nitric acid at 80° C. and mixed for 1 hour. Thereafter, the fired product was thoroughly washed with pure water and thoroughly dried.
[0064] [Elutriation step] After the acid treatment step, elutriation was carried out. That is, the sintered product was placed in an aqueous medium, allowed to stand for a certain period of time, and then the supernatant (in which the ultrafine particles were floating without settling) was removed, thereby removing the ultrafine particles from the sintered product. Specific conditions were as follows: Container used: 0.5 L capacity styrene rod bottle (opening 81.1 mm, depth 128 mm) Height from the bottom of the container to the liquid surface: 111 mm Aqueous medium: 0.05 mass % aqueous solution of sodium hexametaphosphate Standing time: As shown in Table 1 Siphoning of supernatant: Siphoned up to a height of 66 mm from the liquid surface Number of times: 5 times
[0065] <Particle size distribution measurement> Using a Microtrac MT3300EX II (manufactured by Microtrac Bell Corporation), measurements were made by the laser diffraction scattering method in accordance with JIS R1629:1997. 0.5 g of phosphor powder was added to 100 cc of ion-exchanged water, and the mixture was dispersed for 3 minutes using an Ultrasonic Homogenizer US-150E (manufactured by Nippon Seiki Seisakusho Co., Ltd., tip size φ20 mm, amplitude 100%, oscillation frequency 19.5 kHz, amplitude approximately 31 μm). Then, particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer MT3300EX II. From the obtained particle size distribution, the volume-based D50 and other parameters were determined.
[0066] <Manufacture and Evaluation of Package (White LED)> The phosphor powder obtained in the Examples or Comparative Examples was added to a thermosetting silicone resin material, degassed, and kneaded to obtain a kneaded mixture. The ratio (mass of phosphor powder / mass of curable silicone resin material) was adjusted to 0.6. This kneaded mixture was potted into a surface-mount package to which a blue LED element with a peak wavelength of 450 nm was bonded, and the resulting package was then thermally cured to produce a white LED. The total luminous flux of the fabricated white LED when energized was measured using a total luminous flux measuring device manufactured by Otsuka Electronics Co., Ltd. (a device combining a 500 mm diameter integrating hemisphere and a spectrophotometer / MCPD-9800). This measurement was performed on 10 white LEDs. The average value obtained for each LED was used as the measured value.
[0067] The light-emitting characteristics of the package were evaluated by dividing the obtained total luminous flux value by the chromaticity y. The larger this value, the higher the performance of the package. The reason for dividing the total luminous flux value by the chromaticity y is as follows: if the total luminous flux values were compared directly between the examples and comparative examples, the chromaticity would not match, and even if the values (mass of phosphor / mass of curable silicone resin material) were the same, the chromaticity would shift and the total luminous flux would change, making a simple comparison difficult.
[0068] Various information is summarized in Table 1.
[0069]
[0070] As shown in Table 1, when the packages manufactured using the α-sialon phosphors of Examples 1 to 3, which were manufactured using silicon nitride containing a large amount of β-silicon nitride as a raw material, were evaluated, the values obtained by dividing the total luminous flux value by the chromaticity y were larger than those of the comparative example. This indicates that the α-sialon phosphor manufactured using β-silicon nitride as a raw material is preferably used for manufacturing high-performance packages. Incidentally, a comparison of Examples 1 to 3 reveals that the reduction annealing step 2 It is understood that the performance can be further improved by using O or by carrying out an elutriation process.
[0071] This application claims priority based on Japanese Patent Application No. 2023-051847, filed March 28, 2023, the disclosure of which is incorporated herein by reference in its entirety.
[0072] REFERENCE SIGNS LIST 1 Phosphor particle 30 Sealant 40 Composite (wavelength conversion member) 100 Light emitting device 120 Light emitting element 130 Heat sink 140 Case 150 First lead frame 160 Second lead frame 170 Bonding wire 172 Bonding wire
Claims
1. A method for producing an α-sialon phosphor, comprising: a mixture preparation step of preparing a mixture containing silicon nitride, an aluminum source, a calcium source, and a europium source; and a firing step of firing the mixture to obtain a fired product, wherein more than 50 mass% of the silicon nitride is β-silicon nitride.
2. A method for producing an α-SiAlON phosphor as described in claim 1, wherein the silicon nitride has an oxygen content of 0.5 mass % or less.
3. A method for producing an α-SiAlON phosphor according to claim 1 or 2, further comprising a reduction annealing step of heating the fired product in a reducing atmosphere to reduce it.
4. A method for producing an α-SiAlON phosphor according to claim 3, wherein the reduction annealing step is a step of heating the fired product in an atmosphere containing hydrogen gas.
5. The method for producing an α-SiAlON phosphor according to claim 3, wherein the fired product is added with lithium oxide (Li 2 O) is added to the phosphor, and then the reduction annealing step is carried out.
6. A method for producing an α-SiAlON phosphor according to claim 3, wherein the fired product is heated to 1300 to 1500° C. in the reduction annealing step.
7. A method for producing an α-sialon phosphor according to claim 1 or 2, wherein in the firing step, the mixture is fired at 1800° C. or higher.
8. A method for producing an α-SiAlON phosphor according to claim 1 or 2, wherein the aluminum source contains aluminum nitride.
9. A method for producing an α-sialon phosphor according to claim 1 or 2, wherein the calcium source contains calcium nitride.
10. A method for producing an α-sialon phosphor according to claim 1 or 2, wherein the europium source contains europium oxide.
11. A method for manufacturing a light emitting device, comprising combining a wavelength conversion member containing an α-SiAlON phosphor obtained by the method for manufacturing an α-SiAlON phosphor according to claim 1 or 2 with a light emitting element to manufacture a light emitting device.
Citation Information
Patent Citations
alpha-SIALON POWDER AND ITS MANUFACTURING METHOD
JP2006045271A
Ca-CONTAINING α-SIALON PHOSPHOR AND METHOD FOR PRODUCING THE SAME
JP2012224757A
Fluophor, manufacturing method therefor, light-emitting element using the same, and silicon nitride powder for manufacturing fluophor
JP2019026657A
In-situ toughened alpha prime-sialon-based ceramics
US5908798A
Oxynitride phosphor powder and method for producing same
WO2014157695A1