Method for recovering dusting powder and method for producing sintered ceramic object
The method of using a vibrating cleaning liquid to separate and recover bedding powder from ceramic scraps addresses the challenge of reusing ceramic scraps by ensuring effective powder removal and maintaining substrate properties, enhancing productivity and reducing waste.
Patent Information
- Application Number
- PCT/JP2024/011514
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to separate and recover bedding powder from ceramic scraps to prevent its adhesion, which is essential for reusing scraps as raw materials in ceramic substrate production without compromising properties like insulation and strength.
A method involving a cleaning step where ceramic scraps with adhered bedding powder are washed using a vibrating cleaning liquid, followed by a recovery step to separate and recover the bedding powder, utilizing ultrasonic cleaning and potentially other vibration-based methods to effectively remove the powder from the scraps.
This method allows for the efficient separation and recovery of bedding powder, enabling its reuse, which improves productivity, reduces waste, and maintains the properties of ceramic substrates, such as strength and thermal conductivity.
Smart Images

Figure JP2024011514_03102024_PF_FP_ABST
Abstract
Description
Method for recovering bedding powder and method for manufacturing ceramic sintered body
[0001] The embodiments described below generally relate to a method for recovering bedding powder and a method for producing a ceramic sintered body.
[0002] Ceramic sintered bodies are excellent in strength, wear resistance, heat dissipation, and the like. One example of the use of ceramic sintered bodies is a plate-shaped ceramic sintered body. Plate-shaped ceramic sintered bodies are used, for example, as ceramic sintered bodies for substrates used in circuits and the like (hereinafter simply referred to as "ceramic substrates"). In the process of manufacturing ceramic substrates, for example, a long sheet-shaped ceramic compact is produced by a doctor blade method, and the sheet-shaped ceramic compact is cut to a required size, and the plate-shaped ceramic compact is then sintered to obtain a ceramic substrate.
[0003] In recent years, in order to increase the mass productivity of ceramic substrates, multiple plate-shaped ceramic green bodies coated with a spreading powder (mold release agent) have been stacked and sintered with the aim of sintering many plate-shaped ceramic green bodies at once. The spreading powder serves to prevent the stacked plate-shaped ceramic green bodies from adhering to each other during sintering. For example, in Japanese Patent No. 5673847 (Patent Document 1), the size and amount of spreading powder made of boron nitride (BN) is controlled. This reduces waviness in the resulting ceramic substrate when multiple plate-shaped ceramic green bodies are stacked and sintered with the spreading powder interposed therebetween, and also suppresses adhesion between the resulting ceramic substrates (the plate-shaped ceramic green bodies before sintering).
[0004] When a ceramic sheet is sintered to obtain a ceramic sintered plate (ceramic substrate), the ceramic sheet is cut to the desired size. Cutting the ceramic sheet generates scraps of the ceramic sheet (hereinafter simply referred to as "scrap"). Scraps are primarily ceramic parts that were originally part of the ceramic sheet. In addition, defective products generated during the manufacturing and transportation processes of ceramic sheet and ceramic plate are also removed and turned into scraps.
[0005] Therefore, the reuse of scraps as raw materials has been considered. For example, Japanese Patent No. 3779481 (Patent Document 2) proposes a ceramic molded body that is easy to recover and reuse by improving the binder in the raw material. Japanese Patent Laid-Open Publication No. 2015-091742 (Patent Document 3) proposes a method of immersing scraps in a solvent, mixing them, and then reusing them as a recycled slurry.
[0006] Patent No. 5673847 Patent No. 3779481 JP 2015-091742 A
[0007] It is desirable to reuse the above-mentioned scraps from the viewpoints of improving productivity and reducing waste. However, when reusing scraps generated after coating with bedding powder as raw materials for new ceramic substrates or other new sintered ceramic bodies, a problem arises in how to separate and recover the bedding powder attached to the scraps from the scraps or the ceramic powder generated from the scraps. Using scraps from which the bedding powder has not been separated or ceramic powder generated from the scraps as raw materials for new ceramic substrates or other new sintered ceramic bodies may result in a deterioration of various properties, such as insulation and strength. For example, the inventions described in Patent Documents 2 and 3 are suitable for reusing scraps without bedding powder attached, but are unable to separate the scraps from the bedding powder, and therefore are unable to reuse scraps with bedding powder attached.
[0008] The embodiments are intended to address such issues and to provide a method for separating and recovering the bedding powder from scrap material to which the bedding powder has adhered or from ceramic powder produced from the scrap material.
[0009] The method for recovering bedding powder according to the embodiment is characterized by having a cleaning process in which a cleaning liquid is vibrated to clean ceramic molded body pieces to which bedding powder has adhered, and a recovery process in which at least the bedding powder is recovered from the mixed liquid produced in the cleaning process.
[0010] Fig. 1 is a diagram showing an example of an adhering step of adhering a laying powder to a sheet-shaped ceramic molded body. Fig. 2 is a diagram showing an example of a sheet-shaped ceramic molded body. Fig. 3 is a diagram showing an example of a cutting step of cutting a sheet-shaped ceramic molded body. Fig. 4 is a diagram showing an example of a cleaning step of cleaning scraps in a method for recovering laying powder according to an embodiment. A flowchart showing an example of a method for manufacturing a ceramic sintered body according to an embodiment. A flowchart showing an example of a cleaning step according to an embodiment. Embodiment
[0011] The method for recovering bedding powder and the method for manufacturing a ceramic sintered body according to the embodiment will be described with reference to FIGS.
[0012] The method for recovering bedding powder according to the embodiment is characterized by including a cleaning process in which the bedding powder is washed by vibrating a cleaning solution 9 in which scrap material 12, which is composed of a ceramic molded body and bedding powder attached thereto, is immersed, and a recovery process in which the bedding powder is separated from the scrap material or ceramic powder produced from the scrap material by the cleaning process and recovered.
[0013] FIG. 1 shows an example of a coating step in which a laying powder (release agent) 4 is applied to a sheet-shaped ceramic green body 1a. FIG. 2 shows an example of a sheet-shaped ceramic green body 1b (a sheet-shaped ceramic green body 1a to which the laying powder 4 is applied). FIG. 3 shows an example of a cutting step in which the sheet-shaped ceramic green body 1b is cut. FIG. 4 shows an example of a cleaning step in a method for recovering laying powder according to an embodiment. In FIGS. 1 to 4, reference numeral 1 denotes a sheet-shaped ceramic green body (reference numeral 1a: a sheet-shaped ceramic green body that does not include a laid-powder applied thereto; reference numeral 1b: a sheet-shaped ceramic green body that includes the sheet-shaped ceramic green body 1a and the laid-powder applied thereto), reference numeral 2 denotes a member for arranging the sheet-shaped ceramic green body 1, reference numeral 3 denotes a laying powder application device, reference numeral 4 denotes the laid-powder, reference numeral 5 denotes a laid-powder layer, reference numeral 6 denotes a plate-shaped ceramic green body (reference numeral 6a: a plate-shaped ceramic green body that does not include a laid-powder applied thereto; reference numeral 6b: a plate-shaped ceramic green body that includes the laid-powder applied thereto), reference numeral 7 denotes a plate-shaped ceramic green body (reference numeral 7a: a plate-shaped ceramic green body that does not include a laid-powder applied thereto; reference numeral 7b: a plate-shaped ceramic green body that includes the laid-powder applied thereto), reference numeral 8 denotes a plate-shaped ceramic green body (reference numeral 8b: a plate-shaped ceramic green body that does not include a laid-powder applied thereto; reference numeral 8c: a plate-shaped ceramic green body that includes the laid-powder applied thereto), reference numeral 9 denotes a plate-shaped ceramic green body (reference numeral 9d: a plate-shaped ceramic green body that does not include a laid-powder applied thereto; reference numeral 9 A plate-shaped ceramic formed body including a ceramic formed body 6a and a bedding powder applied thereto, i.e., a sheet-shaped ceramic formed body 1b, was cut, while reference numeral 6c denotes scrap material not including the applied bedding powder), reference numeral 7 denotes a cutting jig, reference numeral 8 denotes an ultrasonic cleaning device, reference numeral 9 denotes cleaning liquids (reference numeral 9a: cleaning liquid for the first cleaning step, reference numeral 9b: cleaning liquid for the second cleaning step), reference numeral 10 denotes a water cleaning tank, reference numeral 11 denotes a mixed liquid (reference numeral 11a: mixed liquid for the first cleaning, reference numeral 11b: mixed liquid for the second cleaning), and reference numeral 12 denotes scrap material.
[0014] A method for manufacturing a ceramic sintered body according to an embodiment is shown in Fig. 5. In Fig. 5, ST1 is a molding step, ST2 is a powder coating step, ST3 is a cutting step, ST4 is a sintering step, ST5 is a cleaning step, and ST6 is a separation and recovery step.
[0015] The ceramic sheet compact 1a refers to a ceramic powder formed into a sheet shape. The ceramic sheet compact 1a may be formed by adding an organic binder, a sintering aid, or the like to the ceramic powder as needed. The shape of the front and back surfaces of the ceramic sheet compact 1a is not limited to a square, but may be a circle, a shape with irregularities, or the like.
[0016] The ceramic powder constituting the sheet-shaped ceramic compact 1a may be a powder containing one selected from silicon nitride, aluminum nitride, aluminum oxide, zirconium oxide, and silicon carbide as its main component. Here, the main component of the sheet-shaped ceramic compact 1a or the plate-shaped ceramic sintered body produced by cutting and sintering it refers to the component with the largest mass ratio among the components constituting the sheet-shaped ceramic compact 1a or the plate-shaped ceramic sintered body. A sheet-shaped ceramic compact 1a containing silicon nitride as its main component becomes a silicon nitride sintered body after sintering. Furthermore, a sheet-shaped ceramic compact 1a containing aluminum oxide as its main component becomes an aluminum oxide sintered body after sintering.
[0017] Furthermore, in a sheet-shaped ceramic compact 1a made of a raw material powder mixture of two or more selected from silicon nitride, aluminum nitride, aluminum oxide, zirconium oxide, and silicon carbide, or a plate-shaped ceramic sintered body produced by cutting and sintering the sheet-shaped ceramic compact 1a, the component with a larger mass ratio may be regarded as the main component. For example, an alu-zir sintered body is a sintered ceramic compact made of a raw material powder mixture of aluminum oxide and zirconium oxide. If the alu-zir sintered body has aluminum oxide as the main component, it may be regarded as a plate-shaped aluminum oxide sintered body.
[0018] In the forming step ST1 (shown in FIG. 5), a sheet-shaped ceramic green body 1a is formed by a doctor blade method, die molding, cold isostatic pressing (CIP), injection molding, or the like. As will be described later, the doctor blade method is preferred when producing a ceramic substrate. The doctor blade method can produce a long sheet-shaped ceramic green body 1a. This can improve the mass productivity of ceramic substrates (plate-shaped ceramic sintered bodies). Hereinafter, an example of obtaining a sheet-shaped ceramic green body 1a by the doctor blade method will be described.
[0019] In the forming step ST1 (shown in FIG. 5 ), the sheet-shaped ceramic molded body 1a is subjected to a degreasing treatment as needed. The degreased body that has been degreased is also included in the sheet-shaped ceramic molded body 1a. Alternatively, the degreasing treatment may be performed on the sheet-shaped ceramic molded body 1b in the spreading powder application step ST2 after the spreading powder 4 has been applied, or on the plate-shaped ceramic molded body 6b in the cutting step ST3 after cutting. The sheet-shaped ceramic molded body 1b also includes a degreased body obtained by degreasing the sheet-shaped ceramic molded body 1b, and the plate-shaped ceramic molded body 6b also includes a degreased body obtained by degreasing the plate-shaped ceramic molded body 6b.
[0020] Next, in the spreading powder application step ST2 (shown in FIG. 5 ), spreading powder 4 is applied to the sheet-shaped ceramic compact 1a to form a spreading powder layer 5. The spreading powder 4 may be one or more selected from boron nitride, zirconium oxide, aluminum oxide, and aluminum nitride. The spreading powder 4 is applied to the surface of the sheet-shaped ceramic compact 1a to form the spreading powder layer 5. The spreading powder layer 5 serves to prevent adhesion between the stacked plate-shaped ceramic compacts 6b obtained by cutting the sheet-shaped ceramic compact 1b when they are stacked and sintered. Furthermore, the spreading powder 4 is preferably boron nitride. As described below, the plate-shaped ceramic compact 6b is fired at approximately 1600 to 2000°C. Boron nitride is suitable for use as the spreading powder 4 because it does not easily adhere to the plate-shaped ceramic compact 6b, even in high-temperature environments. There are various types of boron nitride, such as hexagonal, cubic, and rhombohedral crystals, among which hexagonal boron nitride (h-BN) is preferred.
[0021] The average particle size of the spreading powder 4 is preferably 20 μm or less. By reducing the average particle size of the spreading powder 4, it becomes easier to form a spreading powder layer 5 with a uniform thickness on the surface of the sheet-shaped ceramic compact 1a. If the average particle size of the spreading powder 4 is larger than 20 μm, the spreading powder layer 5 will be non-uniform, which may have an adverse effect on the surface properties of the ceramic sintered body. Preferably, the average particle size of the spreading powder 4 is 10 μm or less, more preferably 6 μm or less. There is no particular lower limit for the average particle size of the spreading powder 4, but 2 μm or more is preferred. If the average particle size is less than 2 μm, handling may be impaired.
[0022] As shown in FIG. 1 , a ceramic sheet 1a is formed on a placement member 2. Examples of the placement member 2 include a film and a plate-like member. The ceramic sheet 1a may be formed directly on the placement member 2, or may be placed on the placement member 2 during the forming process. For example, a doctor blade method may be used to form the ceramic sheet 1a on the film-like placement member 2, thereby producing a long ceramic sheet 1a.
[0023] The sheet-shaped ceramic compact 1a can be coated with the base powder 4 by various methods, including spraying, passing the compact through a solution containing the base powder 4, using a brush, using static electricity, gravure printing, and immersing the compact in a solution containing the base powder 4. When using a solution containing the base powder 4, water or an organic solvent may be used as the solvent. Examples of organic solvents include alcohol, cellulose, carboxymethyl cellulose, acrylic polymers, polyvinyl alcohol, polyvinylpyrrolidone, and amine-functionalized polymers. Examples of acrylic polymers include acrylic acid, acrylamide, and maleic anhydride. Examples of amine-functionalized polymers include allylamine, ethyleneimine, and oxazoline. Examples of alcohols include ethanol, methanol, butanol, and propanol.
[0024] FIG. 1 illustrates an example of a coating method for coating a sheet-shaped ceramic formed body 1a with a coating powder 4 using a spray-type coating powder coating device 3. The coating powder coating device 3 is preferably a spray-type device. A spray-type device can stabilize the amount of coating powder 4 sprayed. Furthermore, by providing multiple spray nozzles, the coating powder 4 can be applied over a wide area. Furthermore, with the spray-type device, a long sheet-shaped ceramic formed body 1a can be placed on a film-like placement member 2 and the coating powder 4 can be applied while the body is being transported. Furthermore, with the spray-type device, a solution containing the coating powder 4 may be sprayed.
[0025] A powder layer 5 (shown in FIG. 2) made of powder 4 is formed on the ceramic sheet-shaped body 1a to form a ceramic sheet-shaped body 1b.
[0026] Next, in the cutting step ST3 (shown in FIG. 5), the sheet-shaped ceramic green body 1b is cut to a size appropriate for the purpose. The cutting is performed using, for example, a cutting jig 7. To increase the mass productivity of ceramic substrates, it is preferable to produce long or wide sheet-shaped ceramic green bodies 1b. Furthermore, ceramic green bodies shrink during sintering. For this reason, the sheet-shaped ceramic green body 1b is cut to a size larger than the intended ceramic substrate. By cutting the sheet-shaped ceramic green body 1b, a plate-shaped ceramic green body 6b with a uniform powder layer 5 and defective scraps 12 are obtained (shown in FIG. 3).
[0027] Subsequently, in the sintering step ST4 (shown in FIG. 5), the plate-shaped ceramic compact 6b is sintered to produce a plate-shaped ceramic sintered body, i.e., a ceramic substrate. In the sintering step ST4, sintering is performed by heat treatment under normal pressure or pressure, typically at 1600 to 2000°C. Alternatively, the sintering step ST4 may be performed in two stages, with the heat treatment temperature ranges being different.
[0028] When the sheet-shaped ceramic green body 1b is cut to the desired size in the cutting process ST3 (shown in FIG. 5), scraps 12 are produced in addition to the plate-shaped ceramic green body 6b. The scraps 12 have the laying powder 4 attached to them. In the cleaning process ST5 and the separation and recovery process ST6 (shown in FIG. 5), the scraps 12 are cleaned and the laying powder 4 is separated and recovered. The amount of the laying powder 4 applied to the sheet-shaped ceramic green body 1b may be inspected, and any portions where the amount of the laying powder 4 applied is outside the appropriate range (i.e., portions where the amount of the laying powder 4 is too little or too much) may be cut and deemed defective, and the laying powder 4 may be recovered from these defective portions. Furthermore, any portions of the sheet-shaped ceramic green body 1b that are damaged during transport may be cut and deemed defective, and the laying powder 4 may be recovered from these defective portions. Similarly, plate-shaped ceramic green bodies 6b with insufficient application or damage may be deemed defective, and the laying powder 4 may be recovered from these defective portions. Note that the defective portions are also included in the scraps 12 here.
[0029] Next, in the cleaning step ST5 (shown in FIG. 5 ), one or more scraps 12 are immersed in the cleaning solution 9, and the cleaning solution 9 is vibrated to clean the scraps 12. Cleaning that vibrates the cleaning solution 9 includes at least one method selected from ultrasonic cleaning, bubbling cleaning, swinging cleaning, stirring cleaning, and jet cleaning. When the cleaning that vibrates the cleaning solution 9 includes two or more cleaning methods, these cleaning methods may be performed simultaneously or sequentially. Note that in the cleaning step ST5, all of the scraps 12 may be decomposed into ceramic powder, only a portion of the scraps 12 may be decomposed into ceramic powder, or the scraps 12 may not be decomposed into ceramic powder at all.
[0030] Ultrasonic cleaning is a cleaning method that uses ultrasonic waves added to the cleaning liquid. It is a cleaning method that utilizes ultrasonic cavitation, and is primarily based on the following mechanism. When ultrasonic vibrations are transmitted through the liquid, bubbles are generated due to pressure fluctuations that correspond to the frequency. The bubbles repeatedly expand and contract in response to the pressure fluctuations, increasing their pressure, and then collapse. Jets and shock waves generated when the bubbles collapse remove any deposits from the object being cleaned. The action of the collapsing bubbles removing deposits from the object being cleaned is referred to here as the "cavitation effect."
[0031] Bubbling cleaning is a cleaning method that uses the physical action of bubbles by adding or generating bubbles in the cleaning solution. Oscillating cleaning is a cleaning method that involves oscillating the cleaning solution. For example, an example of oscillating cleaning is a cleaning method that involves oscillating the cleaning tank itself. Agitating cleaning is a cleaning method that involves agitating the cleaning solution. Jet cleaning is a cleaning method that involves spraying the cleaning solution. Jet cleaning is also called jet bath cleaning.
[0032] Among ultrasonic cleaning, bubbling cleaning, swing cleaning, stirring cleaning, and jet cleaning, ultrasonic cleaning is preferred as a cleaning method that applies vibrations to the cleaning solution 9. This is because ultrasonic cleaning can clean scraps 12 regardless of their shape and size, and the cavitation effect makes it easy to remove deposits from the scraps 12 and break them down. Furthermore, ultrasonic cleaning allows the degree of cleaning to be controlled by controlling the generation of cavitation.
[0033] On the other hand, jet cleaning and bubbling cleaning tend to insufficiently clean areas not hit by the jet or bubbles. Oscillating cleaning and agitating cleaning cannot sufficiently agitate the cleaning liquid in areas such as small gaps formed in the scrap 12, which may result in insufficient cleaning of deposits in such areas. In particular, because the scrap 12 is in a soft state before sintering and is often cleaned in a bundle of long, thin string-like pieces, jet cleaning, bubbling cleaning, oscillating cleaning, and agitating cleaning may result in incomplete cleaning. In contrast, ultrasonic cleaning can clean even small areas by immersing the cleaning liquid in the area, as cavitation acts on the area, regardless of the shape of the scrap 12.
[0034] On the other hand, a drawback of ultrasonic cleaning is that the number of cavitations generated varies depending on the distance from the ultrasonic generator, which can lead to variations in the cleaning results within the cleaning tank. Therefore, by combining ultrasonic cleaning with at least one of jet cleaning, bubbling cleaning, oscillating cleaning, and agitation cleaning, either simultaneously or in sequence, the scraps 12 can be cleaned uniformly.
[0035] The following description will be given taking as an example a case where the cleaning step ST5 (shown in FIG. 5) includes ultrasonic cleaning. In cases where the cleaning step ST5 does not include ultrasonic cleaning but includes at least one of jet cleaning, bubbling cleaning, oscillating cleaning, and agitation cleaning, the descriptions relating to ultrasonic cleaning should be interpreted with appropriate substitutions. For example, if at least one of bubbling cleaning, oscillating cleaning, agitation cleaning, and jet cleaning is included instead of ultrasonic cleaning, each cleaning method uses vibrations corresponding to the cleaning ability at that frequency instead of the ultrasonic frequency. Furthermore, in cases where the cleaning step ST5 combines ultrasonic cleaning with another cleaning method, the descriptions relating to the single ultrasonic cleaning should be interpreted with appropriate substitutions.
[0036] As an example of the cleaning process ST5, ultrasonic cleaning is performed as the first cleaning ST51, as shown in FIG. 6 . As described above, the first cleaning ST51 may include at least one of ultrasonic cleaning, jet cleaning, bubbling cleaning, oscillating cleaning, and agitation cleaning. Ultrasonic cleaning can break down the scraps 12 ( FIG. 4(A) ) immersed in the cleaning solution 9a in the cleaning tank 8, and separate the bedding powder 4 from the scraps 12 or the ceramic powder resulting from the decomposition of the scraps 12. After ultrasonic cleaning, the ceramic powder and the bedding powder 4 are mixed into the cleaning solution 9a. The cleaning solution after the first cleaning ST51 is also referred to as the mixed solution 11a (shown in FIG. 4(B)).
[0037] The ultrasonic cleaning in the first cleaning ST51 preferably has a frequency of 10 kHz or higher. If the ultrasonic frequency is less than 10 kHz, the cavitation effect may be insufficient. If the cavitation effect is insufficient, cleaning may take a long time. There is no particular upper limit to the frequency, but 5 MHz or lower is preferable. If the frequency exceeds 5 MHz, no further effect can be obtained and this may actually lead to increased costs. For this reason, the ultrasonic frequency in the first cleaning is preferably 10 kHz or higher and 5 MHz or lower. Preferably, it is more preferably 20 kHz or higher and 200 kHz or lower.
[0038] In the first cleaning ST51, it is preferable to use an aqueous cleaning solution as the cleaning solution 9a. Here, an aqueous cleaning solution refers to water or a cleaning solution to which a chemical solution containing components such as a surfactant has been added. Tap water or other suitable water can be used. The sheet-shaped ceramic compact 1a generally contains an organic binder as a binding agent and may also contain an organic solvent. An organic solvent may also be used when applying the spreading powder 4 to the sheet-shaped ceramic compact 1a. The chemical solution makes it easier to separate the organic binder and organic solvent.
[0039] A water-soluble surfactant is preferred as the chemical solution. Examples of water-soluble surfactants include cationic, anionic, and nonionic surfactants. Of these, nonionic surfactants are preferred. Nonionic surfactants do not remain as ions in the recovered ceramic powder and bedding powder 4. This makes it possible to suppress a decrease in sinterability during reuse.
[0040] The cleaning time for the first cleaning ST51 is preferably 3 minutes or more. Here, the cleaning time refers to the time for applying ultrasonic waves to the cleaning solution 9a. If the cleaning time is less than 3 minutes, the cleaning effect may be insufficient. Furthermore, although there is no particular upper limit on the cleaning time for the first cleaning ST51, 120 minutes or less is preferable. If the cleaning time exceeds 120 minutes, no further effect can be obtained and this may actually result in increased costs. Therefore, the cleaning time for the first cleaning ST51 is preferably 3 minutes or more and 120 minutes or less. More preferably, 5 minutes or more and 60 minutes or less are more preferable. The above-mentioned preferable cleaning time applies to a single first cleaning. As will be described later, if the first cleaning ST51 is performed multiple times, it is preferable that each cleaning time be within the range of 3 minutes or more and 120 minutes or less.
[0041] As an example of the cleaning process ST5 (shown in FIG. 5 ), a water cleaning, optionally vibrating the cleaning solution, is preferably performed as a second cleaning ST52 after the first cleaning ST51. Water cleaning refers to cleaning using water without added chemicals as the cleaning solution 9 (i.e., when water is used as the aqueous cleaning solution 9a in the first cleaning ST51, this first cleaning ST51 is a water cleaning). After the first cleaning ST51, the scrap 12 is removed from the mixed solution 11a and immersed in the cleaning solution 9b in the water cleaning tank 10 for the second cleaning ST52 (shown in FIG. 4(C)). The same equipment may be used for the cleaning tank 8 and the water cleaning. In this case, the mixed solution 11a is replaced with the cleaning solution 9b for the second cleaning ST52. By performing the second cleaning ST52, cleaning can be performed with the cleaning solution 9b, which has been freed from the bedding powder 4, ceramic powder, sintering aid, binder, organic solvent, and other separated substances that were mixed into the cleaning solution 9a in the first cleaning ST51. In other words, the second cleaning ST52 has a rinsing effect. The cleaning time of the second cleaning ST52 is preferably in the range of 3 minutes to 120 minutes. The cleaning time of the second cleaning ST52 refers to the time during which ultrasonic waves or other effects are applied to the cleaning liquid 9b.
[0042] Ultrasonic cleaning may be performed in the second cleaning ST52. By performing ultrasonic cleaning in the second cleaning ST52, the rinsing effect can be improved. The frequency when performing ultrasonic cleaning in the second cleaning ST52 is preferably in the range of 10 kHz to 200 kHz.
[0043] The first cleaning ST51 and the second cleaning ST52 may be combined and performed multiple times. By performing the combined steps multiple times, the cleaning can proceed while removing separated matter from the cleaning solution 9. This can enhance the effect of the chemical solution, for example. It is preferable to alternately perform the first cleaning ST51 and the second cleaning ST52. When a combination of performing the first cleaning ST51 and then performing the second cleaning ST52 is defined as one set, it is preferable to perform this series of combinations one set or more and ten sets or less.
[0044] The final cleaning in the cleaning step ST5 is referred to as the finishing cleaning. The finishing cleaning is preferably performed with water. When the cleaning step ST5 (shown in FIG. 5) includes multiple cleanings, the final cleaning is the finishing cleaning. When the cleaning step ST5 (shown in FIG. 5) includes only one cleaning, the cleaning also serves as the finishing cleaning.
[0045] The cleaning process ST5 (shown in FIG. 5 ) may include a rough cleaning ST50. Here, rough cleaning ST50 refers to the first cleaning performed in the cleaning process ST5, which is a water cleaning performed to break down the scrap 12. By breaking down the scrap 12 to reduce its size in advance, the cleaning efficiency of the subsequent cleanings ST51 and ST52 can be improved. Furthermore, from the viewpoint of the ability to break down the scrap 12, rough cleaning ST50 is preferably a cleaning that applies vibrations to the cleaning solution 9, and more preferably ultrasonic cleaning. When ultrasonic cleaning is performed as rough cleaning ST50, from the viewpoint of the ability and efficiency to break down the scrap 12, the frequency is preferably in the range of 10 kHz to 200 kHz, and the cleaning time is preferably 3 minutes to 80 minutes, and more preferably shorter than the first cleaning.
[0046] The cleaning step ST5 has been described above using an example involving ultrasonic cleaning. This step allows the bedding powder 4 adhering to the scrap 12 to be separated. Note that the cleaning step ST5 does not necessarily have to separate all of the bedding powder 4 adhering to the scrap 12 or the ceramic powder produced by decomposition of the scrap 12; it may simply separate a portion of the adhering bedding powder. Furthermore, the scrap 12 from which the bedding powder has been separated may be recovered and used as a raw material for the recycled slurry.
[0047] Next, in the separation and recovery step ST6 (shown in FIG. 5), the ceramic powder and / or the laying powder 4 are separated and recovered from the mixed solution 11 (mixed solution 11a produced in the first cleaning and / or mixed solution 11b produced in the second cleaning and / or mixed solution 11c produced in the rough cleaning) produced in the cleaning step ST5. In this step, the sintering aid may also be separated and recovered.
[0048] The process of separating and recovering the ceramic powder, the base powder 4, or both can be carried out using methods such as a method using a filter or a method using a centrifuge. In the method using a filter, a mesh filter is used, for example. The mesh filter has a mesh diameter that matches the particle size of the powder to be separated, for example. The filter may be multi-layered, or filters with different mesh diameters may be multi-layered. In the method using a centrifuge, the ceramic powder and the base powder 4 are separated by utilizing the difference in mass.
[0049] The step of separating and recovering the ceramic powder and / or the laying powder 4 may be carried out on the mixed liquid 11 or on the mixed liquid 11 from which the solvent has been evaporated.
[0050] By performing the above-described cleaning step ST5 and separation and recovery step ST6, it is possible to recover the ceramic powder, the laying powder 4, or both, and also the sintering aid. As shown in Fig. 5, the recovered ceramic powder and sintering aid can be reused in the molding step ST1, and the laying powder 4 can be reused in the laying powder application step ST2.
[0051] The spreading powder 4 obtained by the spreading powder recovery method of the embodiment can be applied to the surface of the sheet-shaped ceramic formed body 1a in the spreading powder application step ST2. When the spreading powder 4 is to be reused, the recovered spreading powder 4 may be used alone, or new spreading powder and the recovered spreading powder 4 may be mixed and used.
[0052] Furthermore, the ceramic powder obtained by the method for recovering the spread powder according to the embodiment can be reused when producing the sheet-shaped ceramic compact 1a in the forming step ST1. When reusing the ceramic powder, the recovered ceramic powder may be used alone, or a mixture of new ceramic powder and the recovered ceramic powder may be used. Furthermore, the sintering aid obtained by the method for recovering the spread powder according to the embodiment can be reused when producing the sheet-shaped ceramic compact 1a in the forming step ST1. When reusing the sintering aid, the sintering aid may be used alone, or a mixture of new sintering aid and the recovered sintering aid may be used.
[0053] The method for manufacturing a ceramic sintered body according to the embodiment is characterized by comprising a powder application process ST2 in which the powder 4 obtained by the powder recovery method according to the embodiment is applied to the surface of a sheet-shaped ceramic molding 1a, a cutting process ST3 in which the sheet-shaped ceramic molding 1b to which the powder 4 has been applied is cut, and a sintering process ST4 in which the plate-shaped ceramic molding 6b after cutting is sintered.
[0054] Alternatively, the method for manufacturing a ceramic sintered body according to the embodiment is characterized by comprising a forming process ST1 in which a sheet-shaped ceramic molding 1a is formed using ceramic powder obtained by the method for recovering the laying powder according to the embodiment as raw material powder, a laying powder application process ST2 in which a laying powder 4 is applied to the surface of the sheet-shaped ceramic molding 1a, a cutting process ST3 in which the sheet-shaped ceramic molding 1b to which the laying powder 4 has been applied is cut, and a sintering process ST4 in which the plate-shaped ceramic molding 6b after cutting is sintered.
[0055] Alternatively, the method for manufacturing a ceramic sintered body according to the embodiment is characterized by comprising a forming process ST1 in which a sheet-shaped ceramic molding 1a is formed using ceramic powder obtained by the method for recovering the laying powder according to the embodiment as raw material powder, a laying powder application process ST2 in which the laying powder 4 obtained by the method for recovering the laying powder according to the embodiment is applied to the surface of the sheet-shaped ceramic molding 1a, a cutting process ST3 in which the sheet-shaped ceramic molding 1b to which the laying powder 4 has been applied is cut, and a sintering process ST4 in which the plate-shaped ceramic molding 6b after cutting is sintered.
[0056] The method for manufacturing a ceramic sintered body according to the embodiment can obtain a good plate-shaped ceramic sintered body even when the spreading powder 4 obtained by the above-described recovery method is reused. Similarly, a good plate-shaped ceramic sintered body can be obtained even when the ceramic powder obtained by the above-described recovery method is reused. For example, a ceramic substrate using the spreading powder 4 or ceramic powder obtained by the above-described recovery method has equivalent peelability between substrates after sintering and equivalent properties such as strength, thermal conductivity, and insulation, compared to a similar ceramic substrate not using the recovered spreading powder 4 or ceramic powder.
[0057] The sintering process of the plate-shaped ceramic compact 6b is carried out in a high-temperature environment of about 1600 to 2000°C. The laying powder 4 is required to have the performance to withstand high-temperature environments. For this reason, expensive materials such as boron nitride and zirconium oxide are used for the laying powder 4. The ability to reuse the laying powder 4 is effective in reducing costs and improving productivity. Furthermore, the reuse of ceramic powder is also effective in reducing costs and improving productivity. Furthermore, scraps that previously had to be discarded can now be reused, which is effective in reducing waste.
[0058] (Examples) (Examples 1 to 7, Comparative Example 1) In order to verify the laying powder recovery method according to Examples 1 to 7 and Comparative Example 1, plate-shaped ceramic molded bodies (hereinafter referred to as "ceramic molded body pieces") cut from a sheet-shaped ceramic molded body coated with BN (boron nitride) laying powder were prepared as simulants of scrap material 12. Specifically, in order to verify the laying powder recovery method according to Examples 1 to 6 and Comparative Example 1, plate-shaped silicon nitride molded bodies (an example of a ceramic molded body piece) were prepared by cutting a sheet-shaped silicon nitride molded body coated with BN laying powder. Furthermore, in order to verify the laying powder recovery method according to Example 7, plate-shaped aluminum nitride molded bodies (an example of a ceramic molded body piece) were prepared by cutting a sheet-shaped aluminum nitride molded body coated with BN laying powder.
[0059] The ceramic molded body pieces were treated as scrap material 12 and were cleaned under the conditions of Examples 1 to 7 and Comparative Example 1 shown in Table 1. In the ultrasonic cleaning of the first cleaning ST51, a cleaning solution containing a chemical solution was used. In Examples 3 and 6, in which the first cleaning ST51 was performed multiple times, the cleaning solution 9a was replaced after each cleaning. In Examples 1, 3 to 7 and Comparative Example 1, in which the second cleaning ST52 was performed, the second cleaning step was a finish cleaning, and was performed with water. On the other hand, in Example 2, in which the second cleaning ST52 was not performed, the first cleaning once also served as the finish cleaning.
[0060] [Table 1]
[0061] All of the bedding powder recovery methods according to Examples 1 to 7 include a first cleaning step ST51 using ultrasonic cleaning. Furthermore, the bedding powder recovery methods according to Examples 3 to 6 include a rough cleaning step ST50. Furthermore, the bedding powder recovery methods according to Examples 4 to 6 include ultrasonic cleaning as the rough cleaning step ST50.
[0062] Furthermore, the method for recovering bedding powder according to Example 2 does not include second cleaning ST52. In the methods for recovering bedding powder according to Examples 3 to 6, second cleaning ST52, i.e., finishing cleaning, is ultrasonic cleaning. In Examples 3 and 6, the cleaning liquid 9a is replaced and first cleaning ST51 is performed multiple times. In Comparative Example 1, at least first cleaning ST51, which applies vibrations to the cleaning liquid, is not performed.
[0063] After washing the ceramic compact pieces, the BN powder was recovered and separated from the mixed liquid 11 containing the BN powder, ceramic powder, and sintering aid powder. The amount of BN powder applied to the ceramic test pieces and the amount of BN powder recovered were measured, and the recovery rate (%) of the powder was calculated using the following formula: Recovery rate (%) of powder = (amount of BN powder recovered / amount of BN powder applied) x 100. The results obtained using this formula are shown in Table 2, with a recovery rate of 60% or more and 100% or less designated as "A," a recovery rate of 40% or more and less than 60% designated as "B," and a recovery rate of less than 40% designated as "C."
[0064] [Table 2]
[0065] As shown in Table 2, in the bedding powder recovery methods of Examples 1 to 7, the effect of the first cleaning ST51 resulted in an improved bedding powder recovery rate of 40% or more. Furthermore, in the bedding powder recovery methods of Examples 3 to 6, the rough cleaning ST50 was performed, which further improved the bedding powder recovery rate to 60% or more. This demonstrates the effectiveness of rough cleaning. On the other hand, in contrast to Examples 1 to 7, Comparative Example 1 did not perform at least the first cleaning ST51, which vibrates the cleaning liquid, and therefore the bedding powder recovery rate was reduced to less than 40%.
[0066] Furthermore, when the BN bedding powder obtained by the bedding powder recovery method according to Examples 1 to 7 was reused in the manufacturing process of silicon nitride substrates and aluminum nitride substrates, the silicon nitride substrates and aluminum nitride substrates could be used without any problems, demonstrating that the BN bedding powder obtained by the bedding powder recovery method can be reused.
[0067] Furthermore, when the ceramic powders obtained by the BN bedding powder recovery method, i.e., silicon nitride powder, aluminum nitride powder, and sintering aid powder, were reused in the manufacturing process of silicon nitride substrates and aluminum nitride substrates, silicon nitride substrates and aluminum nitride substrates with equivalent strength, thermal conductivity, and insulation properties were obtained. Thus, it was demonstrated that the bedding powder recovery method according to Examples 1 to 7 is also effective for recovering and reusing ceramic powder.
[0068] According to at least one of the embodiments described above, the laying powder 4 can be separated from the ceramic powder of the mill waste 12, and the laying powder 4 can be recovered and reused.
[0069] Although several embodiments of the present invention have been described above, these embodiments are presented by way of example only and are not intended to limit the scope of the invention. These novel embodiments can be embodied in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the spirit of the invention. Modifications of these embodiments are included within the scope and spirit of the invention, as well as within the scope of the invention and its equivalents as set forth in the claims. Furthermore, the above-described embodiments can be implemented in combination with each other.
Claims
1. A method for recovering bedding powder, comprising: a cleaning step of applying vibration to a cleaning liquid to clean ceramic molded pieces to which bedding powder has adhered; and a recovery step of recovering at least the bedding powder from the mixed liquid produced in the cleaning step.
2. The method for recovering bedding powder according to claim 1, characterized in that the cleaning step includes ultrasonic cleaning.
3. The method for recovering bedding powder according to claim 2, characterized in that the cleaning step is a step of applying vibrations at an ultrasonic frequency of 10 kHz or more.
4. The method for recovering bedding powder according to claim 3, characterized in that the cleaning step further comprises washing with water after the ultrasonic cleaning.
5. The method for recovering bedding powder according to claim 3, characterized in that the cleaning step further includes rough cleaning for dismantling the ceramic molded pieces prior to the ultrasonic cleaning.
6. The method for recovering bedding powder according to claim 4, characterized in that the cleaning step further includes rough cleaning for dismantling the ceramic molded pieces prior to the ultrasonic cleaning.
7. A method for recovering the bedding powder according to claim 2, characterized in that the ceramic molded body pieces are scraps produced by cutting a sheet-like ceramic molded body to which the bedding powder is attached.
8. A method for recovering the bedding powder according to claim 6, characterized in that the ceramic molded body pieces are scraps produced by cutting a sheet-like ceramic molded body to which the bedding powder is attached.
9. The method for recovering bedding powder according to claim 1, characterized in that the bedding powder is boron nitride, and the ceramic molded body pieces are silicon nitride molded bodies.
10. The method for recovering bedding powder according to claim 2, characterized in that the bedding powder is boron nitride, and the ceramic molded body pieces are silicon nitride molded bodies.
11. The method for recovering bedding powder according to claim 8, characterized in that the bedding powder is boron nitride, and the ceramic molded body pieces are silicon nitride molded bodies.
12. A method for producing a ceramic sintered body, comprising: a powder application step of applying the powder obtained by the recovery method described in claim 1 onto the surface of a sheet-shaped ceramic body; a cutting step of cutting the sheet-shaped ceramic body after the powder application; and a sintering step of sintering the plate-shaped ceramic body after the cutting.
13. A method for producing a ceramic sintered body, comprising: a powder application step of applying the powder obtained by the recovery method described in claim 2 to the surface of a sheet-shaped ceramic body; a cutting step of cutting the sheet-shaped ceramic body after the powder application; and a sintering step of sintering the plate-shaped ceramic body after the cutting.
14. A method for producing a ceramic sintered body, comprising: a powder application step of applying the powder obtained by the recovery method described in claim 11 to the surface of a sheet-shaped ceramic body; a cutting step of cutting the sheet-shaped ceramic body after the powder application; and a sintering step of sintering the plate-shaped ceramic body after the cutting.
15. A method for producing a ceramic sintered body, characterized in that the recovery process comprises recovering ceramic powder in addition to the spreading powder, a forming process for forming a sheet-shaped ceramic body using the ceramic powder obtained by the recovery method described in claim 1, a spreading powder application process for applying the spreading powder to the sheet-shaped ceramic body, a cutting process for cutting the sheet-shaped ceramic body after the spreading powder application, and a sintering process for sintering the plate-shaped ceramic body after cutting.
16. A method for producing a ceramic sintered body, characterized in that the recovery step recovers ceramic powder in addition to the spreading powder, and comprises: a forming step of forming a sheet-shaped ceramic body using the ceramic powder obtained by the recovery method described in claim 2; a spreading powder application step of applying the spreading powder to the sheet-shaped ceramic body; a cutting step of cutting the sheet-shaped ceramic body after the spreading powder application; and a sintering step of sintering the plate-shaped ceramic body after cutting.
17. A method for producing a ceramic sintered body, characterized in that the recovery step recovers ceramic powder in addition to the spreading powder, and comprises: a forming step of forming a sheet-shaped ceramic body using the ceramic powder obtained by the recovery method described in claim 11; a spreading powder application step of applying the spreading powder to the sheet-shaped ceramic body; a cutting step of cutting the sheet-shaped ceramic body after the spreading powder application; and a sintering step of sintering the plate-shaped ceramic body after cutting.
18. The method for producing a ceramic sintered body according to any one of claims 12 to 17, characterized in that the ceramic sintered body is a ceramic substrate.
Citation Information
Patent Citations
Ceramic green sheet, ceramic sheet using the same, and manufacturing method thereof
JP3779481B2
Silicon nitride substrate and method for manufacturing a silicon nitride substrate
JP5673847B2
New cutting and separating method of ceramic blank
CN101712185A
Silicon fragment cleaning device
CN213728226U
Zirconia-base placing powder
JP1997157014A