Pellicle film and pellicle
By controlling the coefficient of variation of void diameters and distances in the carbon nanotube-based pellicle membrane, the issues of strength and EUV transmittance uniformity are addressed, resulting in improved performance and stability for EUV lithography applications.
Patent Information
- Application Number
- PCT/JP2024/011768
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Current pellicle membranes using carbon nanotubes for EUV lithography lack uniformity in pore characteristics, affecting their strength and EUV permeability, leading to variations in transmittance.
A pellicle membrane with a porous structure formed by carbon nanotubes, where the coefficient of variation of void diameters and distances between nearest centers of gravity is controlled within specific ranges to ensure uniformity, enhancing strength and reducing EUV transmittance variations.
The controlled pore characteristics improve the strength of the pellicle membrane and stabilize EUV transmittance, reducing variations and enhancing the membrane's performance in EUV lithography.
Smart Images

Figure JP2024011768_03102024_PF_FP_ABST
Abstract
Description
Pellicle membrane and pellicle
[0001] The present invention relates to a pellicle membrane and a pellicle.
[0002] In a manufacturing process of a semiconductor device or the like, for example, a photoresist is applied to a substrate such as a semiconductor wafer, and the substrate with the photoresist applied is irradiated with light using a photomask, and the photoresist is removed, thereby forming a desired circuit pattern on the substrate.
[0003] When a photomask is irradiated with light while foreign matter is attached to it, the attached foreign matter may interfere with the circuit pattern formed on the substrate. For this reason, a pellicle equipped with a pellicle film for capturing foreign matter may be used to prevent foreign matter from adhering to the photomask. The pellicle is placed above the photomask at a distance such that the pellicle film does not come into contact with the photomask.
[0004] In recent years, the use of extreme ultraviolet (EUV) has been considered in order to form finer circuit patterns. EUV refers to light with a wavelength of 1 nm or more and 100 nm or less. Specifically, light rays of approximately 13.5 nm±0.3 nm are beginning to be used as EUV. When EUV is irradiated onto a pellicle film, the EUV passes through the pellicle film, but a portion of the irradiated EUV is absorbed by the pellicle film. The absorbed EUV light energy is converted into thermal energy, causing the temperature of the pellicle film to rise. For this reason, pellicle films are required to have EUV transmittance, heat resistance, durability, etc.
[0005] Carbon nanotubes are being considered as one of the materials to be used for the pellicle film of a pellicle used in a process of forming a circuit pattern using EUV.
[0006] For example, Patent Document 1 discloses a pellicle film containing carbon nanotubes, at least on the surface side of which contains a silicon carbide layer in which at least a portion of carbon has been replaced with silicon.
[0007] International Publication No. 2021-172104
[0008] The pellicle film containing carbon nanotubes disclosed in Patent Document 1 is said to have excellent strength and EUV transmittance. However, the pellicle film disclosed in Patent Document 1 does not mention variations in void characteristics on the surface of the pellicle film. Variations in void characteristics are likely to affect the strength and EUV transmittance of the pellicle film, and further improvements in pellicle films have been required.
[0009] The present invention provides a pellicle film containing carbon nanotubes, which has improved strength and reduced variation in EUV transmittance, and a pellicle using the pellicle film.
[0010] [1] A pellicle membrane having a porous structure, the pellicle membrane containing carbon nanotubes, wherein the coefficient of variation of the pore diameter of pores measured on the surface of the porous structure is 0.7 or less, and the coefficient of variation of the distance between nearest centroids of the pores is 0.6 or less.
[0011] [2] The pellicle membrane according to [1], wherein the coefficient of variation of the pore diameter is 0.4 or more and 0.7 or less.
[0012] [3] The pellicle membrane according to [1] or [2], wherein the coefficient of variation of the distance between the nearest centers of gravity is 0.2 or more and 0.5 or less.
[0013] [4] The pellicle membrane according to any one of [1] to [3], wherein the length of the carbon nanotubes is 0.1 μm or more and 1000 μm or less.
[0014] [5] The pellicle membrane according to any one of [1] to [4], wherein the cross-sectional diameter of the carbon nanotubes is 0.2 nm or more and 50 nm or less.
[0015] [6] The pellicle membrane according to any one of [1] to [5], wherein the average pore diameter is 20 nm or more and 60 nm or less.
[0016] [7] The pellicle membrane according to any one of [1] to [6], wherein the pellicle membrane is a porous structure formed by depositing the carbon nanotubes.
[0017] [8] The pellicle membrane according to any one of [1] to [7], which is self-supporting.
[0018] [9] A pellicle comprising: the pellicle membrane according to any one of [1] to [8]; and a support having a frame and an opening surrounded by the frame, and supporting the pellicle membrane.
[0019] According to one aspect of the present invention, it is possible to provide a pellicle film containing carbon nanotubes, which has improved strength and reduced variation in EUV transmittance, and a pellicle using the pellicle film.
[0020] Fig. 1 is a plan view schematically showing an example of a pellicle according to the present embodiment. Fig. 2 is a cross-sectional view showing the II-II cross section of Fig. 1. Fig. 3 is a plan view schematically showing a pellicle for evaluating the strength of a pellicle film. Fig. 4 is a side view schematically showing a pellicle for evaluating the strength of a pellicle film. Fig. 5 is an explanatory view schematically showing the strength evaluation of a pellicle film.
[0021] The pellicle membrane according to the present embodiment has a porous structure. The pellicle membrane contains carbon nanotubes, and the coefficient of variation of the pore diameter of the pores measured on the surface of the porous structure is 0.7 or less, and the coefficient of variation of the distance between nearest centroids of the pores is 0.6 or less.
[0022] The pellicle membrane according to the present embodiment, having the above-described configuration, is believed to have voids that are nearly uniform. Therefore, it is believed that the pellicle membrane suppresses variations in strength and suppresses variations in the in-plane characteristics of transmitted light that passes through the pellicle membrane. As a result, the pellicle membrane according to the present embodiment is believed to improve the strength of the pellicle membrane and suppress variations in EUV transmittance.
[0023] There are no particular limitations on the means for adjusting the pellicle membrane so that the coefficient of variation of the pore diameter of the pores measured on the surface of the porous structure is 0.7 or less and the coefficient of variation of the distance between nearest centers of gravity of the pores is 0.6 or less. Examples of such means include, in an example of a preferred method for producing a pellicle membrane described below, a means for adjusting the amount of carbon nanotubes contained in the pellicle membrane (for example, the amount of carbon nanotubes contained in a carbon nanotube film that is an intermediate product when forming the pellicle membrane, or the amount of carbon nanotubes in a carbon nanotube dispersion when forming a carbon nanotube film) and the dispersion strength of the carbon nanotubes.
[0024] The carbon nanotubes contained in the pellicle film according to this embodiment are not particularly limited, and are preferably at least one type selected from the group consisting of multi-walled carbon nanotubes (MWCNT: Multi-Walled Carbon Nanotubes), few-walled carbon nanotubes (FWCNT: Few-Walled Carbon Nanotubes), double-walled carbon nanotubes (DWCNT: Double-Walled Carbon Nanotubes), and single-walled carbon nanotubes (SWCNTS: Single-Walled Carbon Nanotubes).
[0025] Carbon nanotubes can be obtained by known manufacturing methods such as arc discharge, laser ablation, and chemical vapor deposition.
[0026] The length of the carbon nanotubes is, for example, preferably 0.1 μm or more and 1000 μm or less, more preferably 0.5 μm or more, and even more preferably 1 μm or more, and more preferably 600 μm or less, and even more preferably 400 μm or less.
[0027] The cross-sectional diameter of the carbon nanotube is preferably 0.2 nm or more and 50 nm or less. The cross-sectional diameter of the carbon nanotube is more preferably 0.5 nm or more, and even more preferably 1 nm or more. The cross-sectional diameter of the carbon nanotube is more preferably 30 nm or less, and even more preferably 20 nm or less. In this specification, the cross-sectional diameter may be simply referred to as the diameter.
[0028] The pellicle membrane according to this embodiment has a coefficient of variation of pore diameters measured on the surface of the porous structure of 0.7 or less. From the viewpoint of further improving the strength of the pellicle membrane and further suppressing variations in EUV transmittance, the coefficient of variation of pore diameters is preferably 0.68 or less, and more preferably 0.67 or less. The lower limit of the coefficient of variation of pore diameters is not particularly limited, and may be, for example, 0.40 or more, or 0.42 or more.
[0029] In this specification, the void diameter means the diameter of a hypothetical circle having the same area as the void area (i.e., the equivalent circle diameter). 1 ) is the average value of the pore diameter (D 1 [unit: nm]) and standard deviation (σ 1 [unit: nm]) and the coefficient of variation of the pore diameter can be calculated based on the following formula (Formula 1): 1 = σ 1 / D 1 ...(Equation 1)
[0030] In the pellicle membrane according to the present embodiment, the coefficient of variation of the distance between nearest centroids of voids in the voids measured on the surface of the porous structure is 0.6 or less. From the viewpoint of further improving the strength of the pellicle membrane and further suppressing variations in EUV transmittance, the coefficient of variation of the distance between nearest centroids is preferably 0.5 or less, more preferably 0.45 or less, and even more preferably 0.43 or less. The lower limit of the coefficient of variation of the distance between nearest centroids is not particularly limited and may be, for example, 0.2 or more or 0.25 or more.
[0031] In this specification, the distance between the nearest centroids of voids is the distance between the centroid of one void and the centroid of the void closest to that void. In other words, it means the distance from the centroid of one void to the centroid of the other void between adjacent voids. The coefficient of variation (CV) of the distance between the nearest centroids of voids is 2 ) is the average distance between the nearest centroids of the gap (D 2 [unit: nm]) and standard deviation (σ 2 [unit: nm]) and the coefficient of variation of the distance between the nearest centers of gravity of the gap can be calculated based on the following formula (Formula 2): 2 = σ 2 / D 2 ...(Equation 2)
[0032] The pellicle membrane of this embodiment may, for example, have a coefficient of variation of the pore diameter of the pores measured on the surface of the porous structure of 0.4 or more and 0.7 or less, and may have a coefficient of variation of the distance between nearest centers of gravity of the pores of 0.2 or more and 0.6 or less.
[0033] From the viewpoint of further improving the strength of the pellicle membrane and further suppressing variations in EUV transmittance, the average pore diameter of the pores measured on the surface of the porous structure of the pellicle membrane may be, for example, 20 nm or more and 60 nm or less. The average pore diameter may be 25 nm or more, or 30 nm or more. The average pore diameter may be 55 nm or less, or 50 nm or less.
[0034] From the viewpoint of further improving the strength of the pellicle membrane and further suppressing variations in EUV transmittance, the average value of the distance between nearest centroids of voids measured on the surface of the porous structure of the pellicle membrane is preferably, for example, 40 nm or more and 95 nm or less. The average value of the distance between nearest centroids may be 50 nm or more, or may be 55 nm or more. The average value of the distance between nearest centroids may be 80 nm or less, 68 nm or less, or 67 nm or less.
[0035] In the void characteristics measured on the surface of the porous structure of a pellicle membrane, the void characteristics of the average void diameter and the coefficient of variation of the void diameter, as well as the average distance between nearest centroids of the voids and the coefficient of variation of the distance between nearest centroids of the voids, may be measured by a method including the following steps (1) to (10). By adopting the measurement method described below, a unique threshold value is determined, making it easier to obtain plausible results, for example, regardless of the measurer. The method for measuring the void characteristics is specifically as shown in the examples described below.
[0036] (1) A step of preparing a pellicle membrane. (2) A step of imaging the surface of the prepared pellicle membrane to obtain image data of the pellicle membrane. (3) A step of setting three or more different thresholds as initial thresholds at equal intervals within a range from a first pixel value to a second pixel value greater than the first pixel value for the image data, performing binarization processing based on each of the initial thresholds, and obtaining binarized image data based on the initial thresholds. (4) A step of performing blob analysis on the binarized image data based on the initial thresholds to obtain initial measured values that calculate the distribution of void characteristics of voids on the surface of the pellicle membrane. (5) A step of calculating initial theoretical values of the distribution of void characteristics calculated using a log-normal probability density function based on the initial measured values. (6) A step of calculating the error between the initial measured values and the initial theoretical values. (7) If the error between the initial measured value and the initial theoretical value is not smallest, the threshold is reset, the image data is binarized based on the reset threshold, binarization processing is performed on the image data based on the reset threshold, and the binarized image data based on the reset threshold is subjected to blob analysis to obtain a remeasurement measured value that calculates the distribution of void characteristics of voids on the surface of the pellicle membrane. (8) Based on the remeasurement measured value, an error is calculated between the remeasurement measured value and a theoretical value of the distribution of void characteristics calculated using a log-normal distribution probability density function. (9) If the error between the remeasurement measured value and the theoretical value is not smallest, the steps of obtaining the remeasurement measured value and calculating the error between the remeasurement measured value and the theoretical value are repeated until the error between the remeasurement measured value and the theoretical value is smallest. (10) A step of obtaining the distribution of void characteristics calculated based on the threshold value when the error between the initial measured value and the initial theoretical value, or the error between the re-measured measured value and the re-measured theoretical value, is smallest as the final measured value.
[0037] The threshold value at which the error is minimized is preferably determined by using various known optimization algorithms. For example, in steps (4) to (9) above, it is preferable to use various known optimization algorithms to search for the threshold value at which the error is minimized. In this case, after the initial threshold value is determined, a unique threshold value is determined by using the optimization algorithm.
[0038] In the step of acquiring the binarized image data based on the initial thresholds, the initial thresholds are not limited to the above. Five or more different thresholds may be set at equal intervals within a range from a first pixel value to a second pixel value greater than the first pixel value, or seven or more different thresholds may be set. The interval between the first pixel value and the second pixel value is preferably 100 or more. The first pixel value is preferably set in the range of 20 to 50. The second pixel value is preferably set in the range of 150 to 240. "Equal intervals" refers to the equal intervals between adjacent thresholds, such as when n thresholds are set as the three or more different thresholds, the interval between the nth threshold and the n-1th threshold and the interval between the n-1th threshold and the n-2th threshold are equal. Specifically, the initial thresholds may be set as a plurality of equal intervals within a range from a pixel value of 20 to a pixel value of 240, with an interval of 3 to 12. In the step of obtaining the actual value of the remeasurement, the threshold value that is reset is not three or more different threshold values, but a single threshold value.
[0039] The void characteristics may be measured, for example, by an apparatus having a program that causes a computer to execute the above steps (1) to (10). The program may be recorded on a recording medium.
[0040] The thickness of the pellicle film is preferably 3 nm or more and 1000 nm or less. The thickness of the pellicle film is preferably 10 nm or more, and more preferably 20 nm or more. The thickness of the pellicle film is preferably 500 nm or less, and more preferably 300 nm or less. If the thickness of the pellicle film is, for example, 3 nm or more and 1000 nm or less, the strength of the pellicle film is further improved and variations in EUV transmittance are more easily suppressed. In addition, the operability of the pellicle film is improved.
[0041] The weight per unit area of the pellicle membrane is not particularly limited, and is, for example, 0.1 μg / cm 2 Above, 20μg / cm 2 The weight per unit area of the pellicle membrane is preferably 0.5 μg / cm or less. 2 More preferably, it is 1 μg / cm or more. 2 The weight per unit area of the pellicle membrane is more preferably 15 μg / cm or more. 2 More preferably, it is 10 μg / cm or less. 2 It is more preferable that the weight per unit area of the pellicle membrane is, for example, 0.1 μg / cm or less. 2 Above, 20μg / cm 2 If it is below this value, the strength of the pellicle film is further improved and variations in EUV transmittance are more easily suppressed.
[0042] The pellicle membrane according to this embodiment is preferably a porous structure formed by the deposition of carbon nanotubes. The porous structure formed by the deposition of carbon nanotubes can be manufactured by an example of a preferred method for manufacturing a pellicle membrane, which will be described later. If the pellicle membrane is a porous structure formed by the deposition of carbon nanotubes, the strength of the pellicle membrane is further improved, and variations in EUV transmittance are more easily suppressed.
[0043] The pellicle film according to the present embodiment is preferably self-supporting from the viewpoint of improving transparency to exposure light. The term "self-supporting" refers to a film that is self-supporting by itself, and indicates that the pellicle film is a film that has self-supporting properties (also referred to as a self-supporting film). In other words, a self-supporting pellicle film is a film that can maintain its shape by itself, even without the presence of a substrate or the like.
[0044] (Method for manufacturing a pellicle membrane) The method for manufacturing a pellicle membrane is not particularly limited. An example of a preferred method for manufacturing a pellicle membrane includes, for example, a step of dispersing carbon nanotubes (step P1), a step of precipitating and depositing the dispersed carbon nanotubes on an air-permeable member to obtain a carbon nanotube film formed in a mat shape on the air-permeable member (step P2), and a step of removing the air-permeable member from the carbon nanotube film to obtain a pellicle membrane (step P3).
[0045] First, in step P1, carbon nanotubes are dispersed in a liquid as a dispersion medium to prepare a carbon nanotube dispersion in which carbon nanotubes are dispersed in the liquid. The liquid may be a liquid containing water. The carbon nanotube dispersion may contain only carbon nanotubes as a dispersoid. The carbon nanotube dispersion may contain, in addition to carbon nanotubes, various additives such as dispersants that disperse the carbon nanotubes.
[0046] For example, by adjusting the balance between the dispersion strength when dispersing carbon nanotubes in a liquid in step P1 and the weight per unit area of carbon nanotubes when producing a carbon nanotube film in step P2, it becomes easier to obtain a pellicle film having a void diameter coefficient of variation of 0.7 or less and a void gap distance coefficient of variation of 0.6 or less. Specifically, for example, if the weight per unit area of the carbon nanotubes is at least a certain amount, the void diameter coefficient of variation tends to be in the range of 0.7 or less, while if the weight per unit area of the carbon nanotubes is reduced too much, the void diameter coefficient of variation tends to exceed 0.7. Furthermore, for example, if the dispersion strength is kept within a certain range, the void gap distance coefficient of variation tends to be in the range of 0.6 or less, while if the dispersion strength is increased too much, the void gap distance coefficient of variation tends to exceed 0.6.
[0047] The weight per unit area of the carbon nanotubes and the dispersion strength are, for example, 0.1 μg / cm 3 as the amount of carbon nanotubes contained in the carbon nanotube film produced in step P2. 2 Above, 20μg / cm 2 Furthermore, when a stirrer is used as a disperser for dispersing carbon nanotubes, the dispersion strength may be, for example, in the range of 10 m / s or more and 60 m / s or less as the peripheral speed of the stirrer, and the stirring time of the stirrer may be, for example, in the range of 5 minutes or more and 60 minutes or less.
[0048] Next, in step P2, the dispersed carbon nanotubes are precipitated and deposited on an air-permeable member. For example, the carbon nanotube dispersion prepared in step P1 is filtered through a filter membrane as an air-permeable member, causing the carbon nanotubes to precipitate and deposit, forming a mat-like carbon nanotube film on the filter membrane. The filter membrane is preferably, for example, a membrane filter.
[0049] Next, in step P3, the filtration membrane is removed from the mat-shaped carbon nanotube membrane to obtain a pellicle membrane containing carbon nanotubes. A drying step may be performed, if necessary, before or after removing the filtration membrane from the mat-shaped fiber membrane. The obtained pellicle membrane is a free-standing membrane.
[0050] (Pellicle) The pellicle according to this embodiment includes the pellicle membrane according to the embodiment described above, and a support that has a frame and an opening surrounded by the frame and supports the pellicle membrane.
[0051] The pellicle according to the present embodiment will be described below with reference to the drawings. Note that in the drawings in this specification, some parts are illustrated enlarged or reduced in size for ease of explanation.
[0052] FIG. 1 shows a plan view of a pellicle 100 viewed from the surface on which the pellicle membrane 10 is installed, and FIG. 2 shows a cross-sectional view of the pellicle 100 shown in FIG. 1. The pellicle 100 comprises a pellicle membrane 10 and a support 30 that supports the pellicle membrane 10. The support 30 comprises a frame 31 and an opening 32 surrounded by the frame 31, with the opening 32 penetrating from one surface of the support 30 to the other. The frame 31 and the opening 32 are both rectangular, and all four corners of the outer shape of the frame 31 are rounded. The frame 31 comprises a support surface 33 facing the pellicle membrane 10. The pellicle membrane 10 is rectangular, and comprises a first pellicle membrane surface 11 facing the support surface 33 of the support 30 and a second pellicle membrane surface 12 opposite the first pellicle membrane surface 11. The pellicle membrane 10 has its peripheral edge 13 fixed to a part of the support surface 33 of the frame 31 , and covers the opening 32 of the support 30 .
[0053] The pellicle membrane according to the present embodiment described above is used as the pellicle membrane 10. Examples of materials that can be used for the support 30 include resin materials (polyethylene, etc.), metal materials (aluminum, aluminum alloys, magnesium alloys, stainless steel, titanium, etc.), ceramic materials (SiC, etc.), and fiber-reinforced plastic materials (carbon fiber-reinforced plastic, etc.).
[0054] In addition, in order to clarify the positional relationship between the surface of the pellicle film 10 facing the support surface 33 of the support 30 and the surface on the opposite side thereof, the terms first pellicle film surface 11 and second pellicle film surface 12 are used for convenience. Therefore, in some cases, the first pellicle film surface 11 and the second pellicle film surface 12 can be used interchangeably, and the first pellicle film surface 11 and the second pellicle film surface 12 can be used interchangeably.
[0055] While an example of a pellicle according to the present embodiment has been described above with reference to Figures 1 and 2, the pellicle according to the present embodiment is not limited to this. The pellicle according to the present embodiment may adopt various forms as long as the effects of the pellicle using the pellicle membrane according to the present embodiment described above can be obtained. The shape and dimensions of each part of each component constituting the pellicle according to the present embodiment may be determined, for example, according to the dimensions of the photomask (not shown) when the pellicle according to the present embodiment is used.
[0056] For example, the pellicle membrane 10 and the support 30 of the pellicle 100 shown in Figures 1 and 2 are both formed in a rectangular shape. The pellicle according to this embodiment is not limited to this, and may be formed in any desired shape, such as a circle, an ellipse, or a polygon.
[0057] 1 and 2, for example, the peripheral edge 13 of the pellicle membrane 10 is fixed to a portion of the support surface 33 of the support body 30. The pellicle 100 is not limited to this, and the peripheral edge 13 of the pellicle membrane 10 may be fixed to the entire surface of the support surface 33 of the support body.
[0058] 1 and 2, the pellicle membrane 10 and the support 30 may be fixed by providing an adhesive layer (not shown). The adhesive layer is a layer that is provided as needed. The material constituting the adhesive layer is not particularly limited, and may be, for example, various adhesives such as acrylic resin, epoxy resin, silicone resin, polyimide resin, and fluororesin, as well as carbon nanotubes.
[0059] (Method for Manufacturing a Pellicle) An example of a preferred method for manufacturing a pellicle according to the present embodiment includes the steps of: preparing a pellicle membrane according to the present embodiment; preparing a support having a frame and an opening surrounded by the frame and supporting the pellicle membrane; and providing the pellicle membrane on the support so as to cover the opening and be supported by the support surface of the frame. The manufacturing method may optionally include the step of providing an adhesive layer on at least a portion of the support surface of the frame.
[0060] The step of preparing a pellicle membrane according to this embodiment may involve preparing a pellicle membrane according to the above-described embodiment. The step of preparing a support may involve preparing a support formed into the desired shape using the material constituting the support described above by a known method. The step of providing a pellicle membrane may involve covering the opening and installing the pellicle membrane by a known method so that it is supported by the support surface of the frame. When an adhesive layer is provided on at least a portion of the support surface of the frame, the pellicle membrane is installed so that it is supported by the support surface of the frame via the adhesive layer. When various adhesives are used for the adhesive layer, the step of providing the adhesive layer involves applying an adhesive to the support surface to provide an adhesive-containing adhesive layer. When carbon nanotubes are used for the adhesive layer, the step of providing the adhesive layer involves, for example, applying a carbon nanotube dispersion to the support surface and drying it to provide an adhesive layer containing carbon nanotubes.
[0061] The pellicle according to this embodiment is used, for example, by being placed above the photomask at a distance from the photomask so that the first pellicle film surface faces the photomask. By using the pellicle according to this embodiment, adhesion of foreign matter to the photomask is suppressed and variations in EUV transmittance are suppressed. Furthermore, since the pellicle film according to this embodiment has improved strength, breakage during installation and transportation of the pellicle is suppressed.
[0062] The present invention is not limited to the above-described embodiment, and includes modifications and improvements within the scope of achieving the object of the present invention.
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0064] [Example 1] <Preparation of Pellicle Film> Carbon nanotubes (hereinafter referred to as CNT) having a diameter of 0.2 nm or more and 50 nm or less and a length of 1 μm or more and 250 μm or less were prepared. The prepared CNTs were weighed so that the concentration of the CNTs in the aqueous dispersion was 0.02 mass%. In addition, carboxymethyl cellulose (hereinafter referred to as CMC) was weighed as a dispersant so that the concentration in the aqueous dispersion was 0.2 mass%. The weighed CNTs and weighed CMC were put into water, and the CNTs were dispersed in water using a thin film rotary high-speed mixer (manufactured by Primix Corporation, product name "Filmix") at a peripheral speed of 40 m / s for a dispersion time of 10 minutes, thereby preparing an aqueous dispersion of CNTs. The shear rate when dispersing the CNTs was approximately 4.0 × 10 5 s -1 Next, the aqueous dispersion of CNT was diluted so that the CNT concentration was 1 ppm. Then, the mass of CNT contained in the pellicle membrane (referred to as the mass in the CNT membrane in Table 1) was 0.88 μg / cm 2The diluted CNT aqueous dispersion was placed in a filter so that the CNT concentration was 0.01%. Next, the CNT aqueous dispersion placed in the filter was filtered through a membrane filter to form a mat-like CNT film on the membrane filter. The mat-like CNT film was then peeled off from the membrane filter to produce a pellicle film containing CNT. The pellicle film was a self-supporting film. From the obtained pellicle film, the coefficient of variation of the pore size, the average value of the pore size, the coefficient of variation of the distance between the nearest centers of gravity of the pores, and the average value of the distance between the nearest centers of gravity of the pores were calculated according to the pore analysis of the pellicle film described below.
[0065] <Analysis of voids in pellicle membrane> The surface of the pellicle membrane obtained in each example was observed with a scanning electron microscope (SEM) (CrossBeam 550, manufactured by Carl Zeiss), and image data of the SEM image was obtained. The imaging conditions were an acceleration voltage of 1 kV and a magnification of 10,000 times. The field of view was three or more fields of view.
[0066] From the image data of the obtained SEM image, the pore diameter (pore size) was analyzed as a circle equivalent diameter. First, for one field of view of the image data of the SEM image, the initial binarization threshold was set at seven values: 40, 60, 80, 100, 120, 140, and 160, at equal intervals of 20 pixel values between the pixel value 40 and the pixel value 160, and seven binarized processed image data were obtained at each binarization threshold. This operation was performed on image data of three or more fields of view. Next, the initial pore diameter distribution based on the initial binarization threshold was measured for the obtained binarized processed image data. Then, by fitting using Bayesian optimization so that the measured value of the pore diameter distribution closely approximates (fits) a log-normal distribution, a binarization threshold that minimizes the error between the measured value of the pore diameter distribution and the theoretical value of the pore diameter distribution was automatically searched for. The coefficient of variation of the void diameter and the coefficient of variation of the distance between the nearest centers of gravity of the voids were calculated from the void diameter distribution and the distribution of the distance between the nearest centers of gravity of the voids measured based on the binarization threshold when the error between the actual measured value of the void diameter distribution and the theoretical value of the void diameter distribution was minimized.
[0067] <Evaluation of pellicle membrane strength> An acrylic plate measuring 2 cm × 5 cm and 2 mm thick was prepared as a support. A frame-shaped opening measuring 1 cm × 1 cm was provided near the center of one end of the acrylic plate, penetrating the acrylic plate. The area extending from the opening outward to 5 mm from the outer periphery of the opening served as a support surface, and double-sided adhesive tape was attached to the entire support surface. The peripheral portion of the pellicle membrane obtained in each example was attached and fixed on the adhesive tape so as to cover the opening, thereby producing a pellicle for evaluating the strength of the pellicle membrane (see Figures 3A and 3B).
[0068] Here, the strength evaluation of a pellicle film will be described with reference to Figures 3A, 3B, and 4. Figure 3A is a schematic plan view of a pellicle WK for strength evaluation of a pellicle film (hereinafter referred to as the strength evaluation pellicle WK) as viewed from the pellicle film 10W. Figure 3B is a schematic side view of the strength evaluation pellicle WK as viewed from the longitudinal direction. The strength evaluation pellicle WK is the pellicle for strength evaluation of a pellicle film prepared as described above. The strength evaluation pellicle WK has an opening 32W penetrating the support 30W on the first end E1 side of the support 30W. Double-sided adhesive tape is disposed as an adhesive layer 20W in the outer region of the opening 32W. The pellicle film 10W is attached so that the adhesive layer 20W contacts the peripheral edge of the pellicle film 10W. The pellicle film 10W is attached to the support 30W via an adhesive layer 20W so as to cover the opening 32W.
[0069] The evaluation method was performed using the following procedure. FIG. 4 schematically illustrates a method for evaluating the strength of a pellicle film using a strength evaluation pellicle WK, showing the strength evaluation pellicle WK viewed from the longitudinal side. As shown in FIG. 4, first, the strength evaluation pellicle WK was placed on a horizontal table T. A stopper S was placed so as to contact the second end E2 side of the strength evaluation pellicle WK. Next, while preventing the second end E2 side of the strength evaluation pellicle WK from slipping, the first end E1 side was lifted, and a plate-like member B having a thickness of 1 mm was sandwiched between the table T and the strength evaluation pellicle WK. Next, the plate-like member B was removed in the horizontal direction H, and the strength evaluation pellicle WK was dropped. After dropping the strength evaluation pellicle WK, the presence or absence of damage to the pellicle film 10W was visually confirmed. If no damage was found, 1 mm thick plate-like members B were stacked, two plate-like members B were sandwiched between them, and the two plate-like members B were removed in the horizontal direction H, and the strength evaluation pellicle WK was dropped. This operation was repeated until damage occurred to the pellicle membrane 10W, and the maximum height when no damage occurred to the pellicle membrane 10W was evaluated as the strength of the pellicle membrane 10W. Note that this maximum height corresponds to the maximum number of plate-like members B when 1 mm thick plate-like members B are stacked. The strength evaluation of the pellicle membrane 10W was performed three times using the above procedure, and the average value of the three measurements was used.
[0070] <Evaluation of transmittance at a wavelength of 550 nm> For the pellicles obtained in each example, the light transmittance from wavelengths of 200 nm to 800 nm was measured using an ultraviolet-visible-near-infrared spectrophotometer (manufactured by Shimadzu Corporation, product name "UV-VIS-NIR SPECTROPHOTOMETER UV-3600"), and the light transmittance (%) at a wavelength of 550 nm was extracted. The measurement was performed using the attached large sample chamber MPC-3100, without using the built-in integrating sphere. The light transmittance at a wavelength of 550 nm was measured at the center of each of six pellicles produced under the same conditions, and the average value was calculated.
[0071] It is known that there is a correlation between the transmittance of a pellicle film containing CNTs at a wavelength of 13.5 nm and that at a wavelength of 550 nm (see, for example, Figure 4(a) of Marina, Y, et al. “CNT EUV pellicle tunability and performance in a scanner-like environment,” Proc. SPIE 11609, Extreme Ultraviolet (EUV) Lithography XII, 116090Y, (23 March 2021). Figure 4(a). ; doi: 10.1117 / 12.2584519). Therefore, by evaluating the variation in the transmittance at a wavelength of 550 nm, it is possible to evaluate the variation in the transmittance at a wavelength of 13.5 nm (i.e., the variation in EUV transmittance). If the light transmittance at a wavelength of 550 nm is 85% or more, it is easy to ensure, for example, a high EUV transmittance (for example, an EUV transmittance of 94% or more).
[0072] [Examples 2 to 7 and Comparative Examples 1 to 4] Pellicle films were prepared in the same manner as in Example 1, except that the dispersion strength and the mass of CNTs contained in the pellicle film (mass within the CNT film) were changed according to Table 1, and void analysis of the pellicle film, strength evaluation of the pellicle film, and transmittance evaluation at a wavelength of 550 nm were performed.
[0073]
[0074] From the above results, it can be seen that pellicle membranes having a void diameter coefficient of variation of 0.7 or less and a void gap distance coefficient of variation of 0.6 or less have excellent evaluation results for pellicle membrane strength and transmittance at a wavelength of 550 nm. Therefore, according to one embodiment of the present invention, a pellicle membrane having improved pellicle membrane strength and reduced variation in EUV transmittance, and a pellicle using said pellicle membrane are provided.
[0075] 10, 10W... pellicle film, 11... first pellicle film surface, 12... second pellicle film surface, 13... peripheral portion, 20W... adhesive layer, 30, 30W... support, 31... frame portion, 32, 32W... opening, 33... support surface, 100... pellicle, WK... pellicle for strength evaluation.
Claims
1. A pellicle membrane having a porous structure, the pellicle membrane comprising carbon nanotubes, the coefficient of variation of the pore diameter of the pores measured on the surface of the porous structure being 0.7 or less, and the coefficient of variation of the distance between nearest center of gravity of the pores being 0.6 or less.
2. A pellicle membrane according to claim 1, wherein the coefficient of variation of the pore size is 0.4 or more and 0.7 or less.
3. A pellicle membrane according to claim 1 or 2, wherein the coefficient of variation of the distance between the nearest centers of gravity is 0.2 or more and 0.5 or less.
4. A pellicle membrane according to claim 1 or 2, wherein the length of the carbon nanotubes is 0.1 μm or more and 1000 μm or less.
5. A pellicle membrane according to claim 1 or 2, wherein the cross-sectional diameter of the carbon nanotubes is 0.2 nm or more and 50 nm or less.
6. A pellicle membrane according to claim 1 or 2, wherein the average pore size is 20 nm or more and 60 nm or less.
7. A pellicle membrane according to claim 1 or 2, wherein the pellicle membrane is a porous structure formed by depositing the carbon nanotubes.
8. The pellicle membrane according to claim 1 or 2, which is self-supporting.
9. A pellicle comprising: a pellicle membrane according to claim 1 or 2; and a support having a frame and an opening surrounded by the frame, the support supporting the pellicle membrane.
Citation Information
Patent Citations
Pellicle film, pellicle, original plate for exposure, exposure device, method for producing pellicle, and method for producing semiconductor device
WO2021172104A1
Method for forming pellicle
JP2018194838A
Films of a mixture of multi-walled, few-walled, and single-walled carbon nanotubes
JP2022534476A
Treatment of nanofiber filtration films and soluble substrates
JP2022553694A
Pellicle film, and pellicle
WO2014142125A1