Aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, production method therefor, and method for producing active material for lithium secondary battery

The use of an aqueous solution with niobium polyacid, lithium, and phosphate ions for coating the positive electrode active material in lithium ion batteries addresses the interfacial resistance and stability issues, resulting in improved performance and storage stability for all-solid-state batteries by forming a stable and non-porous lithium niobate layer.

WO2024204115A1PCT designated stage expired Publication Date: 2024-10-03DOWA HOLDINGS CO LTD

Patent Information

Application Number
PCT/JP2024/011789
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

All-solid-state lithium ion secondary batteries face issues with increased interfacial resistance and capacity deterioration due to the formation of high resistance sites on the positive electrode active material surface, which is exacerbated by the reaction between the positive electrode active material and the solid electrolyte, and existing coating techniques using volatile organic compounds and unstable peroxo complexes are costly and chemically unstable.

Method used

An aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions is used to coat the positive electrode active material, with a specific molar ratio of phosphorus to the sum of niobium and lithium, and hydrogen peroxide, to form a stable lithium niobate coating layer that suppresses the increase in specific surface area and improves storage stability.

Benefits of technology

The proposed method achieves excellent storage stability and reduces interfacial resistance, thereby enhancing the performance of all-solid-state lithium ion secondary batteries by forming a non-porous lithium niobate coating layer with improved ionic conductivity and chemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011789_03102024_PF_FP_ABST
    Figure JP2024011789_03102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide an aqueous solution and a production method therefor, the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, suppressing an increase in the specific surface area of a coated positive electrode active material when the surfaces of positive electrode active material particles of a lithium-ion secondary battery are coated with a coating layer containing niobium, lithium, and phosphorus, which are solid electrolytes, and having excellent storage stability. [Solution] This aqueous solution contains niobium polyacid ions, lithium ions, and phosphate ions, wherein: the ratio P / (Nb+Li+P) of the molar number of the phosphorus to the sum of the molar numbers of the niobium, lithium, and phosphorus contained in the aqueous solution is at least 0.04 and less than 0.5; the molar ratio Li / Nb of the lithium and the niobium is greater than 0.6 and at most 2.0; and 0.01-10 mass% of hydrogen peroxide is preferably further contained.
Need to check novelty before this filing date? Find Prior Art

Description

Aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, method for producing the same, and method for producing active material for lithium secondary batteries

[0001] The present invention relates to an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions for coating the surfaces of positive electrode active material particles of a lithium ion secondary battery with lithium niobate as a solid electrolyte, a method for producing the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, and a method for producing an active material for a lithium secondary battery having a coating layer containing lithium niobate.

[0002] The positive electrode active material of lithium-ion secondary batteries has generally been composed of a composite oxide of lithium and a transition metal. Among them, lithium cobalt oxide (LiCoO), which is a composite oxide containing Co as a component, has been particularly popular. 2 ) is widely used. Recently, lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 ), or ternary (LiNi 1/3 Mn 1/3 Co 1/3 O 2 The use of these types of devices and their combinations is also increasing.

[0003] The electrolyte for lithium ion secondary batteries is LiPF 6 , LiBF 4 These electrolytes are primarily composed of lithium salts such as those listed above dissolved in a mixed solvent of a cyclic carbonate ester such as PC (propylene carbonate) or EC (ethylene carbonate) and a chain ester such as DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), or DEC (diethyl carbonate). Such organic solvents are vulnerable to oxidative atmospheres and are prone to oxidative decomposition reactions, particularly when they come into contact with transition metals such as Co, Ni, or Mn on the positive electrode surface. This is likely due to the high potential of the positive electrode surface and the catalytic action of highly oxidized transition metals. Therefore, preventing contact between the electrolyte and the transition metals (e.g., one or more of Co, Ni, and Mn) that make up the positive electrode active material as much as possible is effective in maintaining the performance of the electrolyte.

[0004] Furthermore, as a method for fundamentally solving the problems of the organic solvent-based electrolyte, all-solid-state lithium-ion secondary batteries have been proposed, in which the electrolyte is replaced with a non-flammable solid electrolyte. Generally, the electrode reaction in a battery occurs at the interface between the electrode active material and the electrolyte. When a liquid electrolyte is used, the electrolyte penetrates the surface of the electrode active material present on the electrode, forming a reaction interface for charge transfer. In all-solid-state batteries, a solid electrolyte with ion conductivity serves as the electrolyte. However, since the solid electrolyte itself does not have the fluidity of a liquid, it is necessary to form a composite in advance by mixing the powder of the electrode active material with the solid electrolyte or by coating the powder of the electrode active material with the solid electrolyte before constructing the secondary battery.

[0005] However, in the case of all-solid-state lithium-ion secondary batteries, there has been a problem in that the resistance (hereinafter sometimes referred to as "interface resistance") that occurs when lithium ions move across the interface between the positive electrode active material and the solid electrolyte increases, and the performance of the all-solid-state lithium-ion secondary battery, such as battery capacity, is likely to decrease. The increase in the interface resistance is believed to be caused by the reaction between the positive electrode active material and the solid electrolyte, resulting in the formation of high-resistance sites on the surface of the positive electrode active material, and it is known that the interface resistance can be reduced by coating the surface of lithium cobalt oxide, which is the positive electrode active material, with lithium niobate.

[0006] For example, Patent Document 1 discloses a technique for wet coating the surface of a positive electrode active material with a lithium ion conductive oxide containing niobium or tantalum and lithium by a wet method, with the aim of improving the interfacial resistance between the positive electrode active material and the solid electrolyte. However, this coating technique uses alkoxides of niobium or tantalum as the niobium or tantalum source and absolute alcohol, a volatile organic compound, as the solvent, which raises concerns about a deterioration in the working environment. Furthermore, this coating technique also presents cost issues, such as the need for explosion-proofing measures for the coating equipment.

[0007] To solve these problems, for example, Patent Document 2 discloses a lithium niobate coating method using water as a solvent. The lithium niobate coating solution disclosed in Patent Document 2 is a solution in which poorly water-soluble niobium oxide is rendered water-soluble by converting it into a peroxo complex or an oxalate complex. Therefore, in the case of the lithium niobate coating solution using the peroxo complex disclosed in Patent Document 2, it is necessary to add 8 moles or more of hydrogen peroxide per mole of niobic acid. Because niobic acid is insoluble in hydrogen peroxide water, it is also necessary to add 1 mole or more of ammonia per mole of niobic acid. However, this coating solution has the problem of poor storage stability due to the chemical instability of the peroxo complex. Furthermore, this coating solution also has the problem of ammonia added to the coating solution leaching out metal components of the cathode active material to be coated.

[0008] As a technique for improving the chemical stability of niobium peroxo complexes, for example, Patent Document 3 discloses a technique of adding phosphate ions to a coating solution of lithium niobate. In this case, although not explicitly stated in Patent Document 3, it is believed that the phosphate ions act as a negative catalyst against the decomposition reaction of hydrogen peroxide. However, in the case of this coating solution, large amounts of hydrogen peroxide and ammonia are required to convert niobium into a peroxo complex, and the chemical stability is insufficient, and the problem of elution of metal components from the positive electrode active material remains unresolved.

[0009] As an aqueous solution-based lithium niobate coating liquid with excellent chemical stability, Patent Document 4 discloses an aqueous lithium niobate precursor solution using niobium polyacid ions and a method for producing the same. In the case of this precursor aqueous solution, niobium is water-soluble in the form of polyacid ions, and ammonia is not used, so there is no problem of elution of metal components of the positive electrode active material.

[0010] International Publication No. 2007 / 004590 JP 2012-074240 A JP 2017-191667 A JP 2020-066570 A

[0011] The lithium niobate precursor aqueous solution disclosed in Patent Document 4 is a coating solution having excellent characteristics, such as excellent storage stability of the solution and suppressing dissolution of the positive electrode active material during coating. However, when the surface of the positive electrode active material is coated with lithium niobate using the precursor aqueous solution, there is a problem in that the specific surface area of ​​the lithium niobate-coated positive electrode active material is larger than that of the positive electrode active material before coating.

[0012] The increase in specific surface area after coating is presumably due to the formation of extremely fine pores in the lithium niobate coating layer. If the coating layer becomes porous, moisture may be adsorbed onto the surface of the positive electrode active material through the pores, which may lead to deterioration of the positive electrode active material. Furthermore, if the coating layer becomes porous, the area of ​​the interface between the coating layer (solid electrolyte) and the positive electrode active material will decrease, which is undesirable.

[0013] The present invention aims to provide a lithium niobate precursor aqueous solution that, when the surfaces of positive electrode active material particles of a lithium ion secondary battery are coated with lithium niobate as a solid electrolyte, suppresses an increase in the specific surface area of ​​the lithium niobate-coated positive electrode active material and has excellent storage stability, and a method for producing the same.

[0014] [1] To achieve the above object, the present invention provides an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, in which the ratio of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution, P / (Nb+Li+P), is 0.04 or more and less than 0.5, and the molar ratio of lithium to niobium, Li / Nb, is more than 0.6 and not more than 2.0. [2] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the above item [1] may further contain 0.01% by mass or more and 10% by mass or less of hydrogen peroxide. [3] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the above item [2] is provided with a ratio of the number of moles of hydrogen peroxide to niobium (PO CIt is preferable that the value of (Nb) is 0.01 or more and 1 or less. [4] It is preferable that the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [1] has an absorbance of 0.1 or less at a wavelength of 660 nm. [5] The present invention also provides a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, the method comprising the steps of: dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions; and adding phosphate ions to the aqueous solution containing niobium polyacid ions and lithium ions. [6] The present invention also provides a method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, comprising the steps of dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions, and adding phosphate ions and hydrogen peroxide to the aqueous solution containing niobium polyacid ions and lithium ions. [7] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions described in [5] or [6] above, it is preferable that the ratio of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus, P / (Nb + Li + P), is 0.04 or more and less than 0.5, and the molar ratio of lithium to niobium, Li / Nb, is greater than 0.6 and less than 2.0. [8] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions described in [6] above, it is preferable that the concentration of hydrogen peroxide in the aqueous solution is 0.01% by mass or more and 10% by mass or less. [9] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [6], the ratio of the number of moles of niobium to the amount of hydrogen peroxide added (PO AIt is preferable that the value of (Nb) is 0.1 or more and 1.0 or less.

[10] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to the above item [5] or [6], it is preferable that phosphate ions are added at a rate of 0.07 mol / min or more and 3.07 mol / min or less per mole of lithium in the aqueous solution containing niobium polyacid ions and lithium ions.

[11] The present invention further provides a method for producing a lithium secondary battery having a coating layer containing lithium niobate, comprising the steps of: coating a surface of an active material for a lithium secondary battery with the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions according to any one of the above items [1] to [4]; and heat-treating the coated active material for a lithium secondary battery.

[0015] The aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions obtained by the production method of the present invention has excellent storage stability, and even when the aqueous solution is used to form a coating layer on the surface of a positive electrode active material for a lithium ion secondary battery, an increase in specific surface area is suppressed. Therefore, the present invention can contribute to improving the performance of all-solid-state lithium ion secondary batteries.

[0016] 1 shows FT-IR spectra of the aqueous solutions obtained in Comparative Example 1 and Example 3.

[0017] [Positive Electrode Active Material] The positive electrode active material coated with an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention is outside the scope of the present invention, but examples thereof include the following. The positive electrode active material is made of a composite oxide of Li and a transition metal M, and is not limited to materials conventionally used in lithium ion secondary batteries, such as lithium cobalt oxide (Li 1+X CoO 2 , -0.1≦X≦0.3), Li 1+X NiO 2 , Li 1+X Mn 2 O 4 , Li 1+X Ni 1/2 Mn 1/2 O 2 , Li 1+X Ni 1/3 Co 1/3 Mn1/3 O 2 (-0.1≦X≦0.3 in both cases), Li 1+X [Ni Y Li 1/3-2Y/3 Mn 2/3-Y/3 ]O 2 (0≦X≦1, 0<Y<1 / 2), etc., and lithium transition metal oxides in which part of these Li or transition metal elements is replaced with Al or other elements, and Li 1+X FePO 4 , Li 1+X MnPO 4 (in all cases, -0.1≦X≦0.3) and lithium manganese oxide (LiMnO 4 ) and those in which a part of Mn is replaced with Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Ni, Co, Fe, etc. (LiAl 0.1 Mn 0.9 O 4 , LiNi 0.5 Mn 1.5 O 4 etc.)

[0018] [Nb source] Anhydrous niobium oxide (Nb 2 O 5 Since niobium oxide is poorly soluble in water, the production method of the present invention uses amorphous, water-soluble niobium oxide as the Nb source. 2 O 5 ・nH 2 O (n is not 0, for example, 3≦n≦16).

[0019] [Polyacid ions] Polyacids are anionic species formed by the condensation of oxoacids, and polyacids of transition metal elements can be considered to be molecular ionic species of metal oxides. When there is one type of metal element, they are called isopolyacids, and when there are multiple metal elements, they are called heteropolyacids.

[0020] Although the potential-pH diagram for niobium has not yet been established, niobium hydroxide precipitates in the neutral region, and therefore Nb(OH) 5 or HNbO 3When an alkali is added to an aqueous solution containing these solid phases to raise the pH of the system, excess OH - The presence of ions causes niobium to react with, for example, Nb(OH) 6 - and NbO 3 - It begins to dissolve in the form of, etc. As the pH of the system is further increased, it is thought that soluble niobium oxide will take on various condensation states depending on the pH of the system, but in this specification, niobium oxide solubilized on the alkaline side is considered to collectively become niobium polyacid ions. Note that niobium polyacid ions once solubilized on the alkaline side maintain the polyacid form even when phosphoric acid is added and the pH of the system is lowered to about 4. The aqueous solution of the present invention containing niobium polyacid ions, lithium ions, and phosphate ions contains niobium in the form of a polyacid, and therefore has excellent storage stability. The form of niobium may be a soluble polyacid ion, and its structure is not particularly limited. The fact that niobium in an aqueous solution is a polyacid ion can be confirmed by FT-IR measurement. When niobium in an aqueous solution is in the form of a polyacid ion, it is possible to obtain a polyacid ion at a wave number of 850 cm. -1 ±20cm -1 An absorption peak due to Nb—O bonds is observed around this point.

[0021] [Li Source] In the manufacturing method of the present invention, lithium hydroxide (LiOH) is used as the Li source. The LiOH may be anhydrous or hydrated. The LiOH added to the aqueous solution is Li + and OH - and exhibits strong alkalinity. In the methods for producing a lithium niobate precursor aqueous solution described in Patent Documents 2 and 3, niobic acid and hydrogen peroxide are first reacted with each other, then ammonia water is added to increase the pH, and finally a Li salt is added to adjust the precursor aqueous solution. In contrast, the method for producing an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions of the present invention is characterized in that LiOH is first added to an aqueous solution containing niobic acid to dissolve the niobic acid.

[0022] Since LiOH itself is a strong alkali, when LiOH is added to an aqueous solution containing niobic acid, the pH of the system rises, dissolving the niobium oxide and forming stable niobium polyoxide ions. Hydrogen peroxide is then added to the alkaline aqueous solution containing the niobium polyoxide ions and lithium ions; the effect of hydrogen peroxide will be described later.

[0023] Since a coating layer of a solid electrolyte having ion conductivity is ultimately formed, the amount of lithium added is preferably such that the molar ratio Li / Nb to 1 mole of niobium contained in the niobium polyoxide ion is greater than 0.6 and less than 2.0. A Li / Nb ratio of 0.6 or less is undesirable because lithium ion conductivity deteriorates due to lithium deficiency. Furthermore, a Li / Nb ratio of more than 2.0 is undesirable because storage stability deteriorates due to an increase in pH caused by excess lithium hydroxide. From the viewpoint of ionic conductivity, Li / Nb is preferably 0.9 or more, more preferably 0.95 or more. Furthermore, from the viewpoint of ionic conductivity, Li / Nb is preferably 1.5 or less, more preferably 1.4 or less.

[0024] The reason why the storage stability of the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions of the present invention is better than that of the precursor aqueous solution obtained by the techniques described in Patent Documents 2 and 3 is presumed to be as follows. In the techniques described in Patent Documents 2 and 3, niobium exists in the form of a peroxo complex in the aqueous solution, and it is known that the peroxo ions coordinated to niobium are easily detached and unstable. In contrast, it is believed that the niobium in the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions of the present invention is mainly in the form of a relatively stable polyacid. Adding hydrogen peroxide to the aqueous solution further improves storage stability. Because the aqueous solution of the present invention does not contain organic substances like the coating solution described in Non-Patent Document 1, a coating layer with low volume resistivity can ultimately be obtained.

[0025] [Phosphate ion] The greatest technical feature of the present invention is that phosphate ions are present in an aqueous solution containing niobium polyphosphate ions and lithium ions. The source of phosphate ions can be water-soluble phosphoric acid (PO ) such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, or their sodium salts or ammonium salts. 4 3- ) salts can be used. Phosphoric acid is a tribasic acid and undergoes three-stage dissociation in an aqueous solution, so it can exist in various forms in the aqueous solution, such as phosphate ions, monohydrogen phosphate ions, dihydrogen phosphate ions, and pyrophosphate ions. However, the form of existence is determined by the pH of the aqueous solution, not by the type of chemical used as a phosphate ion supply source, and therefore, the above-mentioned ions containing a phosphate group are collectively referred to as phosphate ions. In the case of an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention, FT-IR measurement shows that the peak wavelength is 1000 to 1150 cm -1 An absorption peak due to phosphate ions is observed.

[0026] The reason why the coexistence of phosphate ions in an aqueous solution of niobium polyoxide ions and lithium ions suppresses an increase in the specific surface area of ​​the coated positive electrode active material is currently unknown, but the present inventors speculate as follows: That is, possible mechanisms include the presence of phosphate ions contained in the aqueous solution of the present invention containing niobium polyoxide ions, lithium ions, and phosphate ions improving the wettability of the aqueous solution to the surface of the positive electrode active material, the action of phosphate ions contained in the aqueous solution changing the double layer structure at the interface and thereby changing the structure of the coating layer, or the trace amounts of phosphate ions contained in the coating layer suppressing the generation of pores in the coating layer during drying.

[0027] In the method for producing an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention, the phosphate ion aqueous solution is added to an aqueous solution containing lithium and niobium polyacid in which niobium polyacid ions have been stably formed, thereby making it possible to suppress the precipitation of niobic acid in the aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions. 3 P.O. 4A large amount of precipitate (colloid) mainly composed of niobium polyoxide ions, lithium ions, and phosphate ions may be generated. If the concentration of colloidal particles in the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions is high, this is undesirable because it increases the specific surface area of ​​the coated positive electrode active material.

[0028] To prevent the generation of colloids, it is preferable to adjust the rate at which the aqueous phosphate ion solution is added to the aqueous solution containing niobium polyacid ions and lithium ions. To prevent the generation of colloids, the rate at which the aqueous phosphate ion solution is added is preferably 3.07 mol / min or less of phosphate ions per mole of lithium in the aqueous solution containing niobium polyacid ions and lithium ions. More preferably, it is 2 mol / min or less, and even more preferably, it is 1 mol / min or less or 0.6 mol / min or less. While there are no particular limitations on the lower limit of the addition rate, it may be, for example, 0.07 mol / min or more from the viewpoint of production time.

[0029] The presence or absence of the colloid generation can be confirmed by the absorbance value at a wavelength of 660 nm in an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions. This is because the absorbance at a wavelength of 660 nm indicates the intensity of scattered light caused by colloidal microparticles present in an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions. Therefore, high absorbance in the precursor solution according to the present invention suggests a high concentration of microparticles present in the aqueous solution (see, for example, JIS-K0101).

[0030] Furthermore, if a positive electrode active material is coated with an aqueous solution having a high concentration of such fine particles, the fine particles may adhere to the surface of the positive electrode active material, causing the coating layer to become uneven, resulting in an uneven thickness of the coating layer and an increase in specific surface area. According to the inventors' studies, if the absorbance value at a wavelength of 660 nm of an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions is 0.1 or less, even if colloidal fine particles are present in the aqueous solution, the amount is small, preventing unevenness in the coating layer thickness and an increase in specific surface area. More preferably, the absorbance value is 0.08 or less, and even more preferably 0.07 or less. In the present invention, the lower limit of the absorbance is not particularly specified, but may be, for example, 0.001 or more.

[0031] Regarding the content of phosphate ions in an aqueous solution containing niobium polyphosphate ions, lithium ions, and phosphate ions, the ratio of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution, P / (Nb + Li + P), is preferably 0.04 or more and less than 0.5. If this ratio is less than 0.04, the effect of adding phosphate ions is insufficient. From the viewpoint of ionic conductivity, P / (Nb + Li + P) is preferably 0.08 or more. If the value of P / (Nb + Li + P) is 0.5 or more, the effect of adding phosphate ions becomes saturated. From the viewpoint of ionic conductivity, P / (Nb + Li + P) is preferably 0.35 or less. The range of P / (Nb + Li + P) is more preferably 0.1 or more and 0.4 or less, and even more preferably 0.2 or more and 0.4 or less.

[0032] The sum of the lithium, niobium, and phosphorus contents in the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 10% by mass or less, and even more preferably 5% by mass or more and 8% by mass or less. If the sum of the lithium, niobium, and phosphorus contents is less than 1% by mass, the amount of the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions must be increased to obtain the required coating layer thickness, which increases the water content and is therefore cost-inefficient. If the concentration is too low, the water content increases to achieve the required coating thickness, which is uneconomical. If the sum of the lithium, niobium, and phosphorus contents exceeds 20% by mass, the viscosity of the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions increases, which may cause clogging of the narrow piping in the coating treatment equipment.

[0033] The amount of impurity elements other than lithium, niobium, phosphorus, oxygen, and hydrogen in the aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions is preferably 10% by mass or less, more preferably 1% by mass or less. Potential unavoidable impurities include carbonate ions. The term "impurities" used herein refers to impurities contained in the evaporation residue when the precursor aqueous solution is evaporated to dryness at 200°C. When evaporated to dryness at 200°C, carbonate ions combine with counter cations to precipitate as carbonate salts.

[0034] [Hydrogen Peroxide] Hydrogen peroxide can be further added to the aqueous solution of the present invention to improve storage stability. In this case, hydrogen peroxide is preferably added so that the concentration in the aqueous solution is 0.01% by mass or more and 10% by mass or less. If the hydrogen peroxide concentration is less than 0.01% by mass, the generated niobium polyacid reacts with hydroxide ions and is prone to decomposition. On the other hand, if the hydrogen peroxide concentration exceeds 10% by mass, the generated niobium polyacid may react with hydrogen peroxide to form an unstable peroxo complex. Hydrogen peroxide is preferably added so that the concentration in the aqueous solution is 0.05% by mass or more and 5% by mass or less, more preferably 0.1% by mass or more and 1% by mass or less.

[0035] The ratio of the number of moles of hydrogen peroxide to the amount of niobium added (PO A The ratio of the number of moles of hydrogen peroxide to the number of moles of niobium (PO / Nb) is preferably in the range of 0.1 or more and 1 or less. Setting it to 0.1 or more is advantageous in avoiding decomposition of the niobium polyacid by reaction with hydroxide ions. Setting it to 1 or less is advantageous in avoiding the formation of an unstable peroxo complex by reaction of the generated niobium polyacid with hydrogen peroxide. The ratio of the number of moles of hydrogen peroxide to the amount of niobium added (PO / Nb) is preferably in the range of 0.1 or more and 1 or less. Setting it to 0.1 or more is advantageous in avoiding decomposition of the niobium polyacid by reaction of the generated niobium polyacid with hydrogen peroxide. A / Nb) is preferably 0.05 or more and 0.5 or less, and more preferably 0.1 or more and 0.35 or less. From the viewpoint of reactivity, the addition of hydrogen peroxide is preferably carried out after dissolving hydrous niobium oxide with LiOH to form stable niobium polyphosphate ions. It is not important whether the addition of the phosphate ions or the addition of hydrogen peroxide in this section is carried out first.

[0036] Although the added hydrogen peroxide decomposes over time, it is preferable that the aqueous solution contain 0.01% to 6.7% by mass of hydrogen peroxide. If the hydrogen peroxide content is less than 0.01% by mass, the effect of maintaining the stability of the precursor aqueous solution is small. If the hydrogen peroxide content exceeds 6.7% by mass, the effect of adding hydrogen peroxide becomes saturated. The concentration of hydrogen peroxide in the aqueous solution is preferably 0.05% to 5% by mass, and more preferably 0.1% to 1% by mass.

[0037] The ratio of the number of moles of hydrogen peroxide to 1 mole of niobium (PO C The ratio (PO / Nb) is preferably in the range of 0.01 to 1. If the ratio exceeds the above range, not only will the effect of adding hydrogen peroxide be saturated, but when used as a coating solution, there is a risk of dissolving the positive electrode active material. If the amount of hydrogen peroxide is too small, the niobium polyacid will react with hydroxide ions and be easily decomposed. C A more preferable range of / Nb is 0.05 or more and 0.5 or less, and a more preferable range is 0.1 or more and 0.35 or less.

[0038] [pH] In the production method of the present invention, the pH of the aqueous solution used to form niobium polyacid ions is determined almost automatically by the amounts of LiOH (a strong alkali), phosphoric acid, and hydrogen peroxide added, so no special pH adjustment is required. However, the pH is preferably 7.5 to 12.5, which is on the alkaline side. To ensure stable formation of niobium polyacid ions, a pH of 9.0 to 12.0 is preferred. Adding phosphoric acid to a solution containing this niobium polyacid and lithium lowers the pH of the system, but it has been confirmed that niobium polyacids remain stable at a pH of 3 or higher. The pH of the solution to which phosphoric acid has been added is preferably 12.5 or less, more preferably 12 or less. The pH values ​​herein are measured using a glass electrode with a pH meter equipped with a temperature-compensated electrode, calibrated according to JIS Z8802 using an appropriate buffer solution appropriate for the pH range to be measured.

[0039] [Production Method] In the method for producing an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions of the present invention, hydrous niobium oxide is used as the niobium starting material, as described above. Hydrous niobium oxide and LiOH are dissolved in water to obtain an aqueous solution containing niobium polyoxide ions and lithium, and phosphate ions are then added to the aqueous solution to obtain an aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions. In this process, the ratio of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus (P / (Nb + Li + P)) is preferably 0.04 or more and less than 0.5, and the molar ratio of niobium to lithium (Li / Nb) is preferably greater than 0.6 and less than 2.0. The total concentration of niobium is preferably 1% by mass or more and 20% by mass or less. When hydrogen peroxide is added, it is preferably added so that the concentration of hydrogen peroxide in the aqueous solution is 0.01% by mass or more and 10% by mass or less.

[0040] [Coating Treatment] The following is an embodiment of the coating treatment of a positive electrode active material for a lithium ion secondary battery using an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions of the present invention. The positive electrode active material to be coated has a specific surface area of ​​0.1 to 2 m. 2 / g can be used. Since the specific surface area of ​​a positive electrode active material is inversely proportional to its particle size, the specific surface area of ​​the positive electrode active material is appropriately selected depending on the application of the lithium-ion secondary battery. The thickness of the coating layer coated on the positive electrode active material is preferably 3 to 20 nm, more preferably 5 to 15 nm. For the coating treatment, known methods such as a tumbling fluidized bed coating method or a high-velocity airflow collision shear method are used, and a positive electrode active material having a coating layer can be obtained by contacting the positive electrode active material with an aqueous solution containing niobium polyoxide ions of the present invention, lithium ions, and phosphate ions, followed by a heat treatment such as drying.

[0041] [Qualitative Evaluation of Aqueous Solution] Qualitative evaluation of dissolved chemical species in the aqueous solution was performed by Fourier transform infrared spectroscopy (FT-IR) using a NICOLET 7600 manufactured by Thermo Fisher Scientific. In order to remove the low-wavenumber peak of the water solvent, water was used for background measurement, and the measurement was performed by the attenuated total reflectance (ATR) method. A germanium prism was used for the measurement, and the angle of incidence was set to 45°. By performing the FT-IR measurement, it can be confirmed that niobium exists as a polyacid ion and phosphorus exists as a phosphate ion in the aqueous solution of the present invention containing niobium polyacid ions, lithium ions, and phosphate ions.

[0042] [Quantitative Analysis of Li, Nb, and P in Aqueous Solution] The components of the aqueous solution were analyzed using an inductively coupled plasma atomic emission spectrometer (ICP-AES, Agilent Technology 700 Series). A 0.1 g sample was taken from the precursor solution and weighed, to which 15 mL of pure water and 5 mL of hydrochloric acid were added, heated, and then allowed to cool. An additional 2 mL of hydrogen peroxide solution was added, and the solution was allowed to cool. The volume was then adjusted to 100 mL and analyzed by ICP-AES. The mole numbers of the elements in the present invention were calculated from the niobium, lithium, and phosphorus contents obtained by this ICP quantitative analysis.

[0043] [Method for Quantifying Hydrogen Peroxide in Aqueous Solution] Prior to the quantification procedure, a Ti-PAR solution is prepared in advance. The Ti-PAR solution is prepared by mixing 20 mL of a Ti solution with a titanium concentration of 1 mmol / L, prepared using a commercially available titanium standard solution, with 15 mL of a PAR solution prepared by dissolving 11 mg of PAR (4-(2-pyridylazo)-resorcinol) in a 1% by mass aqueous solution of sodium hydroxide and adjusting the volume to 50 mL with ultrapure water. 0.1 mL of the aqueous solution as a sample is added to a plastic container previously charged with 0.05 mL of reagent-grade nitric acid and 20 mL of reagent-grade methanol, and gently shaken to mix. After the precipitate has settled, the solution is filtered using a 0.45 μm filter. It is preferable to wait approximately one minute between the addition of the solution and the start of filtration. A 0.25 mL aliquot of the filtrate was added, followed by 5 mL of methanol, 1 mL of Ti-PAR solution, and 1.2 mL of a pH 8.6 buffer solution prepared by mixing 5 mL of 1 mol / L aqueous ammonia and 40 mL of 1 mol / L ammonium chloride. The resulting solution was adjusted to a final volume of 10 mL with methanol and allowed to stand at 40-45°C for 30 minutes. The absorbance was measured at a wavelength of 520 nm using a Hitachi High-Technologies U-2800 spectrophotometer. The hydrogen peroxide concentration was quantified using the standard addition method, based on the relative absorbance intensity compared to a standard solution of hydrogen peroxide. The molar ratio of the hydrogen peroxide content was calculated from the hydrogen peroxide content obtained in this quantitative analysis.

[0044] [Absorbance Measurement] 3.5 mL of the aqueous solution was dispensed into a quartz cell (10 mm x 10 mm x 45 mm), and the absorbance was measured at wavelengths of 400 to 700 nm using a Hitachi High-Technologies U-2800 spectrophotometer. The precursor solution temperature during measurement was 25°C. The zero point of absorbance was the absorbance measured when ultrapure water with an electrical conductivity of 17 MΩ cm or more and a temperature of 25°C was placed in the measurement cell. Note that the absorbance at a wavelength of 660 nm indicates the intensity of scattered light caused by the fine particles in the precursor aqueous solution, and a high absorbance indicates a high fine particle concentration (see JIS-K0101).

[0045] [Measurement of BET Specific Surface Area] The BET specific surface area of ​​the positive electrode active material before and after coating was determined by the BET single-point method using 4Sorb US manufactured by Yuasa Ionics Co., Ltd. The increase rate of the BET specific surface area before and after coating is defined by the following formula (1): BET specific surface area increase rate = 100 × (BET A -BET B ) / BET B …(1) BET HERE A is the BET specific surface area after coating, BET B is the BET specific surface area before coating. In the present invention, it is determined that the increase in the specific surface area is suppressed when the BET specific surface area increase rate is 100% or less.

[0046] [Evaluation of Ionic Conductivity] The ionic conductivity of the coating layer obtained from the aqueous solution of the present invention was evaluated using a bulk powder formed from the aqueous solution. The aqueous solution was evaporated to dryness in a dryer set at 100°C, and the resulting powder was further calcined in air at 300°C for 12 hours. 0.5 g of the calcined powder was placed in a 10 mm diameter mold and pressed at 20 MPa using a press to obtain a green compact. Impedance measurements were performed on the resulting green compact in an Ar atmosphere at 25°C using a potentio / galvanostat (Solartron 1470E) and a frequency response analyzer (Solartron 1255B) in the frequency range of 100 Hz to 4 MHz. The resistance of the oxide powder sample was determined from the intercept of a Cole-Cole plot (complex impedance plane plot) of the measured values, and the ionic conductivity was calculated from the obtained resistance value.

[0047] [Calculation of the thickness of the coating layer] The thickness of the coating layer obtained by the above coating treatment is calculated on the assumption that the entire amount of the aqueous solution used in the coating treatment is used to form the coating layer. In this case, the lithium, niobium, and phosphorus contained in the aqueous solution are respectively calculated as Li 2 O, Nb 2 O 5 and P 2 O 5 The thickness of the coating layer is defined by the following formula (2): [Coating layer thickness (nm)] = 10 3 × [Li 2 O, Nb 2 O5 and P 2 O 5 Volume (cm) of the mixture 3 ) )] / [amount of positive electrode active material × specific surface area of ​​positive electrode active material (m 2 / g)] ... (2) Here, the volume of the above mixture is calculated as follows: If the Li content in the aqueous solution is a (mass %), the Nb content is b (mass %), and the P content is c (mass %), the atomic weights of Li, Nb, and P and the Li 2 O, Nb 2 O 5 and P 2 O 5 From the molecular weight of Li 2 O content (mass%) a'=a×Li 2 Molecular weight of O / (atomic weight of Li×2) Nb 2 O 5 Content (mass%) b' = b x Nb 2 O 5 Molecular weight of Nb / (atomic weight of Nb×2) P 2 O 5 Content (mass%) c'=c×P 2 O 5 The amount of aqueous solution used for the coating treatment is x (g), and the amount of Li 2 The density of O is 2.0 g / cm 3 , Nb 2 O 5 The density is 4.6 g / cm 3 , P 2 O 5 The density is 2.4 g / cm 3 Then, Li 2 O, Nb 2 O 5 and P 2 O 5 Volume (cm) of the mixture 3 ) = (a' / 2.0 + b' / 4.6 + c' / 2.4) x / 100.

[0048] Comparative Example 1: 81.6 g of pure water and 1.5 g of lithium hydroxide monohydrate (LiOH·H 2 4.195 g of niobium hydroxide (NbO) was added and stirred to dissolve the lithium hydroxide. 2 O 5 ・nH2 13.84 g of niobium oxide (O, Nb concentration: 67.4 mass%) was mixed and stirred at 70°C for 8 hours to solubilize the hydrous niobium oxide, yielding a clear aqueous solution containing niobium polyoxide ions and lithium ions. The pH of the resulting aqueous solution was 11.8. In this case, the molar ratio of lithium to 1 mole of niobium in the niobium polyoxide ions (Li / Nb) was 1.0. While maintaining the aqueous solution containing niobium and lithium at 20°C, 3.2 g of a 30% aqueous solution of hydrogen peroxide was added, and 71 g of purified water was added for final concentration adjustment to obtain an aqueous solution containing niobium polyoxide ions and lithium ions. In this case, the hydrogen peroxide concentration in the aqueous solution was 0.49 mass%. No turbidity was observed visually in the aqueous solution. Absorbance measurement of the aqueous solution of Comparative Example 1 revealed an absorbance value of 0.01 at a wavelength of 660 nm. The conditions for preparing the aqueous solution of this comparative example are shown in Table 1, and the calculated values ​​of the concentrations of each element in the aqueous solution and the hydrogen peroxide concentration are shown in Table 2. When the aqueous solution of this comparative example was subjected to FT-IR measurement, -1 ±20cm -1 An absorption peak due to Nb—O bonds was observed near , and it is believed that the solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. The FT-IR spectrum of the aqueous solution obtained in this comparative example is shown in Figure 1.

[0049] A rolling fluidized coating device (MP-micro manufactured by Powrex Corporation) was used to coat a substrate with a BET specific surface area of ​​0.636 m 2 / g of positive electrode active material (LiNi 1/3 Mn 1/3 Co 1/3 O 2 25.2 g of the aqueous solution obtained in this comparative example was sprayed onto a coating machine (EQ-Lib-LNCM111, manufactured by MTI) while drying the aqueous solution in parallel, thereby coating the surface of the positive electrode active material. The operating conditions of the rolling fluidized coating machine were: intake gas: atmospheric air, intake temperature: 100°C, intake air flow rate: 0.1 m 3 / h, rotor rotation speed: 1000 rpm, spray rate: 0.5 g / min. The amount of the aqueous solution was equivalent to a coating layer thickness of 10 nm. The BET specific surface area after coating was 1.91 m 2 / g, and the increase in BET specific surface area when the coating treatment was carried out using the aqueous solution of this comparative example was 200%. The coating treatment conditions and the increase in BET specific surface area are shown in Table 3.

[0050] Example 1: The procedure was the same as in Comparative Example 1, up to the addition of hydrogen peroxide. 1.0 g of phosphoric acid (80% by mass, manufactured by Wako Pure Chemical Industries, Ltd.) was added, followed by 75 g of pure water for concentration adjustment, to obtain an aqueous solution containing niobium polyphosphate ions, lithium ions, and phosphate ions in Example 1. During the phosphoric acid addition, the solution was stirred while adding phosphate ions at a rate of 0.25 mol / min per 1 mol of lithium in the aqueous solution containing niobium polyphosphate ions and lithium ions. In this case, the P / (Nb + Li + P) ratio was 0.04, and no white colloid formation was observed. Absorbance measurement of the aqueous solution in Example 1 revealed an absorbance value of 0.01 at a wavelength of 660 nm.

[0051] The aqueous solution obtained in this example was subjected to FT-IR measurement, and the wave number was 850 cm -1 ±20cm -1 An absorption peak due to Nb—O bonds was observed around 1000 to 1150 cm, which suggests that the solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed at 1.225 × 10. The ionic conductivity of the powder obtained by evaporating the aqueous solution obtained in this example to dryness at 300°C was 1.225 × 10. -8 S / cm. When 25.2 g of the aqueous solution obtained in this example was used to carry out a coating treatment under the same conditions as in Comparative Example 1, the thickness of the coating layer was 10 nm and the BET specific surface area increase rate was 90%, demonstrating an effect of suppressing the increase in BET specific surface area compared to Comparative Example 1. Table 1 shows the preparation conditions for the aqueous solution in this example, Table 2 shows the calculated concentrations of each element and the hydrogen peroxide concentration in the aqueous solution, Table 3 shows the coating treatment conditions and the BET specific surface area increase rate, and Table 4 shows the ionic conductivity of the powder obtained by evaporation to dryness.

[0052] [Examples 2 to 5] Up to the addition of hydrogen peroxide, the same procedure as in Example 1 was followed, but the amounts of phosphoric acid and pure water for concentration adjustment and the rate of phosphate ion addition were varied as shown in Table 1 to obtain aqueous solutions containing niobium polyoxide ions, lithium ions, and phosphate ions in Examples 2 to 5. In these cases, P / (Nb+Li+P) was set to 0.10 to 0.40, but no white colloid was observed in any of the Examples. Furthermore, absorbance measurements were performed for each Example in the same manner as in Example 1, and the results are also shown in Table 2. FT-IR measurements were performed in all Examples, and a white colloid was observed at a wave number of 850 cm. -1 ±20cm -1 An absorption peak due to Nb—O bonds was observed around 1000 to 1150 cm, which suggests that the solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed. Figure 3 also shows the FT-IR spectrum of the aqueous solution obtained in this example. Using the aqueous solutions obtained in Examples 2 to 5, coating treatment was performed under the same conditions as Comparative Example 1. The amount of aqueous solution used was adjusted so that the thickness of the coating layer would be 10 nm in all cases, and the BET specific surface area increase rate was -1% to 27%. Table 1 shows the preparation conditions for the aqueous solutions in Examples 2 to 5, Table 2 shows the calculated concentrations of each element and the hydrogen peroxide concentration in the aqueous solution, Table 3 shows the coating treatment conditions and the BET specific surface area increase rate, and Table 4 shows the ionic conductivity of the powder obtained by evaporation to dryness. From the results in Table 4, it can be said that from the standpoint of ionic conductivity, a P / (Li + Nb + P) ratio of 0.35 or less is preferable, and a ratio of 0.08 or more is more preferable.

[0053] [Examples 6 to 9] Using the same procedure as in Example 1, aqueous solutions containing niobium polyoxide ions, lithium ions, and phosphate ions were obtained in Examples 6 to 9, in which the values ​​of Li / Nb and P / (Nb + Li + P) were varied by varying the amounts of lithium hydroxide, phosphoric acid, and pure water added for concentration adjustment, and the rate of addition of phosphate ions, as shown in Table 1. In these cases, Li / Nb was 0.78 to 2.00, and P / (Nb + Li + P) was 0.20 to 0.40. No white colloid was observed in any of the Examples. Furthermore, absorbance measurements were performed for each Example in the same manner as in Example 1, and the results are also shown in Table 2. FT-IR measurements were performed for all Examples, and the results were as follows: -1 ±20cm -1 An absorption peak due to Nb—O bonds was observed around 1000 to 1150 cm, which suggests that the solubilized hydrous niobium oxide exists in the form of niobium polyacid ions. -1 An absorption peak due to phosphate ions was observed. Using the aqueous solutions obtained in Examples 6 to 9, coating treatments were performed under the same conditions as in Comparative Example 1. The amount of aqueous solution used was adjusted so that the thickness of the coating layer would be 10 nm in all cases, and the BET specific surface area increase rate was -2% to -3%. Table 1 shows the preparation conditions for the aqueous solutions in Examples 6 to 9, Table 2 shows the calculated concentrations of each element and the hydrogen peroxide concentration in the aqueous solutions, Table 3 shows the coating treatment conditions and the BET specific surface area increase rate, and Table 5 shows the ionic conductivity of the powders obtained by evaporation to dryness for Examples 6 and 7. From the results in Table 5, it can be said that a Li / Nb ratio of 0.9 or higher is preferable from the standpoint of ionic conductivity, and more preferably 0.95 or higher.

[0054] Example 10: Using 36.3 g of the aqueous solution containing niobium polyphosphate ions, lithium ions, and phosphate ions obtained in Example 4, a niobium ion solution having a BET specific surface area of ​​1.085 m 2 When the coating treatment was performed on a positive electrode active material of 0.1g / g, the increase in the BET specific surface area was -1%.

[0055] Example 11 An aqueous solution containing niobium polyoxide ions, lithium ions, and phosphate ions was obtained using the same procedure as in Example 2, except that the phosphate ion addition rate was set to 3.38 mol / min. In this example, the addition of phosphoric acid resulted in the generation of a small amount of white colloid, but no visual cloudiness of the aqueous solution was observed. Table 2 shows the absorbance obtained by measuring the absorbance for this example. Using the aqueous solution obtained in this example, a coating process was performed under the same conditions as in Comparative Example 1. The amount of aqueous solution used was adjusted to achieve a coating layer thickness of 10 nm in all cases. The BET specific surface area increase rate was 73%, demonstrating a suppression of the increase in BET specific surface area compared to Comparative Example 1. Comparison of Examples 2 and 11 revealed that by setting the phosphate ion addition rate to 3.07 mol / min or less of phosphate ions per mole of lithium in the aqueous solution containing niobium polyoxide ions and lithium ions, the generation of colloidal particles was suppressed and the increase in BET specific surface area due to coating could be further suppressed.

[0056] Comparative Example 2: The procedure was the same as in Comparative Example 1 up to the addition of hydrogen peroxide. 24.5 g of phosphoric acid was added at a rate of 0.24 mol / min per mol of lithium in an aqueous solution containing niobium polyphosphate ions and lithium ions. A large amount of white colloid was generated. In this case, P / (Nb + Li + P) was 0.50. The white colloid did not redissolve even when diluted with pure water to adjust the concentration, and the aqueous solution became cloudy with the naked eye. Therefore, a coating treatment using this comparative example was not performed.

[0057] [Comparative Example 3] The same procedure as in Comparative Example 1 was followed, except that the amount of lithium hydroxide added was 2.517 g and the Li / Nb ratio was 0.50. After the addition of hydrogen peroxide, 4.9 g of phosphoric acid was further added to an aqueous solution containing niobium polyoxide ions and lithium ions at a rate of 0.24 mol / min of phosphate ions per mol of lithium, resulting in the generation of a large amount of white colloid. This white colloid did not redissolve even when diluted with pure water to adjust the concentration, and the aqueous solution became cloudy with the naked eye. Therefore, a coating treatment using this comparative example was not performed.

[0058] As described above, by coating the positive electrode active material of a lithium ion battery positive electrode with an aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions as defined in the present invention, it is possible to suppress an increase in the BET specific surface area due to the coating.

[0059]

[0060]

[0061]

[0062]

[0063]

Claims

1. An aqueous solution containing niobium polyacid ions, lithium ions, and phosphate ions, in which the ratio P / (Nb+Li+P) of the number of moles of phosphorus to the sum of the number of moles of niobium, lithium, and phosphorus contained in the aqueous solution is 0.04 or more and less than 0.5, and the molar ratio Li / Nb of lithium to niobium is more than 0.6 and 2.0 or less.

2. An aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions as described in claim 1, further containing hydrogen peroxide at a concentration of 0.01 mass % or more and 10 mass % or less.

3. The ratio of the number of moles of hydrogen peroxide to the number of moles of niobium present in the aqueous solution (PO C 3. The aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 2, wherein the value of (Nb) is 0.01 or more and 1 or less.

4. An aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 1, wherein the aqueous solution has an absorbance of 0.1 or less at a wavelength of 660 nm.

5. A method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions, comprising: dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions; and adding phosphate ions to the aqueous solution containing niobium polyacid ions and lithium ions.

6. A method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions, comprising: dissolving a hydrous oxide of niobium and a salt containing lithium in water to obtain an aqueous solution containing niobium polyacid ions and lithium ions; and adding phosphate ions and hydrogen peroxide to the aqueous solution containing niobium polyacid ions and lithium ions.

7. A method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 5 or 6, wherein the ratio of the number of moles of phosphorus to the sum of the numbers of moles of niobium, lithium and phosphorus, P / (Nb+Li+P), is 0.04 or more and less than 0.5, and the molar ratio of lithium to niobium, Li / Nb, is more than 0.6 and 2.0 or less.

8. A method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 6, wherein the concentration of hydrogen peroxide in the aqueous solution is 0.01% by mass or more and 10% by mass or less.

9. The ratio of the number of moles of hydrogen peroxide added to the number of moles of niobium (PO A 7. The method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions according to claim 6, wherein the value of (Nb) is 0.1 or more and 1.0 or less.

10. A method for producing an aqueous solution containing niobium polyacid ions, lithium ions and phosphate ions as described in claim 5 or 6, in which phosphate ions are added at a rate of 0.07 mol / min or more and 3.07 mol / min or less per mol of lithium in the aqueous solution containing niobium polyacid ions and lithium ions.

11. A method for producing an active material for lithium secondary batteries having a coating layer containing lithium niobate, comprising the steps of: coating the surface of an active material for lithium secondary batteries with an aqueous solution containing niobium polyacid ions according to any one of claims 1 to 4, lithium ions, and phosphate ions; and heat treating the active material for lithium secondary batteries that has been coated.

Citation Information

Patent Citations

  • Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery

    JP2012074240A

  • All-solid lithium battery

    WO2007004590A1

  • Preparation method of carbon-coated niobium doped lithium iron phosphate-lithium cobalt oxide composite positive electrode material

    CN103199248A

  • Solution containing lithium and niobium complex, and method of producing the same

    JP2014210701A

  • Active material coating solution

    JP2017191667A

Cited By

  • Nb complex aqueous solution, method for manufacturing positive electrode active material for all-solid-state lithium ion battery, method for manufacturing positive electrode for all-solid-state lithium ion battery, and method for manufacturing all-solid-state lithium ion battery

    JP7774761B1