Sintered compact composition, green compact, sintered compact, and method for detecting defect in sintered compact
The composition for sintered compacts with a specific binder-to-powder ratio and pre-kneaded organic binder addresses the challenge of defect prediction and prevention in the degreasing process, enhancing production efficiency and recyclability of metal powder.
Patent Information
- Application Number
- PCT/JP2024/012119
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for producing sintered compacts fail to predict and prevent defects such as cracks and blisters during the degreasing process, leading to costly and inefficient production, and the inability to recycle defective metal powder.
A composition for sintered compacts comprising sinterable inorganic powder and an organic binder with a specific ratio of discontinuous binder area to total binder area, pre-kneaded with aggregate resin and wax, allowing for defect prediction and suppression without sintering, and enabling recycling of defective metal powder.
Enables the prediction and prevention of defects in sintered compacts during the degreasing process, improving yield and allowing for the recycling of defective metal powder, thus reducing production costs and enhancing recyclability.
Smart Images

Figure JP2024012119_03102024_PF_FP_ABST
Abstract
Description
Composition for sintered compact, green compact, sintered compact, and method for detecting defects in sintered compact
[0001] The present invention relates to a composition for a sintered compact, a green compact, a sintered compact, and a method for detecting defects in a sintered compact.
[0002] Among sintered bodies made from sinterable inorganic powders such as metals, ceramics, and cermets, a technique for producing precise sintered bodies or sintered bodies with complex shapes is known, which uses a composition for producing sintered bodies containing the sinterable inorganic powder and a binder as a material. The composition for producing sintered bodies is heated and kneaded to form a raw material for the sintered body, which is then injection-molded to form a sintered body, which is then subjected to a debinding process and then sintered.
[0003] In the production of a sintered body using the composition for producing a sintered body described above, the debinding step is the most important step in order to obtain a sintered body of good quality that is free from defects such as cracks, bulges, deformation, etc. This debinding step is a step in which the binder is removed from a compact that is a compact of the composition for producing a sintered body, and known methods for this step include a method in which the compact is heated to thermally decompose and gasify the binder, and a method in which the compact is treated with a solvent to elute and remove the soluble binder components in the compact, and then the remaining binder is thermally decomposed and gasified.
[0004] Various means have been devised to suppress cracking and swelling of molded bodies during the debinding step. For example, Patent Document 1 discloses a technique relating to an injection molding composition having increased strength by blending a component containing a glycidyl group from the viewpoint of shape retention during debinding, and Patent Document 2 proposes a technique relating to an injection molding composition having an increased Vicat softening point.
[0005] Patent No. 5970794 Patent No. 4317916
[0006] However, with the techniques disclosed in Patent Documents 1 and 2, it is not possible to determine whether a defect has occurred until the sintering is actually carried out and the state of the sintered body is confirmed, and a long process and costs are required for determining whether a defect has occurred. Furthermore, when determining whether a defect has occurred based on the sintered body, it is difficult to recover the metal powder used, so the only option is to discard the defective product, and further improvement is desired from the viewpoint of recyclability.
[0007] Therefore, an object of the present invention is to provide a composition for sintered compacts and a green compact that can predict the presence or absence of defects and suppress the occurrence of defects without sintering, as well as to provide a sintered compact in which the occurrence of defects is suppressed. Another object of the present invention is to provide a method for detecting defects in sintered compacts that can predict and detect the presence or absence of defects without sintering and that enables the recycling of defective metal powder.
[0008] The present invention was made based on the above findings, and its gist is as follows: (1) A composition for sintered compacts, comprising a sinterable inorganic powder and an organic binder, characterized in that the ratio of the maximum area (A) of discontinuous organic binder portions, in which the organic binder is surrounded by the inorganic powder, to the total area (B) of the organic binder in one field of view upon cross-sectional observation is 0.5 or less (A / B≦0.5).
[0009] (2) The composition for sintered compacts according to (1), characterized in that the ratio of the maximum area (A) of the discontinuous organic binder portion to the total area (B) of the organic binder in one field of view during cross-sectional observation is 0.3 or less (A / B≦0.3).
[0010] (3) The composition for sintered compacts according to (1) or (2), characterized in that the organic binder is a pre-mixture of an aggregate resin (P) and a wax component (W).
[0011] (4) The composition for sintered compacts according to (1) or (2), characterized in that the organic binder is a pre-mixed composition containing only the aggregate resin (P).
[0012] (5) The composition for sintered compacts according to (1) or (2), wherein the organic binder contains at least a polyacetal resin, a polyolefin resin, and an epoxy resin.
[0013] (6) A green compact formed from the composition for sintered compacts according to (1) or (2).
[0014] (7) A sintered body obtained by sintering the green molded body according to (6).
[0015] (8) A method for detecting defects in a sintered body, comprising: smoothing a cross section of a composition for sintered compacts or a green compact containing a sinterable inorganic powder and an organic binder; observing the cross section; calculating the ratio of the maximum area (A) of discontinuous organic binder portions where the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view; and confirming whether or not the ratio is 0.5 or less (A / B≦0.5).
[0016] According to the present invention, it is possible to provide a composition for sintered compacts and a green compact that can predict the presence or absence of defects and suppress the occurrence of defects without sintering, and also to provide a sintered compact in which the occurrence of defects is suppressed. Furthermore, according to the present invention, it is possible to provide a method for detecting defects in a sintered compact that can predict the presence or absence of defects and detect them without sintering, and that makes it possible to recycle defective metal powder.
[0017] 1A and 1B are enlarged views of a cross section of a composition for sintered compacts, schematically illustrating the state of a sinterable inorganic powder and an organic binder. The cross section of a molded body test piece obtained in an example was observed by SEM and photographed at a magnification of 500x. (a) shows the cross section before binarization, and (b) shows the cross section after binarization.
[0018] Hereinafter, a mode for carrying out the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. The following present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0019] <Composition for sintered compact> The composition for sintered compact of the present embodiment includes a sinterable inorganic powder and an organic binder. In addition to the inorganic powder and the organic binder, the composition for sintered compact of the present embodiment can also include other additives as described below.
[0020] (Sinterable inorganic powder) The composition for a sintered compact of this embodiment contains a sinterable inorganic powder. Note that the sinterable inorganic powder may be used alone or in combination of two or more types.
[0021] In this embodiment, the sinterable inorganic powder can be appropriately selected from known inorganic powders depending on the application. For example, the sinterable inorganic powder can be selected from metal powder, alloy powder, metal carbonyl powder, and mixtures thereof. Among these inorganic powders, it is preferable to use metal powder or ceramic powder to impart functionality.
[0022] Examples of the metal powder include powders of aluminum, magnesium, barium, calcium, cobalt, zinc, copper, nickel, iron, silicon, titanium, tungsten, and metal compounds and metal alloys based on these metals. Here, the metal powder may be not only a completed alloy, but also a mixture of individual alloy components.
[0023] Examples of the ceramic powder include oxides such as zinc oxide, aluminum oxide, and zirconia; hydroxides such as hydroxyapatite; carbides such as silicon carbide; nitrides such as silicon nitride and boron nitride; halides such as fluorite; silicates such as stearite; titanates such as barium titanate and lead zirconate titanate; carbonates; phosphates; ferrite; and high-temperature superconducting materials.
[0024] The sinterable inorganic powder may be used alone or in combination with a plurality of inorganic materials, such as various metals, metal alloys, or ceramics. Particularly preferred metals and alloys include titanium alloys and stainless steel, and preferred ceramics include Al2O3 and ZrO2. Suitable titanium alloys include titanium-6 aluminum-4 vanadium alloys, and suitable stainless steels include SUS316L and SUS630.
[0025] The method for producing the sinterable inorganic powder is not particularly limited, but it is also possible to separate only the organic binder from a molded body that is predicted to be defective by using an acid or heat, and then wash the resulting inorganic powder. However, since there is a possibility that residues may adhere to the inorganic powder depending on the binder component, it is preferable to use a polyacetal resin or the like that leaves little residue after depolymerization.
[0026] (Organic Binder) The composition for a sintered compact according to the embodiment contains an organic binder in addition to the sinterable inorganic powder described above.
[0027] The resin components constituting the organic binder are sometimes collectively referred to as aggregate resin (P). The aggregate resin (P) can be pulverized and then mixed with the sinterable inorganic powder to reduce voids (gaps) that occur in the sintered body. Therefore, the particle size of the aggregate resin (P) powder is preferably such that the sieve passing rate, as measured by JIS Z 8801, is 40% or more, and more preferably 50% or more, on a 50 Mesh (300 μm) screen.
[0028] The organic binder may contain any resin component selected appropriately depending on the application, but preferably contains at least a polyacetal resin, a polyolefin resin, and an epoxy resin.
[0029] The polyacetal resin generates very little residue upon evaporation, improving the quality of the sintered body. The polyolefin resin can increase the strength of the molded body. The epoxy resin can increase the compatibility between the polyacetal resin and the polyolefin resin.
[0030] The volume percentage of the organic binder in the composition for sintered compacts of this embodiment is not particularly limited, but is preferably 25 to 60 volume %, more preferably 30 to 55 volume %, and particularly preferably 35 to 50 volume %, relative to 100 volume % of the composition for sintered compacts of this embodiment. By containing the organic binder within the above-mentioned range, it is possible to obtain a composition for sintered compacts having a melt viscosity suitable for injection molding, and to obtain a sintered product with reduced shrinkage and good dimensional accuracy.
[0031] Polyacetal Resin Examples of the polyacetal resin include polyacetal homopolymers, polyacetal copolymers, and mixtures thereof. Among these, it is preferable to use polyacetal copolymers as the polyacetal resin from the viewpoint of thermal stability. The polyacetal resins may be used alone or in combination.
[0032] The polyacetal may be used in the form of powder other than the pellets that are usually provided. The particle size of the powder is preferably D50=500 μm or less, and more preferably D50=300 μm or less.
[0033] The polyacetal homopolymer may be a polymer having an oxymethylene unit in the main chain, and both ends of the polymer may be blocked with an ester group or an ether group. The polyacetal homopolymer may be obtained from raw materials including formaldehyde and a known molecular weight modifier, and may be obtained from these raw materials by a known slurry method using a known onium salt polymerization catalyst and a hydrocarbon or the like as a solvent, such as the polymerization methods described in JP-B-47-6420 and JP-B-47-10059.
[0034] The polyacetal homopolymer is preferably one in which 99.8 mol % or more of the main chain excluding both terminals is composed of oxymethylene units, and more preferably one in which the main chain excluding both terminals is composed only of oxymethylene units.
[0035] The polyacetal copolymer includes a polymer having an oxymethylene unit and an oxyethylene unit in the main chain, and can be obtained, for example, by copolymerizing trioxane with a cyclic ether and / or a cyclic formal in the presence of a polymerization catalyst.
[0036] The trioxane is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous solution of formalin in the presence of an acid catalyst.
[0037] The cyclic ether and / or cyclic formal are components copolymerizable with the trioxane, and examples thereof include ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epibromohydrin, styrene oxide, oxatane, 1,3-dioxolane, ethylene glycol formal, propylene glycol formal, diethylene glycol formal, triethylene glycol formal, 1,4-butanediol formal, 1,5-pentanediol formal, and 1,6-hexanediol formal. Ethylene oxide and 1,3-dioxolane are particularly preferred. These may be used alone or in combination of two or more.
[0038] The polymerization catalyst used in producing the polyacetal copolymer is not particularly limited, but examples thereof include Lewis acids such as boric acid, tin, titanium, phosphorus, arsenic, and antimonides. Among these, it is particularly preferable to use one or more of boron trifluoride, boron trifluoride hydrates, and coordination complex compounds of boron trifluoride with organic compounds containing oxygen or sulfur atoms. More specifically, suitable examples include boron trifluoride, boron trifluoride diethyl etherate, and boron trifluoride-di-n-butyl etherate. These may be used alone or in combination of two or more.
[0039] The deactivation of the polymerization catalyst in the production of the polyacetal copolymer can be carried out by adding the polyacetal resin obtained by the polymerization reaction to an aqueous solution or an organic solvent solution containing at least one catalyst neutralizing deactivator, such as an amine such as ammonia, triethylamine, or tri-n-butylamine, or a hydroxide, inorganic acid salt, or organic acid salt of an alkali metal or alkaline earth metal, and stirring the resulting slurry for generally several minutes to several hours.
[0040] After the catalyst has been neutralized and deactivated, the slurry is filtered and washed to remove unreacted monomers, catalyst neutralization deactivator, and catalyst neutralization salts, and then dried.
[0041] Furthermore, the polymerization catalyst can be deactivated by contacting the polyacetal copolymer with vapor of ammonia, triethylamine, or the like, or by contacting the polyacetal resin with at least one of hindered amines, triphenylphosphine, calcium hydroxide, or the like in a mixer.
[0042] Furthermore, without deactivating the polymerization catalyst, the polyacetal copolymer can be heated in an inert gas atmosphere at a temperature below the melting point of the polyacetal copolymer, thereby reducing the volatilization of the polymerization catalyst, and the terminal stabilization treatment described below can be performed using the polyacetal copolymer.
[0043] The above-mentioned operation for deactivating the polymerization catalyst and the operation for reducing the volatilization of the polymerization catalyst can be carried out, if necessary, after pulverizing the polyacetal resin obtained by the polymerization reaction.
[0044] The aromatic dicarboxylic acids constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more.
[0045] The terminal stabilization treatment of the obtained polyacetal resin can be carried out by decomposing and removing the unstable terminals as follows: For example, the polyacetal resin can be melted using a vented single-screw extruder or a vented twin-screw extruder in the presence of a known basic substance capable of decomposing unstable terminals, such as ammonia, a fatty acid amine such as triethylamine or tributylamine, a hydroxide of an alkali metal or alkaline earth metal typified by calcium hydroxide, an inorganic weak acid salt, or an organic weak acid salt, as a notching agent, to decompose and remove the unstable terminals.
[0046] The polyacetal resin may be recycled. In the material recycling, polyacetal resin used as a product is collected, and any impurities such as grease are removed, and the resulting pulverized polyacetal resin can be used. In addition to material recycling, polyacetal resin used as a product, such as through chemical recycling, may be recycled into monomers, and the polyacetal resin produced from these monomers may be used. The recycled polyacetal resin may be used alone or mixed with non-recycled polyacetal resin.
[0047] The polyacetal resin may also be a modified polyacetal. A modified polyacetal is generally a block copolymer having a modified segment within the polyacetal. The polyacetal segment may be a homopolymer residue consisting of only oxymethylene units, or a copolymer residue in which oxymethylene units and oxyalkylene units are randomly copolymerized. The modified segment is a component that does not fall under the category of a polyacetal segment, and examples thereof include polyolefin, polyurethane, polyester, polyamide, polystyrene, and alkyl polyacrylate.
[0048] The polyacetal segment is preferably a polyacetal copolymer residue in which oxymethylene units and oxyalkylene units are randomly copolymerized, and the modified segment is preferably a polyolefin or polyurethane.
[0049] The modified segment of the modified polyacetal is preferably a polyolefin, from the viewpoint of reducing residues derived from the organic binder in the degreasing step, and specific examples thereof include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, polybutadiene, and hydrogenated polybutadiene.
[0050] From the same viewpoint, the modified segment of the modified polyacetal is more preferably polyethylene, polypropylene, or hydrogenated polybutadiene, and is particularly preferably hydrogenated polybutadiene from the viewpoint of shape retention in the degreasing step and suppression of cracking and swelling in the degreasing step.
[0051] The modified polyacetal resin may be used alone, or two or more types of modified polyacetal resins may be used together, or may be mixed with an unmodified polyacetal resin.
[0052] Polyolefin Resin The organic binder further contains a polyolefin resin in addition to the polyacetal resin described above. Here, the polyolefin resin is a homopolymer or copolymer having structural units derived from an alkene having 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms.
[0053] Specific examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, and polybutadiene. Polyethylene, polypropylene, and mixtures thereof are preferred, and polyethylene or polypropylene is more preferred from the viewpoints of shape retention during the degreasing process and suppression of cracking and swelling during the degreasing process. Suitable commercially available polyethylenes include, for example, the Suntec HD series (manufactured by Asahi Kasei), the Suntec LD series (manufactured by Asahi Kasei), the Suntec EVA series (manufactured by Asahi Kasei), Neozex, Ultozex, and Evolue (all manufactured by Prime Polymer). Examples of polypropylenes include Sumitomo Noblen (manufactured by Sumitomo Chemical), Novatec PP (manufactured by Japan Polypropylene), the SunAllomer PP series (manufactured by SunAllomer), and Prime Polypro (manufactured by Prime Polymer).
[0054] In addition, from the viewpoints of kneadability with sinterable inorganic powders and injection moldability, the polyolefin resin preferably has a melt flow index of 40 g / 10 min or more. The melt flow index of the polyolefin resin can be measured under conditions of 230°C and 2.16 kg.
[0055] Epoxy Resin The organic binder further contains an epoxy resin in addition to the polyacetal resin and polyolefin resin described above. The inclusion of the epoxy resin increases compatibility with the polyacetal resin and the polyolefin resin, and at the same time enhances interaction (adhesion) with the metal powder, thereby improving the dispersibility and sintered density of the metal powder.
[0056] The epoxy resin refers to a resin composed of an aggregate of multiple epoxy compounds, and the epoxy compound refers to a compound having an epoxy group in the molecule. The multiple epoxy compounds constituting the epoxy resin may have the same or different molecular structures. Furthermore, from the viewpoints of mixability with sinterable inorganic powders and injection moldability, the epoxy resin preferably has a melt flow index of 40 g / 10 min or more. The melt flow index of the polyolefin resin can be measured at 190°C and 2.16 kg according to ASTM-D-1238-57T.
[0057] The type of epoxy resin is not particularly limited, but examples include bisphenol A type epoxy, bisphenol F type epoxy, novolac type epoxy, aliphatic type epoxy, and epoxy resins containing glycidyl, which will be described later.
[0058] A preferred epoxy resin is a copolymer of a glycidyl ester of an unsaturated acid and an olefin, and particularly preferred is ethylene-glycidyl methacrylate copolymer (EGMA).
[0059] Here, the unsaturated acid glycidyl ester is represented by the general formula (1): (wherein R represents an alkenyl group having 2 to 18 carbon atoms, and X represents a carbonyloxy group), and has a structure in which an unsaturated acid is esterified with an alcohol compound having a glycidyl group. Specific examples of the compound include glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, and glycidyl itaconate. Of these, glycidyl methacrylate is preferably used.
[0060] In addition to the glycidyl esters, examples of the unsaturated acid and / or derivative thereof, which are optional components, include unsaturated compounds having one or more carboxylic acid groups, unsaturated compounds having one or more carboxylic acid anhydride groups, and esters of compounds having a carboxylic acid group with alkyl alcohols. Specific compounds include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, citraconic acid, and mesaconic acid, unsaturated carboxylic acid anhydrides such as maleic anhydride, vinyl esters of saturated carboxylic acids such as vinyl acetate, vinyl propionate, and vinyl butyrate, and alkyl esters of unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate. Among these, vinyl acetate, methyl acrylate, ethyl acrylate, and methyl methacrylate are preferred.
[0061] Furthermore, examples of the olefin to be copolymerized with the glycidyl ester of an unsaturated acid include α-olefins having 2 to 10 carbon atoms, and among these, ethylene, propylene, and 1-butene are particularly preferred. The method for copolymerizing the glycidyl ester of an unsaturated acid with the olefin is not particularly limited, and can be carried out by a conventionally known method.
[0062] Among the copolymers of glycidyl esters of unsaturated acids and olefins, ethylene-glycidyl methacrylate copolymer (EGMA) is preferred. Commercially available EGMA can be used, and suitable examples include Celloxide manufactured by Daicel Chemical Industries, Ltd. and Bondfast manufactured by Sumitomo Chemical Co., Ltd.
[0063] Furthermore, EGMA can be synthesized by various methods. For example, it can be produced by bulk polymerization, emulsion polymerization, solution polymerization, etc. using a free radical initiator. Representative polymerization methods include those described in Japanese Patent Publication No. 46-45085 and Japanese Patent Laid-Open Publication No. 61-127709, in which EGMA can be produced in the presence of a polymerization initiator that generates free radicals under conditions of a pressure of 500 kg / cm or more and a temperature of 40 to 300°C. Other examples include a method in which an unsaturated epoxy compound and a radical generator are mixed with a resin composed of at least one monomer selected from ethylene and olefinically unsaturated compounds other than ethylene, and the mixture is melt-graft-copolymerized in an extruder. Another method includes a method in which an unsaturated epoxy compound and an olefinically unsaturated compound are copolymerized in an inert medium such as water or an organic solvent in the presence of a radical generator.
[0064] The copolymer of the unsaturated acid glycidyl ester and the olefin resin has an unsaturated acid glycidyl ester unit content of 1 to 25 wt%, preferably 3 to 20 wt%, and more preferably 13 to 20 wt%. Having an unsaturated acid glycidyl ester unit content of 1% or more enhances the interaction with other resin components and metal powders, leading to improved dispersibility. Furthermore, having an unsaturated acid glycidyl ester unit content of 25% or less provides excellent thermal stability during kneading and injection molding.
[0065] The content of the unsaturated acid glycidyl ester can be determined by measuring the infrared absorption spectrum of a press sheet of the ethylene polymer having an epoxy group. The absorbance of the characteristic absorption in the infrared absorption spectrum is corrected by the thickness of the sheet used for the measurement, and the content of the unsaturated compound having a glycidyl group is determined by a calibration curve method based on the corrected absorbance. The peak of the characteristic absorption is at 910 cm -1 This can be used as an indicator as it often appears near
[0066] Furthermore, when EGMA is used as the epoxy resin, the melt flow index of the EGMA is preferably 3 g / 10 min or more and 400 g / 10 min or less, more preferably 10 g / 10 min or more and less than 400 g / 10 min, and even more preferably 50 g / 10 min or more and less than 400 g / 10 min. Having the melt flow index of EGMA within the above range tends to suppress separation from other resins during injection molding and shorten debinding time. The melt flow index of the EGMA can be measured at 190°C and 2.16 kg according to ASTM-D-1238.
[0067] (Compatibilizer) The composition for sintered compacts of this embodiment may further contain a compatibilizer. By including the compatibilizer, the quality of the composition for sintered compacts can be further improved. The compatibilizer has properties different from those of the resin described above and the wax described below, and has the effect of further increasing the compatibility between the metal and the resin and wax, for example, by having an effect similar to that of a surfactant.
[0068] Examples of the compatibilizer include Sannix (Sanyo Chemical), Sunflex (Sanyo Chemical), Tafmer DF&A (Mitsui Chemicals), Tafmer XM (Mitsui Chemicals), Tafmer BL (Mitsui Chemicals), Tafmer M (Mitsui Chemicals), Tafmer PN (Mitsui Chemicals), and Maricon (Osaka Gas Chemicals).
[0069] (Fluidity Imparting Agent) The composition for sintered compact of this embodiment preferably further contains a fluidity imparting agent in addition to the sinterable inorganic powder and organic binder described above. By including the fluidity imparting agent, the fluidity of the composition for sintered compact can be further improved.
[0070] The fluidity imparting agent is a compound other than the resin components such as the polyacetal resin, polyolefin resin, and epoxy resin, and examples thereof include waxes. For convenience, the present specification distinguishes between those with a melting point of 100°C or less as "wax" and those with a melting point above 100°C as "resin." These fluidity imparting agents are collectively referred to as the wax component (W).
[0071] Examples of waxes include paraffin wax, polyethylene wax, polypropylene wax, carnauba wax, polyethylene glycol, polytetramethylene glycol, polytetraethylene glycol, polyisobutylene, microcrystalline wax, montan wax, beeswax, Japan wax, synthetic wax, poly-1,3-dioxolane, poly-1,3-dioxepane, etc. Among these, paraffin wax, polyethylene glycol, and polytetramethylene glycol are preferred from the viewpoint of achieving even better fluidity of the composition for sintered compacts in injection molding. Furthermore, one type of wax may be used alone, or multiple types may be used in combination.
[0072] In the resin composition for a sintered body of this embodiment, the ratio of the maximum area (A) of the discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view during cross-section observation is 0.5 or less (A / B≦0.5).
[0073] The discontinuous organic binder portion is a region of the organic binder that is surrounded by inorganic powder. Since the volatilization path during degreasing is blocked, if the resin volatilizes within this region, the volatilized binder that is not completely released to the outside may cause swelling or cracking. Therefore, in the resin composition for sintered bodies of this embodiment, by reducing the ratio of the maximum area (A) of the discontinuous organic binder portion where the organic binder is surrounded by inorganic powder to the total area (B) of the organic binder in one field of view during cross-section observation (specifically, to 0.5 or less (A / B≦0.5)), the occurrence of swelling and cracking due to the volatilized binder can be reduced, thereby increasing the yield of the sintered body. In addition, since the ratio (A / B) can be confirmed at the resin composition for sintered bodies or green compact stage, it is possible to predict the presence or absence of defects in the sintered body without performing a sintering process, and it is also possible to recycle defective metal powder. From the same viewpoint, the ratio (A / B) is preferably 0.3 or less, and more preferably 0.2 or less.
[0074] FIG. 1 is an enlarged view of a portion of the cross section of the composition for sintered compacts of this embodiment, schematically illustrating the sinterable inorganic powder and organic binder. As shown in FIG. 1, the discontinuous organic binder portion refers to the portion surrounded by the sinterable inorganic powder. When observing the cross section of the composition for sintered compacts of this embodiment, multiple discontinuous organic binder portions are observed, and the area of the largest discontinuous organic binder portion among the discontinuous organic binder portions observed in one field of view is defined as the maximum area (A). Furthermore, the total area (B) of the organic binder is the total area of the organic binder portions observed in one field of view.
[0075] The conditions for observing the cross section of the composition for sintered compacts of this embodiment are not particularly limited as long as they allow for accurate confirmation of the area of the organic binder. For example, observation can be performed using a scanning electron microscope (SEM). While the optimal magnification varies depending on the particle size of the inorganic powder, it is desirable to select an observation method with as wide a field of view as possible at a magnification that allows for clear identification of the organic binder. For example, if the average particle size of the inorganic powder is approximately 10 μm, a magnification of approximately 500x is preferred, and if the average particle size of the inorganic powder is approximately 0.1 μm, a magnification of approximately 2500x is preferred.
[0076] Furthermore, from the viewpoint of determining the area of the organic binder with higher accuracy, it is preferable to obtain a cross-sectional image of the composition for sintered compacts of this embodiment using an SEM, and then perform a binarization process on the cross-sectional image to distinguish between the sinterable inorganic powder and the organic binder. For example, Otsu's binarization can be used as this binarization process. Furthermore, when performing the binarization process, it is preferable to distinguish noise such as processing marks from the sinterable inorganic powder and the binder, and it is necessary to control the threshold value for binarization and set it to a value that can distinguish between the inorganic powder and the organic binder.
[0077] Furthermore, although the cross section of the composition for sintered compacts of this embodiment can be obtained by a microtome, polishing, or the like, it is preferable to obtain the cross section by Ar ion milling, because this makes the cross section as smooth as possible and minimizes processing marks, thereby minimizing noise generated during the binarization process described below and enabling clear binarization.
[0078] When a cross-section of a composition for sintered compacts is observed, if the ratio of the maximum area (A) of the discontinuous organic binder portion where the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view exceeds 0.5 (A / B>0.5), the composition for sintered compacts is judged to be defective. A composition for sintered compacts judged to be defective is expected to cause a decrease in density and strength when subsequently sintered. This ratio is discovered when the composition of the organic binder, the properties of the sinterable inorganic powder, or processing conditions such as kneading and molding conditions are not within the preferred range, and is said to be correlated with the dispersibility of the organic binder or the sinterable inorganic powder.
[0079] <Method for Producing Composition for Sintered Compact> (Kneading Method) The method for producing the composition for sintered compact of this embodiment is not particularly limited, and the composition can be produced by a known method. For example, the composition can be produced by mixing the above-mentioned sinterable inorganic powder and organic binder, as well as other optional components, using, for example, a Henschel mixer, a tumbler, a V-shaped blender, or the like, and then melt-kneading the mixture in a semi-molten state using a kneader such as a single-screw extruder, a twin-screw extruder, a heating roll, a kneader, or a Banbury mixer. The obtained composition for sintered compact can be in various forms, such as strands or pellets.
[0080] When kneading is performed using a pressure kneader, the kneading temperature is preferably set to 160°C to 210°C, more preferably 170°C to 190°C. The blade rotation speed is preferably 10 rpm to 50 rpm, more preferably 15 rpm to 40 rpm. Furthermore, the kneading time is preferably 45 minutes or more and 2 hours or less. By kneading within the above conditions, it is possible to improve the compatibility between the resins and suppress the organic binder phenomenon caused by thermal decomposition.
[0081] (Pre-mixing) The organic binder can be pre-mixed (pre-mixed) before being mixed with the sinterable inorganic powder. Specifically, pre-mixing can be performed by kneading the aggregate resin (P) using a kneader such as a pressure kneader, a twin-screw extruder, a heated roll, a kneader, or a Banbury mixer, and then kneading the aggregate resin (P) and the wax component (W) using a kneader such as a Henschel mixer, a tumbler, a V-shaped blender, or a mixer / stirrer. It is also possible to perform only one of these pre-mixing processes. The yield of the sintered body can be improved by subsequently mixing and using the pre-mixed organic binder with the sinterable inorganic powder.
[0082] <Green molded body> The green molded body of this embodiment is formed using the composition for a sintered molded body of this embodiment described above as a raw material. The green molded body of this embodiment is obtained by using the composition for a sintered molded body in a screw or piston injection molding machine.
[0083] In the injection molding, the cylinder temperature is preferably set to 160 to 210° C., more preferably 170 to 190° C. Setting the temperature to 160° C. or higher can improve the fluidity of the resin, while setting it to 200° C. or lower can reduce mold contamination due to resin decomposition.
[0084] The mold temperature is preferably 30 to 90° C., and more preferably 50 to 70° C. By setting the mold temperature to 30° C. or higher, dimensional stability during molding is improved, and by setting it to 90° C. or lower, it is possible to prevent poor appearance of the green molded product caused by waxes with a melting point of 100° C. or lower.
[0085] <Sintered Body> The sintered body of this embodiment is obtained by sintering the above-described green body of this embodiment.
[0086] The green compact can be placed in a sealed debinding / sintering furnace and debinding / sintered under desired conditions to produce a debinding body and a sintered body.
[0087] In the case of debinding by heating, the debinding is carried out by raising the temperature from room temperature to about 500-600°C in a nitrogen or argon atmosphere. A fluidity imparting agent may be dissolved in a solvent before heating. The temperature is then raised to the sintering temperature of the sinterable inorganic powder to obtain a sintered compact.
[0088] In the case of degreasing with acid, nitric acid gas is passed through in a nitrogen atmosphere and the temperature is raised from room temperature to 110-120°C. The temperature is then raised to the sintering temperature of the sinterable inorganic powder to obtain a sintered compact.
[0089] <Method for detecting defects in sintered bodies> In this embodiment, the method for detecting defects in sintered bodies involves smoothing the cross section of a composition for sintered bodies or a green body containing a sinterable inorganic powder and an organic binder, observing the smoothed cross section, calculating the ratio of the maximum area (A) of discontinuous organic binder portions where the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view, and confirming whether or not this ratio is 0.5 or less (A / B≦0.5). This makes it possible to predict and detect defects without actually performing sintering.
[0090] The conditions for the composition for sintered compact and the green compact are the same as those for the composition for sintered compact and the green compact of the present embodiment described above.
[0091] Furthermore, in the method for detecting defects in sintered bodies according to this embodiment, when a sample (a composition for sintered body or a green body) in which defects are predicted is found, the organic binder can be separated and removed from the sample by acid, heating, washing, etc., thereby recycling the sinterable inorganic powder. This further reduces the cost of producing sintered bodies. Note that once a sintered body has been produced, it is difficult to extract only the inorganic powder from a sample in which a defect has been found because the powder is molten.
[0092] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.
[0093] <Constituent Components> The components contained in each sample of the Examples and Comparative Examples are as follows: (A) Polyacetal resin Tenac (registered trademark)-C FF520 manufactured by Asahi Kasei Corporation
[0094] (B) Epoxy resin (B-1) Bondfast CG5001 manufactured by Sumitomo Chemical Co., Ltd. (B-2) Bondfast BF-7B manufactured by Sumitomo Chemical Co., Ltd. (B-3) Bondfast BF-7M manufactured by Sumitomo Chemical Co., Ltd.
[0095] (C) Polyolefin resin (C-1) Polypropylene: SunAllomer PP PMB60A manufactured by SunAllomer Co., Ltd. (C-2) Polyethylene: Suntec (registered trademark) HDPE J300 manufactured by Asahi Kasei Corporation
[0096] (D) Fluidity imparting agent (D-1) Paraffin wax: Paraffin wax SP-0145 manufactured by Nippon Seiro Co., Ltd. (D-2) Carnauba wax: Refined carnauba wax No. 1 manufactured by Nippon Wax Co., Ltd. (D-3) Montan wax: LicoWax E manufactured by Clariant Japan
[0097] (E) Compatibilizer (E-1) Mitsui Chemicals, Inc., Tafmer PN-2070 (E-2) Sanyo Chemicals, Inc., Sannix GL-3000 (E-3) Mitsui Chemicals, Inc., Tafmer XM-7070S (E-4) Mitsubishi Chemical Corporation, PTMG3000
[0098] Aggregate Resin (P) The above components (A), (B), (C), and (E) are collectively referred to as aggregate resin (P). Wax (W) In the following description, the fluidity imparting agent (D) is referred to as wax (W).
[0099] [Examples 1 to 5 and Comparative Examples 1 to 2] Each material was weighed to achieve the blending ratios listed in Tables 1 and 2. For samples marked with a circle in the "Pulverization" column for aggregate resin (P), the aggregate resin (P) was kneaded at 180°C using a twin-screw extruder, followed by freeze-pulverization (-196°C) to obtain a powder with a sieve pass rate of 55% (50 Mesh, 300 μm). For samples marked with a circle in the "Pre-mixing" column for aggregate resin (P) and wax (W), the aggregate resin (P) was kneaded at 180°C using a twin-screw extruder, followed by kneading the wax (W) and aggregate resin (P) at 300 rpm for approximately 5 minutes using a Henschel mixer. Furthermore, for samples with a mark "〇" for both "Pulverization" and "Pre-mixing" for the aggregate resin (P), the aggregate resin (P) was kneaded using a twin-screw extruder at 180°C, followed by freeze-grinding (-196°C) to obtain a powder with a sieve pass rate of 55% on a 50Mesh (300μm) screen. The wax (W) and aggregate resin (P) were then kneaded using a Henschel mixer at 300 rpm for approximately 5 minutes. Each kneaded product obtained by the above method was prepared by using SUS316L (average particle size 10μm) as the sinterable inorganic powder, weighing out 65% by volume of the sinterable inorganic powder and 35% by volume of the organic binder, and then using a pressure kneader under the conditions of temperature, blade rotation speed, and kneading time shown in Tables 1 and 2 to produce each sample of the composition for sintered compacts. Thereafter, each sample of the composition for sintered compact obtained was cooled, crushed, and pelletized to prepare a raw material for injection molding, and then a plurality of molded test pieces were prepared using an injection molding machine (ROBOSHOT α-50iA manufactured by Fanuc Corporation) under the molding temperature, mold temperature, injection pressure, and injection rate conditions shown in Tables 1 and 2. The prepared molded test pieces were all tensile type No. 2 dumbbell test pieces conforming to JIS K 6251, with a total length of 100 mm and a thickness of 3 mm.
[0100] Each of the prepared green test specimens was degreased by heating or acid. The prepared green test specimens were placed in a degreasing furnace at 50 mm intervals and then degreased and sintered as described below to obtain sintered samples. (Thermal Degreasing) The degreasing furnace was purged with nitrogen gas and heated to 150°C at a rate of 50°C / hr. The temperature was then increased from 150 to 200°C at a rate of 30°C / hr and held for 1 hour. The temperature was then increased from 200 to 400°C at a rate of 30°C / hr, and then increased from 400 to 600°C at a rate of 120°C / hr. The furnace was then cooled to obtain degreased samples. (Acid Degreasing) The degreasing furnace was first heated to 110°C and purged with nitrogen at 500 L / h for 30 minutes. Then, 98% nitric acid was supplied at 30 mL / h while maintaining the nitrogen purge. The acid supply was maintained for 2.5 hours, followed by replacing the furnace with nitrogen at 500 L / h for 45 minutes and cooling to room temperature to obtain degreased samples. (Sintering) The obtained degreased samples were sintered by gradually increasing the temperature from room temperature at 200°C / hr in an argon atmosphere and maintaining the maximum temperature at 1350°C for 2 hours to obtain sintered samples.
[0101] <Evaluation> (1) Cross-section preparation Cross-sections were prepared from each prepared molded body test piece using Ar ion milling (X) or a microtome (Y). (Ar ion milling X) The center of the parallel section of each molded body test piece was cut in the direction perpendicular to the flow using a diamond disc cutter, and then a cross-section was prepared using Ar ion milling. The Ar ion milling device used was an IM-4000 (manufactured by Hitachi High-Technologies Corporation). (Microtome Y) The center of the parallel section of each molded body test piece was cut in the direction perpendicular to the flow using a diamond disc cutter, and then a cross-section was prepared using a microtome. The microtome device used was a rotary microtome (manufactured by Leica).
[0102] (2) Cross-Section Observation The cross-sections were observed using a SEM, and 10 images were taken at 500x magnification. A JSM IT-800 (manufactured by JEOL Ltd.) was used. (Binarization) The obtained images were separated into the sinterable inorganic powder portion and the organic binder portion using Otsu's binarization method. Figure 2(a) shows an example of a cross-section of a molded body test piece before binarization, and (b) shows an example of a cross-section of a molded body test piece after binarization. After binarizing the cross-sectional image, the organic binder portion was separated into discontinuous organic binder portions (A) and the total binder area (B). The ratio (A / B) of the largest discontinuous organic binder portion (A) to the total binder area (B) was calculated, and the results are shown in Tables 1 and 2. Regarding Example 1, cross-sections of 10 random particles were observed not only for the molded body but also for the injection molding raw material sample. Similar results (A / B ratio) were obtained for the molded body.
[0103] (3) Density of Sintered Body The density (g / cm) of the obtained sintered body was measured in accordance with JIS Z 8807 using an electronic hydrometer (manufactured by Alpha Mirage) at a water temperature of 25°C. 3 The number of samples was 30, and the average relative densities of the SUS316L powder used are shown in Tables 1 and 2.
[0104] (4) Tensile strength of sintered body A tensile test was carried out on the obtained sintered body to measure its tensile strength. The measurement was carried out using a 5900R 5582 model universal testing machine (manufactured by Instron Corporation) at a test speed of 3.0 mm / min with a chuck distance of 30 mm. The number of samples was 30.
[0105] (5) Yield rate of sintered body Based on the results of (3) Density of sintered body and (4) Tensile strength of sintered body, samples with a relative density of 95% or more and a tensile strength of 480 MPa or more were considered to be good products, and the percentage of good products out of 30 samples was calculated as the yield rate. The results are shown in Tables 1 and 2.
[0106] (6) Recyclability of Metal Powders: In the cross-sectional observation in the above evaluation (2), for images in which the ratio (A / B) of the largest discontinuous organic binder portion (A) to the total binder area (B) was 0.5 or greater, the compacts were heated at 500°C for 5 hours to remove the binder, and then immersed in o-dichlorobenzene at 150°C for cleaning to obtain inorganic powders. Sintered bodies were produced using the obtained inorganic powders under the conditions of Example 1, and samples with equivalent yields were obtained in all cases. Furthermore, for images in which the ratio (A / B) of the largest discontinuous organic binder portion (A) to the total binder area (B) was 0.5 or greater, inorganic powders were extracted from some of the compacts using the method described above. Sintered bodies were produced using the obtained inorganic powders under the same conditions as in Example 1, and samples with equivalent yields were obtained.
[0107] From the results in Tables 1 and 2, it can be seen that the yield rate of the sintered bodies obtained in each Example is significantly higher than that of the sintered body of Comparative Example 1. It can also be seen that the yield rate of the sintered bodies obtained in each Example is significantly higher than that of the sintered body of Comparative Example 1.
[0108] According to the present invention, it is possible to provide a composition for sintered compacts and a green compact that can predict the presence or absence of defects and suppress the occurrence of defects without sintering, and also to provide a sintered compact in which the occurrence of defects is suppressed. Furthermore, according to the present invention, it is possible to provide a method for detecting defects in a sintered compact that can predict the presence or absence of defects and detect them without sintering, and that makes it possible to recycle defective metal powder.
Claims
1. A composition for sintered compacts comprising a sinterable inorganic powder and an organic binder, characterized in that the ratio of the maximum area (A) of discontinuous organic binder portions in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view when observing a cross section is 0.5 or less (A / B≦0.5).
2. A composition for sintered compacts as described in claim 1, characterized in that the ratio of the maximum area (A) of the discontinuous organic binder portion to the total area (B) of the organic binder in one field of view during cross-sectional observation is 0.3 or less (A / B≦0.3).
3. A composition for sintered compacts according to claim 1 or 2, characterized in that the organic binder is a pre-mixture of an aggregate resin (P) and a wax component (W).
4. A composition for sintered compacts according to claim 1 or 2, characterized in that the organic binder is a premixed mixture of only the aggregate resin (P).
5. A composition for sintered compacts according to claim 1 or 2, characterized in that the organic binder contains at least a polyacetal resin, a polyolefin resin and an epoxy resin.
6. A green compact formed from the composition for sintered compacts according to claim 1 or 2.
7. A sintered body obtained by sintering the green molded body according to claim 6.
8. A method for detecting defects in a sintered body, comprising: smoothing a cross-section of a composition for sintered bodies or a green body containing a sinterable inorganic powder and an organic binder; observing the cross-section; calculating the ratio of the maximum area (A) of discontinuous organic binder portions in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view; and verifying whether this ratio is 0.5 or less (A / B≦0.5).
Citation Information
Patent Citations
Injection molding composition
JP2003252676A
Composition for sintered compact and sintered compact
WO2022215472A1
Composition for inorganic powder injection molding, and molded body and sintered body each using same