Filler for ion exchange chromatography, method for producing same, and method for measuring hemoglobin component
Core-shell particles with specific characteristics address the challenge of high separation performance at reduced column pressure in ion exchange chromatography, enabling accurate hemoglobin measurement and efficient production, particularly for HbA1c and other hemoglobin species.
Patent Information
- Application Number
- PCT/JP2024/012138
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing ion exchange chromatography packing materials face challenges in achieving high separation performance at reduced column pressure, leading to inefficient separation of hemoglobins like HbA1c, and require improved manufacturing methods for efficient production.
Development of core-shell type particles with a cation exchange group, having a specific particle size distribution and cation exchange capacity, formed through seed polymerization and subsequent polymerization of a cation exchange group-containing monomer, which reduces column pressure and enhances separation performance.
The core-shell particles achieve high separation performance for hemoglobins, including HbA1c, with reduced column pressure, enabling accurate measurement and efficient production, and can simultaneously separate components like HbA1a, HbA1b, and HbF with improved resolution.
Smart Images

Figure JP2024012138_03102024_PF_FP_ABST
Abstract
Description
Packing material for ion exchange chromatography, its manufacturing method and method for measuring hemoglobins
[0001] The present invention relates to a packing material for ion exchange chromatography, a method for producing the same, and a method for measuring hemoglobins.
[0002] Ion-exchange liquid chromatography is widely used for analyzing components in samples in various fields, including organic chemistry, biochemistry, and medicine. This method separates target substances by utilizing the electrostatic interaction between the ion-exchange groups of the packing material and the ions in the target substances. It can be divided into cation-exchange and anion-exchange methods. The former separates cationic substances using a column packing material with anionic functional groups as cation-exchange groups, while the latter separates anionic substances using a column packing material with cationic functional groups as anion-exchange groups.
[0003] Ion exchange chromatography, with its high accuracy and rapid measurement time, is an effective method for separating and analyzing various biologically relevant substances, such as hemoglobins. Hemoglobin (also referred to as Hb) non-enzymatically binds (i.e., glycates) with blood glucose and its metabolites to form glycated Hb. HbA1, which is the glycated form of HbA, which accounts for the majority of total Hb, is not strictly the entirety of glycated hemoglobin, but is often clinically treated as synonymous with glycated hemoglobin. HbA1 can be further separated into A1a, A1b, and A1c. Of these, HbA1c reflects the average glucose concentration in the blood over the past one to two months and is therefore widely used as a test item for diabetes screening and for assessing the glycemic control status of diabetic patients. Other known Hb types include HbA0, HbA2, HbC, HbD, HbE, HbF, and HbS.
[0004] Regarding ion exchange chromatography technology, Patent Document 1 discloses a method for measuring HbA1c using a column packing material comprising core particles made of a crosslinked polymer, a nonionic hydrophilic polymer layer polymerized on the surface of the core particles, and a compound having an ion exchange group bound to the polymer layer. Patent Document 2 discloses a method for separating HbA0, HbA2, HbE, etc. using a packing material obtained by introducing an alkane or aromatic to the surface of a crosslinked polymer particle via oxygen, further introducing a polyether, and introducing a cation exchange group to the other end of the polyether. Patent Document 3 discloses a carrier for separating HbA0, HbA1c, etc., obtained by adding a polymerizable monomer to a seed polymer, followed by seed polymerization to obtain an enlarged polymer, and then introducing a cation exchange group.
[0005] JP 2010-112794 A JP 2018-017560 A JP 3-82963 A
[0006] As mentioned above, Patent Documents 1 to 3 propose various packing materials for use in ion exchange chromatography. However, there is room for improvement in order to enable packing materials to exhibit sufficiently high separation performance even at low column pressures. There is also room for improvement in order to manufacture packing materials more efficiently and simply. For example, Example 3 of Patent Document 2 discloses that seed particles are reacted with a monomer to obtain crosslinked polymer particles, which are then reacted with benzenemethanol or allyl glycidyl ether and further sulfonic acid groups are introduced to obtain a packing material, which is then packed into a column to separate hemoglobin. However, with such a method, there is room for improvement in separation performance, as some components are eluted in a state where they are not clearly separated.
[0007] The present invention has been made in view of the above-mentioned current situation, and aims to provide a packing material for ion exchange chromatography that has an extremely high level of separation performance even when the column pressure is reduced and is particularly useful for measuring hemoglobins such as hemoglobin A1c, and a method for producing the packing material efficiently and simply. Another aim of the present invention is to provide a method for measuring hemoglobins that can measure hemoglobins with extremely high accuracy.
[0008] Disclosure 1 relates to a packing material for use in ion exchange chromatography, the packing material being core-shell particles comprising a core portion and a shell portion covering at least a portion of the core portion, with cation exchange groups on the surface of the shell portion, and the CV value (%) represented by the following formula (1): CV value (%) = (standard deviation of particle size / average particle size) × 100 (1) is 18% or less. Disclosure 2 relates to the packing material for ion exchange chromatography of Disclosure 1, in which the average particle size of the core-shell particles is 3.0 to 10.0 μm. Disclosure 3 relates to the packing material for ion exchange chromatography of Disclosure 1 or 2, in which the core portion includes seed particles. Disclosure 4 relates to the packing material for ion exchange chromatography of any one of Disclosures 1 to 3, in which the shell portion is formed using a cation exchange group-containing polymerizable monomer. Disclosure 5 relates to the packing material for ion exchange chromatography of Disclosure 4, in which the cation exchange group-containing polymerizable monomer includes a sulfonic acid group and a vinyl group. Disclosure 6 relates to the ion exchange chromatography packing of any one of Disclosures 1 to 5, which is used for measuring hemoglobins by ion exchange chromatography. Disclosure 7 relates to a method for measuring hemoglobins by ion exchange chromatography, using the ion exchange chromatography packing of any one of Disclosures 1 to 6 as a column packing. Disclosure 8 relates to the hemoglobin measurement method of Disclosure 7, which is a method for measuring at least hemoglobin A1c. Disclosure 9 relates to the hemoglobin measurement method of Disclosure 7, which is a method for simultaneously measuring at least hemoglobin A1c and hemoglobin F. Disclosure 10 relates to a method for producing the ion exchange chromatography packing of any one of Disclosures 1 to 6, which includes a step (1) of polymerizing a first composition containing seed particles and a polymerizable monomer, and a step (2) of adding a second composition containing a cation exchange group-containing polymerizable monomer and polymerizing the resulting mixture. The present invention is described in detail below.
[0009] As a result of extensive research into packing materials used in ion exchange chromatography, the present inventors have discovered that core-shell particles comprising a core and a shell covering at least a portion of the core, with cation exchange groups on the surface of the shell, and with a CV value within a predetermined range, exhibit extremely high levels of separation performance even at reduced column pressure. Furthermore, among the above core-shell particles, they have found that core-shell particles (also referred to as seed core particles) obtained by forming a core (also referred to as seed core particles) by seed polymerization and then forming a shell using a polymerizable monomer exhibit extremely high levels of separation performance compared to, for example, particles obtained by forming a core by suspension polymerization and then forming a shell, or particles obtained by surface-treating seed core particles. This is how the present invention was completed.
[0010] The packing material for ion exchange chromatography (hereinafter also simply referred to as "packing material") of the present invention is a core-shell particle having a core and a shell covering at least a portion of the core, and having cation exchange groups on the surface of the shell. The shape of the particle is not particularly limited, but is preferably spherical. In particular, it is more preferable that the shape of the core-shell particle is a perfect sphere.
[0011] In this specification, "spherical" means that the average sphericity is 0.8 or more. The sphericity (minor diameter / major diameter) can be measured by analyzing an electron micrograph taken with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) using an image analyzer. The average sphericity can be calculated by visually determining the minor diameter and major diameter of, for example, 100 particles randomly selected from the electron micrograph and calculating the average value of the sphericity.
[0012] The packing material has a CV value (also referred to as the CV value of particle size distribution) of 18% or less, expressed by the following formula (1): CV value (%) = (standard deviation of particle size / average particle size) × 100 (1). This allows the packing material to maintain an extremely high level of separation performance even when the column pressure is reduced. The CV value is preferably 18.0% or less, more preferably 16.0% or less, even more preferably 15.0% or less, even more preferably 14.0% or less, and most preferably 12.0% or less. A CV value of 10.0% or less is also preferable. Normally, high column pressure requires a measuring device with pressure resistance, which can lead to concerns about device component failure and increased costs, as well as increased strain on the packing material, which may affect separation performance and measured values. However, the use of the packing material of the present invention allows the column pressure to be reduced, eliminating these concerns.
[0013] In this specification, the term "column pressure" refers to the liquid pressure of an eluent flowing into a separation column in ion exchange chromatography. Specifically, the column pressure is measured in an ion exchange chromatography apparatus by a pressure gauge installed in the flow path of the eluent flowing into the separation column. The pressure gauge used to measure this column pressure is not particularly limited as long as it is one that is commonly used in ion exchange chromatography apparatuses. For example, a Bourdon tube pressure gauge specified in JIS B7505 (1980) is preferably used.
[0014] The packing material preferably has a standard deviation of particle size of 1.8 μm or less, more preferably 1.5 μm or less, even more preferably 1.2 μm or less, still more preferably 1.0 μm or less, and most preferably 0.9 μm or less, thereby further enhancing the effect of maintaining an extremely high level of separation performance even when the column pressure is reduced.
[0015] The packing material (i.e., the core-shell particles) more preferably has an average particle size of 1.0 to 10.0 μm. Within this range, the separation performance of the packing material is further enhanced. The lower limit of the average particle size is more preferably 2.0 μm or more, and even more preferably 3.0 μm or more. The upper limit of the average particle size is more preferably 9.0 μm or less, and even more preferably 8.0 μm or less. The average particle size of the core-shell particles is preferably in the range of 3 to 10 μm, more preferably 3.0 to 10.0 μm, even more preferably 3.0 to 9.0 μm, and particularly preferably 3.0 to 8.0 μm. While reducing the particle size of a packing material typically increases the specific surface area in a column, improving separation performance, it can also increase column pressure. However, the packing material of the present invention is extremely useful because it can exhibit extremely high levels of separation performance while sufficiently reducing column pressure, even within the small particle size range described above.
[0016] In this specification, the standard deviation and average particle size of the filler particle size are both values based on the number of particles and are determined by the following measurement method. (Measurement of standard deviation and average particle size of particle size) The particle size distribution is measured using a Coulter counter (manufactured by Beckman Coulter, Inc. under the trade name "Multisizer 4e", manufactured in 2021), and the number average particle size and standard deviation of particle size are calculated. However, to measure the particle size distribution, either a 10 μm aperture with a measurable range of 0.2 μm to 6 μm, a 30 μm aperture with a measurable range of 0.6 to 18 μm, or a 100 μm aperture with a measurable range of 2.0 to 60 μm is used. The aperture used is appropriately selected to suit the particle size range of the particles to be measured. The measurement sample is a dispersion prepared by dispersing 1 g of each filler in 5 mL of pure water. A beaker filled with a measurement electrolyte (trade name "ISOTON (registered trademark) II" manufactured by Beckman Coulter, Inc.) is placed in the measuring section of a Coulter counter, and the dispersion liquid is dropped into the beaker while gently stirring the contents of the beaker. After the reading of the concentration meter on the Coulter counter main screen is adjusted to 5 to 10%, measurement is started. The contents of the beaker are gently stirred during measurement, and the measurement is stopped when 100,000 particles have been measured.
[0017] The packing material preferably has a cation exchange capacity of 0.1 to 150 μeq / gel mL, more preferably 0.1 to 100 μeq / gel mL. This further enhances the separation performance of the packing material. The lower limit of the cation exchange capacity is more preferably 1 μeq / gel mL or more, even more preferably 10 μeq / gel mL or more, particularly preferably 20 μeq / gel mL or more, and most preferably 40 μeq / gel mL or more. The upper limit of the cation exchange capacity is more preferably 90 μeq / gel mL or less, even more preferably 80 μeq / gel mL or less.
[0018] In this specification, the cation exchange capacity of a packing material is determined by the following measurement method. (Measurement of Cation Exchange Capacity) A target sample (packing material) is packed into a column with an inner diameter of 4.6 mm and a length of 8 mm. A 0.1 mol / L hydrochloric acid solution is passed through this column at a flow rate of 1.0 mL / min for 10 minutes, followed by ion-exchange water at a flow rate of 1.0 mL / min until the electrical conductivity of the column eluate decreases and then stabilizes. Thereafter, a 0.5 mol / L aqueous sodium chloride solution is passed through the column at a flow rate of 1.0 mL / min for 1 minute, and the treated solution is recovered. The treated solution is then automatically titrated with a 0.01 mol / L aqueous sodium hydroxide solution, with the neutralization point of the electrical conductivity as the endpoint, to measure the electrical conductivity.
[0019] As described above, the filler is a core-shell particle, which has a core and a shell that covers at least a part of the core, and has cation exchange groups on the surface of the shell.
[0020] The shape of the core is not particularly limited, but is preferably spherical, and more preferably a perfect sphere.
[0021] The core preferably includes seed particles. The seed particles can be obtained by polymerizing a monomer using a polymerization method such as dispersion polymerization, emulsion polymerization, soap-free emulsion polymerization, or suspension polymerization. Among these, soap-free emulsion polymerization is preferred. This allows the seed particles to be free of any dispersant or emulsifier. The polymerization conditions are not particularly limited.
[0022] The monomer for obtaining the seed particles is not particularly limited as long as it is a compound having a polymerizable group, and one or more types can be used. The polymerizable group is preferably a group containing an unsaturated double bond, such as a (meth)acryloyl group, a (meth)acrylamide group, a vinyl group, an allyl group, an ethynyl group, or a styryl group, and one or more of these groups are contained in the compound. Among these, a (meth)acryloyl group and / or a vinyl group is more preferred.
[0023] The monomer preferably contains at least one monomer selected from the group consisting of aliphatic monomers having a linear or branched aliphatic hydrocarbon group and aromatic monomers.
[0024] Examples of the aliphatic hydrocarbon group constituting the aliphatic monomer include methyl, ethyl, propyl, butyl (n-butyl, tert-butyl), pentyl, hexyl, and octyl groups. Among linear or branched aliphatic hydrocarbon groups, tert-butyl is preferred. As the aliphatic monomer, tert-butyl(meth)acrylate is preferred.
[0025] The aromatic monomer is preferably an aromatic monomer having a vinyl group and / or a (meth)acryloyl group.
[0026] Examples of the aromatic monomer having a vinyl group include styrene-based monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, dimethylstyrene, ethylstyrene, propylstyrene, p-t-butylstyrene, p-methoxystyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, and bromostyrene; monofunctional monomers such as vinylnaphthalene, 4-vinylbiphenyl, and p-styryltrimethoxysilane; and polyfunctional monomers such as divinylbenzene, divinylnaphthalene, and divinylbiphenyl. Among these, it is preferable to use at least a styrene-based monomer as the aromatic monomer having a vinyl group, and styrene is more preferable.
[0027] Examples of the aromatic monomer having a (meth)acryloyl group include benzyl (meth)acrylate, phenyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenoxybenzyl (meth)methacrylate, biphenylmethyl (meth)acrylate, and phenol EO-modified (meth)acrylate. Among these, aromatic monomers having a methacryloyl group are preferred. Benzyl (meth)acrylate is also preferred, and benzyl methacrylate is more preferred.
[0028] The seed particles are preferably polymers obtained using at least one monomer selected from the group consisting of aliphatic monomers and aromatic monomers. That is, the seed particles are preferably at least one polymer selected from the group consisting of polymer (a) obtained using only aliphatic monomers, polymer (b) obtained using only aromatic monomers, and polymer (c) obtained using both aliphatic and aromatic monomers. Suitable examples of the polymer (b) (i.e., aromatic polymer) include styrene-based polymers such as polystyrene, styrene-sulfonic acid copolymer, styrene-methacrylic acid copolymer, and acrylonitrile-butadiene-styrene copolymer, with polystyrene being particularly preferred. Suitable examples of the polymer (b) include aromatic polymers containing structural units derived from aromatic monomers having a (meth)acryloyl group, such as benzyl (meth)acrylate.
[0029] The average particle size of the seed particles is preferably 0.2 to 3.0 μm. The lower limit of the average particle size is more preferably 0.4 μm or more, and the upper limit of the average particle size is more preferably 2.0 μm or less. The average particle size of the seed particles is also a value based on the number of particles, and is determined by the same measurement method as for the filler.
[0030] The core portion can be obtained, for example, by polymerizing a first composition containing a seed particle and a polymerizable monomer. More specifically, as in step (1) described below, the seed particle is swollen with a polymerizable monomer, and then the polymerizable monomer is polymerized within the seed particle to obtain the core portion. The core portion can be suitably obtained by step (1) described below.
[0031] The average particle size of the core portion is preferably 1.0 to 10.0 μm. The lower limit of the average particle size is more preferably 2.0 μm or more, and even more preferably 3.0 μm or more. The upper limit of the average particle size is more preferably 9.0 μm or less, and even more preferably 8.0 μm or less. The average particle size of the core portion is also a value based on the number of particles, and is determined by the same measurement method as for the filler.
[0032] The shell portion is present on at least a portion or the entire surface of the core portion. The thickness of the shell portion is not particularly limited, but for example, the maximum thickness of the shell portion is preferably 5 nm or more. More preferably, it is 20 nm or more, even more preferably 30 nm or more, even more preferably 40 nm or more, and most preferably 50 nm or more. The maximum thickness of the shell portion is also preferably 1 μm or less. More preferably, it is 500 nm or less, even more preferably 200 nm or less. The shell portion may be a single layer, or may be composed of two or more layers. The thickness of the shell portion can be determined, for example, by subtracting the average particle size of the core portion from the average particle size of the core-shell particles.
[0033] The shell portion has cation exchange groups on its surface. Examples of cation exchange groups include sulfonic acid groups, carboxyl groups, and phosphate groups. Among these, sulfonic acid groups are preferred because they can stably dissociate the target substance ionically. That is, the filler of the present invention preferably comprises a core portion and a shell portion that covers at least a portion of the core portion, and has sulfonic acid groups on the surface of the shell portion.
[0034] In this specification, unless otherwise specified, the term "cation exchange group" refers to a cation exchange group in the narrow sense (-SO 3 H, -COOH, -OPO 3 H2 For example, the term "sulfonic acid group" includes a sulfonic acid group in the narrow sense (-SO ) such as a sulfoalkyl group. 3 The term "sulfonic acid group" refers to the entire functional group formed by bonding a sulfonic acid group (H) and an alkyl group.
[0035] The amount of cation exchange groups such as sulfonic acid groups on the surface of the shell can be measured by, for example, combustion ion chromatography or time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0036] The shell portion can be obtained, for example, by obtaining the core portion, and then adding a second composition containing a cation-exchange group-containing monomer and polymerizing the resulting mixture. In this way, the shell portion can be suitably obtained by the step (2) described below. That is, a preferred embodiment of the present invention is one in which the shell portion is formed using a cation-exchange group-containing polymerizable monomer.
[0037] Here, core-shell particles differ from particles obtained by surface-treating the core (also referred to as surface-treated particles). Core-shell particles are produced by obtaining the core and then polymerizing a monomer, whereas surface-treated particles are produced by reacting a surface-treating compound with the core after obtaining it, but without polymerizing the monomer. Therefore, the two types can be distinguished by observing the cross-section of the particle. The two types can be distinguished, for example, by thinly slicing each particle using a microtome and observing the cross-section with a transmission electron microscope (TEM) or a scanning electron microscope (SEM). When preparing a sample for observation, an embedding material may be used, for example, with reference to the method described in the known paper "TEM Observation of Water-Based Resin Emulsions - Fixation Method of Core-Shell Epoxy Emulsions Using Gelatin" (Collection of Polymers, Society of Polymer Science, Public Interest Incorporated Association, published May 25, 2018, Vol. 75, No. 3, pp. 290-292). To facilitate structural observation, the sample may be stained appropriately with a staining agent. Examples of staining agents that may be used include osmium tetroxide, which is effective for unsaturated polymeric materials; ruthenium tetroxide, which is effective for saturated polymeric materials; and phosphotungstic acid, which is effective for polyamides. For details on these staining agents and staining methods, see, for example, "SCAS NEWS" (Sumika Chemical Analysis Center, Ltd., Issue 15, pp. 12-14, published January 24, 2002). Other staining agents may also be used. When observing the cross section of a particle, surface-treated particles typically have a homogeneous interior, whereas core-shell particles may exhibit layered structures within the particle (see, for example, Figure 3 on p. 292 of the above-mentioned known paper). Furthermore, when stained, surface-treated particles exhibit almost no unevenness in the staining across the particle cross section, whereas core-shell particles may exhibit different degrees of staining between the core and shell. Furthermore, when focusing on the particle surface, the components bonded to the particle surface by the surface treatment are often distributed in a mottled pattern (also called an island pattern) on the particle surface, and the proportion of the uncoated portion is larger than that of core-shell type particles, which have a homogeneous surface.
[0038] The filler of the present invention is preferably a core-shell type particle (seed core-shell particle) obtained by forming a core portion (seed core particle) by seed polymerization and then forming a shell portion using a polymerizable monomer. Compared to particles obtained by surface-treating seed core particles, the filler can more clearly separate not only HbA1c but also Hb species (e.g., HbA1a, HbA1b, HbF, etc.) that have a weaker retention capacity than HbA1c.
[0039] The filler of the present invention can be produced, for example, by a production method including step (1) of polymerizing a first composition containing seed particles and a polymerizable monomer, and step (2) of adding a second composition containing a cation exchange group-containing monomer and polymerizing the resulting mixture. This production method can obtain particles having a CV value within the above range without a classification step, and step (2) can be performed continuously after step (1), resulting in excellent production efficiency and high-quality fillers. Therefore, this production method is an extremely useful industrial technique. This production method is also one of the inventions of the present inventors.
[0040] <Step (1)> Step (1) is a step of polymerizing a first composition containing seed particles and a polymerizable monomer. Among these, step (1) is preferably a seed polymerization step. Specifically, step (1) is preferably a step of swelling seed particles with a polymerizable monomer and polymerizing the polymerizable monomer within the swollen seed particles. This preferably produces core particles that will become the core portion of the final filler. The core portion thus formed by seed polymerization is also referred to as a seed core particle. It is particularly preferable that the filler of the present invention is a particle obtained by a production method including a seed polymerization step.
[0041] The seed particles swell by absorbing the polymerizable monomer. To allow the seed particles to absorb the polymerizable monomer, it is preferable to first add the seed particles to an emulsion containing the polymerizable monomer and an aqueous medium. The emulsion can be prepared by a known method. For example, the emulsion can be obtained by adding the polymerizable monomer to an aqueous medium and dispersing it using a microemulsifier such as a homogenizer, an ultrasonicator, or a Nanomizer (registered trademark). Examples of the aqueous medium include water (alone) and a mixture of water and a water-soluble organic solvent. The water-soluble organic solvent is not particularly limited, and examples include lower alcohols such as methanol, ethanol, and isopropyl alcohol. Among these, water is preferred as the aqueous medium from the viewpoint of wastewater treatment.
[0042] The seed particles may be added to the emulsion as they are, or may be added to the emulsion in a state where they are dispersed in an aqueous medium. After adding the seed particles to the emulsion, it is preferable to stir the emulsion at room temperature (about 25°C) for 1 to 12 hours, for example, so that the polymerizable monomer is suitably absorbed into the seed particles. To promote the absorption of the polymerizable monomer into the seed particles, the emulsion may be heated, for example, to about 30 to 50°C. The completion of the absorption of the polymerizable monomer into the seed particles can be determined, for example, by confirming the increase in particle size by observation with an optical microscope.
[0043] Although the mixing ratio of the seed particles and the polymerizable monomer is not particularly limited, it is preferable that the total amount of the polymerizable monomer is 1 to 5,000 parts by mass per 1 part by mass of the seed particles. When the mixing ratio is equal to or less than this upper limit, the swelling of the seed particles becomes smooth, the production efficiency improves, and the particle size of the final filler becomes more uniform.
[0044] The polymerizable monomer to be absorbed into the seed particles is not particularly limited as long as it is a compound having a polymerizable group, and one or more types may be used. The polymerizable group is as described above.
[0045] As the polymerizable monomer, for example, a hydrophobic crosslinkable monomer or a monomer mixture containing a hydrophobic crosslinkable monomer as a main component can be used. By using a hydrophobic crosslinkable monomer, a filler with high pressure resistance can be realized and swelling and shrinkage can be prevented.
[0046] Examples of the hydrophobic crosslinkable monomer include styrene derivatives such as divinylbenzene, divinyltoluene, divinylxylene, divinylethylbenzene, and divinylnaphthalene; (meth)acrylic acid ester derivatives such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,6-hexane glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate; aliphatic diene compounds such as 1,3-butadiene, isoprene, and 1,4-hexanediene; and derivatives of the above monomers. Among these, (meth)acrylic acid ester derivatives are preferred. These may be used alone or in combination of two or more.
[0047] The polymerization (preferably seed polymerization) is suitably carried out in the presence of a surfactant. The surfactant is not particularly limited, but anionic surfactants, nonionic surfactants, etc. are suitable, and one type may be used alone, or two or more types may be used in combination.
[0048] Examples of anionic surfactants include carboxylic acid compounds (e.g., sodium laurate, sodium myristate, sodium palmitate, sodium stearate, sodium oleate, potassium laurate, potassium myristate, potassium palmitate, potassium stearate, potassium oleate, etc.), alkyl ether carboxylates (e.g., sodium laureth-4 carboxylate, etc.), higher alcohol compounds (e.g., sodium lauryl sulfate, ammonium lauryl sulfate, triethanolamine lauryl sulfate, etc.), sulfonic acid compounds (e.g., disodium lauryl sulfosuccinate, disodium laureth sulfosuccinate, diethylhexyl sodium sulfosuccinate, sodium lauryl sulfate, etc.), and the like.
[0049] Examples of nonionic surfactants include ethylene oxide condensation compounds (e.g., polyoxyethylene alkyl ethers, polyoxyethylene steryl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene fatty acid esters, polyoxyethylene polyhydric alcohol fatty acid esters, polyoxyethylene sorbitan fatty acid esters, etc.), glycol fatty acid esters, sorbitan fatty acid esters, alkyl glycosides, etc. Commercially available products include polyoxyethylene alkyl ether compounds such as Emulgen (registered trademark) 120, 147, 210, and 420 manufactured by Kao Corporation.
[0050] The amount of the surfactant used is not particularly limited, but is preferably 0.01 to 20 parts by mass per 100 parts by mass of the total amount of polymerizable monomers. This not only improves polymerization stability but also sufficiently reduces the amount of surfactant remaining in the polymerization product. The amount is more preferably 0.3 to 15 parts by mass.
[0051] The polymerization is preferably carried out using one or more polymerization initiators. The polymerization initiator is not particularly limited, but a radical polymerization initiator is preferred, and a thermal polymerization initiator is more preferred.
[0052] Examples of the thermal polymerization initiator include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; hydrogen peroxide; organic peroxides such as cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, dimethylbis(tert-butylperoxy)hexane, dimethylbis(tert-butylperoxy)hexyne-3, bis(tert-butylperoxyisopropyl)benzene, bis(tert-butylperoxy)trimethylcyclohexane, butyl-bis(tert-butylperoxy)valerate, 2-ethylhexaneperoxy acid tert-butyl, dibenzoyl peroxide, paramenthane hydroperoxide, and tert-butyl peroxybenzoate; and 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile). ), 2,2'-azobis(2-isopropylbutyronitrile), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis(2,4-dimethylbutyronitrile), 2,2'-azobis(2-methylcapronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), 2,2'-azobis(2,4,4-trimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2, Nitrile-azo compounds such as 2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(4-ethoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(4-n-butoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(carbamoylazo)isobutyronitrile, and 4,4'-azobis(4-cyanopentanoic acid); and the like.
[0053] The polymerization initiator may also be a redox initiator that combines the above-mentioned persulfate or organic peroxide with a reducing agent, such as sodium sulfoxylate formaldehyde, sodium hydrogen sulfite, ammonium hydrogen sulfite, sodium thiosulfate, ammonium thiosulfate, hydrogen peroxide, sodium hydroxymethanesulfinate, L-ascorbic acid and its salts, cuprous salts, and ferrous salts.
[0054] Among the above polymerization initiators, at least one selected from the group consisting of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 4,4'-azobis(4-cyanopentanoic acid), cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, and lauroyl peroxide is preferred.
[0055] The amount of the polymerization initiator used is, for example, preferably 0 to 5 parts by mass, more preferably 0 to 3 parts by mass, and even more preferably 0.2 to 3 parts by mass, per 100 parts by mass of the total amount of polymerizable monomers.
[0056] In the polymerization, a dispersant may be added to the polymerization reaction system to stabilize the dispersibility of the polymerizable monomer droplets and seed particles. Examples of dispersants include organic dispersants such as partially saponified polyvinyl alcohol, polyacrylates, polyvinylpyrrolidone, carboxymethyl cellulose, and methyl cellulose; and inorganic dispersants such as magnesium pyrophosphate, calcium pyrophosphate, calcium phosphate, calcium carbonate, magnesium phosphate, magnesium carbonate, and magnesium oxide. One or more of these dispersants may be used. When using an inorganic dispersant, it is preferable to use a surfactant in combination. Among these, polyvinyl alcohol and / or polyvinylpyrrolidone are preferred. The amount of dispersant added is not particularly limited, but is preferably 0.3 to 50 parts by mass per 100 parts by mass of the polymerizable monomer.
[0057] In the above polymerization, a water-soluble polymerization inhibitor may be added to the aqueous medium in order to suppress the generation of by-products (e.g., resin fine particles with an excessively small particle size) in the aqueous medium during the polymerization reaction. Examples of polymerization inhibitors include nitrites such as sodium nitrite, sulfites, hydroquinones, ascorbic acids, water-soluble B vitamins, citric acid, polyphenols, and ammonium thiocyanate. The amount of polymerization inhibitor added is preferably, for example, 0.002 to 0.2 parts by mass per 100 parts by mass of polymerizable monomer.
[0058] Regarding the polymerization conditions, the polymerization temperature and polymerization time may be appropriately selected depending on the type of polymerizable monomer and the type of polymerization initiator used as needed. For example, the polymerization temperature is preferably 25 to 110°C, more preferably 50 to 100°C, and the polymerization time is preferably 1 to 12 hours. The polymerization is preferably carried out by raising the temperature after the polymerizable monomer and the polymerization initiator used as needed have been completely absorbed into the seed particles. The polymerization may also be carried out in an inert gas (e.g., nitrogen) atmosphere. The process of absorbing the polymerizable monomer into the seed particles and polymerizing them may be repeated multiple times.
[0059] <Step (2)> Step (2) is a step of adding a second composition containing a cation exchange group-containing polymerizable monomer to the product obtained in step (1) above and polymerizing the resulting mixture. The product obtained in step (1) above contains core particles (seed core particles) that will become the core portion of the filler. The particles finally obtained through step (2) above (i.e., the filler of the present invention) can be called seed core-shell particles.
[0060] The second composition contains one or more cation-exchange-group-containing polymerizable monomers. The cation-exchange-group-containing polymerizable monomers contain a sulfonic acid group (—SO 3 H), carboxyl group (-COOH), phosphate group (-OPO 3 H 2The polymerizable monomer is not particularly limited as long as it has a cation exchange group such as methyl acrylate, methyl meth ...
[0061] The compound having a vinyl group and a sulfonic acid group is preferably a compound represented by the following general formula (2) or (3): (R 1 -Z) m -R 2 - (SO 3 H) n (2) R 4 - (R 2 ) p - (SO 3 H) n (3) (wherein, R 1 is CH 2 = C(R 3 )-C(=O)-. R 3 are the same or different and represent a hydrogen atom or a methyl group. Z represents an oxygen atom or an imino group (—NH—). R 2 represents a divalent to hexavalent organic residue having 1 to 30 carbon atoms. 4 is CH 2 = C(R 3 )-. m represents a number of 1 to 4. n is 1 or 2. p is 0 or 1. ) is a compound represented by the formula (2). The compound represented by the formula (2) or (3) may be in the form of a salt such as a metal salt (for example, a sodium salt).
[0062] In the above general formula (2), Z preferably represents an imino group. That is, the sulfonic acid group-containing monomer preferably has a (meth)acrylamide structure. 2preferably represents an alkyl group having 1 to 30 carbon atoms, preferably 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 3 to 5 carbon atoms. Among alkyl groups, branched alkyl groups are preferred. It is preferable that m and n are each 1. A particularly preferred compound represented by the above general formula (2) is acrylamido t-butylsulfonic acid.
[0063] In the above general formula (3), when p is 1, R 2 is preferably a methylene group. It is also suitable that p is 0. It is preferable that n is 1. That is, the compound represented by the above general formula (3) is preferably methallylsulfonic acid, allylsulfonic acid, or vinylsulfonic acid. Among them, vinylsulfonic acid or methallylsulfonic acid is more preferable.
[0064] The second composition may contain one or more other polymerizable monomers together with the cation-exchange group-containing polymerizable monomer. As the other polymerizable monomer, it is preferable to use at least a compound having a polymerizable group and exhibiting hydrophilicity (also referred to as a hydrophilic monomer).
[0065] Preferred examples of the hydrophilic monomer include hydroxyalkyl(meth)acrylate, hydroxyalkyl(meth)acrylamide, (poly)(alkylene glycol)(meth)acrylate, (poly)(alkylene glycol)vinyl ether, and N-vinylpyrrolidone. The number of carbon atoms in the alkyl group of the hydroxyalkyl(meth)acrylate and hydroxyalkyl(meth)acrylamide is preferably 1 to 30, more preferably 1 to 10, and even more preferably 1 to 5. The number of carbon atoms in the alkylene glycol group of the (poly)(alkylene glycol)(meth)acrylate and (poly)(alkylene glycol)vinyl ether is preferably 1 to 30, more preferably 1 to 10, and even more preferably 1 to 5, and the average number of repeating units (moles) of the alkylene glycol group is preferably 1 to 50, more preferably 2 to 20, and even more preferably 5 to 15.
[0066] Examples of the hydroxyalkyl (meth)acrylates include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, etc. Examples of the hydroxyalkyl (meth)acrylamides include n-hydroxyethyl (meth)acrylamide, hydroxypropyl (meth)acrylamide, etc. Examples of the poly(alkylene glycol) (meth)acrylates include poly(ethylene glycol) (meth)acrylate, poly(propylene glycol) (meth)acrylate, etc. Examples of the (poly)(alkylene glycol) (poly)vinyl ethers include ethylene glycol monovinyl ether, diethylene glycol monovinyl ether, diethylene glycol divinyl ether, etc. Among the hydrophilic monomers, (poly)(alkylene glycol) (meth)acrylates are preferred, and poly(ethylene glycol) (n=10) mono(meth)acrylate is more preferred.
[0067] The amount of the cation-exchange-group-containing polymerizable monomer is preferably 5 to 500 parts by mass relative to 100 parts by mass of the core particles obtained in step (1). This ensures that the resulting core-shell particles have a sufficient number of cation-exchange groups on the shell surface, thereby further improving separation performance. The amount of the cation-exchange-group-containing polymerizable monomer relative to 100 parts by mass of the core particles obtained in step (1) is more preferably 50 to 300 parts by mass. Furthermore, when the cation-exchange-group-containing monomer is used in combination with another polymerizable monomer, the amount of the other polymerizable monomer is preferably 10 to 200 parts by mass, more preferably 50 to 100 parts by mass, relative to 100 parts by mass of the cation-exchange-group-containing monomer.
[0068] The polymerization in the step (2) is carried out continuously following the step (1). Therefore, each reactant such as a polymerization initiator may already be present in the system, but may be further added in the step (2). For example, a polymerization initiator may be further added. The polymerization initiator is as described above, and a radical polymerization initiator is preferred, and a thermal polymerization initiator is more preferred.
[0069] Regarding the polymerization conditions, the polymerization temperature and polymerization time may be appropriately selected depending on the type of monomer and the type of polymerization initiator used as needed. For example, the polymerization temperature is preferably 25 to 110°C, more preferably 50 to 100°C, and the polymerization time is preferably 1 to 12 hours. The polymerization may also be carried out under an atmosphere of an inert gas (e.g., nitrogen).
[0070] The packing material of the present invention has an extremely high level of separation performance and can reduce column pressure, thereby improving measurement accuracy compared to when conventional column packing materials are used. Thus, a method for measuring a sample by ion exchange chromatography (preferably ion exchange liquid chromatography) using the above packing material is a preferred embodiment of the present invention. The sample to be measured by the measurement method can be any sample that can be measured by conventional ion exchange chromatography, and is not particularly limited. Examples include biological samples such as proteins and nucleic acids; drugs; sugars; surfactants; various ions; and the like. In particular, the above packing material is effective for measuring hemoglobins such as hemoglobin A1c. That is, a method for measuring hemoglobins by ion exchange chromatography using the above packing material as a column packing material also constitutes one aspect of the present invention. Furthermore, the use of the above packing material as a column packing material for measuring hemoglobins by ion exchange chromatography is also a preferred embodiment of the present invention.
[0071] The ion exchange liquid chromatograph used for the measurement may be a known one, and may be composed of, for example, a liquid delivery pump, a sample injection device (sampler), a column, a detector, etc. Other auxiliary devices (e.g., a column thermostat, an eluent degassing device, etc.) may also be attached as appropriate. Particularly when measuring hemoglobins, a conventionally known HPLC system equipped with a pump for delivering an eluent, a sampler, a detector, etc. can be used. For measurement, a column packed with the packing material of the present invention is connected to such a system, and a blood sample is measured.
[0072] When various measurements are performed using the above packing material, the column pressure is preferably set to, for example, 5 MPa or less. The column pressure is more preferably 3 MPa or less, even more preferably 2 MPa or less, and most preferably 1.5 MPa or less. There are no particular restrictions on the lower limit of the column pressure, but from the viewpoint of suppressing pressure fluctuations and performing stable measurements, it is preferable to set the column pressure to, for example, 0.098 MPa or more. The column pressure is more preferably 0.2 MPa or more.
[0073] The eluent used in the measurement is selected from known eluents used in ion exchange chromatography. Specific examples of the eluent include inorganic buffer solutions containing phosphoric acid, boric acid, and salts thereof; organic acid buffer solutions containing various amino acids, citric acid, succinic acid, phthalic acid, and salts thereof; Good's buffer solutions such as Bis-Tris (bis(2-hydroxyethyl)iminotris-(hydroxymethyl)methane), HEPES (N-2-hydroxyethylpiperazine-N'-2-ethanesulfonic acid), and MES (2-(N-morpholino)ethanesulfonic acid); and the like. Furthermore, various salts such as sodium chloride, potassium chloride, sodium sulfate, and sodium bicarbonate; inorganic acids such as hydrochloric acid; organic acids such as acetic acid; bases such as sodium hydroxide and potassium hydroxide; water-soluble organic solvents such as methanol, ethanol, and acetonitrile may be added or used alone, as needed.
[0074] The concentration of the eluent varies depending on other measurement conditions, but is preferably 1 to 1000 mM, more preferably 5 to 800 mM. A mixture of the above eluents may also be used. The eluent may be switched during measurement, or gradient elution may be performed.
[0075] When measuring hemoglobins such as hemoglobin A1c, it is preferable to use a buffer solution having a salt concentration of 10 mM to 1000 mM. When the salt concentration of the buffer solution is 10 mM or more, the ion exchange reaction proceeds favorably, and hemoglobin can be sufficiently separated. Furthermore, when the salt concentration of the buffer solution is 1000 mM or less, salt precipitation can be sufficiently prevented.
[0076] Here, by using the packing material of the present invention, hemoglobin A1c (also referred to as HbA1c) can be clearly separated. Furthermore, components (e.g., HbA1a, HbA1b, HbF, etc.) that have a smaller retention force on the packing material than HbA1c can also be clearly separated. Therefore, the above measurement method is useful as a method for measuring at least one selected from the group consisting of HbA1a, HbA1b, HbA1c, and HbF. Among these, the above measurement method is preferred as a method for measuring at least HbA1c, and is also suitable as a method for simultaneously measuring HbA1c and at least one selected from the group consisting of HbA1a, HbA1b, and HbF. Furthermore, the above measurement method is also useful as a method for simultaneously measuring at least HbA1c and HbF. Currently, analytical columns for HbF etc. and analytical columns for HbA1c are sold separately, and HbA1c cannot be separated using analytical columns for HbF etc., and HbA1c cannot be separated using analytical columns for HbA1c. Therefore, the effect of being able to simultaneously measure components with low retention (HbA1a, HbA1b, HbF etc.) and HbA1c can be said to be an extremely unique effect that could not be achieved with conventional technology, and is extremely useful from a technical standpoint.
[0077] According to the present invention, there are provided a packing material for ion exchange chromatography that has an extremely high level of separation performance even at reduced column pressure and is particularly useful for measuring hemoglobins such as hemoglobin A1c, a method for producing the packing material efficiently and simply, and a method for measuring hemoglobins that can measure hemoglobins with extremely high accuracy.
[0078] 7A is a chromatogram obtained when hemoglobins were measured using the packing material of Example 1. This is an enlarged view of the portion of the chromatogram shown in FIG. 1 where the analysis time was 0 to 1.5 minutes. This is an enlarged view of the portion of the chromatogram obtained when hemoglobins were measured using the packing material of Example 2 where the analysis time was 0 to 1.5 minutes. This is an enlarged view of the portion of the chromatogram obtained when hemoglobins were measured using the packing material of Example 3 where the analysis time was 0 to 1.5 minutes. This is an enlarged view of the portion of the chromatogram obtained when hemoglobins were measured using the packing material of Example 4 where the analysis time was 0 to 1.5 minutes. This is an enlarged view of the portion of the chromatogram obtained when hemoglobins were measured using the packing material of Example 5 where the analysis time was 0 to 1.5 minutes. This is an image obtained by slicing the packing material of Example 1 using an ultramicrotome, staining it with osmium tetroxide, and then observing it with a transmission electron microscope (TEM). This is an enlarged view of FIG. 7A.
[0079] The present invention will be described in more detail below with reference to examples, but is not limited to these examples. Unless otherwise specified, "%" means "% by mass." The methods for measuring the standard deviation and average particle size of the packing material, and the method for measuring the cation exchange capacity, are as described above. The column was prepared and Hb measurements were performed as follows.
[0080] (Column Preparation) Each packing material was packed into a stainless steel vessel having an inner diameter of 4.6 mm and a length of 8 mm to obtain a column. This column was connected to an HPLC system (Shimadzu Corporation, LC-20A) and the following Hb measurements were performed.
[0081] (Measurement of Hb) Elution conditions: Step gradient elution was performed using two solutions, eluent A (succinic acid buffer: pH 5) and eluent B (300 mM phosphate buffer: pH 7). The concentration of eluent A was adjusted so that HbA1c had the same retention time for each packing. Flow rate: 1.5 ml / min. Detection wavelength: 415 nm. Measurement sample: healthy human blood diluted 300-fold with phosphate buffer containing surfactant at pH 7.
[0082] Example 1 Seed particles were synthesized using soap-free emulsion polymerization. Specifically, 40 g of benzyl methacrylate (manufactured by Fujifilm Wako Co., Ltd.) and 300 g of ion-exchanged water were first added to a reactor equipped with a stirrer, and the mixture was heated with stirring under a nitrogen atmosphere until the temperature reached 80°C over one hour. Separately, an aqueous potassium persulfate solution was prepared by dissolving 0.9 g of potassium persulfate (manufactured by Sigma-Aldrich Co.) in 30 g of ion-exchanged water. After the reactor was heated, the aqueous potassium persulfate solution was added, and polymerization was continued for two hours. After polymerization was complete, the seed particle solution was recovered by removing aggregates. The solids concentration of the seed particle solution was 0.5 g / mL, the standard deviation of the particle size was 0.8 μm, the average particle size was 0.8 μm, and the CV value was 12.0%.
[0083] 90 g of tetraethylene glycol dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.), 120 g of triethylene glycol dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.), 0.5 g of benzoyl peroxide (manufactured by Kishida Chemical Co., Ltd.), 1.50 g of sodium dodecyl sulfate (manufactured by Kishida Chemical Co., Ltd.), and 100 g of ion-exchanged water were weighed into a 500 mL glass beaker, a stirrer was added, and the mixture was mixed using a magnetic stirrer. The mixture was then emulsified by stirring at 15,000 rpm for 5 minutes using a high-speed homogenizer. This emulsion and 1 mL of the above seed particle solution were added to a reactor equipped with a stirrer and left at room temperature for 1 hour. 100 g of a 3% aqueous solution of polyvinyl alcohol (manufactured by Mitsubishi Chemical Corporation) were added, heated with stirring, and polymerized at 80°C for 1 hour under a nitrogen atmosphere to obtain seed core particles. The average particle diameter of the seed core particles was 4.471 μm.
[0084] Next, 100 g of 2-(meth)acrylamido-2-methylpropanesulfonic acid (manufactured by Toagosei Chemical Industry Co., Ltd.) and 20 g of polyethylene glycol methacrylate (manufactured by NOF Corporation) were dissolved in 300 mL of ion-exchanged water containing 100 g of methanol. The resulting mixture was added to the reactor and polymerized at 80°C for 2 hours under a nitrogen atmosphere with stirring. The resulting polymerized composition was washed with water and acetone to obtain seed core-shell particles.
[0085] The resulting seed core-shell particles (i.e., filler) had a particle size standard deviation of 0.7 μm, an average particle size of 4.557 μm, a CV value of the particle size distribution of 14.3%, and a cation exchange capacity of 50 μeq / gel mL. The shell layer thickness was 0.086 μm (= 4.557 μm - 4.471 μm).
[0086] The resulting packing material was packed into a column, and sample measurements were performed using this column. The column pressure was as shown in Table 1. The resulting chromatograms are shown in Figures 1 and 2. In Figure 1, Peak 1 is HbA1c. HbA1c was well separated from other hemoglobin fractions within a short period of time. Figure 1 is a chromatogram obtained when hemoglobins were measured using the packing material of Example 1, and Figure 2 is an enlarged view of the portion of the chromatogram shown in Figure 1 where the analysis time was 0 to 1.5 minutes.
[0087] The theoretical plate number N of this column was calculated using the half-width method. That is, it was calculated based on the obtained chromatogram using the following formula (4). The results are shown in Table 1. Theoretical plate number N = 5.54 × (t R / W 0.5h ) 2 (4) However, t R indicates the retention time (seconds) of the HbA1c peak. 0.5h indicates the peak width at the midpoint of the HbA1c peak height.
[0088] Example 2 Seed core particles were obtained in the same manner as in Example 1, except that 10 g of tetraethylene glycol dimethacrylate, 80 g of triethylene glycol dimethacrylate, 0.6 g of benzoyl peroxide, 1.00 g of sodium dodecyl sulfate, 500 g of ion-exchanged water, and 0.4 mL of seed particle solution were used. The average particle diameter of the seed core particles was 6.020 μm.
[0089] Next, seed core-shell type particles were obtained in the same manner as in Example 1, except that 90 g of 2-(meth)acrylamide-2-methylpropanesulfonic acid and 10 g of polyethylene glycol methacrylate were dissolved in 200 mL of ion-exchanged water containing 100 g of methanol.
[0090] The obtained seed core-shell particles had a particle size standard deviation of 0.9 μm, an average particle size of 6.118 μm, a CV value of the particle size distribution of 15.0%, a cation exchange capacity of 98 μeq / gel mL, and a shell layer thickness of 0.098 μm (= 6.118 μm - 6.020 μm).
[0091] Example 3 Seed core particles were obtained by polymerization in the same manner as in Example 2, except that the amount of the seed particle solution added was 0.65 mL. The average particle diameter of the seed core particles was 6.830 μm.
[0092] Seed core-shell particles were obtained in the same manner as in Example 2. The obtained seed core-shell particles had a particle size standard deviation of 1.0 μm, an average particle size of 6.950 μm, a CV value of the particle size distribution of 14.2%, and a cation exchange capacity of 54 μeq / gel mL. The shell layer thickness was 0.120 μm (= 6.950 μm - 6.830 μm).
[0093] Example 4 Polymerization was carried out in the same manner as in Example 1, except that 5 g of tetraethylene glycol dimethacrylate, 25 g of triethylene glycol dimethacrylate, 0.3 g of benzoyl peroxide, 1.00 g of sodium dodecyl sulfate, and 0.12 mL of the above seed particle solution were used, to obtain seed core particles. The average particle diameter of the seed core particles was 4.947 μm.
[0094] Next, seed core-shell type particles were obtained in the same manner as in Example 1, except that 70 g of 2-(meth)acrylamide-2-methylpropanesulfonic acid and 30 g of polyethylene glycol methacrylate were dissolved in 200 mL of ion-exchanged water containing 100 g of methanol.
[0095] The seed core-shell particles obtained had a particle size standard deviation of 0.6 μm, an average particle size of 4.989 μm, a particle size distribution CV value of 11.2%, a cation exchange capacity of 45 μeq / gel mL, and a shell layer thickness of 0.042 μm (= 4.989 μm - 4.947 μm).
[0096] Example 5 Seed core particles were obtained by polymerization in the same manner as in Example 4, except that the amount of sodium dodecyl sulfate added was 0.2 g. The average particle size of the seed core particles was 4.917 μm.
[0097] The obtained seed core-shell particles had a particle size standard deviation of 0.9 μm, an average particle size of 4.992 μm, a particle size distribution CV value of 17.3%, a cation exchange capacity of 63 μeq / gel mL, and a shell layer thickness of 0.075 μm (= 4.992 μm - 4.917 μm).
[0098] Each of the packing materials obtained in Examples 2 to 5 was packed into a column, and sample measurements were performed using this column. The column pressure was as shown in Table 1. The resulting chromatograms are shown in Figures 3 to 6. In Figures 3 to 6, the peak with the largest height, which appeared around 1 minute into the analysis, is HbA1c. As in the case of sample measurements using the packing material obtained in Example 1, HbA1c was well separated from other hemoglobin fractions within a short period of time. Figures 3 to 6 are enlarged views of the portion of the chromatograms obtained when hemoglobins were measured using each of the packing materials in Examples 2 to 5, where the analysis time was 0 to 1.5 minutes.
[0099] Comparative Example 1 A mixture of a 3% aqueous solution of polyvinyl alcohol (manufactured by Mitsubishi Chemical Corporation), 300 g of tetraethylene glycol dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.), 100 g of triethylene glycol dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.), and 1.0 g of benzoyl peroxide (manufactured by Kishida Chemical Co., Ltd.) was charged into a reactor equipped with a stirrer, and then heated with stirring to polymerize at 80°C for 1 hour under a nitrogen atmosphere. Next, 100 g of 2-(meth)acrylamido-2-methylpropanesulfonic acid (manufactured by Toa Gosei Chemical Co., Ltd.) and 20 g of polyethylene glycol methacrylate were dissolved in 300 mL of ion-exchanged water containing 100 g of methanol. The resulting mixture was added to the reactor and polymerized at 80°C for 2 hours under a nitrogen atmosphere with stirring. The resulting polymerized composition was washed with water and acetone to obtain a filler.
[0100] The resulting packing material had a standard deviation of particle size of 2.1 μm, an average particle size of 9.040 μm, a CV value of the particle size distribution of 23.2%, and a cation exchange capacity of 40 μeq / gel mL.
[0101] The resulting packing material was packed into a column, and a sample was measured using this column. The column pressure was as shown in Table 1. The number of theoretical plates, N, was calculated based on the obtained chromatogram (not shown). The results are shown in Table 1.
[0102] Comparative Example 2 Polymerization was carried out in the same manner as in Comparative Example 1, except that the concentration of the aqueous polyvinyl alcohol solution was changed to 5%, to obtain a filler.
[0103] The resulting packing material had a standard deviation of particle size of 1.5 μm, an average particle size of 5.960 μm, a CV value of the particle size distribution of 25.2%, and a cation exchange capacity of 60 μeq / gel mL.
[0104] The resulting packing material was packed into a column, and a sample was measured using this column. The column pressure was as shown in Table 1. The number of theoretical plates, N, was calculated based on the obtained chromatogram (not shown). The results are shown in Table 1.
[0105] Comparative Example 3 Polymerization was carried out in the same manner as in Comparative Example 1, except that the concentration of the aqueous polyvinyl alcohol solution was changed to 7%, to obtain a filler.
[0106] The resulting packing had a standard deviation of particle size of 0.7 μm, an average particle size of 3.684 μm, a CV value of the particle size distribution of 19.0%, and a cation exchange capacity of 75 μeq / gel mL.
[0107] The resulting packing material was packed into a column, and a sample was measured using this column. The column pressure was as shown in Table 1. The number of theoretical plates, N, was calculated based on the obtained chromatogram (not shown). The results are shown in Table 1.
[0108]
[0109] As shown in Comparative Examples 1 to 3, increasing the particle size of the packing to reduce the column pressure resulted in a decrease in the number of theoretical plates. In contrast, when the packing obtained in Example 1 was used for measurement, the pressure was equivalent to that of Comparative Example 1, but the number of theoretical plates was higher than that of Comparative Example 1. That is, when the number of theoretical plates calculated in Example 1 was compared with that of Comparative Example 1, which was performed at the same column pressure, the value was clearly larger, indicating improved separation performance. This is thought to be due to a smaller CV value of the particle size distribution compared to suspension polymerization. Furthermore, in Examples 2 to 5, by setting the CV value of the particle size distribution to 18% or less (preferably 18.0% or less), the column pressure was found to be lower than in the comparative examples with similar average particle sizes. Furthermore, in all of Examples 2 to 5, the number of theoretical plates was higher than that of Comparative Example 1.
[0110] When samples were measured using the packing materials obtained in Examples 1 to 5 as column packing materials, not only was HbA1c separated with high resolution, but also HbA1a, HbA1b, and HbF were clearly separated (see Figures 1 to 6). Thus, the use of the packing material of the present invention unexpectedly achieved excellent separation of not only HbA1c but also components such as HbA1a, HbA1b, and HbF, which have lower retention than HbA1c. Note that when the packing material described in Patent Document 2 was used as a column packing material to measure human blood, clear separation of HbA1c and HbF was not possible (not shown). Furthermore, it is precisely because the packing material described in the present application is capable of not only separating HbA1c with high resolution, but also clearly separating HbA1a, HbA1b, and HbF, while simultaneously suppressing column pressure.
[0111] The filler obtained in Example 1 was embedded in epoxy resin, sliced using an ultramicrotome (Leica, model number: EM UC7), stained with a 1% osmium tetroxide solution diluted with 0.1 M sodium phosphate buffer, and then observed under a transmission electron microscope (Hitachi High-Technologies Corporation, device name: HT7800, model number: 6149-02). Images observed at 6000x magnification are shown in Figures 7A and 7B. As can be seen from Figures 7A and 7B, the core region was observed with dark contrast, while the shell region was observed with bright contrast. The thickness of the shell region was approximately 80 nm.
Claims
1. A packing material for ion exchange chromatography, characterized in that the packing material is a core-shell type particle having a core portion and a shell portion covering at least a portion of the core portion, and having a cation exchange group on the surface of the shell portion, and has a CV value (%) represented by the following formula (1): CV value (%) = (standard deviation of particle size / average particle size) x 100 (1) of 18% or less.
2. The packing material for ion exchange chromatography according to claim 1, wherein the average particle size of the core-shell particles is 3.0 to 10.0 μm.
3. The packing material for ion exchange chromatography according to claim 1 or 2, characterized in that the core portion contains seed particles.
4. The packing material for ion exchange chromatography according to claim 1, 2 or 3, characterized in that the shell portion is formed using a cation exchange group-containing polymerizable monomer.
5. The packing material for ion exchange chromatography according to claim 4, characterized in that the cation exchange group-containing polymerizable monomer contains a sulfonic acid group and a vinyl group.
6. The packing material for ion exchange chromatography according to claim 1, 2, 3, 4 or 5, which is used for measuring hemoglobins by ion exchange chromatography.
7. A method for measuring hemoglobin by ion exchange chromatography, comprising using the ion exchange chromatography packing material according to claim 1, 2, 3, 4, 5 or 6 as a column packing material.
8. The method for measuring hemoglobin according to claim 7, which is a method for measuring at least hemoglobin A1c.
9. The method for measuring hemoglobin types according to claim 7, characterized in that it is a method for simultaneously measuring at least hemoglobin A1c and hemoglobin F.
10. A method for producing a packing material for ion exchange chromatography according to claim 1, 2, 3, 4, 5 or 6, characterized in that the method comprises the steps of: (1) polymerizing a first composition containing seed particles and a polymerizable monomer; and (2) adding a second composition containing a cation exchange group-containing polymerizable monomer and polymerizing the resulting composition.
Citation Information
Patent Citations
Filler for cation chromatography and its preparation
JP1995027754A
Method for producing a monodisperse ion exchanger having pores
JP2007535584A
Method of measuring saccharified hemoglobin
JP2009133654A
Separation material and filling column
JP2020044496A
Liquid chromatography column, and method for analyzing hemoglobin
WO2012128276A1
Cited By
Analytical filler for separating glycosylated hemoglobin and preparation method thereof
CN119259009A