Method for producing hydraulic composition slurry
The method of mixing low IM cement clinker powder with TIPA and DEIPA during water addition, along with limestone and gypsum, addresses the need for improved strength development in hydraulic composition slurries, enhancing energy efficiency and waste utilization in cement production.
Patent Information
- Application Number
- PCT/JP2024/012240
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
The cement industry faces challenges in resource and energy conservation, particularly in producing Portland cement, which requires high-temperature firing and significant energy costs, while also needing to address environmental issues through effective use of waste materials. There is a need for a hydraulic composition slurry that exhibits improved strength development.
A method involving the use of low IM cement clinker powder with a specific mineral composition, mixed with water and additives like triisopropanolamine (TIPA) and diethanolisopropanolamine (DEIPA) during mixing, rather than grinding, to enhance strength development, while incorporating limestone and gypsum powder, optimizing the water-cement ratio and additive amounts for improved strength.
The method results in a hydraulic composition slurry with enhanced compressive strength, allowing for increased waste utilization and reduced firing temperatures, achieving better physical properties and efficient energy use.
Smart Images

Figure JP2024012240_03102024_PF_FP_ABST
Abstract
Description
Method for producing hydraulic composition slurry
[0001] The present invention relates to a method for producing a hydraulic composition slurry.
[0002] The present invention relates to a method for producing a hydraulic composition slurry containing cement clinker, gypsum, limestone, additives, and water. More specifically, the present invention relates to improving the strength development of the hydraulic composition by adding a specific additive when mixing a mixture of cement clinker, gypsum, and limestone with water.
[0003] The cement industry is a mass-production, mass-consumption industry, and resource and energy conservation has been and will continue to be a top priority. For example, to produce Portland cement, the most widely produced cement, raw materials prepared to a specific chemical composition must be fired at high temperatures of 1,450 to 1,550°C to produce cement clinker, and the energy costs required to achieve this temperature are enormous.
[0004] Meanwhile, in relation to recent global environmental problems, the effective use of waste, by-products, etc. has become an important issue. Taking advantage of the characteristics of the cement industry and cement manufacturing facilities, it is considered effective to use or treat waste as raw materials or fuel during cement manufacturing, as it allows for safe and large-scale disposal.
[0005] The present inventors have developed a cement clinker containing a high proportion of waste-derived minerals, which allows for low-temperature firing and also has good physical properties such as strength. 2 O 3 (Hereinafter, C 3 A) and 4CaO.Al 2 O 3 Fe 2 O 3 (Hereinafter, C 4 AF) total amount is 22% or more, C 3 A cement clinker having an S content of 60% or more and an iron content (I.M.) of 1.3 or less (hereinafter also referred to as low-IM cement clinker) has already been proposed (Patent Document 1: JP 5665,638B).
[0006] Conventionally, grinding aids such as diethylene glycol have been used in the grinding process of Portland cement production to improve the grinding efficiency of cement clinker, and triethanolamine and triisopropanolamine have also been used in some cases (see, for example, Non-Patent Document 1).
[0007] The present inventors have also found that the compressive strength of cement can be improved by using a grinding aid such as diethanolisopropanolamine (JP 6825,171B).
[0008] JP 5665,638BJP 6825,171B
[0009] "Ceramic Engineering Handbook (2nd Edition)" edited by the Ceramic Society of Japan, Gihodo Publishing, published March 31, 2002, page 231, left column
[0010] The use of the low-IM cement clinker makes it possible to increase the amount of waste material used compared to conventional cement, and also to reduce the firing temperature during production. There is a demand for hydraulic composition slurries with even better strength development.
[0011] An object of the present invention is to improve the strength development of a hydraulic composition slurry.
[0012] In this invention, C calculated by the Borg method 3 A and C 4 A hydraulic composition slurry is produced by mixing low-IM cement clinker powder, which has a total AF content of 22% by mass to 40% by mass and an iron ratio (IM), which represents the mass ratio of Al2O3 to Fe2O3 in the cement clinker, of 0.8 to 1.3, with water. The low-IM cement clinker powder contains at least limestone powder and gypsum powder in addition to the low-IM cement clinker, and triisopropanolamine (TIPA) and / or diethanolisopropanolamine (DEIPA) are added during mixing with water.
[0013] In Patent Document 2, DEIPA is added during the grinding of low-IM cement clinker, and DEIPA is a grinding aid. In contrast, in the present invention, DEIPA and / or TIPA are added during mixing with water. As is clear from Table 4 and Figure 2, when DEIPA and / or TIPA are added during mixing with water rather than during grinding, and when the low-IM cement clinker powder contains limestone powder, both TIPA and DEIPA provide high strength development, with TIPA in particular providing extremely high strength development. In contrast, when the low-IM cement clinker powder does not contain limestone powder, TIPA does not contribute to strength development, and DEIPA only slightly improves strength development (Table 3 and Figure 1). Furthermore, when TIPA and DEIPA are added during grinding without limestone, DEIPA contributes only slightly to strength development, and TIPA does not contribute to strength development at all (Table 2).
[0014] TIPA and / or DEIPA may be added to the slurry immediately after starting to mix the water with the low IM cement clinker powder, but adding them to the water before mixing with the low IM cement clinker powder allows them to act uniformly and sufficiently.
[0015] Preferably, 30 to 100 parts by mass of water, more preferably 40 to 65 parts by mass of water, is mixed with 100 parts by mass of low IM cement clinker powder. The water temperature during mixing is, for example, 5° C. to 35° C. The mixing time with water, the equipment used for mixing, etc. are determined, for example, according to standard methods.
[0016] Preferably, TIPA and / or DEIPA are added in a total amount of 0.01 to 0.05 parts by mass per 100 parts by mass of the low-IM cement clinker powder. The strength-enhancing effect of TIPA and DEIPA is manifested when added in an amount of 0.01 part by mass or more, and addition of 0.05 parts by mass or more does not increase the effect. More preferably, TIPA and / or DEIPA are added in a total amount of 0.02 to 0.04 parts by mass per 100 parts by mass of the low-IM cement clinker powder. It is particularly preferred that TIPA be added in an amount of 0.01 to 0.05 parts by mass per 100 parts by mass of the low-IM cement clinker powder, and most preferably, TIPA be added in an amount of 0.02 to 0.04 parts by mass per 100 parts by mass of the low-IM cement clinker powder. Hydraulic compositions often contain aggregates such as sand and gravel, which have small specific surface areas and low reactivity. Since TIPA and DEIPA act on low IM cement clinker powder, the amount to be added is determined based on the amount of low IM cement clinker powder.
[0017] Preferably, the low IM cement clinker powder contains limestone powder at a concentration of 2% by mass or more and 10% by mass or less, more preferably 3% by mass or more and 8% by mass or less, and gypsum powder at a concentration of 1.5% by mass or more and 5% by mass or less, more preferably 1.8% by mass or more and 3% by mass or less, calculated as SO3.
[0018] The hydraulic composition slurry produced according to the present invention exhibits extremely good strength development (see Table 4 and FIG. 2).
[0019] 10A and 10B are characteristic diagrams showing the results of a strength test in a comparative example and an example, respectively.
[0020] C in the present invention 3 A, C 4 AF and C 3 The amount of S is determined by the Bogue formula.
[0021] The Bogue formula is used alongside coefficients and ratios to calculate the approximate composition of major compounds using the values of major chemical components, and is well known to those skilled in the art. Just to be sure, the method for calculating the amount of each mineral in cement clinker using the Bogue formula is described below, with units in mass%. C 3S amount = (4.07 x CaO) - (7.60 x SiO 2 ) - (6.72 x Al 2 O 3 ) - (1.43 x Fe 2 O 3 ) C 2 S amount=(2.87×SiO 2 ) - (0.754 x C 3 S) C 3 Amount = (2.65 x Al 2 O 3 ) - (1.69 x Fe 2 O 3 ) C 4 AF amount = 3.04 x Fe 2 O 3
[0022] The iron percentage (I.M.) is calculated using the values of the main chemical components, along with the hydraulic percentage (H.M.), silica percentage (S.M.), activity index (A.I.), and lime saturation degree (LSD). These percentages and coefficients are used as characteristic values for managing cement clinker production, as one of the coefficients and ratios, and are well known to those skilled in the art. Just to be sure, the calculation method for the iron percentage is described below along with other percentages and coefficient values, which are mass ratios. Note that "CaO" and "SiO" in the above formula are 2 " "Al 2 O 3 " and "Fe 2 O 3 " can be measured in accordance with JIS R5202 "Chemical analysis method for Portland cement" or JIR 5204 "Fluorescence X-ray analysis method for cement".
[0023] Hydraulic modulus (HM)=CaO / (SiO 2 +Al 2 O 3 +Fe 2 O 3 ) Silicate ratio (S.M.) = SiO 2 / (Al 2 O 3 +Fe 2 O 3 ) Activity Coefficient (A.I.) = SiO 2 / Al 2 O 3 Iron rate (I.M.) = Al 2 O3 / Fe 2 O 3 Lime saturation (L.S.D.) = CaO / (2.8 x SiO 2 +1.18 x Al 2 O 3 +0.65×Fe 2 O 3 )
[0024] In this specification, when the upper and lower limits of a range are indicated, such as "A to B," they are included, such as "A or more and B or less." When composition or content is expressed in percentages, it means mass percent. Furthermore, powder containing at least limestone and gypsum in addition to cement clinker is called cement clinker powder. The amount of water to be mixed is indicated in parts by mass as the amount of water mixed with 100 parts by mass of cement clinker powder. This ratio is called the water-to-cement ratio (W / C). If the cement clinker powder contains blast furnace slag, fly ash, etc. in addition to cement clinker, lime, and gypsum, the mass of these materials is also included. However, cement clinker powder does not include the aggregates sand or gravel.
[0025] As described above, in the low IM cement clinker used in the present invention, C 3 A, C 4 The total amount of AF must be 24% or more. If the amount of these is less than 24%, it becomes difficult to obtain cement clinker with good physical properties such as strength development by firing at a temperature of 1300 to 1400°C. As will be described later, in order to obtain high strength development, it is necessary to 3 S must be 63% or more. 3 A and C 4 The total amount of AF is 24% or more and 37% or less, preferably 24% or more and 35% or less, more preferably 24% or more and 32% or less, and particularly preferably 24% or more and 28% or less.
[0026] Of these two components, C 4 AF is preferably present alone in an amount of 15% or more, since it allows sufficient sintering even at low temperatures and reduces the amount of f-CaO in the cement clinker.
[0027] C 3The amount of S is extremely important for the strength development of a cement composition (hereinafter simply referred to as "cement"). If this amount falls below 63%, C 3 A and C 4 Even if the total amount of AF and the iron content described later are set within the predetermined ranges, good strength development cannot be obtained. 3 A and C 4 Since the total amount of AF is at least 24%, C 3 The upper limit of the S content is 76%. In order to ensure a certain amount of time from the start to the end of coagulation, the S content is preferably 63% to 70%, and more preferably 63% to 65%.
[0028] The low IM cement clinker used in the present invention further contains C 2 S may be contained. The amount thereof is 15% or less, and preferably 3% or more. From the viewpoint of obtaining long-term strength, C is particularly preferable. 2 S and C 3 The total amount of S is 69% or more and 76% or less.
[0029] The most important thing about the cement clinker used in the present invention is that the iron content (I.M.) is 0.8 or more and 1.3 or less, preferably 1.14 to 1.27. If the iron content exceeds 1.3, sufficient strength development (more specifically, development of mortar strength, for example) cannot be obtained even if the cement clinker satisfies other requirements. Furthermore, if the iron content exceeds 1.3, the time from the start to the end of setting tends to become too long, and for this reason too, the iron content is set to 1.3 or less. The iron content is preferably 1.14 to 1.27.
[0030] The hydraulic ratio and silicic acid ratio are not particularly limited, but in order to obtain an excellent balance of various physical properties, the hydraulic ratio is preferably 1.8 to 2.2, particularly preferably 1.9 to 2.1, and the silicic acid ratio is preferably 1.0 to 2.0, particularly preferably 1.1 to 1.7.
[0031] There are no particular limitations on the method for producing low-IM cement clinker, and it can be easily obtained by preparing and mixing known cement clinker raw materials in predetermined proportions so as to achieve the above-mentioned mineral ratios and coefficients, and then burning the mixture by a known method (for example, an SP kiln or an NSP kiln).
[0032] The cement raw materials may be prepared and mixed by any known method. For example, waste materials, by-products, and other raw materials (CaO sources such as limestone, quicklime, and slaked lime, SiO sources such as silica stone, etc.) may be mixed in advance. 2 Al from sources, clay, etc. 2 O 3 Fe source, iron source, etc. 2 O 3 The composition of the raw materials (sources, etc.) is measured, and the blending ratio of each raw material is calculated from the proportion of each component in these raw materials so that the blending ratio falls within the above range, and the raw materials are blended in that ratio.
[0033] The raw materials used in the production of low IM cement clinker are the same as those used in the production of conventional cement clinker, and are not particularly limited. Of course, waste materials, by-products, etc. can also be used.
[0034] In the production of low-IM cement clinker, it is preferable to use one or more waste materials, by-products, etc., from the viewpoint of promoting the effective utilization of waste materials, by-products, etc. Specific examples of usable waste materials and by-products include blast furnace slag, steelmaking slag, non-ferrous slag, coal ash, sewage sludge, water purification sludge, papermaking sludge, construction soil, foundry sand, soot and dust, incineration fly ash, molten fly ash, chlorine bypass dust, wood chips, waste clay, slag, waste tires, shells, municipal waste, and its incineration ash. Some of these materials can be used as both a cement raw material and a thermal energy source.
[0035] Low IM cement clinker is C 3 A and C 4 It contains a large amount of AF, a mineral whose constituent element is aluminum. Therefore, compared to conventional cement clinker, it has the advantage of being able to be produced using more waste and by-products that are high in aluminum.
[0036] In the present invention, the low IM cement clinker powder comprises gypsum and limestone in addition to the low IM cement clinker.
[0037] As the gypsum, any known gypsum as a raw material for cement production, such as gypsum dihydrate, gypsum hemihydrate, gypsum anhydride, etc., can be used without any particular limitation. The amount of gypsum added is determined by the amount of SO in the low IM cement clinker powder. 3 It is preferable to add the amount so that it is 1.5 to 5.0 mass %, and more preferably 1.8 to 3 mass %.
[0038] The limestone can be any limestone known as a cement admixture. For example, natural limestone or synthetic calcium carbonate can be used. Adding limestone results in better strength development than when not adding limestone.
[0039] The limestone content in the low-IM cement clinker powder is preferably 2 to 10% by mass. If the limestone content is less than 2%, the synergistic effect with the additives is not sufficiently obtained. To better demonstrate the strength-improving effect, the limestone content is more preferably 3 to 8% by mass.
[0040] The low-IM cement clinker powder may contain, in addition to the limestone, fly ash and / or blast furnace slag and / or siliceous admixture, etc. In this case, the total concentration of the limestone and blast furnace slag and the fly ash and / or siliceous admixture in the low-IM cement clinker powder is 10 mass% or less.
[0041] The above cement clinker, gypsum, limestone and other admixtures have a fineness of 2800 to 4500 cm 3 in terms of Blaine specific surface area. 2 It is preferable that the molecular weight is adjusted to be / g.
[0042] The pulverization method for preparing the powder to the desired fineness may be any known technique without particular limitation, and the components may be pulverized separately and then mixed, or may be mixed and then pulverized. As the pulverizer, a ball mill, a vertical mill, etc. may be used.
[0043] The hydraulic composition slurry produced by the present invention can be used as a Portland cement slurry, particularly a slurry using Portland cement conforming to JIS standards. Examples of Portland cement include ordinary Portland cement, high-early-strength Portland cement, and ultra-high-early-strength Portland cement. In addition to being used as Portland cement, it can also be used as a component of various blended cements and solidifying materials such as soil solidification agents. When preparing Portland cement, blended cement, soil solidification agents, etc., aggregates such as sand and gravel may be added.
[0044] In the method for producing hydraulic composition slurry of the present invention, triisopropanolamine (TIPA) and / or diethanolisopropanolamine (DEIPA) are added when low-IM cement clinker powder is mixed with water. The low-IM cement clinker powder contains limestone powder and gypsum powder in addition to cement clinker itself. High strength development is achieved when TIPA and / or DEIPA and limestone powder are included. Table 3 and Figure 1 show the strength when limestone is not included, and Table 4 and Figure 2 show the strength when limestone is included.
[0045] The mixing method is not particularly limited, and known methods using a cement mixer, a propeller mixer, etc. may be used. It is preferable that TIPA and / or DEIPA be uniformly mixed with water in advance. However, TIPA and / or DEIPA may also be added to the slurry immediately after starting to mix water and low-IM cement clinker powder.
[0046] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0047] Industrial raw materials including limestone, coal ash, and waste soil from construction were mixed and fired in an electric furnace at 1,350°C for 90 minutes to obtain a low-IM cement clinker having the mineral composition and coefficient values according to the Bogue method shown in Table 1.
[0048] 100% by mass of low IM cement clinker, SO 3Gypsum was added so that the conversion was 2±0.2 mass%, and limestone was further added to obtain a specific surface area of 3200±50 cm by the Blaine method. 2 The mixture was pulverized to produce each cement (hydraulic composition) so that the mortar compressive strength of the obtained cement was measured.
[0049] The various measurement methods are as follows.
[0050] Measurement of chemical composition of raw materials and cement clinker: Measurement was carried out by fluorescent X-ray analysis in accordance with JIS R5204.
[0051] Measurement of mortar compressive strength: Measured by a method conforming to JIS R5201, and compared with the compressive strength of DEG, which has been conventionally used as a grinding aid, set at 100.
[0052]
[0053] <Production of hydraulic composition slurry using additives as grinding aids> Based on 100% by mass of the cement clinker obtained as described above, 3 Gypsum was added in an amount equivalent to 2.0±0.2% by mass (weight ratio: gypsum dihydrate / gypsum hemihydrate = 1). Furthermore, 0.03 parts by mass of an additive was added to a mixture of 100 parts by mass of cement clinker and gypsum, and the specific surface area measured by the Blaine method was 3200±50 cm 2 The resulting low IM cement clinker powder was mixed and pulverized in a ball mill so that the water-cement ratio was 50%.
[0054] The additives used were diethylene glycol (hereinafter referred to as DEG), triisopropanolamine (hereinafter referred to as TIPA), diethyleneisopropanolamine (hereinafter referred to as DEIPA), and triethanolamine (hereinafter referred to as TEA).
[0055] The hydraulic composition slurry produced using the above additive as a grinding aid was subjected to a compressive strength test in accordance with JIS R5201. The results are shown in Table 2.
[0056]
[0057] <Production of hydraulic composition slurry when additives are mixed with mixing water> The hydraulic composition slurry was prepared by mixing 100% by mass of the cement clinker obtained as described above with SO 3 Gypsum was added in an amount equivalent to 2.0±0.2 mass% (weight ratio: gypsum dihydrate / gypsum hemihydrate = 1) to obtain a granule having a specific surface area of 3200±50 cm2 by Blaine method. 2 The mixture was mixed and pulverized in a ball mill so that the total weight of the clinker powder was 100g / g, to produce a low IM cement clinker powder.
[0058] The mixing water used in measuring the compressive strength of the mortar was mixed with 0.03 parts by mass of an additive per 100 parts by mass of cement clinker.
[0059] Table 3 shows the results of the compressive strength test of the hydraulic composition slurry obtained by mixing the above additives with mixing water.
[0060]
[0061] <Production of hydraulic composition slurry when mixing low IM cement clinker powder containing limestone with mixing water containing additives> For the low IM cement clinker in Table 1, SO 3 A 2.0±0.2 mass% amount of gypsum (weight ratio: gypsum dihydrate / gypsum hemihydrate = 1, total weight 3.42 g) was added to 100 mass parts of cement clinker, and 5.26 mass parts of limestone was added to 100 mass parts of cement clinker. The specific surface area measured by the Blaine method was 3200±50 cm 2 The low-IM cement clinker powder was produced by mixing and grinding the materials in a ball mill so that the limestone concentration was 4.84% by mass and the gypsum concentration was 3.15% by mass.
[0062] The hydraulic composition slurry was prepared by mixing 0.03 parts by mass of additive per 100 parts by mass of cement clinker with the mixing water used to measure the compressive strength of mortar, and the compressive strength was measured in accordance with JIS R5201. The test results are shown in Table 4.
[0063]
[0064] Comparative Examples 1 to 4 are examples in which various additives were used as grinding aids when grinding cement clinker. Compared to Comparative Example 1, which used DEG, a general-purpose additive, Comparative Examples 2, 3, and 4 did not show any significant strength-enhancing effect.
[0065] Comparative Examples 5 to 8 are examples in which various additives were mixed into the mixing water during mortar production.Comparative Examples 5, 6, and 7 do not show any significant strength-enhancing effect compared to Comparative Example 4, which used the general-purpose additive DEG.
[0066] Comparative Examples 9 and 10 and Examples 1 and 2 are examples in which various additives were mixed with the mixing water used in producing hydraulic slurry, and limestone was also mixed in. Compared to Comparative Example 9, which used the general-purpose additive DEG, Examples 1 and 2, which used the additive of the present invention, showed good strength at 3 days, and also showed significant increases in strength at 7 days and 28 days.
Claims
1. C calculated by the Borg formula 3 A and C 4 A method for producing a hydraulic composition slurry by mixing a low-IM cement clinker powder, in which the total amount of AF is 22 mass% or more and 40 mass% or less, and the iron ratio (IM), which represents the mass ratio of Al2O3 to Fe2O3 in the cement clinker, is 0.8 to 1.3, with water, wherein the low-IM cement clinker powder contains at least limestone powder and gypsum powder in addition to the low-IM cement clinker, and triisopropanolamine (TIPA) and / or diethanolisopropanolamine (DEIPA) are added when the low-IM cement clinker powder is mixed with water.
2. A method for producing a hydraulic composition slurry according to claim 1, characterized in that triisopropanolamine (TIPA) and / or diethanolisopropanolamine (DEIPA) are added to the water before mixing with the low IM cement clinker powder.
3. A method for producing a hydraulic composition slurry according to claim 2, characterized in that 30 parts by mass or more and 100 parts by mass or less of water are mixed with 100 parts by mass of the low IM cement clinker powder.
4. A method for producing a hydraulic composition slurry according to claim 3, characterized in that triisopropanolamine (TIPA) and / or diethanolisopropanolamine (DEIPA) are added in a total amount of 0.01 to 0.05 parts by mass per 100 parts by mass of the low IM cement clinker powder.
5. A method for producing a hydraulic composition slurry according to claim 4, characterized in that triisopropanolamine (TIPA) is added in an amount of 0.01 part by mass or more and 0.05 part by mass or less per 100 parts by mass of the low IM cement clinker powder when mixed with water.
6. A method for producing a hydraulic composition slurry according to claim 4 or 5, characterized in that the low IM cement clinker powder contains limestone powder at a concentration of 2% by mass or more and 10% by mass or less, and gypsum powder at a concentration of 1.5% by mass or more and 5% by mass or less, calculated as SO3.
Citation Information
Patent Citations
Method for manufacturing cement clinker
JP5665638B2
Method for producing hydraulic composition
JP6825171B1
Reinforced blended cement composition and reinforced portland cement composition
JP1991183647A
Cement admixture and cement and concrete compounded with the cement admixture
JP1997142900A
High activity cement clinker, high activity cement, and early strength cement composition
JP2012091992A