Biodegradable resin composition and molded body

The biodegradable resin composition, featuring a zinc element and a specific polyester structure, addresses hydrolysis susceptibility in conventional bioplastics by enhancing thermal and hydrolytic stability, ensuring effective degradation and reduced environmental impact.

WO2024204351A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/012259
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional biodegradable plastics suffer from hydrolysis susceptibility, leading to decreased physical properties during processing, storage, and use, and their enhanced hydrolysis resistance methods result in prolonged degradation, causing environmental persistence.

Method used

A biodegradable resin composition incorporating a zinc element within specific concentration ranges, combined with a polyester derived from aliphatic and aromatic dicarboxylic acids, enhances thermal and hydrolytic stability while maintaining biodegradability.

Benefits of technology

The zinc-enhanced biodegradable resin composition achieves balanced hydrolysis resistance and biodegradability, ensuring excellent thermal stability during processing and hydrolytic stability during use, thereby reducing environmental persistence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided are: a biodegradable resin composition having excellent thermal stability during heating and melting and having excellent hydrolysis stability during use; and a molded body thereof. The problem is solved by a biodegradable resin composition comprising a biodegradable resin (A) and a zinc element, wherein: the content of the zinc element is 0.001-7,000 ppm by mass; and the biodegradable resin (A) contains at least either (i) a polyester containing an aliphatic diol-derived constitutional unit and an aliphatic dicarboxylic acid-derived constitutional unit as main constitutional units or (ii) a polyester containing an aliphatic diol-derived constitutional unit, an aliphatic dicarboxylic acid-derived constitutional unit, and an aromatic dicarboxylic acid-derived constitutional unit as main constitutional units.
Need to check novelty before this filing date? Find Prior Art

Description

Biodegradable resin composition and molded article

[0001] The present invention relates to a biodegradable resin composition and a molded article thereof.

[0002] In recent years, concerns about ecosystem and environmental pollution due to marine disposal of plastic products have become apparent. For example, in Europe, regulations and laws are being enacted that prohibit the use of disposable plastic shopping bags in retail stores and disposable plastic containers such as cups and plates. Various regulations are being enacted around the world from the perspective of preventing environmental pollution. Recently, there has been a demand for biodegradable plastic products that can be composted, and that also combine moldability and quality from the perspectives of cost and practical use.

[0003] Conventionally, known biodegradable plastics (resins) include, for example, polybutylene succinate (hereinafter abbreviated as PBS), polybutylene terephthalate / adipate (hereinafter abbreviated as PBAT), polybutylene succinate / terephthalate (hereinafter abbreviated as PBST), polylactic acid (hereinafter abbreviated as PLA), polybutylene succinate / adipate (hereinafter abbreviated as PBSA), and polyhydroxyalkanoate (hereinafter abbreviated as PHA). PHAs include poly(3-hydroxybutyrate) (hereinafter abbreviated as PHB), poly(3-hydroxybutyrate / 3-hydroxyvalerate) (hereinafter abbreviated as PHBV), poly(3-hydroxybutyrate / 3-hydroxyhexanoate) (hereinafter abbreviated as PHBH), and poly(3-hydroxybutyrate / 4-hydroxybutyrate).

[0004] Due to their structure, these biodegradable polyesters are susceptible to hydrolysis by water in the environment, and there is concern that they may deteriorate during processing, storage, and use, resulting in a decrease in their physical properties.

[0005] As a method for solving this problem, Patent Document 1 shows that by blending a specific amount of a polycarbodiimide compound and a specific antioxidant together with a biodegradable plastic, the hydrolysis resistance and heat resistance of the resulting biodegradable plastic composition can be improved.

[0006] Japanese Patent Application Laid-Open No. 2003-313436

[0007] The technology described in Patent Document 1 is a technology in which hydrolysis is suppressed by reacting a carbodiimide with a biodegradable polyester, but at the same time, there is a problem that the biodegradation rate is significantly reduced, the process of decomposing after use is prolonged, and the polyester remains in the environment for a long period of time.

[0008] The present invention has been made in view of the above-mentioned problems of the conventional technology, and aims to provide an excellent material that has a balance between hydrolysis resistance and biodegradability compared to conventional methods for imparting hydrolysis resistance.

[0009] As a result of extensive research aimed at solving the above problems, the present inventors have found that by incorporating a specific amount of zinc element into a biodegradable resin, the resulting biodegradable resin composition has improved thermal stability and hydrolytic stability. That is, the gist of the present invention resides in the following [1] to

[12] .

[0010] [1] A biodegradable resin composition comprising a biodegradable resin (A) and zinc element, wherein the zinc element content is 0.001 ppm by mass or more and 7000 ppm by mass or less, and wherein the biodegradable resin (A) comprises at least one of (i) a polyester having as main structural units structural units derived from an aliphatic diol and structural units derived from an aliphatic dicarboxylic acid, and (ii) a polyester having as main structural units structural units derived from an aliphatic diol, structural units derived from an aliphatic dicarboxylic acid, and structural units derived from an aromatic dicarboxylic acid. [2] The biodegradable resin composition according to [1], wherein the structural units derived from an aliphatic dicarboxylic acid have 2 to 30 carbon atoms. [3] The biodegradable resin composition according to [1] or [2], wherein the structural units derived from an aromatic dicarboxylic acid have 6 to 12 carbon atoms. [4] The biodegradable resin composition according to any one of [1] to [3], wherein the structural units derived from an aliphatic diol have 2 to 30 carbon atoms. [5] The biodegradable resin composition according to any one of [1] to [4], wherein the structural units derived from an aromatic dicarboxylic acid are terephthalic acid. [6] The biodegradable resin composition according to any one of [1] to [5], wherein the structural units derived from an aliphatic dicarboxylic acid are succinic acid. [7] The biodegradable resin composition according to any one of [1] to [6], wherein the content of structural units derived from an aliphatic dicarboxylic acid is 40 mol% or more relative to the total of structural units derived from an aliphatic dicarboxylic acid and structural units derived from an aromatic dicarboxylic acid contained in all resins in the biodegradable resin composition. [8] The biodegradable resin composition according to any one of [1] to [7], wherein the bio-content of the biodegradable resin (A) calculated according to ASTM D6866 is 20% or more. [9] The biodegradable resin composition according to any one of [1] to [8], further comprising an inorganic filler.

[10] The biodegradable resin composition according to [9], wherein the inorganic filler is calcium carbonate.

[11] The biodegradable resin composition according to

[10] , wherein the calcium carbonate is heavy calcium carbonate.

[12] A molded article made using the biodegradable resin composition according to any one of [1] to

[11] .

[0011] According to the present invention, it is possible to provide a biodegradable resin composition that has excellent thermal stability when heated and melted and excellent hydrolytic stability when used, and a molded article thereof.

[0012] The present invention is not limited to the following description and can be modified as desired without departing from the spirit of the present invention. In this specification, when a numerical value or physical property value is enclosed between "-" and "-", the lower and upper limits are included as endpoints. In this specification, the expression "A or B" can be interpreted as "at least one selected from the group consisting of A and B." In this specification, "heat resistance" and "thermal stability" are synonymous, and "hydrolysis resistance" and "hydrolytic stability" are synonymous. Although multiple embodiments are described in this specification, various conditions in each embodiment can be applied to each other to the extent applicable.

[0013] <Biodegradable Resin Composition> A biodegradable resin composition according to one embodiment of the present invention (hereinafter also simply referred to as "biodegradable resin composition" or "resin composition") comprises a biodegradable resin (A) and zinc element, wherein the zinc element content is 0.001 ppm by mass or more and 7000 ppm by mass or less, and the biodegradable resin (A) comprises at least either (i) a polyester having as main structural units structural units derived from an aliphatic diol and structural units derived from an aliphatic dicarboxylic acid, or (ii) a polyester having as main structural units structural units derived from an aliphatic diol, structural units derived from an aliphatic dicarboxylic acid, and structural units derived from an aromatic dicarboxylic acid.

[0014] From the viewpoints of heat resistance and hydrolysis resistance, the biodegradable resin composition contains elemental zinc at a content of 0.001 ppm by mass or more and 7000 ppm by mass or less. The method for incorporating elemental zinc into the biodegradable resin composition is not particularly limited; zinc may be incorporated as simple zinc, or, if other components are included in the composition, zinc may be incorporated in the other components. Examples of compositions containing elemental zinc and other components include zinc salts such as zinc acetate dihydrate, zinc carbonate, zinc chloride, zinc fatty acid, zinc oxalate, zinc phosphate, and zinc oxide, as well as calcium carbonate containing elemental zinc, such as heavy calcium carbonate. Heavy calcium carbonate differs from light calcium carbonate, which is chemically produced using limestone as a raw material, in that it is calcium carbonate produced by physically crushing and classifying natural limestone.

[0015] The zinc element content in the biodegradable resin composition is not particularly limited as long as it is 0.001 mass ppm or more and 7000 mass ppm or less, but is preferably 0.01 mass ppm or more, more preferably 0.05 mass ppm or more, particularly preferably 0.1 mass ppm or more, and is preferably 5000 mass ppm or less, more preferably 3000 mass ppm or less, even more preferably 2000 mass ppm or less, and particularly preferably 1000 mass ppm or less. If the content is above the lower limit of the above range, the thermal stability and hydrolysis resistance of the biodegradable resin composition are ensured. Furthermore, if the content is below the upper limit of the above range, the biodegradable resin composition is less likely to be decomposed by acids or alkalis derived from the zinc component.

[0016] The zinc element content in the biodegradable resin composition can be measured by weighing a sample, adding nitric acid to dissolve it, adjusting the volume to a constant level with pure water, and then using an ICP light emitting device (Agilent 5800, manufactured by Agilent) to measure the zinc element content by the standard addition method.

[0017] [Biodegradable Resin (A)] The biodegradable resin (A) contains at least one of (i) a polyester whose main structural units are structural units derived from an aliphatic diol and structural units derived from an aliphatic dicarboxylic acid, and (ii) a polyester whose main structural units are structural units derived from an aliphatic diol, structural units derived from an aliphatic dicarboxylic acid, and structural units derived from an aromatic dicarboxylic acid. Here, structural units derived from an aliphatic diol are also referred to as "aliphatic diol units," structural units derived from an aliphatic dicarboxylic acid are also referred to as "aliphatic dicarboxylic acid units," and structural units derived from an aromatic dicarboxylic acid are also referred to as "aromatic dicarboxylic acid units."

[0018] The content of the biodegradable resin (A) in the biodegradable resin composition is not particularly limited, but from the viewpoint of moldability and mechanical properties, it is usually 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. There is no need to set an upper limit, and it is sufficient if it is 100% by mass or less.

[0019] Each structural unit of the biodegradable resin (A) will be described below.

[0020] (Aliphatic diol) As the aliphatic diol, those usually used as raw materials for polyesters can be used without any particular limitation. The carbon number of the aliphatic diol is not particularly limited, but is preferably 2 to 30, more preferably 2 to 20, even more preferably 4 to 12, and particularly preferably 4 to 10. When the carbon number of the aliphatic diol is equal to or greater than the lower limit of the above range, a good balance between biodegradability and mechanical properties is achieved. Furthermore, when the carbon number of the aliphatic diol is equal to or less than the upper limit of the above range, good crystallinity is achieved.

[0021] Examples of aliphatic diols include alkylene diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and neopentyl glycol; oxyalkylene diols such as diethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol; and cycloalkylene diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol. From the viewpoints of mechanical properties, biodegradability, and heat resistance, among these, ethylene glycol, 1,4-butanediol, and 1,10-decanediol are preferred, and ethylene glycol and 1,4-butanediol are particularly preferred. These aliphatic diols may or may not be derivatives thereof.

[0022] The above aliphatic diol compounds may be compounds having a structure in which one or more kinds of compounds are mutually dehydrated and condensed.

[0023] The above aliphatic diols may be used alone or in combination of two or more.

[0024] Furthermore, ethylene glycol, 1,3-propanediol, 1,4-butanediol, and the like derived from plant materials can be used.

[0025] - Content of Aliphatic Diol Units in Biodegradable Resin (A) The content of aliphatic diol units in the biodegradable resin (A) is not particularly limited, but from the viewpoint of mechanical properties, it is usually 10 mol% or more, preferably 30 mol% or more, more preferably 45 mol% or more, and even more preferably 49 mol% or more, relative to 100 mol% of all structural units constituting the biodegradable resin (A). Also, it is usually 55 mol% or less, and even more preferably 50 mol% or less.

[0026] (Dicarboxylic Acid) From the viewpoint of ensuring excellent thermal stability and hydrolysis resistance, the biodegradable resin (A) may be an embodiment in which, as a structural unit derived from a dicarboxylic acid, a structural unit derived from an aliphatic dicarboxylic acid is included in the main structural unit (hereinafter also referred to as "Aspect A"), or an embodiment in which, in addition to the structural unit, a structural unit derived from an aromatic dicarboxylic acid is included in the main structural unit (hereinafter also referred to as "Aspect B"). Alternatively, both the polyester of Aspect A and the polyester of Aspect B may be used.

[0027] The number of carbon atoms in the aliphatic dicarboxylic acid is not particularly limited, but is preferably 2 to 30, more preferably 4 to 20, even more preferably 4 to 12, and particularly preferably 4 to 10. When the number of carbon atoms in the aliphatic dicarboxylic acid is equal to or greater than the lower limit of the above range, the thermal stability is excellent. When the number of carbon atoms in the aliphatic dicarboxylic acid is equal to or less than the upper limit of the above range, the biodegradability and thermal stability are excellent.

[0028] Specific examples of aliphatic dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, succinic anhydride, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecadicarboxylic acid, dodecadicarboxylic acid, and dimer acid. Among these, from the viewpoints of heat resistance and crystallinity, aliphatic dicarboxylic acids such as succinic acid, succinic anhydride, adipic acid, and sebacic acid are preferred. In particular, from the viewpoints of biodegradability, cost, and thermal stability, aliphatic dicarboxylic acids having 4 carbon atoms such as succinic acid or succinic anhydride are preferred, and succinic acid is more preferred.

[0029] The number of carbon atoms in the aromatic dicarboxylic acid is not particularly limited, but is preferably 6 to 12, and more preferably 6 to 8. When the number of carbon atoms in the aromatic dicarboxylic acid is equal to or greater than the lower limit of the above range, the thermal stability is good. When the number of carbon atoms in the aromatic dicarboxylic acid is equal to or less than the upper limit of the above range, the biodegradability is good.

[0030] Specific examples of aromatic dicarboxylic acids include 2,5-furandicarboxylic acid, phthalic acid, isophthalic acid, terephthalic acid, dibromoisophthalic acid, sulfoisophthalic acid, 1,4-phenylenedioxydicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylketonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, hexahydrophthalic acid, hexahydroisophthalic acid, and hexahydroterephthalic acid. Of these, from the viewpoints of raw material availability and biodegradability, 2,5-furandicarboxylic acid and terephthalic acid are preferred, and terephthalic acid is particularly preferred.

[0031] The aromatic dicarboxylic acid may be a derivative thereof or may not be a derivative. For example, derivatives of the aromatic dicarboxylic acids exemplified above are preferred, and among them, lower alkyl esters having 1 to 4 carbon atoms or acid anhydrides, etc. are mentioned. Specific examples of the derivatives of aromatic dicarboxylic acid compounds include lower alkyl esters such as methyl esters, ethyl esters, propyl esters, or butyl esters of the aromatic dicarboxylic acids exemplified above; or cyclic acid anhydrides of the aromatic dicarboxylic acids exemplified above, such as phthalic anhydride; etc.

[0032] The above aliphatic dicarboxylic acids and aromatic dicarboxylic acids may each be used alone or in combination of two or more kinds.

[0033] Furthermore, succinic acid, succinic anhydride, adipic acid, etc., derived from plant materials can be used.

[0034] Content of each dicarboxylic acid unit in the biodegradable resin (A) In the case of embodiment A, from the viewpoint of biodegradability and crystallinity, the content is usually 30 mol% or more, preferably 40 mol% or more, more preferably 45 mol% or more, and even more preferably 49 mol% or more, relative to 100 mol% of all structural units constituting the biodegradable resin (A), and is usually 70 mol% or less, preferably 60 mol% or less, more preferably 55 mol% or less, and even more preferably 50 mol% or less.

[0035] In the case of aspect B, the content of the aliphatic dicarboxylic acid unit in the biodegradable resin (A) is not particularly limited, but from the viewpoint of biodegradability and crystallinity, it is usually 20 mol% or more, preferably 25 mol% or more, more preferably 27 mol% or more, based on 100 mol% of all structural units constituting the biodegradable resin (A). Also, in the case of aspect B, the content of the aromatic dicarboxylic acid unit in the biodegradable resin (A) is not particularly limited, but from the viewpoint of biodegradability and crystallinity, it is usually 5 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, more preferably 22 mol% or more, based on 100 mol% of all structural units constituting the biodegradable resin (A).

[0036] The content of aliphatic dicarboxylic acid units in all resins in the biodegradable resin composition is preferably 40 mol% or more, more preferably 45 mol% or more, and particularly preferably 50 mol% or more, based on the total of the aliphatic dicarboxylic acid units and aromatic dicarboxylic acid units in all resins in the biodegradable resin composition. When the content is equal to or greater than the lower limit of the above range, the composition has excellent biodegradability, thermal stability, and hydrolysis resistance.

[0037] The biodegradable resin composition may contain a resin other than the biodegradable resin (A). In this case, the "content of the aliphatic dicarboxylic acid units contained in all the resins in the biodegradable resin composition" can be adjusted to satisfy the preferred range by adjusting the amount of the aliphatic dicarboxylic acid units in the resins other than the biodegradable resin (A).

[0038] (Other Copolymerization Components) In the production of polyesters, components (other copolymerization components) other than the diols and dicarboxylic acids described above may be copolymerized. Examples of copolymerization components that can be used in this case include hydroxycarboxylic acids such as lactic acid, glycolic acid, hydroxybutyric acid, hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, malic acid, maleic acid, citric acid, and fumaric acid; esters, lactones, and hydroxycarboxylic acid polymers of these hydroxycarboxylic acids; trifunctional or higher polyhydric alcohols such as glycerin, trimethylolpropane, and pentaerythritol; and trifunctional or higher polyvalent carboxylic acids or anhydrides thereof such as propanetricarboxylic acid, pyromellitic acid, and trimellitic acid, benzophenonetetracarboxylic acid, and anhydrides thereof.

[0039] Furthermore, adding a small amount of a trifunctional or higher functional hydroxycarboxylic acid, a trifunctional or higher functional alcohol, or a trifunctional or higher functional carboxylic acid makes it easy to obtain a polyester with high viscosity. Among these, hydroxycarboxylic acids such as malic acid, citric acid, and fumaric acid are preferred, and malic acid is particularly preferred. Examples of components constituting trifunctional or higher functional polyhydric alcohol units include glycerin, trimethylolpropane, and pentaerythritol. These may be used alone or in combination of two or more.

[0040] The amount of the tri- or higher functional compound is preferably 0.001 to 5 mol %, and more preferably 0.05 to 0.5 mol %, relative to 100 mol % of all dicarboxylic acid components in the polyester raw material. If the amount exceeds the upper limit of this range, gel (unmelted material) is likely to form in the resulting polyester, while if it is below the lower limit, the advantage of using the multifunctional compound (usually, the ability to increase the viscosity of the resulting polyester) is difficult to obtain.

[0041] [Characteristics of Biodegradable Resin (A)] (Bio-content) The bio-content of the biodegradable resin (A) calculated according to ASTM D6866 is not particularly limited, but from the viewpoint of greenhouse gas reduction, it is preferably 10% or more, more preferably 20% or more, even more preferably 30% or more, and particularly preferably 50% or more. Furthermore, there is no particular upper limit, and it may be 100%, 100% or less, 70% or less, or 65% or less. The bio-content can be controlled by adjusting the ratio of monomer units produced from plant-derived raw materials to the total structural units constituting one or more biodegradable resins (A). Furthermore, the bio-content may be satisfied by one type of biodegradable resin (A), or by the entire one or more biodegradable resins (A), and it is preferable that at least one type of biodegradable resin (A) satisfies the bio-content.

[0042] (Intrinsic Viscosity) The intrinsic viscosity (IV, dL / g) of the biodegradable resin (A) is not particularly limited, but the intrinsic viscosity of at least one of the biodegradable resins (A) is preferably 1.2 dL / g or more, more preferably 1.4 dL / g or more, and particularly preferably 1.6 dL / g or more. The intrinsic viscosity is preferably 2.8 dL / g or less, more preferably 2.5 dL / g or less, and particularly preferably 2.3 dL / g or less. All of the one or more biodegradable resins (A) may satisfy this intrinsic viscosity. If the intrinsic viscosity is below the lower limit of the above range, it is difficult to obtain sufficient mechanical strength when molded into a molded article. If the intrinsic viscosity exceeds the upper limit of the above range, the melt viscosity during molding is high, making molding difficult.

[0043] (Amount of terminal carboxyl groups) The amount of terminal carboxyl groups in the biodegradable resin (A) is not particularly limited, but is usually 80 (equivalents / ton) or less, preferably 60 (equivalents / ton) or less, more preferably 40 (equivalents / ton) or less, and particularly preferably 25 (equivalents / ton) or less. The lower the lower limit, the better the thermal stability and hydrolysis resistance, but it is usually 5 (equivalents / ton) or more. If the upper limit is exceeded, the viscosity will decrease significantly due to hydrolysis, which may significantly impair the quality.

[0044] (Melt Flow Rate (MFR)) The melt flow rate (MFR) of the biodegradable resin (A) is not particularly limited, but the MFR of at least one of the biodegradable resins (A) is preferably 0.5 to 50 g / 10 min, as measured at 190°C under a load of 2.16 kg according to JIS K7210 (2014). For film applications and extrusion molding applications, it is more preferably 0.5 to 20 g / 10 min, and even more preferably 1.0 to 10 g / 10 min. If the MFR is above the lower limit, the fluidity required for molding is obtained, and if it is below the upper limit, the resin will have excellent bubble stability during film molding. On the other hand, for injection molding applications and fiber applications, it is more preferably 0.5 to 50 g / 10 min, and even more preferably 3.0 to 40 g / 10 min. All of one or more biodegradable resins (A) may satisfy this MFR. If the MFR is equal to or higher than the lower limit, the fluidity required for molding is obtained, and if it is equal to or lower than the upper limit, the resin will have excellent mechanical properties such as impact strength of injection molded products.

[0045] (Weight-Average Molecular Weight) The weight-average molecular weight (Mw) of the biodegradable resin (A) is not particularly limited, but the weight-average molecular weight of at least one of the biodegradable resins (A) is preferably 10,000 or more, more preferably 25,000 or more, even more preferably 50,000 or more, and particularly preferably 100,000 or more. It is also preferably 1,000,000 or less, more preferably 500,000 or less, and particularly preferably 300,000 or less. The weight-average molecular weight may be satisfied by all of the one or more biodegradable resins (A). If the weight-average molecular weight (Mw) is equal to or greater than the lower limit of the above range, the material will have excellent moldability and mechanical properties. Furthermore, if the weight-average molecular weight (Mw) is equal to or less than the upper limit of the above range, molding at low temperatures of approximately 100 to 200°C is possible, which is excellent. The weight average molecular weight (Mw) is determined as a value converted into monodisperse polystyrene from a measurement value obtained by gel permeation chromatography (GPC) at a measurement temperature of 40° C. using chloroform as a solvent.

[0046] (Melting point, glass transition temperature, crystallization temperature) The melting point (Tm) of the biodegradable resin (A) is not particularly limited, but is usually 50 ° C or higher, preferably 70 ° C or higher, more preferably 80 ° C or higher, and even more preferably 85 ° C or higher. Also, it is usually 200 ° C or lower, preferably 180 ° C or lower, more preferably 150 ° C or lower, and even more preferably 130 ° C or lower. If the melting point is above the lower limit of the range, it is excellent in terms of crystallization and heat resistance. Furthermore, if the melting point is above the lower limit of the range, it is excellent in that it can be molded at low temperatures. The glass transition temperature (Tg) of the biodegradable resin (A) is not particularly limited, but is usually -70 ° C or higher, preferably -50 ° C or higher, more preferably -40 ° C or higher, and even more preferably -35 ° C or higher. Also, it is usually 60 ° C or lower, preferably 30 ° C or lower, more preferably 20 ° C or lower, and even more preferably 10 ° C or lower. If the glass transition temperature is above the lower limit of the range, the crystallinity is good. Furthermore, if the glass transition temperature is above the lower limit of the range, the resin will have excellent biodegradability. When the biodegradable resin is crystalline, the crystallization temperature (crystallization peak temperature) (Tc) of the biodegradable resin (A) is not particularly limited, but is usually 0°C or higher, preferably 10°C or higher, more preferably 20°C or higher, and even more preferably 30°C or higher, and is usually 150°C or lower, preferably 100°C or lower, and even more preferably 85°C or lower. If the crystallization temperature is above the lower limit of the range, a sufficient crystallization rate is achieved during molding. If the crystallization temperature is below the upper limit of the range, stable molding is possible. The melting point, glass transition temperature, and crystallization temperature can be measured using a differential scanning calorimeter (Seiko Corporation, product name: DSC220). Specifically, a sample of about 5 mg is precisely weighed, heated and melted under a nitrogen gas flow at a flow rate of 40 mL / min, and then cooled at a rate of 10°C / min, allowing the crystallization temperature Tc to be measured. Subsequently, the sample is heated at a rate of 10°C / min, allowing the glass transition temperature and melting point to be measured.Furthermore, the above melting point, glass transition temperature, and crystallization temperature may be satisfied by one type of biodegradable resin (A), or by all of one or more types of biodegradable resins (A), and it is preferable that at least one type of biodegradable resin (A) satisfies these requirements.

[0047] [Method for producing biodegradable resin (A)] The method for producing biodegradable resin (A) is not particularly limited, and known methods can be used. Below, a method for producing biodegradable resin (A) will be described, but it is merely an example, and the method for producing biodegradable resin (A) is not limited to this embodiment.

[0048] First, a reaction treatment including an esterification reaction of raw materials containing a diol and a dicarboxylic acid in the presence of a catalyst is carried out, followed by a polycondensation reaction treatment in which a polycondensation reaction is carried out.

[0049] (Esterification reaction treatment) Esterification reaction is a reaction that converts carboxylic acid into ester, and transesterification reaction is a reaction that reacts an ester with an alcohol to exchange the main chain moieties. The method for performing the esterification reaction treatment is not particularly limited, and known methods can be used. Furthermore, the esterification reaction treatment and other subsequent treatments can be performed in multiple consecutive reaction tanks or in a single reaction tank, but it is preferable to perform them in multiple consecutive reaction tanks in order to reduce fluctuations in the physical properties of the resulting polyester.

[0050] The reaction temperature in the esterification reaction treatment is not particularly limited as long as it is a temperature at which the esterification reaction can be carried out. However, in terms of being able to increase the reaction rate, it is preferably 200°C or higher, and more preferably 210°C or higher, and in order to prevent discoloration of the polyester, it is preferably 250°C or lower, more preferably 245°C or lower, and particularly preferably 240°C or lower.

[0051] If the reaction temperature is too low, the esterification reaction rate is slow, requiring a long reaction time, and undesirable reactions such as dehydration decomposition of the diol occur frequently. If the reaction temperature is too high, decomposition of the diol and dicarboxylic acid increases, and the amount of scattered material in the reaction vessel increases, which can easily cause the generation of foreign matter and make the reaction product hazy. It is also preferable that the esterification temperature be a constant temperature. A constant temperature stabilizes the esterification rate. The constant temperature may be within ±5°C of the set temperature, and is preferably within ±2°C.

[0052] The reaction atmosphere is not particularly limited, but an inert gas atmosphere such as nitrogen or argon is preferred. The reaction pressure is preferably 50 kPa to 200 kPa, preferably 60 kPa or more, more preferably 70 kPa or more, and preferably 130 kPa or less, more preferably 110 kPa or less. If the reaction pressure is below the lower limit of the above range, the amount of flying material in the reaction vessel increases, the haze of the reaction product increases, and this is likely to cause an increase in foreign matter. In addition, the diol component is likely to be distilled out of the reaction system, which is likely to result in a decrease in the polycondensation reaction rate. On the other hand, if the reaction pressure exceeds the upper limit of the above range, the dehydration decomposition of the diol component increases, which is likely to result in a decrease in the polycondensation rate.

[0053] The reaction time is not particularly limited, but is preferably 1 hour or more, and is preferably 10 hours or less, and more preferably 4 hours or less.

[0054] When the reaction step includes a polycondensation reaction treatment described below, it is preferable to subject an esterification reaction product having an esterification rate of 80% or more to the polycondensation reaction treatment. The polycondensation reaction generally refers to a high-molecular-weight reaction of polyester carried out at a reaction pressure of 50 kPa or less. The esterification reaction is generally carried out at 50 to 200 kPa and is preferably carried out in an esterification reaction tank, while the polycondensation reaction is generally carried out at 50 kPa or less, preferably 10 kPa or less, and is preferably carried out in a polycondensation reaction tank. In this specification, the esterification rate indicates the ratio of esterified dicarboxylic acid components to all dicarboxylic acid components in the polyester raw material, and is expressed by the following formula: Esterification rate (%) = (saponification value - acid value) / saponification value x 100

[0055] By continuously subjecting the reaction product obtained in the esterification reaction treatment to the polycondensation reaction described below, a high-quality polyester resin with low haze and little foreign matter can be efficiently obtained.

[0056] (Polycondensation Reaction Treatment) Next, the reaction product obtained by the esterification reaction treatment is subjected to a polycondensation reaction, which can be carried out under reduced pressure using a plurality of continuous reaction vessels.

[0057] The reaction pressure in the polycondensation reaction tank (particularly the final polycondensation reaction tank) is not particularly limited, but is usually 0.01 kPa or more, preferably 0.03 kPa or more, and usually 1.4 kPa or less, preferably 0.4 kPa or less. If the pressure during the polycondensation reaction is too high, the polycondensation time becomes long, which leads to a decrease in molecular weight and coloration due to thermal decomposition of the polyester, and it tends to become difficult to produce a polyester exhibiting sufficient properties for practical use. On the other hand, a production method using ultra-high vacuum polycondensation equipment that sets the reaction pressure to less than 0.01 kPa is a preferred embodiment from the viewpoint of improving the polycondensation reaction rate, but requires extremely expensive capital investment, making it economically disadvantageous.

[0058] The reaction temperature is not particularly limited, but is usually 215°C or higher, preferably 220°C or higher, and usually 270°C or lower, preferably 260°C or lower. If the reaction temperature is below the lower limit of the above range, the polycondensation reaction rate is slow, and not only does it take a long time to produce a polyester with a high degree of polymerization, but it also requires a high-power stirrer, which is economically disadvantageous. On the other hand, if the reaction temperature exceeds the upper limit of the above range, thermal decomposition of the polyester resin during production tends to occur, making it difficult to produce a polyester with a high degree of polymerization.

[0059] The reaction time is not particularly limited, but is usually 1 hour or more and usually 15 hours or less, preferably 10 hours or less, and more preferably 8 hours. If the reaction time is too short, the reaction is insufficient, making it difficult to obtain a polyester with a high degree of polymerization, and the mechanical properties of the molded product tend to be poor. On the other hand, if the reaction time is too long, the molecular weight of the polyester resin decreases significantly due to thermal decomposition, and not only does the mechanical properties of the molded product tend to be poor, but the amount of carboxyl group terminals, which has an adverse effect on the durability of the polyester resin, may increase due to thermal decomposition.

[0060] By controlling the temperature, time and reaction pressure of the polycondensation reaction within the above ranges, a polyester resin having a desired intrinsic viscosity can be obtained.

[0061] (Reaction catalyst) The esterification reaction and polycondensation reaction are accelerated by using a reaction catalyst. A sufficient reaction rate can be achieved in the esterification reaction even without an esterification catalyst. Furthermore, if an esterification catalyst is present during the esterification reaction, the water produced by the esterification reaction can cause the catalyst to form an insoluble precipitate in the reaction product, which can impair the transparency of the resulting polyester (i.e., increase haze) and can also cause the catalyst to become a foreign substance. Therefore, it is preferable not to add a reaction catalyst during the esterification reaction. Furthermore, adding a catalyst to the gas phase of the reaction vessel can increase the haze of the resulting polyester and can also cause the catalyst to become a foreign substance, so it is preferable to add the catalyst to the reaction liquid.

[0062] In polycondensation reactions, the reaction does not proceed easily without a catalyst, so it is preferable to use a catalyst. As a polycondensation reaction catalyst, a compound containing at least one metal element from Groups 1 to 14 of the periodic table is generally used. Specific examples of metal elements include scandium, yttrium, samarium, titanium, zirconium, vanadium, chromium, molybdenum, tungsten, tin, antimony, cerium, germanium, zinc, cobalt, manganese, iron, aluminum, magnesium, calcium, strontium, sodium, and potassium. Among these, scandium, yttrium, titanium, zirconium, vanadium, molybdenum, tungsten, zinc, iron, and germanium are preferred, and titanium, zirconium, tungsten, iron, and germanium are particularly preferred.

[0063] Furthermore, among the above metals, in order to reduce the polyester terminal concentration, which affects the thermal stability of the polyester, metal elements of Groups 3 to 6 of the periodic table that exhibit Lewis acidity are preferred, specifically scandium, titanium, zirconium, vanadium, molybdenum, or tungsten, with titanium and zirconium being particularly preferred from the viewpoint of availability, and titanium being even more preferred from the viewpoint of reactivity.

[0064] In the present embodiment, as the catalyst, a compound containing an organic group, such as a carboxylate, an alkoxy salt, an organic sulfonate, or a β-diketonate salt, containing the above-mentioned metal element; or an inorganic compound, such as an oxide or halide of the above-mentioned metal element, or a mixture thereof, is preferably used.

[0065] In this embodiment, the catalyst is preferably in a liquid state during polymerization or a compound that dissolves in the ester oligomer or polyester, because the polymerization rate increases when the catalyst is in a molten or dissolved state during polymerization. Furthermore, while polycondensation is preferably performed without a solvent, a small amount of solvent may be used separately to dissolve the catalyst. Examples of solvents for dissolving the catalyst include alcohols such as methanol, ethanol, isopropanol, or butanol; the aforementioned diols such as ethylene glycol, butanediol, or pentanediol; ethers such as diethyl ether or tetrahydrofuran; nitriles such as acetonitrile; hydrocarbon compounds such as heptane or toluene; water; and mixtures thereof. The amount of solvent used is typically such that the catalyst concentration in the polyester raw material is 0.0001% by mass or more and 99% by mass or less. To dissolve the catalyst, the catalyst can be diluted with a diol such as 1,4-butanediol or ethylene glycol. In this case, the diol can also function as a raw material for the polyester.

[0066] The titanium compound is preferably a tetraalkyl titanate or a hydrolyzate thereof, and specific examples thereof include tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, tetra-t-butyl titanate, tetraphenyl titanate, tetracyclohexyl titanate, tetrabenzyl titanate, mixed titanates thereof, and hydrolyzates thereof.

[0067] Furthermore, examples of titanium compounds that are preferably used include titanium (oxy)acetylacetonate, titanium tetraacetylacetonate, titanium (diisoproxide)acetylacetonate, titanium bis(ammonium lactate)dihydroxide, titanium bis(ethylacetoacetate)diisopropoxide, titanium (triethanolaminate)isopropoxide, polyhydroxytitanium stearate, titanium lactate, titanium triethanolaminate, and butyl titanate dimer.

[0068] Furthermore, as the titanium compound, a liquid obtained by mixing an alcohol, a Group 2 metal compound in the long periodic table (Nomenclature of Inorganic Chemistry IUPAC Recommendations 2005) (hereinafter, sometimes referred to as a Group 2 metal compound in the long periodic table), a phosphate ester compound, or a titanium compound may also be used.

[0069] Among these, tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, titanium (oxy)acetylacetonate, titanium tetraacetylacetonate, titanium bis(ammonium lactate) dihydroxide, polyhydroxytitanium stearate, titanium lactate, butyl titanate dimer, or a liquid obtained by mixing alcohols, a Group 2 metal compound in the long form periodic table, a phosphate ester compound, and / or a titanium compound are preferred, and tetra-n-butyl titanate, titanium (oxy)acetylacetonate, titanium tetraacetylacetonate, titanium bis(ammonium lactate) dihydroxide, polyhydroxytitanium stearate, titanium lactate, butyl titanate dimer, or a liquid obtained by mixing alcohols, a Group 2 metal compound in the long form periodic table, a phosphate ester compound, and / or a titanium compound are preferred. More preferred are cetyl acetonate, polyhydroxy titanium stearate, titanium lactate, butyl titanate dimer, or liquids obtained by mixing alcohols, a Group 2 metal compound in the long periodic table, a phosphate ester compound, and / or a titanium compound, and particularly preferred are tetra-n-butyl titanate, polyhydroxy titanium stearate, titanium (oxy)acetylacetonate, titanium tetraacetylacetonate, or liquids obtained by mixing alcohols, a Group 2 metal compound in the long periodic table, a phosphate ester compound, and / or a titanium compound.

[0070] Specific examples of zirconium compounds include zirconium tetraacetate, zirconium acetate hydroxide, zirconium tris(butoxy)stearate, zirconyl diacetate, zirconium oxalate, zirconyl oxalate, potassium zirconium oxalate, polyhydroxyzirconium stearate, zirconium ethoxide, zirconium tetra-n-propoxide, zirconium tetraisopropoxide, zirconium tetra-n-butoxide, zirconium tetra-t-butoxide, zirconium tributoxyacetylacetonate, and mixtures thereof.

[0071] Among these, zirconyl diacetate, zirconium tris(butoxy)stearate, zirconium tetraacetate, zirconium acetate hydroxide, ammonium zirconium oxalate, potassium zirconium oxalate, polyhydroxyzirconium stearate, zirconium tetra-n-propoxide, zirconium tetraisopropoxide, zirconium tetra-n-butoxide, and zirconium tetra-t-butoxide are preferred, and zirconyl diacetate, zirconium tetraacetate, zirconium acetate hydroxide, zirconium tris(butoxy)stearate, ammonium zirconium oxalate, zirconium tetra-n-propoxide, or zirconium tetra-n-butoxide is more preferred, with zirconium tris(butoxy)stearate being particularly preferred because a polyester with a high degree of polymerization and little coloration can be easily obtained.

[0072] Specific examples of germanium compounds include inorganic germanium compounds such as germanium oxide or germanium chloride, and organic germanium compounds such as tetraalkoxygermanium. In terms of cost and availability, germanium oxide, tetraethoxygermanium, tetrabutoxygermanium, and the like are preferred, with germanium oxide being particularly preferred.

[0073] Examples of iron compounds include inorganic chlorides such as ferric chloride, inorganic oxides such as triiron tetroxide, and organic iron complexes such as ferrocene, etc. Among these, inorganic oxides are preferred.

[0074] Examples of other metal-containing compounds include scandium compounds such as scandium carbonate, scandium acetate, scandium chloride, and scandium acetylacetonate; yttrium compounds such as yttrium carbonate, yttrium chloride, yttrium acetate, and yttrium acetylacetonate; vanadium compounds such as vanadium chloride, vanadium trichloride oxide, vanadium acetylacetonate, and vanadium acetylacetonate oxide; molybdenum compounds such as molybdenum chloride and molybdenum acetate; tungsten compounds such as tungsten chloride, tungsten acetate, and tungstic acid; and lanthanoid compounds such as cerium chloride, samarium chloride, and ytterbium chloride.

[0075] The amount of polycondensation catalyst added is not particularly limited, but the lower limit of the metal amount relative to the polyester produced is usually 0.1 mass ppm or more, preferably 0.5 mass ppm or more, and more preferably 1 mass ppm or more, and the upper limit is usually 3000 mass ppm or less, preferably 1000 mass ppm or less, more preferably 250 mass ppm or less, and particularly preferably 130 mass ppm or less. This range is particularly suitable when a metal compound is used as the polycondensation catalyst. Using too much catalyst is not only economically disadvantageous, but can also increase the carboxyl group terminal concentration of the polyester resin. This can lead to a decrease in the thermal stability and hydrolysis resistance of the polyester due to an increase in the amount of carboxyl group terminals and residual catalyst concentration. Conversely, if the amount is too small, the polymerization activity will be low, which can induce thermal decomposition of the polyester during polyester production, making it difficult to obtain a polyester exhibiting practically useful physical properties.

[0076] The position of the catalyst to be added to the reaction system is not particularly limited as long as it is added before the polycondensation reaction step, and it may be added when the raw materials are charged. However, if the catalyst is present in a situation where a large amount of water is present or generated, the catalyst may be deactivated, causing the precipitation of foreign matter and impairing the quality of the product. Therefore, it is preferable to add the catalyst after the esterification reaction step.

[0077] (Reaction Tank) As the esterification reaction tank for carrying out the esterification reaction treatment, known ones can be used, and they may be any of the types such as a vertical stirred complete mixing tank, a vertical thermal convection mixing tank, or a tower-type continuous reaction tank, and may be a single tank or a plurality of tanks of the same or different types connected in series. Among them, a reaction tank having a stirring device is preferred, and as the stirring device, in addition to a normal type having a power unit, bearings, a shaft, and stirring blades, high-speed rotating types such as a turbine stator type high-speed rotating stirrer, a disk mill type stirrer, or a rotor mill type stirrer can also be used.

[0078] There are no limitations on the mode of stirring, and in addition to the usual stirring method of directly stirring the reaction liquid in the reaction tank from the top, bottom, or side of the reaction tank, a method can also be used in which a portion of the reaction liquid is taken out of the reaction tank via piping or the like and stirred with a line mixer or the like to circulate the reaction liquid. The type of stirring blade can also be selected from known types, and specific examples include propeller blades, screw blades, turbine blades, fan turbine blades, disk turbine blades, Pfaudler blades, full zone blades, and Max Blend blades.

[0079] There are no particular limitations on the type of polycondensation reaction tank, and examples thereof include a vertical stirring polymerization tank, a horizontal stirring polymerization tank, a thin-film evaporation polymerization tank, etc. The polycondensation reaction tank may be a single tank, or a plurality of tanks of the same or different types connected in series, but in the later stage of polycondensation when the viscosity of the reaction liquid increases, it is preferable to select a horizontal stirring polymerization tank having a thin-film evaporation function that is excellent in interface renewal property, plug flow property, or self-cleaning property.

[0080] <Inorganic Filler> The biodegradable resin composition preferably further contains an inorganic filler. The inclusion of an inorganic filler not only increases the rigidity of the molded body, but also has the effect of acting as an antiblocking agent when formed into a film. Furthermore, the inclusion of an inorganic filler has the effect of accelerating the disintegration of the molded body in soil or seawater during disposal after use.

[0081] The inorganic filler may be fibrous, granular, plate-like, or needle-like depending on its shape, and particularly preferably granular or plate-like.The granular ones include mineral particles such as talc, zeolite, diatomaceous earth, kaolin, clay, silica, and quartz powder; metal carbonate particles such as calcium carbonate, magnesium carbonate, and heavy calcium carbonate; metal silicate particles such as calcium silicate, aluminum silicate, and magnesium silicate; metal oxide particles such as alumina, silica, zinc oxide, and titanium oxide; metal hydroxide particles such as aluminum hydroxide, calcium hydroxide, and magnesium hydroxide; metal sulfate particles such as barium sulfate and calcium sulfate; and carbon particles such as carbon black.Furthermore, the plate-like ones include mica.

[0082] Preferably, talc, calcium carbonate, silica, titanium oxide, barium sulfate, etc. can be used as the inorganic filler, and from the viewpoint of environmental friendliness after biodegradation, talc, calcium carbonate, and silica are more preferred, and calcium carbonate is particularly preferred.

[0083] The particle size of the inorganic filler used is not particularly limited, and may be, for example, 0.001 to 30 μm, 0.01 to 10 μm, 0.1 to 5 μm, or 0.1 to 3 μm.

[0084] Furthermore, when needle-shaped particles are used, the upper limit of the aspect ratio is usually 1000 or less, preferably 500 or less, and more preferably 100 or less, and the lower limit is usually 1 or more, preferably 10 or more, and more preferably 15 or more. If the aspect ratio is too small, expected physical properties such as rigidity and heat resistance tend not to be exhibited, while if it is too large, it tends to cause poor appearance and deteriorate the physical properties of the film. The aspect ratio here refers to the ratio of the major axis to the minor axis of the inorganic filler. The aspect ratio of the particles is the arithmetic average of the ratio of the longest axis to the shortest axis of at least 10 particles observed in a scanning electron microscope photograph with a field of view of 100 μm × 100 μm.

[0085] The volume-average particle size may be measured by any method, including measuring particles dispersed in a dispersion medium by a sedimentation method, laser scattering analysis, or laser Doppler method. In the present invention, the volume-average particle size is measured based on the sedimentation velocity of particles (Stokes' law) using a centrifugal sedimentation particle size distribution analyzer SA-CP4L manufactured by Shimadzu Corporation or an automatic particle size distribution analyzer RS-1000 manufactured by Shimadzu Corporation.

[0086] There is no particular limitation on the specific surface area of ​​the inorganic filler used, but if the specific surface area is too large, the rigidity tends not to be sufficiently improved, and if it is too small, the transparency tends to decrease. The specific surface area of ​​the inorganic filler used is usually 8000 cm 2 / g or more, preferably 10,000 cm 2 / g or more, while usually 50000cm 2 / g or less, preferably 40,000 cm 2 / g or less.

[0087] There is no particular limitation on the hardness of the inorganic filler used, but if the hardness is too low, physical properties such as rigidity and heat resistance tend to be reduced, while if the hardness is too high, it tends to cause poor appearance and a decrease in physical properties such as film strength. The upper limit of the hardness (Mohs hardness) of the filler used is usually 9 or less, preferably 8 or less, more preferably 7 or less, and the lower limit is usually 1 or more, preferably 2 or more, more preferably 3 or more. The Mohs hardness here refers to the value measured by rubbing a standard substance with a sample substance and determining whether or not scratches are left. The standard substances are as follows: Hardness 1: talc, Hardness 2: gypsum, Hardness 3: calcite, Hardness 4: fluorite, Hardness 5: apatite, Hardness 6: orthoclase, Hardness 7: quartz, Hardness 8: topaz, Hardness 9: corundum (corundum), Hardness 10: diamond

[0088] The inorganic filler may be surface-treated, which may improve the dispersibility of the inorganic filler, the fluidity of the resin composition, and the smoothness and opening properties of the resulting film. Furthermore, surface treatment is expected to reduce the amount of inorganic filler and additives such as plasticizers required for incorporation into the resin composition. Surface treatment of the inorganic filler can be carried out by commonly known methods, and the surface treatment method is not particularly limited. Examples of surface treatment agents include linear fatty acids and branched fatty acids having 6 to 40 carbon atoms, and ester compounds thereof.

[0089] These inorganic fillers may be used alone or in combination of two or more different types, which differ in material, physical properties, surface treatment or the like.

[0090] When the biodegradable resin composition contains an inorganic filler, the content of the inorganic filler in the biodegradable resin composition is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, and is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less. If the content of the inorganic filler is equal to or greater than the lower limit, the effect of the inorganic filler can be sufficiently obtained, and if it is equal to or less than the upper limit, deterioration of physical properties due to poor dispersion of the inorganic filler can be prevented.

[0091] [Calcium Carbonate] As described above, calcium carbonate is particularly preferably used as the inorganic filler. As the calcium carbonate, calcium carbonate containing zinc element or calcium carbonate not containing zinc element may be used.

[0092] The biodegradable resin composition preferably contains calcium carbonate containing elemental zinc. By adding calcium carbonate containing elemental zinc to the biodegradable resin composition, the carboxylic acid at the end of the polyester interacts with the zinc element, thereby suppressing intramolecular acid hydrolysis caused by the terminal carboxylic acid, and at the same time, the nucleating effect of the calcium carbonate promotes crystallization of the biodegradable resin, resulting in a biodegradable resin composition with excellent thermal stability and hydrolysis resistance.

[0093] The form of calcium carbonate is not particularly limited, and known calcium carbonates can be used, such as light calcium carbonate or heavy calcium carbonate. As described above, it is necessary for the biodegradable resin composition to contain a specific amount of zinc. To meet this requirement, it is preferable to use calcium carbonate containing zinc, for example, heavy calcium carbonate produced by physically crushing and classifying limestone and containing zinc. The presence or absence of zinc and its content in heavy calcium carbonate vary depending on the origin and quality of the raw limestone. Therefore, it is preferable to appropriately select heavy calcium carbonate made from limestone of a specific origin and quality. Note that heavy calcium carbonate containing zinc typically contains at least one element selected from the group consisting of magnesium, aluminum, iron, silicon, phosphorus, strontium, sulfur, barium, chromium, copper, potassium, manganese, and sodium in addition to zinc. Therefore, when heavy calcium carbonate containing zinc is used as calcium carbonate, the element will be contained in the polyester resin composition. On the other hand, precipitated calcium carbonate usually does not contain zinc element and the above elements.

[0094] When calcium carbonate is used as the inorganic filler, the content of calcium carbonate in the biodegradable resin composition is not particularly limited, but is usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, and is usually 70% by mass or less, preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 25% by mass or less. If the content is equal to or greater than the lower limit of the above range, a resin composition having excellent thermal stability and hydrolysis resistance can be obtained. On the other hand, if the content is equal to or less than the upper limit of the above range, a resin composition having excellent moldability and mechanical properties can be obtained.

[0095] When calcium carbonate containing zinc is used as the calcium carbonate, the zinc content in the calcium carbonate is not particularly limited, but is preferably 0.01 ppm by mass or more, more preferably 0.1 ppm by mass or more, and particularly preferably 1 ppm by mass or more, and is preferably 10,000 ppm by mass or less, more preferably 500 ppm by mass or less, even more preferably 100 ppm by mass or less, and particularly preferably 50 ppm by mass or less. When the content is equal to or greater than the lower limit of the above range, the resin composition has excellent thermal stability and hydrolysis resistance. When the content is equal to or less than the upper limit of the above range, discoloration and promotion of hydrolysis of the polyester due to the Lewis acidity of zinc are unlikely to occur.

[0096] [Other Components] The biodegradable resin composition may contain components other than the biodegradable resin (A), zinc element, and inorganic filler described above, such as polyesters other than the biodegradable resin (A), resins other than polyesters, carbodiimide compounds, fillers other than inorganic fillers, or plasticizers. In particular, when a resin other than the biodegradable resin (A) is contained, it is preferable to use a biodegradable resin as the resin. For example, polycaprolactone, polyamide, polyvinyl alcohol, cellulose ester, etc., or fine powders of animal or plant substances such as starch, cellulose, paper, wood flour, chitin / chitosan, coconut shell powder, and walnut shell powder, or mixtures thereof, may be blended. Furthermore, additives such as heat stabilizers, plasticizers, lubricants, antiblocking agents, nucleating agents, colorants, pigments, UV absorbers, or light stabilizers, modifiers, or crosslinking agents may be added to adjust the physical properties and processability of the molded body.

[0097] <Characteristics of Biodegradable Resin Composition> [Melt Flow Rate (MFR)] The melt flow rate (MFR) of the biodegradable resin composition is preferably 0.5 to 30 g / 10 min, as measured at 190°C under a load of 2.16 kg according to JIS K7210 (2014). For film applications and extrusion molding applications, it is more preferably 1.0 to 10 g / 10 min, and even more preferably 2.0 to 6.0 g / 10 min. If the MFR is above the lower limit, the fluidity required for molding is obtained, and if it is below the upper limit, the resin will have excellent bubble stability during film molding. On the other hand, for injection molding and fiber applications, it is more preferably 3.0 to 30 g / 10 min, and even more preferably 5.0 to 30 g / 10 min. If the MFR is above the lower limit, the fluidity required for molding is obtained, and if it is below the upper limit, the resin will have excellent mechanical properties, such as the impact strength of injection-molded products.

[0098] <Method for Producing Biodegradable Resin Composition> Known methods can be used to produce a biodegradable resin composition. For example, the method for producing a biodegradable resin composition includes a mixing step of mixing a biodegradable resin (A) with elemental zinc or a component containing zinc (such as a zinc salt or calcium carbonate powder containing zinc). Examples of such a method include melt-mixing the biodegradable resin (A) and the elemental zinc or the component containing zinc all at once in an extruder, or feeding each of these components into a kneader from separate feeders and mixing them. When a zinc salt is used as the component containing zinc, the zinc salt may be added as a powder, or may be added after being dispersed or dissolved in water, a solvent, oil, or the like. Alternatively, the zinc salt and the biodegradable resin (A) may be kneaded in an extruder in advance so that the zinc salt is 10 ppm by mass to 30% by mass, and the resulting mixture may be diluted with the biodegradable resin (A) as a masterbatch and kneaded to adjust the zinc concentration. Furthermore, when using calcium carbonate powder containing zinc as the zinc-containing component, it is possible to adjust the calcium carbonate concentration and zinc concentration in the resin composition by first preparing the biodegradable resin (A) and calcium carbonate containing zinc to a high-concentration calcium carbonate masterbatch of 50% by mass or more, and then diluting and kneading the resulting mixture with the biodegradable resin (A). A single-screw or twin-screw extruder can be used as the extruder. The resin kneaded in the twin-screw extruder can be pelletized using a pelletizer or underwater cutter, and the pellets can be used in various subsequent molding processes. It is also possible to directly feed pellets of the biodegradable resin (A), zinc alone or a component containing zinc, and other raw material pellets into a molding machine to prepare a resin composition and simultaneously produce a molded product such as a film.

[0099] <Molded Article> A molded article according to another embodiment of the present invention is a molded article of the biodegradable resin composition described above. The method for producing the molded article is not particularly limited, and the molded article can be obtained by molding using a known polyester molding method. The molding method is not particularly limited, and known methods such as compression molding, lamination molding, injection molding, extrusion molding, vacuum molding, pressure molding, blow molding, inflation molding, and stretch molding can be used. More specifically, for example, a method can be used in which a film-like, sheet-like, or cylindrical article extruded to a predetermined thickness from a T-die, I-die, or round die is cooled and solidified using a cooling roll, water, compressed air, or the like.

[0100] The uses of the molded articles are not limited, and specific examples include food films, trays for fresh food and fast food containers, outdoor leisure products, fishing lines, fishing nets, vegetation nets, water-retaining sheets, coating materials, agricultural mulch films, fertilizer coating materials, seedling beds, flower pots, etc., striped tape, split yarns, composite fibers, shopping bags, zippers, shrink films, fruit and vegetable bags, shopping bags, garbage bags, compost bags, cosmetic containers, detergent containers, bleach containers, ropes, binding materials, surgical sutures, sanitary cover stock materials, cooler boxes, cushioning materials, and synthetic paper.

[0101] Specific embodiments of the present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as the gist of the invention is not exceeded. Note that the values ​​of various production conditions and evaluation results in the following examples represent preferred upper or lower limit values ​​in the embodiments of the present invention, and preferred ranges may be defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​in the following examples or values ​​between the examples.

[0102] <Production Example 1: Production of Biodegradable Resin (A-1)> [Preparation of Polycondensation Catalyst] 343.5 parts by mass of magnesium acetate tetrahydrate was placed in a reactor equipped with a stirrer, and 1,434 parts by mass of absolute ethanol (purity 99% by mass or higher) was added. 218.3 parts by mass of ethyl acid phosphate (monoester and diester mixed in a weight ratio of 45:55) was then added, and the mixture was stirred at 23°C. After confirming that the magnesium acetate had completely dissolved, 410.0 parts by mass of tetra-n-butyl titanate was added. Stirring was continued for an additional 10 minutes, yielding a homogeneous mixed solution. This mixed solution was concentrated under reduced pressure while maintaining a temperature of 60°C or less. Approximately half of the ethanol added was distilled off, leaving a translucent, viscous liquid. 1,108 parts by mass of 1,4-butanediol was added, and the mixture was further concentrated under reduced pressure while maintaining a temperature of 80°C or less, yielding a catalyst solution with a titanium atom content of 3.5% by mass.

[0103] [Polymerization of biodegradable resin (A-1)] A reaction vessel equipped with a stirrer, nitrogen inlet, heater, thermometer, and pressure reducing port was charged with 33.6 parts by mass of succinic acid, 38.6 parts by mass of terephthalic acid, 69.7 parts by mass of 1,4-butanediol (Dairen Chemical Co., petrochemicals), 0.138 parts by mass of trimethylolpropane (0.200 mol% relative to 100 mol% of the total of succinic acid and terephthalic acid), 0.10 parts by mass of polyethylene wax (Honeywell "ACumist B6", melting point: 124 ° C.), and 0.0017 parts by mass of sodium hydroxide (NaOH), and further added tetra-n-butyl titanate so that the titanium atom content was 30 ppm by mass per polyester resin obtained. While stirring the contents of the vessel, nitrogen gas was introduced into the vessel, and the system was placed under a nitrogen atmosphere by vacuum substitution. Next, the temperature in the system was raised from 160°C to 230°C over 1 hour while stirring, and the reaction was carried out at this temperature for 3 hours. The terminal acid value of the obtained ester oligomer was measured and found to be 90 equivalents / ton. To this ester oligomer, the catalyst solution was added in an amount that resulted in 70 ppm by mass of titanium atoms per the obtained polyester resin, and the temperature was raised to 250°C over 45 minutes. At the same time, 0.07 x 10 3The pressure was reduced to 0.02 Pa or less, and polycondensation was continued while maintaining the heated and reduced pressure state. When a predetermined viscosity was reached, the polymerization was terminated to obtain a polyester copolymer (biodegradable resin (A-1)).

[0104] The melting point, crystallization temperature, and glass transition temperature of the produced biodegradable resin (A-1) were measured using a differential scanning calorimeter (Seiko Corporation, product name: DSC220). Specifically, approximately 5 mg of sample was precisely weighed, heated and melted under a nitrogen gas flow at a flow rate of 40 mL / min, and then the exothermic peak temperature of crystallization when cooled at a rate of 10 ° C. / min was taken as Tc. The temperature at which the baseline shifted when the temperature was subsequently increased at a rate of 10 ° C. / min was taken as the glass transition temperature. The endothermic peak temperature of crystalline melting observed when the temperature was subsequently increased at a rate of 10 ° C. / min was taken as the melting point. The biodegradable resin (A-1) measured as described above had a melting point of 110 ° C., a glass transition temperature of -20 ° C., and a crystallization peak temperature (Tc (A)) of 60 ° C.

[0105] The weight average molecular weight (Mw) of the biodegradable resin (A-1) measured by gel permeation chromatography (GPC) using monodisperse polystyrene as a standard substance was 117,000, and the MFR measured at 190°C and a load of 2.16 kg using a melt indexer according to JIS K7210 (2014) was 4.5 g / 10 min. The mole fraction of each constituent unit was measured using a Bruker NMR "AVANCE 400". 1 H-NMR was measured and the ratio of the integral values ​​of the chemical shifts corresponding to each structural unit was determined. The ratio of succinic acid units to terephthalic acid units in biodegradable resin (A-1) was confirmed to be 55:45 from the integral ratio of 2.63 ppm and 8.10 ppm. The biocontent of biodegradable resin (A-1) was 22%.

[0106] <Production Example 2: Production of Biodegradable Resin (A-2)> Production was carried out in the same manner as in Production Example 1, except that 1,4-butanediol (manufactured by Novamont, a plant-derived raw material) was used instead of 1,4-butanediol (manufactured by Dairen Chemical, a petrochemical product). The produced biodegradable resin (A-2) had a melting point of 110°C, a glass transition temperature of -20°C, and a crystallization peak temperature (Tc(A)) of 60°C. The weight-average molecular weight (Mw) was 117,000, and the MFR was 4.5 g / 10 min. The ratio of succinic acid units to terephthalic acid units was confirmed to be 55:45 from the integral ratio of 2.63 ppm and 8.10 ppm. The biodegradable resin (A-2) had a biodegradability of 63%.

[0107] <Other Materials> Biodegradable resin (A-3): Polybutylene adipate terephthalate, trade name: Ecoflex (registered trademark) (manufactured by BASF, melting point: 120°C, Tc(B): 41°C, MFR: 3.5g / 10min, Mw: 125,000, molar ratio of adipic acid units to terephthalic acid units = 53:47, bio content 0%) Biodegradable resin (A-4): Polybutylene succinate: trade name: BioPBS (registered trademark), model: FZ91PM (manufactured by PTTMCC, melting point: 115°C, MFR 4.5g / 10min, Mw = 160,000, bio content 50%) Biodegradable resin (A-5): Polybutylene succinate adipate: trade name: BioPBS (registered trademark) Model: FD92PB (manufactured by PTTMCC, melting point: 86°C, MFR 4.5g / 10min, Mw=160,000, bio content 35%) Zinc acetate dihydrate (Fujifilm Wako Pure Chemical Industries, purity 99.9%) Light calcium carbonate (zinc content 0.0 ppm, average particle size 2.0 μm) Heavy calcium carbonate (1) (zinc content 4.0 ppm, average particle size 1.8 μm) Heavy calcium carbonate (2) (zinc content 4.0 ppm, average particle size 1.0 μm) Heavy calcium carbonate (3) (zinc content 3.0 ppm, average particle size 1.0 μm) Heavy calcium carbonate (4) (zinc content 1.0 ppm, average particle size 2.0 μm)

[0108] <Measurement of zinc content in calcium carbonate> The zinc content in calcium carbonate was measured by weighing calcium carbonate, dissolving it with nitric acid, and then adjusting the volume with pure water, using an ICP spectrometry device (Agilent 5800) by the standard addition method. It was also confirmed that each of the heavy calcium carbonates (1) to (4) contained at least one element selected from the group consisting of magnesium, aluminum, iron, silicon, phosphorus, strontium, sulfur, barium, chromium, copper, potassium, manganese, and sodium.

[0109] <Measurement of Zinc Element Content in Resin Composition> The zinc element content in the resin composition was measured by the standard addition method using an ICP light emitting device (Agilent 5800 manufactured by Agilent), similar to the zinc element content in calcium carbonate.

[0110] <Evaluation of Thermal Stability of Biodegradable Resin Composition (Heat Retention Test)> For the pellets of the biodegradable resin composition obtained in the Examples and Comparative Examples, conditions optimized for JIS K7210 (2014) were used. That is, when measuring using a melt indexer at 190°C and a load of 2.16 kg, the MFR was measured for both a case where the preheating time was 5 minutes and a case where the preheating time was 6 minutes, and the rate of change was calculated.

[0111] Evaluation of hydrolytic stability of biodegradable resin compositions (hydrolysis test) Pellets of the biodegradable resin compositions obtained in the examples and comparative examples were allowed to stand at 60°C and 70% RH for 72 hours, and their MFR was measured using a melt indexer at 190°C, a load of 2.16 kg, and a preheating time of 5 minutes. The results were compared with the MFR measured by the above-mentioned method with a preheating time of 5 minutes, and the rate of change was calculated.

[0112] Example 1 100% by mass of the biodegradable resin (A-1) described in Production Example 1 was dry-blended with 0.0337 parts by mass of zinc acetate dihydrate and 0.05 parts by mass of Irganox 1010, and the mixture was kneaded at 150°C in a twin-screw extruder. The extruded strand was water-cooled and then cut to obtain pellets of the resin composition. The resulting pellets were evaluated for thermal stability using the method described above. The MFR after 5 minutes of preheating was 5.8 g / 10 min, and the MFR after 6 minutes of preheating was 5.8 g / 10 min. The calculated rate of change was 0%. Furthermore, hydrolytic stability was evaluated using the method described above. After standing for 72 hours at 60°C and 70% RH, the MFR was 7.5 g / 10 min, and the rate of change was 29.3%.

[0113] Example 2 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 0.0000336 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 5.9 g / 10 min, and the MFR after 6 minutes of preheating was 6.0 g / 10 min. The calculated rate of change was 1.7%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 7.2 g / 10 min, and the rate of change was 22.0%.

[0114] Example 3 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 0.00017 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 5.8 g / 10 min, and the MFR after 6 minutes of preheating was 5.9 g / 10 min. The calculated rate of change was 1.7%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 7.1 g / 10 min, a rate of change of 22.4%.

[0115] Example 4 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 0.00168 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 7.0 g / 10 min, and the MFR after 6 minutes of preheating was 7.1 g / 10 min. The calculated rate of change was 1.4%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 8.9 g / 10 min, a rate of change of 27.1%.

[0116] Example 5 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 0.3367 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 7.2 g / 10 min, and the MFR after 6 minutes of preheating was 7.3 g / 10 min. The calculated rate of change was 1.4%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 8.8 g / 10 min, and the rate of change was 22.2%.

[0117] Example 6 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 1.6835 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 9.9 g / 10 min, and the MFR after 6 minutes of preheating was 10.1 g / 10 min. The calculated rate of change was 2.0%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 12.8 g / 10 min, a rate of change of 29.3%.

[0118] Example 7 A resin composition was obtained in the same manner as in Example 1, except that the biodegradable resin (A-2) produced in Production Example 2 was used instead of the biodegradable resin (A-1) in Example 1, and zinc acetate dihydrate was used in an amount of 0.0168 parts by mass. The resin composition was then evaluated in the same manner. The MFR after 5 minutes of preheating was 5.7 g / 10 min, and the MFR after 6 minutes of preheating was 5.8 g / 10 min. The calculated rate of change was 1.8%. Furthermore, the MFR after standing for 72 hours at 60°C and 70% RH was 7.1 g / 10 min, a rate of change of 24.6%.

[0119] Example 8 A resin composition was obtained in the same manner as in Example 7, except that biodegradable resin (A-4): BioPBS FZ91PM was used instead of biodegradable resin (A-2) in Example 7. The same evaluation was carried out on this resin composition. The MFR after 5 minutes of preheating was 5.1 g / 10 min, and the MFR after 6 minutes of preheating was 5.1 g / 10 min. The calculated rate of change was 0%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 6.4 g / 10 min, and the rate of change was 25.5%.

[0120] Example 9 A resin composition was obtained in the same manner as in Example 7, except that biodegradable resin (A-5): BioPBS FD92PM was used instead of biodegradable resin (A-2). The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 4.9 g / 10 min, and the MFR after 6 minutes of preheating was 5.0 g / 10 min. The calculated rate of change was 2.0%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 6.2 g / 10 min, and the rate of change was 26.5%.

[0121] Example 10: 90% by mass of the biodegradable resin (A) described in Production Example 1, 0.0168 parts by mass of zinc acetate dihydrate, and 0.05 parts by mass of Irganox 1010 were dry-blended and then fed into a twin-screw extruder using a feeder. 10% by mass of precipitated calcium carbonate was also fed into the same twin-screw extruder using a separate feeder and kneaded at 150°C. The extruded strands were water-cooled and then cut to obtain pellets of the resin composition. The thermal stability of the resulting pellets was evaluated using the method described above. The MFR after 5 minutes of preheating was 6.2 g / 10 min, and the MFR after 6 minutes of preheating was 6.2 g / 10 min. The calculated rate of change was 0%. Furthermore, hydrolytic stability was evaluated using the method described above. After standing for 72 hours at 60°C and 70% RH, the MFR was 7.6 g / 10 min, and the rate of change was 22.6%.

[0122] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that zinc acetate dihydrate was not added. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 7.2 g / 10 min, and the MFR after 6 minutes of preheating was 7.4 g / 10 min. The calculated rate of change was 2.8%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 9.5 g / 10 min, and the rate of change was 31.9%.

[0123] Comparative Example 2 A resin composition was obtained in the same manner as in Example 7, except that zinc acetate dihydrate was not added. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 5.7 g / 10 min, and the MFR after 6 minutes of preheating was 6.0 g / 10 min. The calculated rate of change was 5.3%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 8.0 g / 10 min, and the rate of change was 40.4%.

[0124] Comparative Example 3 A resin composition was obtained in the same manner as in Example 8, except that zinc acetate dihydrate was not added. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 4.9 g / 10 min, and the MFR after 6 minutes of preheating was 5.2 g / 10 min. The calculated rate of change was 6.1%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 6.4 g / 10 min, and the rate of change was 30.6%.

[0125] Comparative Example 4 A resin composition was obtained in the same manner as in Example 9, except that zinc acetate dihydrate was not added. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 5.0 g / 10 min, and the MFR after 6 minutes of preheating was 5.3 g / 10 min. The calculated rate of change was 6.0%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 6.7 g / 10 min, and the rate of change was 34.0%.

[0126] Comparative Example 5 A resin composition was obtained in the same manner as in Example 10, except that zinc acetate dihydrate was not added. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 6.4 g / 10 min, and the MFR after 6 minutes of preheating was 6.7 g / 10 min. The calculated rate of change was 4.7%. Furthermore, after standing at 60°C and 70% RH for 72 hours, the MFR was 8.8 g / 10 min, and the rate of change was 37.5%.

[0127] Comparative Example 6 A resin composition was obtained in the same manner as in Example 1, except that the amount of zinc acetate dihydrate was changed to 3.3670 parts by mass. The resin composition was evaluated in the same manner. The MFR after 5 minutes of preheating was 11.0 g / 10 min, and the MFR after 6 minutes of preheating was 11.5 g / 10 min. The calculated rate of change was 4.5%. Furthermore, the MFR after standing for 72 hours at 60°C and 70% RH was 16.0 g / 10 min, and the rate of change was 45.5%.

[0128]

[0129] As is clear from Table 1, when the resin composition contains a biodegradable resin (A) and zinc element and the zinc content is 5,000 ppm or less, the resin composition is specifically excellent in thermal stability and hydrolytic stability. On the other hand, when the zinc content exceeds 10,000 ppm, both the thermal stability and hydrolytic stability decrease.

[0130] Example 11: 80% by mass of the biodegradable resin (A-1) described in Production Example 1, 20% by mass of calcium bicarbonate powder (1) containing 4 ppm of zinc element, and 0.05 parts by mass of Irganox 1010 were dry-blended and kneaded in a twin-screw extruder at 150°C. The extruded strands were water-cooled and then cut to obtain pellets of the resin composition. The content of aliphatic dicarboxylic acid units was 27.5 mol% and the content of aromatic dicarboxylic acid units was 22.5 mol% relative to 100 mol% of all structural units constituting the biodegradable resin (A). The heat resistance of the resulting pellets was evaluated according to the method described above. The MFR after 5 minutes of preheating was 3.2 g / 10 min, and the MFR after 6 minutes of preheating was 3.2 g / 10 min. The calculated rate of change was 0%. Furthermore, hydrolysis was evaluated according to the method described above. After standing at 60° C. and 70% RH for 72 hours, the MFR was 4.0 g / 10 min, and the rate of change was 25%.

[0131] Example 12 A resin composition was produced in the same manner as in Example 11, except that the biodegradable resin (A-2) produced in Production Example 2 was used instead of the biodegradable resin (A-1) in Example 11, and the same evaluations were performed. The content of aliphatic dicarboxylic acid units was 27.5 mol%, and the content of aromatic dicarboxylic acid units was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.4 g / 10 min, and the MFR after 6 minutes of preheating was 3.4 g / 10 min. The calculated rate of change was 0%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 4.3 g / 10 min, and the rate of change was 26.5%.

[0132] Example 13: A resin composition was produced in the same manner as in Example 11, except that 91% by mass of biodegradable resin (A-3): polybutylene adipate terephthalate, trade name: Ecoflex (registered trademark), was used instead of the biodegradable resin (A-1) in Example 11, and 9% by mass of calcium bicarbonate powder (1) containing 4.0 ppm of zinc element was used. Based on 100 mol% of all structural units constituting the biodegradable resin (A), the content of aliphatic dicarboxylic acid units was 26.5 mol%, and the content of aromatic dicarboxylic acid units was 23.5 mol%. The MFR after 5 minutes of preheating was 3.6 g / 10 min, and the MFR after 6 minutes of preheating was 3.7 g / 10 min. The calculated rate of change was 2.8. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 4.5 g / 10 min, and the rate of change was 25%.

[0133] Example 14: In Example 11, biodegradable resin (A-1) was replaced with 95% by mass of biodegradable resin (A-4): polybutylene succinate: product name: BioPBS (registered trademark) model: FZ91PM. A resin composition was produced in the same manner as in Example 11, except that 5% by mass of calcium bicarbonate powder (1) containing 4.0 ppm of zinc was used. The aliphatic dicarboxylic acid unit content was 25 mol% relative to 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 4.2 g / 10 min, and the MFR after 6 minutes of preheating was 4.3 g / 10 min. The calculated rate of change was 2.4%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 5.2 g / 10 min, and the rate of change was 23.8%.

[0134] Example 15: In Example 11, 70% by mass of biodegradable resin (A-5): polybutylene succinate adipate (trade name: BioPBS (registered trademark), model: FD92PB) was used instead of the biodegradable resin (A-1), and 30% by mass of calcium bicarbonate powder (1) containing 4.0 ppm of zinc was used. A resin composition was produced in the same manner as in Example 11, and similar evaluations were performed. The content of aliphatic dicarboxylic acid units was 25 mol% relative to 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 2.2 g / 10 min, and the MFR after 6 minutes of preheating was 2.2 g / 10 min. The calculated rate of change was 0%. Furthermore, after standing for 72 hours at 60 °C and 70% RH, the MFR was 2.8 g / 10 min, and the rate of change was 27.3%.

[0135] Example 16 A resin composition was produced in the same manner as in Example 12, except that calcium bicarbonate powder (2) containing 4.0 ppm of zinc and having a particle size of 1.0 micrometers was used instead of calcium bicarbonate powder (1) in Example 12, and similar evaluations were performed. The aliphatic dicarboxylic acid unit content was 27.5 mol% and the aromatic dicarboxylic acid unit content was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.2 g / 10 min, and the MFR after 6 minutes of preheating was 3.2 g / 10 min. The calculated rate of change was 0%. Furthermore, the MFR after standing at 60°C and 70% RH for 72 hours was 4.1 g / 10 min, a rate of change of 28.1%.

[0136] Example 17 A resin composition was produced in the same manner as in Example 12, except that calcium bicarbonate powder (3) containing 3.0 ppm of zinc was used instead of calcium bicarbonate powder (1) in Example 12, and similar evaluations were performed. The aliphatic dicarboxylic acid unit content was 27.5 mol% and the aromatic dicarboxylic acid unit content was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.0 g / 10 min, and the MFR after 6 minutes of preheating was 3.0 g / 10 min. The calculated rate of change was 0%. Furthermore, the MFR after standing for 72 hours at 60°C and 70% RH was 3.8 g / 10 min, a rate of change of 26.7%.

[0137] Example 18 A resin composition was produced in the same manner as in Example 12, except that calcium bicarbonate powder (4) containing 1.0 ppm of zinc was used instead of calcium bicarbonate powder (1) in Example 12, and similar evaluations were performed. The aliphatic dicarboxylic acid unit content was 27.5 mol% and the aromatic dicarboxylic acid unit content was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 2.8 g / 10 min, and the MFR after 6 minutes of preheating was 2.8 g / 10 min. The calculated rate of change was 0%. Furthermore, the MFR after standing for 72 hours at 60°C and 70% RH was 3.5 g / 10 min, a rate of change of 25.0%.

[0138] Comparative Example 7 A resin composition was produced in the same manner as in Example 11, except that precipitated calcium carbonate powder was used, and the same evaluations were performed. The content of aliphatic dicarboxylic acid units was 27.5 mol%, and the content of aromatic dicarboxylic acid units was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.3 g / 10 min, and the MFR after 6 minutes of preheating was 3.5 g / 10 min. The calculated rate of change was 6.1%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 4.5 g / 10 min, and the rate of change was 36.4%.

[0139] Comparative Example 8 A resin composition was produced in the same manner as in Example 12, except that precipitated calcium carbonate powder was used, and the same evaluations were performed. The content of aliphatic dicarboxylic acid units was 27.5 mol%, and the content of aromatic dicarboxylic acid units was 22.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.5 g / 10 min, and the MFR after 6 minutes of preheating was 3.8 g / 10 min. The calculated rate of change was 8.6%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 4.6 g / 10 min, and the rate of change was 31.4%.

[0140] Comparative Example 9 A resin composition was produced in the same manner as in Example 13, except that precipitated calcium carbonate powder was used, and the same evaluations were performed. The content of aliphatic dicarboxylic acid units was 26.5 mol%, and the content of aromatic dicarboxylic acid units was 23.5 mol%, based on 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 3.6 g / 10 min, and the MFR after 6 minutes of preheating was 3.8 g / 10 min. The calculated rate of change was 5.6%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 4.9 g / 10 min, and the rate of change was 36.1%.

[0141] Comparative Example 10: A resin composition was produced in the same manner as in Example 14, except that precipitated calcium carbonate powder was used, and the same evaluations were carried out. The content of aliphatic dicarboxylic acid units was 25 mol% relative to 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 4.4 g / 10 min, and the MFR after 6 minutes of preheating was 4.7 g / 10 min. The calculated rate of change was 6.8%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 6.0 g / 10 min, and the rate of change was 36.4%.

[0142] Comparative Example 11 A resin composition was produced in the same manner as in Example 15, except that precipitated calcium carbonate powder was used, and the same evaluations were carried out. The content of aliphatic dicarboxylic acid units was 25 mol% relative to 100 mol% of all structural units constituting the biodegradable resin (A). The MFR after 5 minutes of preheating was 2.6 g / 10 min, and the MFR after 6 minutes of preheating was 2.9 g / 10 min. The calculated rate of change was 11.5%. Furthermore, after standing for 72 hours at 60°C and 70% RH, the MFR was 3.5 g / 10 min, and the rate of change was 34.6%.

[0143]

[0144] As is clear from Table 2, when the resin composition contains the biodegradable resin (A) and calcium carbonate, and the calcium carbonate contains zinc element, it is found that the resin composition has excellent thermal stability and hydrolysis stability.

[0145] The biodegradable resin composition according to this embodiment has excellent thermal stability when melted and excellent hydrolytic stability during use, and therefore can be suitably used in molding methods involving heating, such as for films, sheets, injection-molded products, blow-molded products, vacuum-molded products, extrusion-molded products, fibers, etc. Furthermore, because the resin composition of the present invention has high hydrolytic stability, it is possible to extend the shelf life of the resin raw material before processing and the shelf life of the processed product.

Claims

1. A biodegradable resin composition comprising a biodegradable resin (A) and zinc element, the zinc element content being 0.001 ppm by mass or more and 7000 ppm by mass or less, the biodegradable resin (A) comprising at least either (i) a polyester having as its main structural units a structural unit derived from an aliphatic diol and a structural unit derived from an aliphatic dicarboxylic acid, or (ii) a polyester having as its main structural units a structural unit derived from an aliphatic diol, a structural unit derived from an aliphatic dicarboxylic acid, and a structural unit derived from an aromatic dicarboxylic acid.

2. The biodegradable resin composition according to claim 1, wherein the structural unit derived from the aliphatic dicarboxylic acid has 2 to 30 carbon atoms.

3. The biodegradable resin composition according to claim 1, wherein the structural unit derived from the aromatic dicarboxylic acid has 6 to 12 carbon atoms.

4. The biodegradable resin composition according to claim 1, wherein the structural unit derived from the aliphatic diol has 2 to 30 carbon atoms.

5. The biodegradable resin composition according to claim 1, wherein the structural unit derived from the aromatic dicarboxylic acid is terephthalic acid.

6. The biodegradable resin composition according to claim 1, wherein the structural unit derived from the aliphatic dicarboxylic acid is succinic acid.

7. A biodegradable resin composition according to claim 1, in which the content of structural units derived from aliphatic dicarboxylic acids is 40 mol% or more relative to the total of structural units derived from aliphatic dicarboxylic acids and structural units derived from aromatic dicarboxylic acids contained in all resins in the biodegradable resin composition.

8. The biodegradable resin composition according to claim 1, wherein the bio-content of the biodegradable resin (A) calculated based on ASTM D6866 is 20% or more.

9. The biodegradable resin composition according to claim 1, further comprising an inorganic filler.

10. The biodegradable resin composition according to claim 9, comprising calcium carbonate as the inorganic filler.

11. The biodegradable resin composition according to claim 10, wherein the calcium carbonate is ground calcium carbonate.

12. A molded article made using the biodegradable resin composition according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Biodegradable plastic composition, its molded article, and method for controlling biodegradation rate

    JP2003313436A

  • Biodegradable resin laminate and its manufacturing process

    JP2009051210A

  • Biodegradable resin film

    JP2014090704A

  • Resin composition and method for producing resin composition

    JP2023024333A

Cited By

  • Biodegradable polyester composition as well as preparation method and application thereof

    CN119955262A