Ceramic electronic component and method for manufacturing same
The ceramic electronic component's innovative electrode layer configuration and manufacturing method address cracking issues by controlling Cu diffusion and stress, enhancing mechanical strength and reliability in ceramic capacitors.
Patent Information
- Application Number
- PCT/JP2024/012713
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Ceramic electronic components face issues with mechanical strength and moisture resistance, particularly when internal electrodes containing low melting point metals like tin expand due to diffusion from external electrodes during baking, leading to cracking and damage.
A ceramic electronic component design with alternately stacked Ni-based internal electrode layers, where the first layer contains a higher concentration of low melting point metal and a narrower width connected to the external electrode, and the second layer has a wider width, reducing Cu diffusion and stress, along with a method involving lamination and specific electrode configurations to suppress cracking.
The design effectively suppresses cracking and enhances mechanical strength by controlling Cu diffusion and stress distribution, ensuring reliable performance and capacitance in multilayer ceramic capacitors.
Smart Images

Figure JP2024012713_03102024_PF_FP_ABST
Abstract
Description
Ceramic electronic component and manufacturing method thereof
[0001] The present invention relates to a ceramic electronic component and a method for manufacturing the same.
[0002] In recent years, the spread of electric vehicles has led to demand for improved reliability in the electronic components they are equipped with, such as improved mechanical strength and moisture resistance. In addition, to achieve even higher performance, the mounting area of ceramic electronic components on circuit boards is being limited, while increasing the number of laminated layers of ceramic electronic components is being demanded.
[0003] JP 2018-198292 A Republished 2014 / 175034 A
[0004] In order to improve the mechanical strength of ceramic electronic components, it has been proposed to dissolve tin in only one of the internal electrodes containing nickel, thereby changing the stress distribution inside the ceramic electronic component and improving its flexural strength (see, for example, Patent Document 1).
[0005] On the other hand, there is a problem that when the external electrode is baked, the internal electrode reacts with the external electrode, and copper, which is a metal component of the external electrode, diffuses to the nickel side of the internal electrode, causing the internal electrode to expand, which generates outward stress in the cover and side margin, which cannot withstand this stress and causes cracks (see, for example, Patent Document 2).
[0006] In particular, when an internal electrode containing a low-melting-point metal such as tin (melting point 231.97°C) is used, the diffusion of the external electrode components into the internal electrode is promoted when the external electrode is baked, making the occurrence of cracks such as those described above a greater problem.
[0007] The present invention has been made in view of the above-mentioned problems, and has an object to provide a ceramic electronic component that can suppress the occurrence of cracks, and a method for manufacturing the same.
[0008] A ceramic electronic component according to the present invention comprises: a laminated chip having a substantially rectangular parallelepiped shape in which first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni are alternately laminated with dielectric layers sandwiched therebetween, the laminated chip being formed so that the first internal electrode layers and the second internal electrode layers are alternately extended to first and second end faces opposing each other of the substantially rectangular parallelepiped shape; a first external electrode provided on the first end face, the contact layer in contact with the first end face being mainly composed of Cu; and a second external electrode provided on the second end face, the contact layer in contact with the second end face being mainly composed of Cu; At least the first internal electrode layer of the external electrode layer and the second internal electrode layer contains a low-melting point metal having a melting point lower than the melting point of Pb, the concentration of the low-melting point metal being higher in the first internal electrode layer than in the second internal electrode layer, the width of the portion of the first internal electrode layer that connects to the first external electrode in a direction perpendicular to the stacking direction is narrower than the width of the portion facing the second internal electrode layer, and the width of the portion of the second internal electrode layer that connects to the second external electrode in a direction perpendicular to the stacking direction is wider than the width of the portion of the first internal electrode layer that connects to the first external electrode.
[0009] In the ceramic electronic component, the low-melting-point metal may be Sn.
[0010] In the ceramic electronic component, the second internal electrode layers may contain a metal element other than the low-melting-point metal that forms a stable compound with hydrogen.
[0011] In the ceramic electronic component, the metal element that forms a stable compound with hydrogen may be at least one of Ag, Au, Ga, and Ge.
[0012] In the ceramic electronic component, a width in a direction perpendicular to the stacking direction of a portion of the second internal electrode layer that is connected to the second external electrode may be the same as a width of a portion of the second internal electrode layer that faces the first internal electrode layer.
[0013] In the ceramic electronic component, a width in a direction perpendicular to the stacking direction of a portion of the first internal electrode layer that is connected to the first external electrode may be 60% or more and 90% or less of a width of a portion that faces the second internal electrode layer.
[0014] In the ceramic electronic component, a third internal electrode layer connected to the first external electrode may be provided in a central portion in the stacking direction, and a width of a portion of the third internal electrode layer connected to the first external electrode in a direction perpendicular to the stacking direction may be the same as a width of a portion facing the second internal electrode layer.
[0015] In the ceramic electronic component, the number of the third internal electrode layers may be 5% to 40% of the internal electrode layers connected to the first external electrode.
[0016] In the ceramic electronic component, in the direction in which the first end face and the second end face face each other, a length of a portion of the first internal electrode layer that is connected to the first external electrode and is narrower than a width of a portion that faces the second internal electrode layer may be greater than or equal to 1 / 4 and less than or equal to 1 / 1 of the length of the first external electrode.
[0017] A method for manufacturing a ceramic electronic component according to the present invention includes: a first internal electrode layer mainly composed of Ni and a second internal electrode layer mainly composed of Ni, which are alternately stacked with a dielectric layer sandwiched therebetween, and which has a substantially rectangular parallelepiped shape; the first internal electrode layer and the second internal electrode layer are alternately extended to a first end face and a second end face opposing the substantially rectangular parallelepiped shape; at least the first internal electrode layer of the first and second internal electrode layers contains a low-melting-point metal having a melting point equal to or lower than the melting point of Pb; and the concentration of the low-melting-point metal is The method includes the steps of preparing a laminated chip in which the first internal electrode layer is higher than the second internal electrode layer, the width of the portion of the first internal electrode layer that is extended to the first end face in a direction perpendicular to the stacking direction is narrower than the width of the portion facing the second internal electrode layer, and the width of the portion of the second internal electrode layer that is extended to the second end face in a direction perpendicular to the stacking direction is wider than the width of the portion of the first internal electrode layer that is extended to the first end face, and firing external electrodes primarily composed of Cu to each of the first end face and the second end face.
[0018] According to the present invention, it is possible to provide a ceramic electronic component that can suppress the occurrence of cracks, and a method for manufacturing the same.
[0019] 1 is a partial cross-sectional perspective view of the multilayer ceramic capacitor according to the first embodiment. FIG. 1 is a cross-sectional view taken along line A-A in FIG. 1. FIG. 1 is a cross-sectional view taken along line B-B in FIG. 1. (a) is an enlarged cross-sectional view of the vicinity of a first external electrode, and (b) is an enlarged cross-sectional view of the vicinity of a second external electrode. FIG. 1 illustrates a crack. (a) is a plan view of a first internal electrode layer, and (b) is a plan view of a second internal electrode layer 12b. FIG. 1 illustrates the wraparound length of the external electrodes. FIG. 1 illustrates a flow of a manufacturing method of a multilayer ceramic capacitor. FIG. 1 illustrates a lamination step. (a) is a plan view of a first internal electrode layer, and (b) is a plan view of a third internal electrode layer. FIG. 1 illustrates a first end face of a laminated chip. FIG. 1 illustrates a lamination step.
[0020] Hereinafter, embodiments will be described with reference to the drawings.
[0021] First Embodiment FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to a first embodiment. FIG. 2 is a cross-sectional view taken along line A-A in FIG. 1 . FIG. 3 is a cross-sectional view taken along line B-B in FIG. 1 . As illustrated in FIGS. 1 to 3 , the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape. A first external electrode 20a and a second external electrode 20b are provided on two opposing end faces (a first end face and a second end face) of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The first external electrode 20a extends from the first end face to four adjacent faces. The second external electrode 20b extends from the second end face to four adjacent faces. However, the first external electrode 20a and the second external electrode 20b are spaced apart from each other.
[0022] 1 to 3, the L direction is the length direction of the laminated chip 10, the direction in which the two end faces of the laminated chip 10 face each other, and the direction in which the first external electrode 20a and the second external electrode 20b face each other. The W direction is the width direction of the internal electrode layers, and the direction in which the two side faces other than the two end faces of the laminated chip 10 face each other. The T direction is the stacking direction, and the direction in which the top face and bottom face of the laminated chip 10 face each other. The L direction, W direction, and T direction are perpendicular to each other.
[0023] The multilayer chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers are alternately stacked. The internal electrode layers include a plurality of first internal electrode layers 12a and a plurality of second internal electrode layers 12b. The first internal electrode layers 12a and the second internal electrode layers 12b are alternately stacked. The edges of the first internal electrode layers 12a extend to a first end surface of the multilayer chip 10 on which a first external electrode 20a is provided. The edges of the second internal electrode layers 12b extend to a second end surface of the multilayer chip 10 on which a second external electrode 20b is provided. As a result, the first internal electrode layers 12a and the second internal electrode layers 12b are alternately electrically connected to the first external electrode 20a and the second external electrode 20b. As a result, the multilayer ceramic capacitor 100 has a configuration in which capacitor units are stacked. In the laminate of the dielectric layers 11 and the internal electrode layers, the internal electrode layers are arranged as the outermost layers in the lamination direction, and the upper and lower surfaces of the laminate are covered with cover layers 13. The cover layers 13 are mainly composed of a ceramic material. For example, the cover layers 13 may have the same composition as or different from the dielectric layers 11.
[0024] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.
[0025] The dielectric layer 11 is, for example, a compound represented by the general formula ABO 3 The main phase is a ceramic material having a perovskite structure represented by the formula: 3-α For example, the ceramic material includes BaTiO 3 (barium titanate), CaZrO 3 (Calcium zirconate), CaTiO 3 (Calcium titanate), SrTiO 3(strontium titanate), MgTiO 3 (magnesium titanate), Ba that forms a perovskite structure 1-x-y Ca x Sr y Ti 1-z Zr z O 3 (0≦x≦1, 0≦y≦1, 0≦z≦1) and the like. 1-x-y Ca x Sr y Ti 1-z Zr z O 3 are barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. The thickness of the dielectric layer 11 is, for example, 0.3 μm or more and 3 μm or less.
[0026] The cover layer 13 may be, for example, a polymer having the general formula ABO 3 The main phase is a ceramic material having a perovskite structure represented by the formula: 3-α For example, the ceramic material includes BaTiO 3 (barium titanate), CaZrO 3 (Calcium zirconate), CaTiO 3 (Calcium titanate), SrTiO 3 (strontium titanate), MgTiO 3 (magnesium titanate), Ba that forms a perovskite structure 1-x-y Ca x Sr y Ti 1-z Zr z O 3 (0≦x≦1, 0≦y≦1, 0≦z≦1) and the like. 1-x-y Ca x Sr y Ti 1-z Zr z O 3Examples of the dielectric layer 11 include barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, and barium calcium titanate zirconate. The main component of the cover layer 13 may be the same as or different from that of the dielectric layer 11.
[0027] Additives may be added to the dielectric layer 11 and the cover layer 13. Examples of additives to the dielectric layer 11 and the cover layer 13 include oxides of magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), rare earth elements (yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), oxides containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or glasses containing Co, Ni, Li, B, Na, K, or Si.
[0028] The first internal electrode layer 12a and the second internal electrode layer 12b are mainly composed of Ni. For example, the first internal electrode layer 12a and the second internal electrode layer 12b contain 85 at% or more of Ni. The first internal electrode layer 12a and the second internal electrode layer 12b may contain ceramic particles or the like as a co-material. The thickness of the first internal electrode layer 12a and the second internal electrode layer 12b is, for example, 0.1 μm or more and 2 μm or less.
[0029] 2, the region where the first internal electrode layer 12a connected to the first external electrode 20a and the second internal electrode layer 12b connected to the second external electrode 20b face each other is a region where capacitance is generated in the multilayer ceramic capacitor 100. Therefore, this region where capacitance is generated is referred to as a capacitance portion 14. In other words, the capacitance portion 14 is a region where adjacent internal electrode layers connected to different external electrodes face each other.
[0030] The region where the first internal electrode layers 12a connected to the first external electrode 20a face each other in the stacking direction without the second internal electrode layer 12b connected to the second external electrode 20b intervening therebetween is referred to as the first end margin 15a. The region where the second internal electrode layers 12b connected to the second external electrode 20b face each other in the stacking direction without the first internal electrode layer 12a connected to the first external electrode 20a intervening therebetween is referred to as the second end margin 15b. Each end margin is a region where internal electrode layers connected to the same external electrode face each other in the stacking direction without the internal electrode layer connected to a different external electrode intervening therebetween. The first end margin 15a and the second end margin 15b are regions that do not generate electrical capacitance.
[0031] As illustrated in Figure 3, in the laminated chip 10, the side margin 16 is a region provided to cover the ends (ends in the W direction) of two side surfaces of the dielectric layer 11, the first internal electrode layer 12a, and the second internal electrode layer 12b. That is, in Figure 3, the side margin 16 is a region provided outside the capacitance section 14 in the W direction. In other words, the side margin 16 is an outer region adjacent to the capacitance section 14 when viewed from the stacking direction, and is an outer region adjacent to the capacitance section 14 on the side where the internal electrode layers are not drawn out. The side margin 16 is also a region that does not generate electrical capacitance.
[0032] Fig. 4(a) is an enlarged cross-sectional view of the vicinity of the first external electrode 20a. Hatching is omitted in Fig. 4(a). As illustrated in Fig. 4(a), the first external electrode 20a has a structure in which a plating layer 22a is provided on an underlayer 21a. The underlayer 21a functions as a contact layer that contacts the first end surface of the laminated chip 10. The underlayer 21a is mainly composed of copper (Cu). The underlayer 21a may also contain a glass component. The underlayer 21a contains 80 at% or more of Cu.
[0033] The plating layer 22a is primarily composed of a metal such as Ni, Cu, Al (aluminum), Zn (zinc), or Sn (tin), or an alloy of two or more of these metals. The plating layer 22a may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, in FIG. 4( a), the plating layer 22a has a structure in which a first plating layer 23a and a second plating layer 24a are formed in this order from the base layer 21a side. The first plating layer 23a is, for example, a Ni plating layer. The second plating layer 24a is, for example, a Sn plating layer.
[0034] 4(b) is an enlarged cross-sectional view of the vicinity of the second external electrode 20b. Hatching is omitted in FIG. 4(b). As illustrated in FIG. 4(b), the second external electrode 20b has a structure in which a plating layer 22b is provided on an underlayer 21b. The underlayer 21b functions as a contact layer that contacts the second end surface of the laminated chip 10. The underlayer 21b is mainly composed of Cu. The underlayer 21b may also contain a glass component. The underlayer 21a contains 80 at % or more of Cu.
[0035] The plating layer 22b is primarily composed of a metal such as Ni, Cu, Al, Zn, or Sn, or an alloy of two or more of these metals. The plating layer 22b may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 22b has a structure in which a first plating layer 23b and a second plating layer 24b are formed in this order from the base layer 21b side. The first plating layer 23b is, for example, a Ni plating layer. The second plating layer 24b is, for example, a Sn plating layer.
[0036] The base layer 21a and the base layer 21b may have the same composition or different compositions. The plating layer 22a and the plating layer 22b may have the same layered structure or different layered structures. For example, the number of layers of the plating layers may be different. The first plating layer 23a and the first plating layer 23b may have the same composition or different compositions. The second plating layer 24a and the second plating layer 24b may have the same composition or different compositions.
[0037] The first internal electrode layer 12a contains a low-melting-point metal in addition to the main component Ni. The low-melting-point metal is a metal having a melting point lower than that of lead (Pb (melting point: 327.5°C)). For example, it includes bismuth (Bi (melting point: 271.4°C)), Sn (melting point: 231.97°C), indium (In (melting point: 156.61°C)), etc. The second internal electrode layer 12b does not contain a low-melting-point metal. The second internal electrode layer 12b may contain a low-melting-point metal, but the concentration of the low-melting-point metal is lower in the second internal electrode layer 12b than in the first internal electrode layer 12a.
[0038] This configuration can change the stress distribution inside the multilayer ceramic capacitor 100, thereby improving mechanical strength such as flexural strength. For example, in the first internal electrode layer 12a, when the main component Ni is 100 at%, the low-melting-point metal is contained at 0.5 at% to 3 at% inclusive, 0.7 at% to 2 at% inclusive, or 1 at% to 1.5 at% inclusive. In the second internal electrode layer 12b, when the main component Ni is 100 at% inclusive, the low-melting-point metal is contained at 0.5 at% or less, 0.3 at% or less, or 0.1 at% or less.
[0039] When multiple types of low melting point metals are contained, the concentration of the low melting point metals means the atomic percentage of the total amount of all the low melting point metals when Ni is taken as 100 atomic percentage.
[0040] In the multilayer ceramic capacitor 100, when the first external electrode 20a and the second external electrode 20b are baked, a crack 40 as shown in Figure 5 may occur in the area where the cover layer and the side margin, which are covered by the external electrodes, overlap (the corner near the external electrodes).
[0041] This occurs based on the following mechanism: When the internal electrode layers react with the base layers 21a, 21b during baking of the base layers 21a, 21b, Cu, a metal component of the base layers 21a, 21b, diffuses toward the Ni side of the internal electrode layers, causing the internal electrode layers to expand. This expansion of the internal electrode layers generates outward stress in the cover layer 13 and the side margins 16, resulting in cracks. In particular, if the internal electrode layers contain a low-melting-point metal, the diffusion of the external electrode components toward the internal electrode side is promoted during baking of the external electrodes, making the occurrence of cracks 40 a greater problem.
[0042] The multilayer ceramic capacitor 100 according to this embodiment has a configuration that can suppress the occurrence of the cracks 40. Details will be described below.
[0043] FIG. 6( a) is a plan view of the first internal electrode layer 12a. As illustrated in FIG. 6( a), the first internal electrode layer 12a has a first region 121 (lead portion) connected to the first external electrode 20a in a region corresponding to the first end margin 15a and having a width W1, and a second region 122 in a region corresponding to the capacitance portion 14 and having a width W2. The second region 122 faces the second internal electrode layer 12b. The width W1 is smaller than the width W2. The widths W1 and W2 refer to the widths in the W direction, i.e., the widths in the direction perpendicular to the stacking direction. This configuration narrows the diffusion path of Cu when the first external electrode 20a is sintered. This suppresses Cu diffusion even if the first internal electrode layer 12a contains a low-melting-point metal. This suppresses the occurrence of cracks 40.
[0044] The first region 121 may have a shape such that its width narrows as it approaches the first external electrode 20 a. In this case, the width W1 refers to the width of the portion where the first region 121 is connected to the first external electrode 20 a.
[0045] 6(b) is a plan view of the second internal electrode layer 12b. As illustrated in FIG. 6(b), the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is wider than the width in the W direction of the first region 121. For example, the width in the W direction of the second internal electrode layer 12b is approximately constant at any point in the L direction. For example, the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is approximately equal to W2. This configuration ensures good contact between the second internal electrode layer 12b and the second external electrode 20b, ensuring the capacitance of the multilayer ceramic capacitor 100.
[0046] For example, if W1 / W2 is small, there is a risk of a decrease in capacity due to poor contact between the first external electrode 20a and the first internal electrode layer 12a. Therefore, it is preferable to set a lower limit for W1 / W2. In this embodiment, when W2 is 100%, W1 is preferably 60% or more, and more preferably 70% or more. On the other hand, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, W1 is preferably 90% or less, and more preferably 80% or less.
[0047] Furthermore, from the viewpoint of suppressing cracks 40 due to expansion of the first internal electrode layer 12a, the length in the L direction of the first region 121 is preferably ¼ or more, and more preferably ½ or more, of the wraparound length in the L direction of the first external electrode 20a (dimension e in FIG. 7 ). On the other hand, from the viewpoint of ensuring the intersection area between the first internal electrode layer 12a and the second internal electrode layer 12b, the length in the L direction of the first region 121 is preferably ½ or less, and more preferably ¾ or less of dimension e.
[0048] Next, a method for manufacturing the multilayer ceramic capacitor 100 according to the first embodiment will be described.
[0049] (Step of Preparing Raw Material Powder) First, a dielectric material is prepared for forming the dielectric layer 11. The A-site elements and B-site elements contained in the dielectric layer 11 are usually ABO 3 The dielectric layer 11 contains a sintered body of BaTiO particles.3 is a tetragonal compound with a perovskite structure and exhibits a high dielectric constant. 3 Generally, it can be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known for synthesizing the ceramic that is the main component of the dielectric layer 11, such as a solid-phase method, a sol-gel method, and a hydrothermal method. Any of these methods can be used in this embodiment.
[0050] To the obtained ceramic powder, a predetermined additive compound is added depending on the purpose. Examples of the additive compound include oxides of Mg, Mn, Mo, V, Cr, rare earth elements (Y, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Yb), oxides containing Co, Ni, Li, B, Na, K, or Si, and glasses containing Co, Ni, Li, B, Na, K, or Si. Of these, SiO is mainly used. 2 functions as a sintering aid.
[0051] For example, a ceramic material is prepared by wet-mixing a ceramic raw material powder with a compound containing an additive compound, followed by drying and pulverization. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. A dielectric material is obtained by the above process.
[0052] (Lamination Process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained raw material powder and wet mixed. Using the obtained slurry, a dielectric green sheet is coated on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film.
[0053] Next, the internal electrode pattern 52a is formed on the dielectric green sheet 51, which constitutes a first lamination unit. The internal electrode pattern 52a corresponds to the shape of the first internal electrode layer 12a. The width of the internal electrode pattern 52a is set to approximately match the width of the dielectric green sheet 51. A metal paste containing the metal component of the first internal electrode layer 12a is used for the internal electrode pattern 52a. The film formation method may be printing, sputtering, vapor deposition, etc. Furthermore, the internal electrode pattern 52 is formed on the dielectric green sheet 51, which constitutes a second lamination unit. The internal electrode pattern 52 corresponds to the shape of the second internal electrode layer 12b. The width of the internal electrode pattern 52 is set to approximately match the width of the dielectric green sheet 51. A metal paste containing the metal component of the second internal electrode layer 12b is used for the internal electrode pattern 52. The film formation method may be printing, sputtering, vapor deposition, etc.
[0054] Next, while peeling the dielectric green sheet 51 from the substrate, the first and second stacking units are alternately stacked as shown in FIG. 9 . Next, a predetermined number of cover sheets 53 (e.g., 2 to 10 layers) are stacked on top and bottom of the laminate obtained by stacking the first and second stacking units, and are thermocompression bonded. The cover sheets 53 can be formed by the same method as the dielectric green sheet 51. Next, a plurality of side margin sheets 54 are attached to each of both side surfaces of the laminate. The side margin sheets 54 can be formed by the same method as the dielectric green sheet 51.
[0055] (Firing step) After that, the oxygen partial pressure is 10 -5 ~10 -8 The mixture is fired in a reducing atmosphere at 1100 to 1300° C. for 10 minutes to 2 hours.
[0056] (Reoxidation treatment step) Then, N 2 A reoxidation treatment may be carried out in a gas atmosphere at 600° C. to 1000° C.
[0057] (Coating Step) Next, a metal paste that will become the underlayers 21a and 21b is coated on the first side surface of the laminate by a dipping method, etc. This metal paste contains a glass component such as glass frit.
[0058] (Baking Step) Next, the metal paste is baked at a temperature of about 700° C. to 900° C. to form the underlayers 21a and 21b.
[0059] (Plating Process) Thereafter, the base layers 21 a, 21 b may be coated with a metal such as Cu, Ni, or Sn by plating. For example, a first plating layer and a second plating layer are formed in this order on the base layers 21 a, 21 b. This completes the multilayer ceramic capacitor 100.
[0060] According to the manufacturing method of this embodiment, the diffusion path of Cu is narrowed when the first external electrode 20a is baked. As a result, even if the first internal electrode layer 12a contains a low-melting-point metal, Cu diffusion is suppressed. As a result, the occurrence of cracks 40 is suppressed. Meanwhile, the width in the W direction of the portion of the second internal electrode layer 12b that connects to the second external electrode 20b is wider than the width in the W direction of the first region 121. As a result, good contact is achieved between the second internal electrode layer 12b and the second external electrode 20b, and the capacitance of the multilayer ceramic capacitor 100 is ensured.
[0061] Second Embodiment In the first embodiment, all of the internal electrode layers connected to the first external electrode 20a include the first region 121, but some of the internal electrode layers may include the first region 121. The multilayer ceramic capacitor 100a according to the second embodiment has a configuration in which some of all of the internal electrode layers connected to the first external electrode 20a include the first region 121.
[0062] Of all the internal electrode layers connected to the first external electrode 20a, some are third internal electrode layers 12c. FIG. 10( a) is a plan view of the first internal electrode layer 12a. FIG. 10( b) is a plan view of the third internal electrode layer 12c. As illustrated in FIG. 10( b), the width in the W direction of the portion of the third internal electrode layer 12c connected to the first external electrode 20a is wider than the width in the W direction of the first region 121. For example, the width in the W direction of the third internal electrode layer 12c is approximately constant at any point in the L direction. For example, the width in the W direction of the portion of the third internal electrode layer 12c connected to the first external electrode 20a is approximately equal to W2. This configuration ensures good contact between the third internal electrode layer 12c and the first external electrode 20a, ensuring the capacitance of the multilayer ceramic capacitor 100.
[0063] FIG. 11 is a diagram illustrating a first end surface of the laminated chip 10. That is, FIG. 11 is a view of the end surface of the laminated chip 10 viewed through the first external electrode 20a in the multilayer ceramic capacitor 100a. As illustrated in FIG. 11, one or more third internal electrode layers 12c are provided in the center of the stacking direction without the first internal electrode layers 12a interposed therebetween. The first internal electrode layers 12a are provided further outward in the T direction than a group of these third internal electrode layers 12c. This configuration narrows the width of the internal electrode layers in the W direction in the region close to the cover layer 13. This suppresses diffusion in corners where cracks 40 are likely to occur, thereby suppressing cracks 40. Meanwhile, good contact between the internal electrode layers and the first external electrode 20a is achieved near the center of the stacking direction. As a result, it is possible to both suppress cracks 40 and ensure capacitance.
[0064] For example, if the number of third internal electrode layers 12c is small, there is a risk that sufficient capacitance cannot be ensured. Therefore, it is preferable to set a lower limit on the number of third internal electrode layers 12c. On the other hand, if the number of third internal electrode layers 12c is large, there is a risk that the occurrence of cracks 40 cannot be sufficiently suppressed. Therefore, it is preferable to set a lower limit and an upper limit on the number of third internal electrode layers 12c. In this embodiment, when all internal electrode layers connected to the first external electrode 20a are taken as 100%, it is preferable that the number of third internal electrode layers 12c is 5% or more and 40% or less.
[0065] In the multilayer ceramic capacitor 100a according to this embodiment, for example, as illustrated in FIG. 12 , when stacking the multilayer units, a third stack unit in which an internal electrode pattern 52b having the same width as the dielectric green sheet 51 is formed on the dielectric green sheet 51 is used in the central portion instead of a first stack unit in which an internal electrode pattern 52a is formed on the dielectric green sheet 51.
[0066] In addition, elements that form stable compounds with hydrogen reduce the effects of hydrogen generated during the plating process and suppress insulation deterioration. Therefore, it is preferable that the second internal electrode layers 12b contain elements that form stable compounds with hydrogen other than low-melting point metals. Specifically, it is preferable that the second internal electrode layers 12b contain Ni as the main component, Ag (silver), Au (gold), Ga (gallium), Ge (germanium), etc.
[0067] Although the above embodiments have been described with reference to a multilayer ceramic capacitor as an example of a ceramic electronic component, the present invention is not limited to this. For example, the configurations of the above embodiments can be applied to other multilayer ceramic electronic components such as varistors and thermistors.
[0068] The multilayer ceramic capacitors according to the respective embodiments were fabricated and their characteristics were examined.
[0069] Example 1 In Example 1, the multilayer ceramic capacitor described in the first embodiment was fabricated. 3A slurry containing the above as a main component was blended and coated to obtain a dielectric green sheet. An internal electrode pattern was printed on each dielectric green sheet to obtain a laminate unit. Nickel powder was used for the internal electrode pattern. In the first laminate unit, the width of the end of the internal electrode pattern was made smaller than the width of the dielectric green sheet. In addition, in the first laminate unit, 1.0 at% Sn was added when Ni was 100 at% in the internal electrode pattern. 250 layers of the obtained laminate unit were stacked to obtain a laminate. In the second laminate unit, Sn was not added to the internal electrode pattern.
[0070] Multiple cover sheets were laminated and pressed onto the top and bottom of the laminate in the stacking direction, followed by a binder removal process. The laminate was then fired and re-oxidized. A Cu-based metal paste was applied to the two end faces of the resulting laminated chip and baked at approximately 800°C. Through these processes, a multilayer ceramic capacitor with a 0603 shape (length L: 600 μm, width W: 300 μm, height T: 300 μm) and 250 internal electrode layers was fabricated.
[0071] In the fired multilayer ceramic capacitor, the thickness of the first internal electrode layer 12a and the second internal electrode layer 12b was 0.5 μm, and the thickness of each dielectric layer 11 was 0.5 μm. The thickness of each cover layer in the T direction was 25 μm. The thickness of each side margin in the W direction was 25 μm. The width W2 of each internal electrode layer in the W direction was 250 μm. The width W1 of the first region of the first internal electrode layer 12a was 200 μm. The length of the first region 121 of the first internal electrode layer 12a in the L direction was 50 μm. The dimension e of the first external electrode 20a was 150 μm.
[0072] Example 2 In Example 2, the multilayer ceramic capacitor described in the second embodiment was fabricated. In Example 2, of the internal electrode layers connected to the first external electrode 20a, the central 75 layers were designated as third internal electrode layers 12c, and the upper and lower 25 layers were designated as first internal electrode layers 12a. The thickness of the third internal electrode layers 12c was 0.5 μm. The width W2 of the third internal electrode layers 12c in the W direction was 250 μm. The other conditions were the same as in Example 1.
[0073] In the comparative example, instead of the 125 first internal electrode layers 12a, internal electrode layers whose width in the W direction is constant at any point in the L direction were used. Other conditions were the same as in Example 1.
[0074] (Crack Generation) For each of Examples 1 and 2 and the Comparative Example, 100 samples were prepared, and the WT cross sections at the locations where the first external electrodes 20a were provided were observed. No cracks were observed in either Example 1 or 2. This is thought to be because the width of the end of the first internal electrode layer 12a on the first external electrode 20a side was narrowed, thereby suppressing expansion of the first internal electrode layer 12a due to diffusion of Cu from the first external electrode 20a. In contrast, in the Comparative Example, cracks were observed at at least one of the four corners. This is thought to be because the width of the internal electrode layer connected to the first external electrode 20a was not narrow.
[0075] (Capacitance) Next, the capacitance of 100 samples each of Examples 1 and 2 was measured under conditions of 1 kHz and 0.5 Vrms. The average capacitance was calculated. In Example 1, the capacitance was 1.89 μF, and in Example 2, the capacitance was 2.03 μF. Thus, sufficient capacitance was obtained in both Examples 1 and 2. This is thought to be because the width of the second internal electrode layer 12b connected to the second external electrode 20b was large.
[0076] Furthermore, the average value of the sample of Example 2 was 5% or more higher than that of the sample of Example 1. This is thought to be because the width of the lead-out portion of the internal electrode at the center in the height direction in the sample of Example 2 was not narrowed, so that the connection with the external electrode was sufficiently secured and a decrease in capacitance due to poor contact (so-called capacitance loss) was suppressed. Note that in the comparative example, poor insulation occurred due to the occurrence of cracks, making it impossible to measure the capacitance.
[0077] The results of Examples 1 and 2 and the Comparative Example are shown in Table 1.
[0078] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and changes are possible within the scope of the gist of the present invention as described in the claims.
[0079] REFERENCE SIGNS LIST 10 laminated chip 11 dielectric layer 12a first internal electrode layer 12b second internal electrode layer 12c third internal electrode layer 13 cover layer 14 capacitance portion 15a first end margin 15b second end margin 16 side margin 20a first external electrode 20b second external electrode 21a, 21b underlayer 22a, 22b plating layer 23a, 23b first plating layer 24a, 24b second plating layer 51 dielectric green sheet 52 internal electrode pattern 53 cover sheet 54 side margin sheet 100 laminated ceramic capacitor 121 first region 122 second region
Claims
1. A laminated chip comprising first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni alternately stacked with a dielectric layer sandwiched therebetween, having a generally rectangular parallelepiped shape, the first internal electrode layers and the second internal electrode layers alternately drawn out to opposing first and second end faces of the generally rectangular parallelepiped shape; a first external electrode provided on the first end face, the contact layer in contact with the first end face being mainly composed of Cu; and a second external electrode provided on the second end face, the contact layer in contact with the second end face being mainly composed of Cu; at least the first internal electrode layer of the first and second internal electrode layers contains a low-melting point metal having a melting point lower than the melting point of Pb, the first internal electrode layer having a higher concentration of the low-melting point metal than the second internal electrode layer; the width of a portion of the first internal electrode layer connected to the first external electrode in a direction perpendicular to the stacking direction is narrower than the width of a portion facing the second internal electrode layer; a width in a direction perpendicular to a stacking direction of a portion of the second internal electrode layer that is connected to the second external electrode is wider than a width of a portion of the first internal electrode layer that is connected to the first external electrode.
2. The ceramic electronic component according to claim 1, wherein the low melting point metal is Sn.
3. The ceramic electronic component according to claim 1, wherein the second internal electrode layer contains a metal element other than the low-melting point metal that forms a stable compound with hydrogen.
4. The ceramic electronic component according to claim 3, wherein the metal element that forms a stable compound with hydrogen is at least one of Ag, Au, Ga, and Ge.
5. A ceramic electronic component as described in claim 1, wherein the width of the portion of the second internal electrode layer that connects to the second external electrode in a direction perpendicular to the stacking direction is the same as the width of the portion of the second internal electrode layer that faces the first internal electrode layer.
6. A ceramic electronic component as described in claim 1, wherein the width of the portion of the first internal electrode layer that connects to the first external electrode in a direction perpendicular to the stacking direction is 60% or more and 90% or less of the width of the portion that faces the second internal electrode layer.
7. A ceramic electronic component as set forth in claim 1, wherein a third internal electrode layer connected to said first external electrode is provided in a central portion in the stacking direction, and the width of the portion of said third internal electrode layer connected to said first external electrode in a direction perpendicular to the stacking direction is the same as the width of the portion facing said second internal electrode layer.
8. The ceramic electronic component according to claim 7, wherein the number of the third internal electrode layers is 5% to 40% of the number of the internal electrode layers connected to the first external electrodes.
9. A ceramic electronic component as described in claim 1, wherein, in the direction in which the first end face and the second end face oppose each other, a length of a portion of the first internal electrode layer that connects to the first external electrode and is narrower than a width of a portion that opposes the second internal electrode layer is between 1 / 4 and 1 / 1 of the length of the first external electrode.
10. A process for preparing a laminated chip, the laminated chip comprising first internal electrode layers mainly composed of Ni and second internal electrode layers mainly composed of Ni, alternately stacked with a dielectric layer sandwiched therebetween, having a substantially rectangular parallelepiped shape, the first internal electrode layers and the second internal electrode layers alternately drawn out to opposing first and second end faces of the substantially rectangular parallelepiped shape, at least the first internal electrode layer of the first and second internal electrode layers contains a low-melting point metal having a melting point lower than the melting point of Pb, the first internal electrode layer has a higher concentration of the low-melting point metal than the second internal electrode layer, the width of a portion of the first internal electrode layer drawn out to the first end face in a direction perpendicular to the lamination direction is narrower than the width of a portion facing the second internal electrode layer, and the width of a portion of the second internal electrode layer drawn out to the second end face in a direction perpendicular to the lamination direction is wider than the width of the portion of the first internal electrode layer drawn out to the first end face; and baking external electrodes mainly composed of Cu onto each of the first end face and the second end face.
Citation Information
Patent Citations
Laminated ceramic capacitor
JP2009027148A
Multilayer ceramic electronic component and manufacturing method for the same
JP2013098525A
Multilayer ceramic capacitor
JP2018198292A
Multilayered ceramic capacitor
WO2022210627A1