Liquid-crystalline resin composition
The liquid crystal resin composition, featuring a combination of a liquid crystal resin, hollow filler, and carbon black, addresses the high dielectric loss tangent issue in conventional compositions, achieving low dielectric constants and excellent blackness for high-frequency components.
Patent Information
- Application Number
- PCT/JP2024/012765
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional liquid crystalline resin compositions containing carbon black have high dielectric loss tangents, which limits their dielectric properties, and they do not achieve optimal blackness and low dielectric constants for high-frequency electronic components.
A liquid crystal resin composition comprising a liquid crystal resin, a hollow filler, and carbon black with a number average particle diameter of 20 to 100 nm, where the hollow filler content is 5 to 85 parts by mass and carbon black content is 0.1 to 7 parts by mass, specifically using aromatic polyester or polyester amide with structural units derived from aromatic hydroxycarboxylic acids, and incorporating glass balloons for improved properties.
The composition achieves a low dielectric constant and low dielectric loss tangent, along with excellent blackness, making it suitable for high-frequency electronic components, particularly in microwave and millimeter wave applications.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Liquid crystalline resin composition
[0001] The present invention relates to a liquid crystalline resin composition.
[0002] Liquid crystalline resins have a good balance of excellent mechanical strength, heat resistance, chemical resistance, electrical properties, etc., and also have excellent dimensional stability, and are therefore widely used as high-performance engineering plastics. Meanwhile, in recent years, remarkable technological developments have been made in the information and communications field, including mobile phones; wireless LANs; and ITS technologies such as GPS, VICS (registered trademark), and ETC. Accordingly, there is a growing need for high-performance high-frequency electronic components that can be used in high-frequency regions such as microwaves and millimeter waves. Materials constituting such electronic components are required to have appropriate dielectric properties depending on the design of each electronic component.
[0003] For example, Patent Document 1 discloses a molded article of a wholly aromatic liquid crystalline polyester resin composition having a relative dielectric constant of 3.0 or less and a dielectric dissipation factor of 0.04 or less, which is obtained by injection molding a composition containing 90 to 45% by weight of a wholly aromatic liquid crystalline polyester having a melting point of 320°C or more, 10 to 40% by weight of inorganic hollow spheres having an aspect ratio of 2 or less, and 0 to 15% by weight of an inorganic filler having an aspect ratio of 4 or more. The molded article has heat resistance such as solder reflow resistance, excellent dielectric properties, and is used as a fixing or holding member for transmitting and receiving parts of information and communication devices used in high frequency bands such as microwaves and millimeter waves.
[0004] Japanese Patent Application Laid-Open No. 2004-27021
[0005] Packages for electronic components, including the above-mentioned high-frequency electronic components, are often colored black to make discoloration due to aging less noticeable. To produce such black-colored packages, for example, a liquid crystalline resin composition containing carbon black is preferably used. However, the inventors' studies have revealed that conventional liquid crystalline resin compositions containing carbon black have significantly high dielectric loss tangents, leaving room for improvement in their dielectric properties.
[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a liquid crystalline resin composition having a low dielectric constant, a low dielectric loss tangent, and excellent blackness.
[0007] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that a liquid crystalline resin composition containing a liquid crystalline resin, a hollow filler, and carbon black in predetermined content ratios, in which the carbon black has a number average particle size of 20 to 100 nm, has a low dielectric constant and a low dielectric loss tangent, and is excellent in blackness, and have completed the present invention. More specifically, the present invention provides the following.
[0008] (1) A liquid crystalline resin composition comprising (A) a liquid crystalline resin, (B) a hollow filler, and (C) carbon black, wherein the content of the (B) hollow filler is 5 to 85 parts by mass and the content of the (C) carbon black is 0.1 to 7 parts by mass, relative to 100 parts by mass of the (A) liquid crystalline resin, and the number average particle diameter of the (C) carbon black is 20 to 100 nm.
[0009] (2) The liquid crystalline resin composition according to (1), wherein the (A) liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent component, a constituent unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
[0010] (3) The liquid crystal resin composition according to (1) or (2), wherein the hollow filler (B) contains glass balloons.
[0011] (4) The liquid crystal resin composition according to any one of (1) to (3), wherein the dielectric loss tangent at a measurement frequency of 5 GHz is 0.0067 or less.
[0012] According to the present invention, it is possible to provide a liquid crystalline resin composition having a low dielectric constant, a low dielectric loss tangent, and an excellent degree of blackness.
[0013] FIG. 1 is a top view showing the cutting positions of the test pieces for evaluating dielectric characteristics used in the examples and comparative examples.
[0014] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0015] <Liquid Crystalline Resin Composition> The liquid crystal resin composition according to the present invention contains (A) a liquid crystal resin, (B) a hollow filler, and (C) carbon black, and the number average particle diameter of the (C) carbon black is 20 to 100 nm.
[0016] [(A) Liquid Crystalline Resin] The (A) liquid crystal resin used in the present invention refers to a melt-processable polymer capable of forming an optically anisotropic molten phase. The properties of the anisotropic molten phase can be confirmed by a conventional polarization examination method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing a molten sample placed on a Leitz hot stage at 40x magnification using a Leitz polarizing microscope under a nitrogen atmosphere. When examined between crossed polarizers, the liquid crystal polymer applicable to the present invention normally transmits polarized light, even in a molten, stationary state, and exhibits optical anisotropy.
[0017] The type of the liquid crystalline resin (A) described above is not particularly limited, but is preferably an aromatic polyester and / or an aromatic polyester amide. Polyesters partially containing aromatic polyesters and / or aromatic polyester amides in the same molecular chain are also included. The liquid crystalline resin (A) preferably has an inherent viscosity (I.V.) of at least about 2.0 dl / g, more preferably 2.0 to 10.0 dl / g, when dissolved in pentafluorophenol at 60°C to a concentration of 0.1% by mass.
[0018] The aromatic polyester or aromatic polyesteramide as the liquid crystal resin (A) applicable to the present invention is particularly preferably an aromatic polyester or aromatic polyesteramide having, as a constituent component, a constituent unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
[0019] More specifically, (1) polyesters mainly composed of structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof; (2) polyesters mainly composed of (a) structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof, and (b) structural units derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and derivatives thereof; (3) polyesters mainly composed of (a) structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof, (b) structural units derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and derivatives thereof, and (c) structural units derived from at least one selected from the group consisting of aromatic diols, alicyclic diols, aliphatic diols, and derivatives thereof; (4) polyesteramides mainly consisting of (a) structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their derivatives, (b) structural units derived from at least one selected from the group consisting of aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c) structural units derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives; (5) polyesteramides mainly consisting of (a) structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their derivatives, (b) structural units derived from at least one selected from the group consisting of aromatic hydroxyamines, aromatic diamines, and their derivatives, (c) structural units derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, and (d) structural units derived from at least one selected from the group consisting of aromatic diols, alicyclic diols, aliphatic diols, and their derivatives. Furthermore, a molecular weight modifier may be used in combination with the above structural components as needed.
[0020] In the (A) liquid crystalline resin, the content of the structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their derivatives is preferably 45 mol% or more, more preferably 50 mol% or more, even more preferably 55 mol% or more, even more preferably 60 mol% or more, and particularly preferably 62 mol% or more, based on all structural units, from the viewpoint of suppressing fluctuations in the molecular structure of the (A) liquid crystalline resin. The upper limit of the content is not particularly limited, and may be 100 mol% or less, 90 mol% or less, 80 mol% or less, 75 mol% or less, or 70 mol% or less, based on all structural units.
[0021] Preferred examples of the compound constituting the (A) liquid crystal resin applicable to the present invention include aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid; aromatic diols such as 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, compounds represented by the following general formula (I) and compounds represented by the following general formula (II); aromatic dicarboxylic acids such as 1,4-phenylenedicarboxylic acid, 1,3-phenylenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid and compounds represented by the following general formula (III); and aromatic amines such as p-aminophenol, p-phenylenediamine and N-acetyl-p-aminophenol. As the aromatic hydroxycarboxylic acid and its derivatives, 4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, or a combination thereof are preferred from the viewpoints of reactivity and the stability of the molecular structure of the (A) liquid crystal resin. (X: alkylene (C 1 ~C 4 ), alkylidene, —O—, —SO—, —SO 2 is a group selected from —, —S—, and —CO—. (Y:-(CH 2 ) n -(n=1 to 4) and -O(CH 2 ) n O- (n = 1 to 4).
[0022] The liquid crystal resin (A) used in the present invention can be prepared by known methods such as direct polymerization or transesterification from the above-mentioned monomer compound (or mixture of monomers). Typically, melt polymerization, solution polymerization, slurry polymerization, solid-state polymerization, or a combination of two or more of these methods is used. Melt polymerization or a combination of melt polymerization and solid-state polymerization is preferred. The above-mentioned compounds capable of forming esters may be used in the polymerization in their original form, or may be modified from a precursor to a derivative capable of forming an ester prior to polymerization. Various catalysts can be used in these polymerizations. Representative examples include metal salt catalysts such as potassium acetate, magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, antimony trioxide, and tris(2,4-pentanedionato)cobalt(III), and organic compound catalysts such as 1-methylimidazole and 4-dimethylaminopyridine. The amount of catalyst used is generally about 0.001 to 1% by mass, and preferably about 0.01 to 0.2% by mass, based on the total mass of the monomers. If necessary, the polymers produced by these polymerization methods can be further subjected to solid-phase polymerization in which they are heated under reduced pressure or in an inert gas to increase the molecular weight.
[0023] The melt viscosity of the liquid crystalline resin (A) obtained by the above method is not particularly limited. Generally, the melt viscosity at the molding temperature is -1 A liquid crystal resin having a viscosity of 3 Pa·s or more and 500 Pa·s or less can be used. However, a liquid crystal resin having a viscosity that is too high is not preferred because it will have a significantly reduced fluidity. The liquid crystal resin (A) may be a mixture of two or more liquid crystal resins.
[0024] [(B) Hollow Filler] The (B) hollow filler is generally called a balloon, and examples of hollow filler materials include inorganic materials such as alumina, silica, glass, and shirasu. Among these, glass and silica are preferred from the viewpoint of heat resistance and strength, and glass is more preferred. That is, glass balloons and silica balloons are preferably used as hollow fillers, and glass balloons are more preferably used. The (B) component may be used alone or in combination of two or more types.
[0025] The aspect ratio of the (B) hollow filler is preferably 1.15 or more, more preferably 1.20 or more and 2.00 or less, even more preferably 1.22 or more and 1.50 or less, and even more preferably 1.25 or more and less than 1.30, from the viewpoints of suppressing an increase in melt viscosity and a deterioration in fluidity, as well as moldability, etc. In this specification, the aspect ratio is determined by measuring the maximum length L, which is the length of the longest part in the particle projection plane, and the maximum perpendicular length S, which is the length of the longest part in the particle projection plane in the direction perpendicular to the maximum length L, for 3,000 particles using a dynamic image analysis method / particle state analyzer, and repeating the measurement several times to obtain the average value of the ratio L / S calculated for each particle.
[0026] From the viewpoint of moldability, the median diameter of component (B) is preferably 5 μm or more, more preferably 10 μm or more, and from the viewpoint of suppressing breakage of component (B) and moldability, it is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. In this specification, the median diameter refers to the volume-based median value measured by a laser diffraction / scattering particle size distribution measurement method.
[0027] The content of the (B) component is 5 to 85 parts by mass, preferably 7 to 65 parts by mass, and more preferably 10 to 45 parts by mass, per 100 parts by mass of the (A) liquid crystalline resin. When the content of the (B) component is 20 parts by mass or more, a liquid crystalline resin composition with excellent dielectric properties is easily obtained. When the content of the (B) component is 75 parts by mass or less, a liquid crystalline resin composition with good fluidity is easily obtained.
[0028] [(C) Carbon Black]
[0029] The carbon black (C) used in the present invention can be any commonly available carbon black used for resin coloring, as long as it has a number-average particle diameter of 20 to 100 nm, and is not particularly limited. Component (C) may be used alone or in combination of two or more. In this specification, the number-average particle diameter is determined by observing carbon black with a transmission electron microscope in accordance with ASTM D3849-14a and measuring the particle diameters of 100 carbon black particles, and the average value is used.
[0030] The number average particle diameter of component (C) is 20 to 100 nm, preferably 22 to 92 nm, more preferably 24 to 84 nm, even more preferably 26 to 76 nm, even more preferably 28 to 68 nm, and particularly preferably 30 to 60 nm. When the number average particle diameter of component (C) is 20 nm or more, a liquid crystalline resin composition having a low dielectric loss tangent is easily obtained. When the number average particle diameter of component (C) is 100 nm or less, a liquid crystalline resin composition having good fluidity is easily obtained.
[0031] The content of the (C) component is 0.1 to 7 parts by mass, preferably 0.3 to 6.5 parts by mass, and more preferably 0.5 to 6 parts by mass, relative to 100 parts by mass of the (A) liquid crystal resin. When the content of the (C) component is 0.1 part by mass or more, the blackness of the resulting resin composition is less likely to decrease. When the content of the (C) component is 7 parts by mass or less, a liquid crystal resin composition with good fluidity is easily obtained.
[0032] [Fillers other than (D) (B) hollow filler and (C) carbon black] The liquid crystalline resin composition according to the present invention may optionally contain fillers other than (D) (C) hollow filler and (C) carbon black. When the liquid crystalline resin composition contains the component (D), the mechanical strength of a molded article of the liquid crystalline resin composition, such as flexural modulus, is likely to be improved. The component (D) may be used alone or in combination of two or more. The component (D) may be an inorganic filler or an organic filler. Examples of the component (D) include a plate-like filler, a fibrous filler, and a granular filler.
[0033] (Flat-like filler) When the liquid crystalline resin composition according to the present invention contains a platy filler, the molded article made of the liquid crystalline resin composition is likely to have improved mechanical strength such as flexural modulus, and warpage is likely to be suppressed. The platy filler may be used alone or in combination of two or more kinds.
[0034] The plate-like filler preferably has a median diameter of 15 to 50 μm. When the median diameter is 15 μm or more, the necessary mechanical strength is likely to be ensured, and the effect of suppressing warpage of the molded article is likely to be enhanced. When the median diameter is 50 μm or less, the fluidity of the composition when melted is likely to be improved. The preferred median diameter is 20 to 30 μm.
[0035] The plate-like filler is not particularly limited, and examples thereof include mica, talc, glass flakes, graphite, various metal foils (e.g., aluminum foil, iron foil, copper foil), etc. In the present invention, it is preferable to use mica as the plate-like filler.
[0036] (Fibrous Filler) When the liquid crystalline resin composition according to the present invention contains a fibrous filler, the molded article made of the liquid crystalline resin composition tends to have improved mechanical strength such as flexural modulus. The fibrous fillers can be used alone or in combination of two or more.
[0037] The average fiber length of the fibrous filler is not particularly limited and may be, for example, 250 μm or more, preferably 350 to 600 μm, and more preferably 450 to 500 μm. When the average fiber length is 250 μm or more, the molded article made from the liquid crystalline resin composition of the present invention is likely to have improved mechanical strength and heat resistance. When the average fiber length is 600 μm or less, the liquid crystalline resin composition is likely to have sufficient fluidity. In this specification, the average fiber length of the fibrous filler is defined as the average of the values measured by importing 10 stereomicroscope images of the fibrous filler from a CCD camera into a PC and processing the images using an image measuring device to measure the fiber lengths of 100 fibrous fillers per stereomicroscope image, i.e., a total of 1,000 fibrous fillers. The average fiber length of the fibrous filler in the liquid crystalline resin composition is measured by applying the above method to the remaining fibrous filler after heating the liquid crystalline resin composition to 600°C for 2 hours to incinerate it.
[0038] The fiber diameter of the fibrous filler is not particularly limited and may be, for example, 20 μm or less, or may be 5 to 15 μm. In this specification, the fiber diameter of the fibrous filler is determined by observing the fibrous filler with a scanning electron microscope and measuring the fiber diameters of 30 fibrous fillers. The fiber diameter of the fibrous filler in the liquid crystalline resin composition is measured by applying the above-mentioned method to the remaining fibrous filler after heating the liquid crystalline resin composition at 600°C for 2 hours to incinerate it.
[0039] Any fiber can be used as long as it satisfies the above-mentioned shape, but examples of the fibrous filler include inorganic fibrous materials such as glass fiber, milled fiber, carbon fiber, asbestos fiber, silica fiber, silica-alumina fiber, zirconia fiber, boron nitride fiber, silicon nitride fiber, boron fiber, potassium titanate fiber, and fibrous materials of metals such as stainless steel, aluminum, titanium, copper, brass, etc. In the present invention, it is preferable to use glass fiber as the fibrous filler from the viewpoint of mechanical strength.
[0040] (Granular filler) When the liquid crystalline resin composition according to the present invention contains a granular filler, the molded article made of the liquid crystalline resin composition is likely to have improved mechanical strength such as flexural modulus and is likely to be inhibited from surface whitening. The granular filler can be used singly or in combination of two or more.
[0041] The median diameter of the granular filler is preferably 0.3 to 5.0 μm. When the median diameter is 0.3 μm or more, the impact resistance of the molded body is likely to be maintained. When the median diameter is 5.0 μm or less, the effect of suppressing surface whitening of the molded body is likely to be enhanced. The median diameter is more preferably 0.5 to 5.0 μm, and even more preferably 0.5 to 4.0 μm. The median diameter of the granular filler in the liquid crystalline resin composition is a value measured for the granular filler remaining after the liquid crystalline resin composition is incinerated by heating at 600° C. for 2 hours.
[0042] Examples of granular fillers include metal oxides such as silica, quartz powder, glass beads, glass powder, potassium aluminum silicate, diatomaceous earth, iron oxide, titanium oxide, zinc oxide, and alumina; metal carbonates such as calcium carbonate and magnesium carbonate; metal sulfates such as calcium sulfate and barium sulfate; phosphates such as calcium pyrophosphate and anhydrous dicalcium phosphate; silicon carbide; silicon nitride; boron nitride, etc. In the present invention, from the viewpoints of suppressing surface whitening of the molded article and reducing dust generation of the molded article, it is preferable to use one or more selected from the group consisting of silica and barium sulfate as the granular filler, and it is more preferable to use silica.
[0043] The content of the component (D) is preferably 2 to 15 parts by mass, more preferably 5 to 12 parts by mass, and even more preferably 7 to 10 parts by mass, relative to 100 parts by mass of the liquid crystal resin (A). When the content of the component (D) is within the above range, the fluidity of the liquid crystal resin composition is sufficiently ensured, and the mechanical strength of a molded article made of the liquid crystal resin composition is likely to be improved.
[0044] [Other Components] The liquid crystalline resin composition of the present invention may contain other polymers and known substances generally added to synthetic resins, i.e., stabilizers such as antioxidants and ultraviolet absorbers, antistatic agents, flame retardants, colorants such as dyes and pigments, lubricants, mold release agents, crystallization accelerators, crystal nucleating agents, etc., depending on the required performance, within the range that does not impair the effects of the present invention. The other polymers refer to polymers other than the (A) liquid crystalline resin, and include, for example, epoxy group-containing copolymers.
[0045] [Preparation of Liquid Crystalline Resin Composition] The preparation of the liquid crystal resin composition according to the present invention is not particularly limited. For example, the liquid crystal resin composition is prepared by blending the components (A), (B), (C), optionally the component (D), and optionally other components, and melt-kneading them using a single-screw or twin-screw extruder.
[0046] [Liquid Crystalline Resin Composition] From the viewpoint of fluidity, the melt viscosity of the liquid crystal resin composition according to the present invention obtained as described above is preferably 100 Pa·sec or less, more preferably 90 Pa·sec or less, and even more preferably 85 Pa·sec or less. The lower limit of the melt viscosity is not particularly limited, and may be 5 Pa·sec or more, 10 Pa·sec or more, or 20 Pa·sec or more. In this specification, the melt viscosity is defined as the viscosity at a cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin, a shear rate of 1000 sec -1 The value obtained by the measurement method in accordance with ISO 11443 under the above conditions is adopted.
[0047] The liquid crystal resin composition according to the present invention has a dielectric constant at a measurement frequency of 5 GHz of preferably 4.0 or less, more preferably 3.9 or less, and even more preferably 3.8 or less, from the viewpoint of dielectric properties. The lower limit of the dielectric constant is not particularly limited, and may be more than 1.0, or may be 1.5 or more, or 2.0 or more.
[0048] The dielectric loss tangent of the liquid crystal resin composition according to the present invention at a measurement frequency of 5 GHz is preferably 0.0067 or less, more preferably 0.0065 or less, and even more preferably 0.0063 or less, from the viewpoint of dielectric properties. The lower limit of the dielectric loss tangent is not particularly limited, and may be 0.001 or more, 0.0015 or more, or 0.0017 or more.
[0049] From the viewpoint of blackness, the L value of the liquid crystal resin composition according to the present invention is preferably 60 or less, more preferably 50 or less, and even more preferably 45 or less. The lower limit of the L value is not particularly limited, and may be 0 or more, 5 or more, or 10 or more.
[0050] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0051] <Liquid Crystalline Resin> Aromatic Polyester The following raw materials were charged into a polymerization vessel, and the temperature of the reaction system was raised to 140°C and allowed to react at 140°C for 1 hour. The temperature was then further raised to 360°C over 5.5 hours, and the pressure was then reduced to 5 Torr (i.e., 667 Pa) over 30 minutes. Melt polymerization was carried out while distilling off acetic acid, excess acetic anhydride, and other low-boiling components. After the stirring torque reached a predetermined value, nitrogen was introduced to change the pressure from reduced pressure to normal pressure and then to pressurized pressure. The polymer was discharged from the bottom of the polymerization vessel, and the strands were pelletized to obtain pellets. The obtained pellets were heat-treated at 300°C for 3 hours under a nitrogen stream to obtain the target polymer. The melting point of the obtained polymer was 348°C, and the melt viscosity at 370°C was 9 Pa·s. The melting point of the above polymer was measured according to the melting point measurement method described below, and the melt viscosity of the above polymer was measured in the same manner as the melt viscosity measurement method described below. 6-Hydroxy-2-naphthoic acid (HNA): 1218 g (48 mol%); 4-hydroxybenzoic acid (HBA): 37 g (2 mol%); 1,4-phenylenedicarboxylic acid: 560 g (TA): (25 mol%); 4,4'-dihydroxybiphenyl (BP): 628 g (25 mol%); metal catalyst (potassium acetate catalyst): 165 mg; acylating agent (acetic anhydride): 1432 g
[0052] Aromatic polyesteramide: After the following raw materials were charged into a polymerization vessel, the temperature of the reaction system was raised to 140°C and the reaction was carried out at 140°C for 1 hour. The temperature was then further raised to 340°C over 4.5 hours, and the pressure was then reduced to 10 Torr (i.e., 1330 Pa) over 15 minutes. Melt polymerization was carried out while distilling off acetic acid, excess acetic anhydride, and other low-boiling components. After the stirring torque reached a predetermined value, nitrogen was introduced to change the pressure from reduced pressure to normal pressure and then to pressurized pressure. The polymer was discharged from the bottom of the polymerization vessel, and the strands were pelletized to obtain pellets. The obtained pellets were heat-treated at 300°C for 2 hours under a nitrogen stream to obtain the target polymer. The melting point of the obtained polymer was 336°C, and the melt viscosity at 350°C was 19.0 Pa·s. The melting point of the above polymer was measured according to the melting point measurement method described below, and the melt viscosity of the above polymer was measured in the same manner as the melt viscosity measurement method described below. 4-Hydroxybenzoic acid (HBA): 1380 g (60 mol%), 6-hydroxy-2-naphthoic acid (HNA): 157 g (5 mol%), 1,4-phenylenedicarboxylic acid (TA): 484 g (17.5 mol%), 4,4'-dihydroxybiphenyl (BP): 388 g (12.5 mol%), N-acetyl-p-aminophenol (APAP): 126 g (5 mol%), metal catalyst (potassium acetate catalyst): 110 mg, acylating agent (acetic anhydride): 1659 g
[0053] [Method of measuring melting point] Using a DSC manufactured by TA Instruments, the liquid crystalline resin was heated from room temperature at a temperature increase rate of 20°C / min to measure the endothermic peak temperature (Tm1) observed, and then held at a temperature of (Tm1+40)°C for 2 minutes. After that, the resin was cooled to room temperature at a temperature decrease rate of 20°C / min, and then heated again at a temperature increase rate of 20°C / min to measure the endothermic peak temperature (Tm2), which was determined as the melting point of the polymer.
[0054] [Method for measuring melt viscosity] The melt viscosity of the liquid crystalline resin was measured using a Capirograph 1B model manufactured by Toyo Seiki Seisakusho, Ltd., at a temperature 10 to 30°C higher than the melting point of the liquid crystalline resin, using an orifice with an inner diameter of 1 mm and a length of 20 mm, at a shear rate of 1000 / sec in accordance with ISO 11443. The specific measurement temperatures were 370°C for aromatic polyesters and 350°C for aromatic polyesteramides.
[0055] <Materials other than liquid crystalline resin> Glass balloon: Y12000 (manufactured by Seishin Enterprise Co., Ltd., aspect ratio (average) 1.264, median diameter 35 μm, true specific gravity 0.6) Carbon black C1: Conductex 7054 Ultra (manufactured by Birla Carbon Korea Co., Ltd., number average particle diameter 54 nm) Carbon black C2: BLACK PEARLS 4350 (manufactured by Cabot Japan Co., Ltd., number average particle diameter 25 nm) Carbon black C3: MONARCH 4750 (manufactured by Cabot Japan Co., Ltd., number average particle diameter 18 nm)
[0056] <Production of Liquid Crystalline Resin Composition> The above components were melt-kneaded in the proportions shown in Table 1 using a twin-screw extruder (TEX30α type, manufactured by The Japan Steel Works, Ltd.) at the following cylinder temperatures to obtain liquid crystal resin composition pellets. [Production conditions] Cylinder temperature: 370°C: for liquid crystal resin compositions containing aromatic polyesters 350°C: for liquid crystal resin compositions containing aromatic polyesteramides
[0057] <L Value> The pellets of the Examples and Comparative Examples were molded using a molding machine ("SE-100DU" manufactured by Sumitomo Heavy Industries, Ltd.) under the following molding conditions to prepare flat test pieces of 80 mm x 80 mm x 1 mm. The L value of these test pieces was measured using a spectrophotometer ("SE6000" manufactured by Nippon Denshoku Industries Co., Ltd.). [Molding Conditions] Cylinder temperature: 370°C (Examples 1 to 5 and Comparative Examples 1 to 4) 350°C (Example 6) Mold temperature: 80°C Injection speed: 33 mm / sec Holding pressure: 60 MPa
[0058] <Dielectric Properties> The pellets of the Examples and Comparative Examples were molded using a molding machine ("SE-100DU" manufactured by Sumitomo Heavy Industries, Ltd.) under the following molding conditions to prepare flat plate-shaped test pieces measuring 80 mm x 80 mm x 1 mm. As shown in FIG. 1 , a test piece measuring 80 mm x 1 mm x 1 mm was cut out from the center of the flat plate-shaped test piece in the flow direction, and this was used as a test piece for evaluating dielectric properties. The relative permittivity and dielectric loss tangent of this test piece at a measurement frequency of 5 GHz were measured using a cavity resonator perturbation method complex permittivity evaluation device manufactured by Kanto Electronics Application Development Co., Ltd. and having the following configuration. Scalar network analyzer: Agilent Technology 8757D Frequency synthesizer: Agilent Technology 83650L Sweep CW Generator Fixed attenuator: Agilent Technology 85025D Detector Cavity resonator: Kanto Electronics Application Development CP431 Measurement program: Kanto Electronics Application Development CPMA-S2 / V2 [Molding conditions] Cylinder temperature: 370°C (Examples 1 to 5 and Comparative Examples 1 to 4) 350°C (Example 6) Mold temperature: 80°C Injection speed: 33 mm / sec Holding pressure: 60 MPa
[0059]
[0060] As is clear from the results shown in Table 1, the liquid crystal resin compositions of the examples had low dielectric constants and low dielectric loss tangents, and were excellent in blackness.
Claims
1. A liquid crystalline resin composition comprising (A) a liquid crystalline resin, (B) a hollow filler, and (C) carbon black, wherein the content of the (B) hollow filler is 5 to 85 parts by mass, the content of the (C) carbon black is 0.1 to 7 parts by mass, and the number average particle diameter of the (C) carbon black is 20 to 100 nm, relative to 100 parts by mass of the (A) liquid crystalline resin.
2. The liquid crystalline resin composition according to claim 1, wherein the (A) liquid crystalline resin is an aromatic polyester or aromatic polyester amide having as a constituent component a structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
3. The liquid crystal resin composition according to claim 1 or 2, wherein the hollow filler (B) contains glass balloons.
4. The liquid crystal resin composition according to claim 1 or 2, wherein the dielectric tangent at a measurement frequency of 5 GHz is 0.0067 or less.
Citation Information
Patent Citations
Glass balloon product and its composition
JP1992295031A
Method for compounding metal to surface of cyclic olefine-based resin molding, and metal-compounded cyclic olefine-based resin molding
JP2004169049A
Manufacturing method of low dielectric wiring board
JP2008034724A
Polymer Composition for Use in Antenna Systems
JP2022545340A
Liquid crystal polymer composition
JP2022546959A