Photocatalyst and preparation method therefor

By doping Cu on the surface of Rutile TiO2, particularly on the (110) plane, the photocatalyst achieves high antibacterial and antiviral efficacy, addressing the limitations of existing photocatalysts in visible light activation and electronic excitation efficiency.

WO2024205060A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG ELECTRONICS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/002888
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current photocatalysts lack effective antibacterial and antiviral properties under visible light, particularly in applications requiring high electronic excitation efficiency and specific crystal structures like Rutile TiO2.

Method used

Doping Cu on the surface of Rutile TiO2 using a hydrothermal method and impregnation process, focusing on the (110) plane to enhance electronic excitation and oxidation-reduction reactions, with specific conditions such as mixing with Cu(NO3)2, heating, and using organic solvents to achieve high Cu doping efficiency.

Benefits of technology

The resulting photocatalyst exhibits strong antibacterial and antiviral efficacy, with increased Cu reduction efficiency on the (110) plane, leading to enhanced visible light activation and virus inactivation capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024002888_03102024_PF_FP_ABST
    Figure KR2024002888_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A photocatalyst and a preparation method therefor are disclosed. The photocatalyst preparation method according to the present disclosure may comprise the steps of: processing a Ti precursor through a hydrothermal method, thereby providing TiO2; and using impregnation to dope, with Cu, the surface of the provided TiO2.
Need to check novelty before this filing date? Find Prior Art

Description

Photocatalyst and method for producing the same

[0001] The present disclosure relates to a photocatalyst and a method for producing the same, and more particularly, to a photocatalyst having high antibacterial and antiviral properties by doping Cu on the surface of TiO2 and a method for producing the same.

[0002] TiO2 can exist thermodynamically in three phases: anatase, rutile, and brookite, and has different band gap energies depending on the phase.

[0003] A band gap is the energy region between the valence band (or "valence band") and the conduction band (or "conduction band") where the electron density is zero. The energy corresponding to the band gap is called the band gap energy. The size of the band gap determines the electrical properties of a material, such as its electrical conductivity.

[0004] Figure 1 is a diagram showing the crystal structure of each of the three phases of TiO2: Anatase, Rutile, and Brookite.

[0005] Referring to Fig. 1, Anatase (300), Rutile (100), and Brookite (200) have different crystal structures, and their respective band gap energies are 3.2 eV for Anatase (300), 3.0 eV for Rutile (100), and 3.4 eV for Brookite (200). Since Rutile (100) has the smallest band gap energy, it has the highest electron excitation efficiency by visible light, which has relatively low energy.

[0006] Rutile TiO2, which has the highest electron excitation efficiency due to low energy, can be used to develop materials using electron movement and oxidation-reduction reactions.

[0007] A method for manufacturing a photocatalyst for achieving the above-described purpose may include a step of preparing TiO2 by processing a Ti precursor through a hydrothermal method; and a step of doping Cu on the surface of the prepared TiO2 through an impregnation process.

[0008] Meanwhile, the doping step may include a step of mixing Cu(NO3)2 into the prepared TiO2; and a step of mixing water into the mixed TiO2 and Cu(NO3)2 and heating the mixture at 90°C for 2 hours.

[0009] Meanwhile, the doping step may include a step of mixing Cu(NO3)2 into the prepared TiO2; and a step of pouring an organic solvent into the mixed TiO2 and Cu(NO3)2 and reacting them at 25°C for 2 hours.

[0010] Meanwhile, the organic solvent may be ethanol or methanol.

[0011] Meanwhile, the doping step may include a step of irradiating ultraviolet rays to the prepared TiO2 surface; and a step of doping Cu to the prepared TiO2 surface by processing the TiO2 on which the ultraviolet rays have been irradiated through an impregnation process.

[0012] Meanwhile, the step of preparing the TiO2 includes a step of obtaining Rutile TiO2 having an area of ​​the (110) plane greater than a critical value; and the doping step may dope Cu onto the surface of the obtained Rutile TiO2 by processing the obtained Rutile TiO2 through an impregnation process.

[0013] Meanwhile, the step of preparing the TiO2 may include a first step of stirring a solution containing 41 mL of Ti(OBu) and 2 M NaCl at 600 rpm at 80°C for 4 hours; a step of obtaining TiO2 seeds by centrifuging the first stirred mixed solution and washing it with at least one of distilled water or ethanol; a second step of stirring the solution containing 2.5 M HCl mixed with the obtained TiO2 seeds at 600 rpm for 20 minutes; a step of subjecting the second stirred solution to a hydrothermal synthesis process at 180°C for 72 hours; a step of subjecting the second stirred solution subjected to the hydrothermal synthesis process to centrifugation and washing it with at least one of distilled water or ethanol to obtain synthesized TiO2; and a step of drying the synthesized TiO2 at 80°C.

[0014] Meanwhile, the above doping step can be performed by depositing Cu on the TiO2 surface using a photodeposition method.

[0015] Meanwhile, the Cu doped on the TiO2 surface may be at least one of a Cu salt, a Cu-metal complex, and a Cu oxide.

[0016] Meanwhile, it may include a TiO2 crystal; and Cu doped in one region of the surface of the TiO2 crystal.

[0017] Meanwhile, the above TiO2 crystal may be Rutile TiO2 in which the area of ​​the (110) plane is greater than a critical value.

[0018] Meanwhile, the photocatalyst may have a greater amount of Cu doped on the (110) plane of the TiO2 crystal than the amount of Cu doped on planes other than the (110) plane.

[0019] Aspects, features and advantages of specific embodiments of the present disclosure will become more apparent from the following description taken in conjunction with the accompanying drawings.

[0020] FIG. 1 is a diagram illustrating the crystal structures of Anatase, Brookite, and Rutile among various crystal forms of TiO2 according to one embodiment of the present disclosure.

[0021] Figure 2a is a drawing for explaining a method of representing a plane of a crystal structure in three-dimensional coordinates.

[0022] FIG. 2b is a diagram illustrating various aspects of TiO2 according to one embodiment of the present disclosure.

[0023] FIG. 3a is a drawing for explaining the excitation of a photocatalyst by light according to one embodiment of the present disclosure.

[0024] FIG. 3b is a diagram illustrating the activation of copper oxide according to one embodiment of the present disclosure.

[0025] FIG. 3c is a diagram illustrating virus inactivation according to one embodiment of the present disclosure.

[0026] FIG. 4a is a drawing for explaining a heating impregnation process according to one embodiment of the present disclosure.

[0027] FIG. 4b is a drawing illustrating an alcohol-based room temperature impregnation process according to one embodiment of the present disclosure.

[0028] FIG. 4c is a table for explaining the doping efficiency of Cu according to the impregnation process according to one embodiment of the present disclosure.

[0029] FIG. 5a is a drawing showing an SEM image of Rutile TiO2 according to one embodiment of the present disclosure.

[0030] FIG. 5b is a drawing for explaining the crystal form of Rutile TiO2 according to the area of ​​the (110) plane of TiO2 according to one embodiment of the present disclosure.

[0031] FIG. 6 is a graph for explaining the antibacterial and antiviral effects according to the area of ​​the (110) plane of TiO2 according to one embodiment of the present disclosure.

[0032] The present embodiments may be modified and have various embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the scope to specific embodiments, but should be understood to encompass various modifications, equivalents, and / or alternatives of the embodiments of the present disclosure. In connection with the description of the drawings, similar reference numerals may be used for similar components.

[0033] In describing the present disclosure, if it is determined that a specific description of a related known function or configuration may unnecessarily obscure the gist of the present disclosure, a detailed description thereof will be omitted.

[0034] Additionally, the following embodiments may be modified in various other forms, and the scope of the technical concepts of the present disclosure is not limited to the following embodiments. Rather, these embodiments are provided to further faithfully and completely convey the technical concepts of the present disclosure to those skilled in the art.

[0035] The terminology used in this disclosure is for the purpose of describing specific embodiments only and is not intended to limit the scope of the rights. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0036] In this disclosure, expressions such as “has,” “can have,” “includes,” or “may include” indicate the presence of a corresponding feature (e.g., a component such as a number, function, operation, or part), and do not exclude the presence of additional features.

[0037] In this disclosure, expressions such as “A or B,” “at least one of A and / or B,” or “one or more of A or / and B” can include all possible combinations of the listed items. For example, “A or B,” “at least one of A and B,” or “at least one of A or B” can all refer to (1) including at least one A, (2) including at least one B, or (3) including both at least one A and at least one B.

[0038] The expressions “first,” “second,” “first,” or “second,” etc., used in this disclosure can describe various components, regardless of order and / or importance, and are only used to distinguish one component from another, but do not limit the components.

[0039] When it is said that a component (e.g., a first component) is “(operatively or communicatively) coupled with / to” or “connected to” another component (e.g., a second component), it should be understood that the component may be directly coupled to the other component, or may be connected through another component (e.g., a third component).

[0040] On the other hand, when it is said that a component (e.g., a first component) is "directly connected" or "directly connected" to another component (e.g., a second component), it can be understood that no other component (e.g., a third component) exists between the component and the other component.

[0041] The expression "configured to" as used in the present disclosure may be used interchangeably with, for example, "suitable for," "having the capacity to," "designed to," "adapted to," "made to," or "capable of." The term "configured to" may not necessarily mean only "specifically designed to" in terms of hardware.

[0042] Meanwhile, the various elements and areas in the drawings are schematically drawn. Therefore, the technical concept of the present invention is not limited by the relative sizes or spacing depicted in the attached drawings.

[0043] Hereinafter, with reference to the attached drawings, embodiments according to the present disclosure will be described in detail so that a person having ordinary knowledge in the technical field to which the present disclosure pertains can easily implement the present disclosure.

[0044] In general, the planes of a crystal structure can be represented by three-dimensional coordinates.

[0045] Figure 2a is a drawing for explaining a method of representing a plane of a crystal structure in three-dimensional coordinates.

[0046] Referring to Fig. 2a, a plane that passes through a point where the x-coordinate is 1 but does not intersect the y-axis or the z-axis is called the (100) plane. A plane that passes through a point where the x-coordinate is 1 and a point where the y-coordinate is 1 but does not intersect the z-axis is called the (110) plane. A plane that intersects all of the x-axis, y-axis, and z-axis at a point where the coordinate is 1 is called the (111) plane.

[0047] FIG. 2b is a diagram illustrating various aspects of TiO2 according to one embodiment of the present disclosure.

[0048] Referring to Fig. 2b, TiO2 can have (001), (100), (110), (111), (101), (011) planes, etc. Depending on the synthesis method and synthesis process of TiO2, it can have various crystal structures, and depending on the crystal structure, electrical conductivity, melting point, band gap energy, etc. can vary.

[0049] The photocatalyst according to the present disclosure may include Cu doped in one region of the surface of the TiO2 crystal.

[0050] Typically, when Rutile TiO2 is synthesized, spherical nanoparticles are formed, and the (110) and (001) planes are evenly formed.

[0051] When TiO2 reacts with light, electron-hole pairs are created, allowing oxidation and reduction reactions to occur simultaneously within a single TiO2 or Cu particle. These oxidation-reduction reactions occur at locations with different energy levels, and these energy levels vary depending on the crystal plane.

[0052] In the case of rutile TiO2, reduction primarily occurs on the (110) plane, while oxidation primarily occurs on the (011) plane. Therefore, the (110) plane is the plane that primarily causes reduction, and if Cu is located on this plane, high Cu reduction [Cu(II) → Cu(I)] efficiency can be expected when irradiated with visible light.

[0053] In one embodiment, the TiO2 crystal may be Rutile TiO2 having an area of ​​the (110) plane greater than a critical value, and the amount of Cu doped on the (110) plane of the TiO2 crystal may be greater than the amount of Cu doped on planes other than the (110) plane.

[0054] As the area of ​​the (110) plane of a TiO2 crystal increases, the TiO2 takes on a rod-shaped crystal form, which is called Rutile TiO2. The purpose of the present invention is to develop and manufacture a visible photocatalyst exhibiting high antibacterial and antiviral efficacy by manufacturing rutile (110) Faceted TiO2 having a high proportion of (110) planes and efficiently grafting it with Cu.

[0055] To manufacture the photocatalyst described above, a Ti precursor can first be processed using a hydrothermal method to produce TiO2. The hydrothermal method is a synthetic method that crystallizes a substance from a high-temperature aqueous solution under high pressure.

[0056] Specifically, a solution containing 2 M NaCl mixed with 41 mL of Ti(OBu) was first stirred at 600 rpm for 4 hours at 80°C.

[0057] The first stirred mixed solution is centrifuged and then washed with at least one of distilled water and ethanol to obtain TiO2 seeds.

[0058] The obtained TiO2 seed is mixed with a solution of 2.5 M HCl and stirred for a second time at 600 rpm for 20 minutes. The second stirred solution is subjected to a hydrothermal synthesis process at 180°C for 72 hours.

[0059] The second stirred solution subjected to the hydrothermal synthesis process is centrifuged and washed with at least one of distilled water and ethanol to obtain synthesized TiO2.

[0060] When preparing TiO2, rutile TiO2 can be obtained with an area of ​​the (110) plane exceeding a critical value. Finally, the synthesized TiO2 is dried at 80°C.

[0061] However, the above-described TiO2 synthesis method is not limited to the above method, and some temperature conditions, time conditions, input raw materials, etc. may be omitted or added.

[0062] As described above, TiO2 can be synthesized by doping Cu onto the prepared TiO2 surface through an impregnation process. The impregnation process refers to infiltrating a liquid into the space of a sintered body, but in metallurgy, it can also mean filling the open pores of a sintered body with oil or fat.

[0063] Here, the TiO2 surface can be irradiated with UV light before the impregnation process. This method of irradiating the TiO2 surface with UV light before the impregnation process has the effect of modifying the hydrophilicity of the TiO2 surface, thereby minimizing the agglomeration of TiO2 particles during the impregnation process. Furthermore, by increasing the Cu doping ratio, efficiency can be enhanced.

[0064] The obtained Rutile TiO2 surface can be doped with Cu by processing it through an impregnation process, and the photocatalyst thus manufactured has high antibacterial and antiviral effects.

[0065] More specifically, Cu(NO3)2 can be mixed with the prepared TiO2. The mixed TiO2 and Cu(NO3)2 can be mixed with water and heated at 50°C to 100°C, preferably 90°C, for 2 hours.

[0066] In another embodiment, Cu(NO3)2 can be mixed with prepared TiO2, and an organic solvent can be poured onto the mixed TiO2 and Cu(NO3)2 to react at 25°C for 2 hours. Here, the organic solvent can be ethanol or methanol.

[0067] In another embodiment, Cu can be doped onto the surface of prepared TiO2 by photodeposition. Here, the photodeposition method refers to a method of depositing metal ions having a redox potential between the band gap energies of the metal oxide by irradiating them with light.

[0068] However, the method of doping Cu on the TiO2 surface described above is not limited to the above method, and some temperature conditions, time conditions, input raw materials, etc. may be omitted or added.

[0069] The Cu doped on the TiO2 surface can be at least one of a Cu salt, a Cu-metal complex, and a Cu oxide. A Cu salt is a general term for a Cu compound formed through an oxidation-reduction reaction, a Cu-metal complex refers to a compound in which Cu and a metal element are combined, and a Cu oxide can refer to, but is not limited to, CuO, CuO2, etc. formed when Cu and oxygen atoms meet.

[0070] FIG. 3a is a drawing for explaining the excitation of a photocatalyst by light according to one embodiment of the present disclosure.

[0071] Referring to Fig. 3a, when irradiated with visible light, Cu doped in TiO2 can receive excited electrons from TiO2 and be converted to Cu(II) → Cu(I).

[0072] Specifically, a photon with energy hv is incident, exciting an electron and generating a hole and an electron. Here, the electron has energy equivalent to the reduction potential between Cu(II) and Cu(I), and the hole is generated in the valence band.

[0073] FIG. 3b is a diagram illustrating the activation of copper oxide according to one embodiment of the present disclosure.

[0074] Referring to Figure 3b, the converted Cu(I) can be reconverted to Cu(II) while transferring electrons to the virus.

[0075] Specifically, the energy corresponding to the electron transfer process is 0.16 V, and holes move on the TiO2 surface.

[0076] FIG. 3c is a diagram illustrating virus inactivation according to one embodiment of the present disclosure.

[0077] Referring to Figure 3c, a virus that has received electrons can be inactivated. The virus or bacteria that has received electrons no longer function properly, rendering them inactive. The above process can be repeated with visible light.

[0078] FIG. 4a is a drawing for explaining a heating impregnation process according to one embodiment of the present disclosure.

[0079] Referring to Fig. 4a, Cu(NO3)2 can be mixed with the prepared TiO2. The mixed TiO2 and Cu(NO3)2 can be mixed with water and heated at 50°C to 100°C, preferably 90°C, for 2 hours.

[0080] FIG. 4b is a drawing illustrating an alcohol-based room temperature impregnation process according to one embodiment of the present disclosure.

[0081] Referring to Fig. 4b, Cu(NO3)2 can be mixed with the prepared TiO2, and an organic solvent can be poured into the mixed TiO2 and Cu(NO3)2 to react at 25°C for 2 hours. Here, the organic solvent can be ethanol or methanol.

[0082] FIG. 4c is a table for explaining the doping efficiency of Cu according to the impregnation process according to one embodiment of the present disclosure.

[0083] Referring to Figure 4c, the heat-impregnation process and the organic solvent-based impregnation process can achieve higher Cu doping ratios compared to the control group. As the Cu doping ratio increases, oxidation-reduction reactions can occur more actively on the surface, further enhancing the virus-neutralizing function.

[0084] FIG. 5a is a drawing showing an SEM image of Rutile TiO2 according to one embodiment of the present disclosure.

[0085] Referring to FIG. 5a, Rutile TiO2 has a rod-shaped shape, and the hydrophobic rod-shaped particles have a property of clumping together to reduce the change in Gibbs Free Energy. To prevent this, Cu can be doped into the rod-shaped Rutile TiO2 using the above-described heating impregnation process and organic solvent impregnation process.

[0086] Here, Gibbs free energy is a concept representing the total amount of energy used or released during a chemical reaction. It is a measure of the energy that can be reversibly or maximally extracted by a system under a given temperature and pressure, and can be used to predict whether a reaction will proceed spontaneously. In nature, reactions occur in a way that causes the change in Gibbs free energy to become zero.

[0087] FIG. 5b is a drawing for explaining the crystal form of Rutile TiO2 according to the area of ​​the (110) plane of TiO2 according to one embodiment of the present disclosure.

[0088] Referring to Fig. 5b, it can be seen that the larger the area of ​​the (110) plane of Rutile TiO2, the larger the ratio of the length of the body to the two ends of the rod. Specifically, when the area of ​​the (110) plane of Rutile TiO2 is larger than the average, it can be expressed as LR (Large aspect ratio) (510), when the area of ​​the (110) plane is the average, it can be expressed as MR (Middle aspect ratio) (520), and when the area of ​​the (110) plane is smaller than the average, it can be expressed as SR (Small aspect ratio) (530).

[0089] The average value of the area of ​​the (110) plane of Rutile TiO2 is experimentally determined, and when the area of ​​the (110) plane of Rutile TiO2 synthesized by the general manufacturing method according to the present disclosure is expressed as a normal distribution, the area of ​​the (110) plane with the largest proportion can be determined as the average value of the area of ​​the (110) plane of Rutile TiO2. Therefore, the average value of the area of ​​the (110) plane of Rutile TiO2 may vary depending on the experimental conditions, such as experimental temperature, time, mixing method, and experimental sequence.

[0090] FIG. 6 is a graph for explaining the antibacterial and antiviral effects according to the area of ​​the (110) plane of TiO2 according to one embodiment of the present disclosure.

[0091] Referring to Figure 6, it can be seen that the antibacterial and antiviral effects of Rutile TiO2, which has a large surface area of ​​the TiO2(110) plane, are the strongest.

[0092] Specifically, it can be seen that Cu / LR doped on the surface of Rutile TiO2 having a larger-than-average area of ​​the (110) plane, Cu / MR doped on the surface of Rutile TiO2 having a larger-than-average area of ​​the (110) plane, and Cu / SR doped on the surface of Rutile TiO2 having a smaller-than-average area of ​​the (110) plane have higher antibacterial and antiviral effects in a shorter time.

[0093] In addition, the larger the area of ​​the (110) plane of Rutile TiO2, the higher the tendency for it to have high antibacterial and antiviral effects in a short period of time.

[0094] That is, when preparing TiO2, Rutile TiO2 having an area of ​​the (110) plane greater than a critical value is obtained, and the obtained Rutile TiO2 is processed through an impregnation process to dope Cu on the surface of the obtained Rutile TiO2, and the photocatalyst thus manufactured has high antibacterial and antiviral effects.

[0095] Although the preferred embodiments of the present disclosure have been illustrated and described above, the present disclosure is not limited to the specific embodiments described above, and various modifications may be made by a person having ordinary skill in the art to which the present disclosure pertains without departing from the gist of the present disclosure as claimed in the claims, and such modifications should not be understood individually from the technical idea or prospect of the present disclosure.

Claims

1. In a method for manufacturing a photocatalyst, Ti precursor is processed by hydrothermal method to produce TiO 2 Steps for preparing; and TiO prepared by the impregnation process 2 A manufacturing method comprising a step of doping Cu on a surface.

2. In paragraph 1, The above doping step is, The above-mentioned TiO 2 In Cu(NO 3 ) 2 a step of mixing; and The above mixed TiO2 and Cu(NO 3 ) 2 A manufacturing method comprising the step of mixing water and heating at 90°C for 2 hours.

3. In paragraph 1, The above doping step is, Cu(NO) on the above prepared TiO2 3 ) 2 a step of mixing; and The above mixed TiO2 and Cu(NO 3 ) 2 A manufacturing method comprising the step of pouring an organic solvent into a solution and reacting it at 25°C for 2 hours.

4. In paragraph 3, The above organic solvent is, A method for producing ethanol or methanol.

5. In paragraph 1, The above doping step is, The above-mentioned TiO 2 A step of irradiating the surface with ultraviolet rays; and TiO irradiated with ultraviolet light on the surface above 2 The TiO prepared above is processed by an impregnation process. 2 A manufacturing method comprising a step of doping Cu on a surface.

6. In paragraph 1, The above TiO 2 The steps to prepare are: (110) Rutile TiO with a surface area greater than a critical value 2 comprising the steps of obtaining; The above doping step is, The above obtained Rutile TiO 2 Rutile TiO obtained by processing through an impregnation process 2 A manufacturing method for doping Cu on the surface.

7. In paragraph 1, The above TiO 2 The steps to prepare are: Ti(OBu) 4 The first step is to stir a solution containing 2 M NaCl in 1 mL at 80°C for 4 hours at 600 rpm; After centrifuging the first stirred mixed solution, wash it with at least one of distilled water or ethanol to obtain TiO 2 Step of obtaining seed; The above obtained TiO 2 A second step of stirring the solution containing 2.5 M HCl mixed with the seed at 600 rpm for 20 minutes; A step of treating the second stirred solution with a hydrothermal synthesis process at 180°C for 72 hours; The second stirred solution, which has undergone the above-mentioned series synthesis process, is centrifuged and washed with at least one of distilled water and ethanol to obtain synthesized TiO. 2 Steps for obtaining; and The above synthesized TiO 2 A manufacturing method comprising a step of drying at 80°C.

8. In paragraph 1, The above doping step is, Cu to TiO by photodeposition method 2 A manufacturing method for doping by depositing on a surface.

9. In paragraph 1, The above TiO 2 Cu doped on the surface, A method for producing at least one of a Cu salt, a Cu-metal complex, and a Cu oxide.

10. In photocatalysis, TiO 2 decision; and The above TiO 2 A photocatalyst comprising Cu doped in one region of the crystal surface.

11. In paragraph 10, The above TiO 2 The decision is, (110) Rutile TiO with a surface area greater than a critical value 2 Photocatalyst.

12. In paragraph 10, The above photocatalyst is, The above TiO 2 A photocatalyst in which the amount of Cu doped on the (110) plane of the crystal is greater than the amount of Cu doped on planes other than the (110) plane.

Citation Information

Patent Citations

  • Cu-doped TiO2 grafted polyacrylonitrile composite antibacterial fibers and preparation method thereof

    CN112481724A

  • Manufacturing method of titanium dioxide nanorod using hydrothermal method and photoelectrode comprising titanium dioxide nanorod prepared therefrom

    KR101724692B1

  • Photocatalytic coating film and method for producing same

    KR1020140027359A