Aromatic polyamide-aromatic polyester copolymer with excellent biodegradability, and preparation method therefor

The aromatic polyamide-aromatic polyester copolymer, synthesized using furan-based dicarboxylic acids and aliphatic diols, addresses the challenge of maintaining mechanical strength and biodegradability, achieving significant biodegradation in seawater and supporting environmental sustainability by using biomass-derived materials.

WO2024205209A1PCT designated stage expired Publication Date: 2024-10-03UNIVERSITY INDUSTRY COOPERATION GROUP OF KYUNG HEE UNIVERSITY +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003807
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional bioplastics face challenges in maintaining mechanical properties like tensile strength while achieving effective biodegradability, particularly in marine environments, where they contribute to environmental pollution and ecological threats such as 'ghost fishing' due to their slow degradation.

Method used

Aromatic polyamide-aromatic polyester copolymers are synthesized by reacting aromatic polyester with aromatic diamine and dicarboxylic acid, using furan-based dicarboxylic acids and aliphatic diols, which are derived from biomass, to create a material with enhanced biodegradability and mechanical strength, specifically designed to degrade more than 30% by weight in seawater within six months and maintain tensile strength of 50 MPa or more.

Benefits of technology

The copolymer exhibits excellent mechanical properties with high tensile strength and rapid biodegradability in seawater, contributing to environmental sustainability and carbon neutrality by using biomass-derived raw materials, while being simple to manufacture and effective in reducing plastic waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003807_03102024_PF_FP_ABST
    Figure KR2024003807_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a biodegradable aromatic polyamide-aromatic polyester copolymer, and a preparation method therefor. The copolymer according to the present invention, can, in particular, attain excellent biodegradability of 30 wt% or higher in seawater within six months, whilst also having excellent mechanical properties of a tensile strength of 50 MPa or higher. Additionally, the biodegradable copolymer of the present invention can be simply and readily prepared and can use a raw material monomer derived from biomass, and thus can contribute to carbon neutrality.
Need to check novelty before this filing date? Find Prior Art

Description

Aromatic polyamide-aromatic polyester copolymer with excellent biodegradability and method for producing the same

[0001] The present invention relates to an aromatic polyamide-aromatic polyester copolymer having satisfactory mechanical properties and excellent biodegradability, and a method for producing the same.

[0002] Plastic has become an indispensable part of modern society. Most products, from furniture and clothing to cell phones and automobiles, are made from plastic. Recently, the rapid increase in packaging and delivery of groceries and food, as well as online shopping, has led to an exponential increase in plastic production and use.

[0003] Accordingly, plastics are hindering the global environment, carbon neutrality, and sustainable growth. The problem of plastic waste, in particular, is becoming increasingly serious, with so much plastic being dumped into the ocean that plastic now accounts for over 80% of marine litter. Polyamide-based nylon fishing nets remain in the wild, creating a phenomenon known as "ghost fishing," posing a threat to marine ecosystems.

[0004] To address the environmental problems caused by waste plastic, biodegradable resins are being developed. Bioplastics are emerging as a solution to the plastic waste issue, and their applications are rapidly expanding beyond disposables and industrial products to include electronics, household goods, and textiles, leading to rapid industrialization. However, these bioplastics face the challenge of maintaining mechanical properties like tensile strength while also struggling to biodegrade.

[0005] The purpose of the present invention is to provide a resin having excellent biodegradability while maintaining mechanical properties and a method for producing the same.

[0006] In order to achieve the above object, according to one aspect of the present invention, a method for producing a biodegradable copolymer of an aromatic polyamide and an aromatic polyester is provided, the method comprising the steps of (a) synthesizing an aromatic polyester, and (b) reacting the synthesized aromatic polyester with an aromatic diamine and an aromatic dicarboxylic acid.

[0007] According to one embodiment, step (a) can be performed by reacting an aromatic dicarboxylic acid with an aliphatic diol.

[0008] According to one embodiment, the step (a) may include heating at a temperature higher than the boiling point of the aliphatic diol and lower than the boiling point of the aromatic dicarboxylic acid.

[0009] According to one embodiment, in step (a), the aliphatic diol may evaporate during the heating to an amount less than 1 stoichiometric equivalent to the aromatic dicarboxylic acid.

[0010] According to one embodiment, the aromatic polyester of steps (a) and (b) may have a carboxylic acid unit at both ends.

[0011] According to one embodiment, the aromatic dicarboxylic acid may be a (5-20) membered heteroaryl compound substituted with two carboxyl groups and containing at least one oxygen atom.

[0012] According to one embodiment, the aromatic dicarboxylic acid used in the synthesis of the aromatic polyamide and the aromatic dicarboxylic acid used in the synthesis of the aromatic polyester may be furan-based dicarboxylic acids.

[0013] According to one embodiment, the aromatic diamine may be an aryl compound having 6 to 20 carbon atoms substituted with two amino groups.

[0014] According to one embodiment, the aliphatic diol may be an alkyl diol having 2 to 12 carbon atoms.

[0015] According to another aspect of the present invention, a biodegradable copolymer of an aromatic polyamide and an aromatic polyester is provided, wherein the ratio of ester functional groups (-COO-) relative to the total polymer weight is 10 wt% or more, and the seawater biodegradability is 30 wt% or more within 6 months.

[0016] According to one embodiment, the biodegradable copolymer may have a tensile strength of 50 MPa or more.

[0017] According to one embodiment, the aromatic polyester may include a unit derived from an aromatic dicarboxylic acid and a unit derived from an aliphatic diol.

[0018] According to one embodiment, the aromatic polyamide may include a unit derived from an aromatic dicarboxylic acid and a unit derived from an aromatic diamine.

[0019] According to one embodiment, the aromatic polyester and the aromatic polyamide may each include a unit derived from a furan-based dicarboxylic acid.

[0020] According to one embodiment, the furan dicarboxylic acid may be at least one selected from 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 2,3-furandicarboxylic acid, and 3,4-furandicarboxylic acid.

[0021] The copolymer according to the present invention exhibits excellent mechanical properties, with a tensile strength of 50 MPa or more, while also exhibiting excellent biodegradability, particularly achieving a seawater biodegradability of 30 wt% or more within 6 months. Furthermore, the biodegradable copolymer of the present invention can be manufactured simply and easily, and because the raw monomers, particularly the aromatic dicarboxylic acid and the aliphatic diol, can be derived from biomass, it can also contribute to carbon neutrality.

[0022] Figure 1 is a schematic diagram of a polymer chemical reaction of Example 1 of the present invention.

[0023] Hereinafter, the present invention will be described in detail.

[0024] The terms used in this specification are used only to describe specific embodiments and are not intended to limit the present invention, and unless otherwise defined, have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs.

[0025] Throughout the specification, when it is said that a part “includes,” “contains,” or “has” a component, this means that it may further include other components, unless specifically stated otherwise.

[0026] According to one aspect of the present invention, a method for producing a biodegradable copolymer of an aromatic polyamide and an aromatic polyester is provided, comprising the steps of (a) synthesizing an aromatic polyester, and (b) reacting the synthesized aromatic polyester with an aromatic diamine and an aromatic dicarboxylic acid.

[0027] According to one embodiment of the present invention, step (a) may be performed by reacting an aromatic dicarboxylic acid with an aliphatic diol. Here, the reaction is an esterification reaction.

[0028] According to one embodiment, step (a) may include a step of heating at a temperature higher than the boiling point of the aliphatic diol and lower than the boiling point of the aromatic dicarboxylic acid. According to one embodiment, step (a) may include a step of heating at a temperature lower than the boiling point of the aliphatic diol and the aromatic dicarboxylic acid to cause an esterification reaction, and a subsequent step of heating at a temperature higher than the boiling point of the aliphatic diol and lower than the boiling point of the aromatic dicarboxylic acid to cause an esterification reaction. In step (a), the aliphatic diol may evaporate during heating at a temperature higher than the boiling point to become an amount less than 1 stoichiometric equivalent with respect to the aromatic dicarboxylic acid. In addition, accordingly, the aromatic polyester of step (a) and step (b) described below may have a carboxylic acid unit at both terminals.

[0029] The aliphatic diol and the aromatic dicarboxylic acid may be used in the same molar amount, or the aliphatic diol may be used in an amount of 0.8 to 1.5 stoichiometric equivalents relative to the aromatic dicarboxylic acid. However, even if the aliphatic diol is used in the same molar amount or a greater amount than the aromatic dicarboxylic acid, it is preferable to heat the mixture to a temperature higher than the boiling point of the aliphatic diol and lower than the boiling point of the aromatic dicarboxylic acid during the reaction of the aromatic dicarboxylic acid, thereby evaporating the aliphatic diol and causing the amount to become stoichiometrically smaller relative to the aromatic dicarboxylic acid during the reaction. As the amount of the aliphatic diol decreases in this way, some of the aliphatic diol participates in the reaction and some of it evaporates, thereby causing a stoichiometric shortage of alcohol functional groups, which can naturally allow both ends of the polyester to become carboxylic acids.

[0030] The above aromatic dicarboxylic acid may be an aromatic aryl or heteroaryl compound substituted with two carboxyl groups, specifically a (5-20) membered heteroaryl compound substituted with two carboxyl groups and containing at least one, for example, one or two, oxygen atoms. More specifically, the above aromatic dicarboxylic acid may be a dicarboxylic acid of a compound selected from the group consisting of benzene, naphthalene, phenylbenzene, furan, oxazole, isoxazole, benzofuran, isobenzofuran, dibenzofuran, benzoxazole, and benzoisoxazole. In one embodiment, the above aromatic dicarboxylic acid may be a furan-based dicarboxylic acid. Examples of the furan-based dicarboxylic acid include 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 2,3-furandicarboxylic acid, and 3,4-furandicarboxylic acid. By using an aromatic dicarboxylic acid in this way, compared to the case where an aliphatic dicarboxylic acid is used, the final copolymer can include more curved or folded structures rather than plain structures, and accordingly, more ester functional groups related to biodegradability can be exposed outside the copolymer structure, so that a copolymer having excellent biodegradability while maintaining mechanical properties can be produced. According to one embodiment, the aromatic dicarboxylic acid may be derived from biomass.

[0031] The above aliphatic diol may be an alkyl diol having 2 to 12 carbon atoms, specifically a straight-chain or branched-chain alkyl diol having 2 to 12 carbon atoms, for example, a straight-chain alkyl diol having 2 to 10 carbon atoms. Examples of the above aliphatic diol include, but are not particularly limited to, one or more selected from ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,4-dimethyl-2-ethyl-1,3-hexanediol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, and 2,2,4-trimethyl-1,6-hexanediol. In one embodiment, the above aliphatic diol may be derived from biomass.

[0032] During the above step (a), if necessary, a catalyst may be further added to promote the reaction between the aliphatic diol and the aromatic dicarboxylic acid. The catalyst is not particularly limited as long as it does not impede the effects of the present invention, but may include metal catalysts, for example, titanium compounds such as titanium methoxide, titanium propoxide, titanium butoxide, titanium chloride, and titanium oxide.

[0033] The above step (b) is a step of reacting the aromatic polyester synthesized in the above step (a) with an aromatic diamine and an aromatic dicarboxylic acid. Here, the reaction is an amide polymerization reaction. By first synthesizing the aromatic polyester in step (a) and then copolymerizing it while synthesizing the polyamide in step (b), a copolymer having excellent tensile strength and biodegradability can be produced.

[0034] The aromatic diamine and the aromatic dicarboxylic acid may each be independently used in a molar amount of 0.7 to 11 times, specifically 0.7 to 10 times, 0.8 to 9 times, 0.8 to 7 times, 0.9 to 5 times, 0.9 to 4 times, or 1 to 3 times, relative to the aromatic polyester. Since the polyester has an ester functional group related to biodegradability and the polyamide has a greater influence on mechanical properties such as tensile strength, by setting the amounts of the aromatic diamine and the aromatic dicarboxylic acid within the above range, a copolymer having excellent biodegradability while maintaining mechanical properties can be produced. As the amount of the aromatic diamine and the aromatic dicarboxylic acid in the polyester decreases, mechanical properties such as tensile strength may decrease and biodegradability may become excellent.

[0035] In the step (b), the aromatic dicarboxylic acid may be an aromatic aryl or heteroaryl compound substituted with two carboxyl groups, specifically, a (5-20) membered heteroaryl compound substituted with two carboxyl groups and containing at least one, for example, one or two, oxygen atoms. In one embodiment, the aromatic dicarboxylic acid may be a furanic dicarboxylic acid. For a specific description of the aromatic dicarboxylic acid, reference may be made to the description of the aromatic dicarboxylic acid in step (a). In one embodiment, both the aromatic dicarboxylic acids in steps (a) and (b) may be furanic dicarboxylic acids. In one embodiment, the aromatic dicarboxylic acid may be derived from biomass.

[0036] In the step (b), the aromatic diamine may be an aryl compound having 6 to 20 carbon atoms substituted with two amino groups. The aromatic diamine is not particularly limited as long as it can be a polyamide and form a copolymer with the polyester and does not impair the effects of the present invention, and examples thereof include p-phenylenediamine, m-phenylenediamine, 2,4-toluenediamine, m-xylylenediamine, p-xylylenediamine, 1,5-diaminonaphthalene, and 2,6-diaminonaphthalene. According to one embodiment, the aromatic diamine may be derived from biomass.

[0037] In the above step (b), the reaction temperature may be, for example, in the range of 100 to 180°C, but is not limited thereto and can be appropriately controlled by a person skilled in the art. In the above step (b), if necessary, a catalyst and / or stabilizer may be further added to promote the reaction. The catalyst is not particularly limited as long as it does not inhibit the effects of the present invention, but a metal catalyst, for example, a lithium compound such as lithium propoxy, lithium chloride, lithium acetate, lithium octylate, or lithium oxide, may be used. The stabilizer is not particularly limited as long as it does not inhibit the effects of the present invention, but a pyridine-based compound or a phosphite-based compound may be used.

[0038] According to another aspect of the present invention, a biodegradable copolymer of an aromatic polyamide and an aromatic polyester is provided, wherein the ratio of ester functional groups (-COO-) relative to the total polymer weight is 10 wt% or more, and the seawater biodegradability is 30 wt% or more within 6 months.

[0039] According to one embodiment, the aromatic polyester may include units derived from an aromatic dicarboxylic acid and units derived from an aliphatic diol. Furthermore, according to one embodiment, the aromatic polyamide may include units derived from an aromatic dicarboxylic acid and units derived from an aromatic diamine. Here, specific descriptions of the aromatic dicarboxylic acid, aliphatic diol, and aromatic diamine may refer to the contents described above in relation to the manufacturing method. According to one embodiment, the biodegradable copolymer of the present invention may be a random copolymer.

[0040] According to the present invention, by manufacturing a copolymer using an aromatic monomer such as an aromatic dicarboxylic acid as described above, a more curved or folded structure can be formed compared to the case where an aliphatic compound is used, so that the ester functional group can be more exposed, and thus the biodegradability, such as seawater biodegradability, is superior compared to other copolymers having a similar ratio of ester functional groups to the total polymer weight. In addition, accordingly, the present invention can exhibit improved biodegradability even without using less units for reinforcing mechanical properties, such as polyamide, to improve biodegradability, so that mechanical properties, such as tensile strength, can also be maintained excellently. According to one embodiment of the present invention, the biodegradable copolymer of the present invention may have a tensile strength of 50 MPa or more.

[0041] According to another aspect of the present invention, packaging materials, packaging containers, vinyls, masks, clothing such as medical gowns, gloves such as medical gloves, etc., comprising a biodegradable copolymer of the above-described aromatic polyamide and aromatic polyester can be provided.

[0042] Hereinafter, the present invention will be described in more detail with reference to examples to aid understanding. However, the following examples are provided solely to facilitate understanding of the present invention and are not intended to limit the scope of the present invention.

[0043]

[0044] [Example 1]

[0045] In the first polymerization step (ester first), 2,5-furandicarboxylic acid (FDCA) (156.09 g, 1.0 mol) and 1,4-butanediol (90.12 g, 1.0 mol) were charged into a reactor and heated and stirred at 100°C to form a homogeneous phase. The temperature was then raised to 150°C, and titanium (IV) butoxide (0.140 g, 0.42 mmol) was added to the reactor. The reaction mixture was heated at 180°C for 2 hours and then at 230°C for 2 hours to induce an esterification reaction. Some of the 1,4-butanediol participated in the reaction, and some was evaporated, so that the alcohol functional group became insufficient stoichiometrically, and a polyester with both terminals naturally formed as carboxylic acids was produced. Through NMR analysis, it was confirmed that the number-average molecular weight of the furan-based polyester manufactured in step 1 was 1000 g / mol.

[0046] Next, in the second polymerization step, the product of the first polymerization step (10.0 g, 0.01 mol), FDCA (1.56 g, 0.01 mol), and 1,4-phenylenediamine (2.16 g, 0.02 mol) were added to N-methyl-2-pyrrolidinone (57 mL; 25 wt% per monomer weight), and lithium chloride (5.7 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. Amide-polymerization was performed at 130°C in a nitrogen environment for 6 hours to produce furan-based aromatic polyamide and furan-based polyester copolymer. The theoretical weight content of ester (COO) functional groups was calculated to be 26.4% of the total polymer weight.

[0047]

[0048] [Example 2]

[0049] A furan-based polyester having a number-average molecular weight of 1000 g / mol was produced by performing polymerization step 1 in the same manner as in Example 1.

[0050] Next, in the second polymerization step, the product of the first polymerization step (10.0 g, 0.01 mol), FDCA (4.68 g, 0.03 mol), and 1,4-phenylenediamine (4.32 g, 0.04 mol) were added to N-methyl-2-pyrrolidinone (76 mL; 25 wt% per monomer weight), and lithium chloride (7.6 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. Amide-polymerization was performed at 130°C in a nitrogen environment for 6 hours to prepare furan-based aromatic polyamide and furan-based polyester copolymer. The theoretical weight content of ester (COO) functional groups was calculated to be 19.7% of the total polymer weight.

[0051]

[0052] [Example 3]

[0053] A furan-based polyester having a number-average molecular weight of 1000 g / mol was produced by performing polymerization step 1 in the same manner as in Example 1.

[0054] Next, in the second polymerization step, the product of the first polymerization step (10.0 g, 0.01 mol), FDCA (14.05 g, 0.09 mol), and 1,4-phenylenediamine (10.8 g, 0.10 mol) were added to N-methyl-2-pyrrolidinone (135 mL; 25 wt% per monomer weight), and lithium chloride (13.5 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. Amide-polymerization was performed at 130°C in a nitrogen environment for 6 hours to produce furan-based aromatic polyamide and furan-based polyester copolymer. The theoretical weight content of ester (COO) functional groups was calculated to be 11.1% based on the total polymer weight.

[0055]

[0056] [Comparative Example 1]

[0057] In Example 1, terephthalic acid (TPA) was used instead of FDCA.

[0058] In the first polymerization step (ester first), TPA (166.13 g, 1.0 mol) and 1,4-butanediol (90.12 g, 1.0 mol) were charged into a reactor and heated and stirred at 100°C to form a homogeneous phase. The temperature was then raised to 150°C, and titanium (IV) butoxide (0.140 g, 0.42 mmol) was added to the reactor. The reaction mixture was heated at 180°C for 2 hours and then at 230°C for 2 hours to induce an esterification reaction. Some of the 1,4-butanediol participated in the reaction, and some was evaporated, so that the alcohol functional group became insufficient stoichiometrically, and a polyester in which both terminals were naturally converted to carboxylic acids was produced. The number-average molecular weight of the aromatic polyester produced in the first step was confirmed to be 1050 g / mol through NMR analysis.

[0059] Next, in the second polymerization step, the product of the first polymerization step (10.5 g, 0.01 mol), TPA (1.66 g, 0.01 mol), and 1,4-phenylenediamine (2.16 g, 0.02 mol) were added to N-methyl-2-pyrrolidinone (57 mL; 25 wt% per monomer weight), and lithium chloride (5.7 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. The aromatic polyamide and aromatic polyester copolymer were manufactured by amide-polymerization at 130°C for 6 hours in a nitrogen environment. The theoretical weight content of ester (COO) functional groups was calculated to be 25.2% based on the total polymer weight.

[0060]

[0061] [Comparative Example 2]

[0062] Only amide-polymerization was performed to ensure that no ester functional group existed.

[0063] FDCA (15.61 g, 0.1 mol), 1,4-phenylenediamine (10.8 g, 0.1 mol) were added to N-methyl-2-pyrrolidinone (105 mL; 25 wt% per monomer weight), and lithium chloride (10.5 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. The furan-based aromatic polyamide was prepared by amide-polymerization at 130°C for 6 h in a nitrogen atmosphere. The theoretical weight content of ester (COO) functional groups was calculated to be 0% based on the total polymer weight.

[0064]

[0065] [Comparative Example 3]

[0066] Instead of conducting the polymerization in two stages as in Example 1,

[0067] FDCA (9.36 g, 0.06 mol), 1,4-butanediol (4.51 g, 0.05 mol), and 1,4-phenylenediamine (2.16 g, 0.02 mol) were added to N-methyl-2-pyrrolidinone (64 mL; 25 wt% per monomer weight), and lithium chloride (6.4 g), pyridine (40 mL), and triphenylphosphite (15.5 g, 0.05 mol) were added as reaction additives. Polymerization was performed at 130°C in a nitrogen atmosphere for 6 h to produce furan-based aromatic polyamides and furan-based polyester copolymers. The theoretical weight content of ester (COO) functional groups was calculated to be 26.4% of the total polymer weight.

[0068]

[0069] [Evaluation example]

[0070] Tensile strength and biodegradability were measured using the copolymers prepared in Examples 1 to 3 and Comparative Examples 1 to 3 according to the following evaluation methods. The results are shown in [Table 1] below.

[0071]

[0072] <Evaluation Method>

[0073] (1) Tensile strength: Measurements were conducted using an Intstron 5943 device in accordance with ASTM D638-Type V. A 500 N load cell was used, and measurements were made at a temperature of 25°C with a crosshead speed of 100 mm / min. The average value was obtained from five measurements.

[0074] (2) Seawater biodegradability test: The seawater biodegradability test was conducted in a stabilized artificial seawater tank (70 X 35 X 35 cm) in which four adult clownfish lived. 3 ) was performed. 20 X 60 X 0.5 mm 3 The specimens of the same size were placed in the fish tank, and after 6 months, the specimens were recovered, washed thoroughly, completely dried, and weighed. The decomposition rate was calculated by multiplying (initial weight - weight after decomposition) / initial weight X 100.

[0075] Manufacturing methodDicarboxylic acid monomeresterFunctional groupWeight contentTensile strengthSeawater biodegradability (6 months, weight loss rate)Example 1Ester firstFDCA26.4%56 MPa51%Example 2Ester firstFDCA19.7%59 MPa42%Example 3Ester firstFDCA11.1%72 MPa33%Comparative example 1Ester firstTPA25.2%63 MPa3%Comparative example 2Ester firstFDCA0%73 MPa1%Comparative example 3All togetherFDCA26.4%Not measurableNot measurable

[0076] As can be seen in Table 1 above, when furan-based aromatic polyamide and furan-based polyester copolymers were manufactured using FDCA derived from biomass in the manner presented in Examples 1 to 3, a high tensile strength of 50 MPa or more was observed, whereas in the case of Comparative Example 3, in which all monomers were polymerized at once, the tensile strength could not be measured due to the low molecular weight.

[0077] It was confirmed that the seawater biodegradability through hydrolysis and microbial activity was higher than expected when the weight content of the ester functional group was 10% or more and the direction of the bent chemical bond of the furan monomer effectively lowered the crystallinity. On the other hand, it was confirmed through Comparative Example 1 that when TPA, not FDCA, was used, biodegradation hardly progressed due to the rigid structure.

[0078] In addition, the polyamide polymer of Comparative Example 2 having an ester functional group weight content of 10% or less had very low seawater biodegradability.

[0079]

[0080] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various modifications and changes may be made to the present invention without departing from the spirit and scope of the present invention as set forth in the claims below.

Claims

1. (a) a step of synthesizing an aromatic polyester, and (b) a step of reacting the above-mentioned synthesized aromatic polyester with an aromatic diamine and an aromatic dicarboxylic acid, A method for producing a biodegradable copolymer of an aromatic polyamide and an aromatic polyester.

2. In paragraph 1, A manufacturing method in which the above step (a) is performed by reacting an aromatic dicarboxylic acid and an aliphatic diol.

3. In paragraph 2, A manufacturing method, wherein the step (a) comprises a step of heating at a temperature higher than the boiling point of the aliphatic diol and lower than the boiling point of the aromatic dicarboxylic acid.

4. In paragraph 3, A manufacturing method wherein, in the step (a), the aliphatic diol evaporates during the heating to an amount less than 1 stoichiometric equivalent with respect to the aromatic dicarboxylic acid.

5. In paragraph 1, A manufacturing method wherein the aromatic polyester of steps (a) and (b) above has a carboxylic acid unit at both ends.

6. In paragraph 1 or 2, A method for producing the above aromatic dicarboxylic acid, wherein the above aromatic dicarboxylic acid is a (5-20) membered heteroaryl compound substituted with two carboxyl groups and containing at least one oxygen atom.

7. In paragraph 2, A manufacturing method wherein the aromatic dicarboxylic acid used in the synthesis of the above aromatic polyamide and the aromatic dicarboxylic acid used in the synthesis of the above aromatic polyester are furan-based dicarboxylic acids.

8. In paragraph 1, A manufacturing method wherein the above aromatic diamine is an aryl compound having 6 to 20 carbon atoms substituted with two amino groups.

9. In paragraph 2, A manufacturing method wherein the above aliphatic diol is an alkyl diol having 2 to 12 carbon atoms.

10. A biodegradable copolymer of an aromatic polyamide and an aromatic polyester, having a ratio of ester functional groups (-COO-) of 10 wt% or more relative to the total polymer weight and a seawater biodegradability of 30 wt% or more within 6 months.

11. In paragraph 10, A biodegradable copolymer having a tensile strength of 50 MPa or more.

12. In paragraph 10, The above aromatic polyester is a biodegradable copolymer comprising a unit derived from an aromatic dicarboxylic acid and a unit derived from an aliphatic diol.

13. In paragraph 10, The above aromatic polyamide is a biodegradable copolymer comprising a unit derived from an aromatic dicarboxylic acid and a unit derived from an aromatic diamine.

14. In paragraph 10, The above aromatic polyester and the above aromatic polyamide are each biodegradable copolymers containing units derived from furan-based dicarboxylic acids.

15. In paragraph 14, A biodegradable copolymer, wherein the above furan-based dicarboxylic acid is at least one selected from 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 2,3-furandicarboxylic acid, and 3,4-furandicarboxylic acid.

Citation Information

Patent Citations

  • Method for producing polyester amide

    JP2016210845A

  • Polyester-amide and method for preparing the same

    KR101813395B1

  • Polyamide, polyester and polyether block copolymer

    KR1020090086024A

  • Learning device for learning convergence education and education method using the same

    KR1020240141221A

  • Aromatic Polyamide-Aromatic Polyester Copolymer Having Good Biodegradability and Method for Preparing the Same

    KR102583184B1