Cement KILN dust (CKD)-based and lime KILN dust (LKD)-based cementitious materials, concrete, and related techniques

Treating CKD and LKD with PVA powder and combining them with perlite and a polycarboxylate material creates a cementitious mixture for concrete production, addressing waste disposal and enhancing durability, resulting in an economically and environmentally friendly concrete production method.

WO2024205584A1PCT designated stage expired Publication Date: 2024-10-03GREEN CEMENT INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2023/016792
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Cement kiln dust (CKD) and lime kiln dust (LKD), byproducts of cement and quick lime manufacturing, are typically disposed of in landfills due to lack of effective utilization, posing environmental concerns and waste management issues.

Method used

A method involving the treatment of CKD and LKD with polyvinyl alcohol (PVA) powder, combined with perlite and a polycarboxylate material, to create a cementitious mixture that can be used to produce concrete, reducing waste disposal and enhancing durability with up to 50% Ordinary Portland Cement (OPC) replacement.

Benefits of technology

The method provides a more economical and environmentally friendly way to produce durable concrete, utilizing waste materials and achieving strength gains equivalent to natural pozzolan materials, thus addressing waste disposal and sustainability in concrete production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000010_0001
    Figure IMGF000010_0001
  • Figure IMGF000010_0002
    Figure IMGF000010_0002
  • Figure IMGF000010_0003
    Figure IMGF000010_0003
Patent Text Reader

Abstract

Cement kiln dust (CKD)-based and lime kiln dust (LKD)-based cementitious materials, concrete, and related techniques are disclosed. In accordance with some embodiments, a cementitious material may be produced by intergrinding (1) at least one of CKD which has been pre-treated with polyvinyl alcohol (PVA) powder and LKD which has been pre-treated with PVA powder, (2) raw perlite ore, and (3) a polycarboxylate material. In accordance with some embodiments, expanded perlite wastes also may be included in the cementitious material. In at least some cases, the cementitious material may be provided as an all-in-one powder blend. In accordance with some embodiments, concrete may be produced by mixing the cementitious material with ordinary Portland cement (OPC), water, and at least one of sand and rock.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CEMENT KILN DUST (CKD)-BASED AND LIME KILN DUST (LKD)- BASED CEMENTITIOUS MATERIALS, CONCRETE, AND RELATED

[0002] TECHNIQUES

[0003] FIELD OF THE DISCLOSURE

[0004] The present disclosure relates to cementitious materials and, more particularly, to cement kiln dust (CKD)-based and lime kiln dust (LKD)-based cementitious materials, concrete, and techniques.

[0005] BACKGROUND

[0006] Cement kiln dust (CKD) is a waste byproduct of making ordinary Portland cement (OPC). Generally, CKD is a fine-grained, highly alkaline solid waste removed from cement kiln exhaust gas by air pollution control devices. Lime kiln dust (LKD) is a waste byproduct of the quick lime manufacturing process. Generally, LKD is a powder residue that collects near the bottom of the kiln stream while calcining limestone. Both CKD and LKD currently are classified as non-hazardous, solid industrial wastes, and much of the CKD and LKD produced annually in the U.S. is disposed of in land-based disposal sites, such as landfills, waste piles, and surface impoundments.

[0007] SUMMARY

[0008] One example embodiment provides a method. The method includes producing a cementitious mixture. The cementitious mixture includes: (a) at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; (b) perlite; and (c) a poly carboxylate material.

[0009] In some cases, the cementitious mixture includes CKD treated with PVA powder but not LKD treated with PVA powder. In some instances, the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm. In some such instances, the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm. In some instances, the CKD treated with PVA powder has a pH of about 11.5 ± 0.5. In some instances, the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5-6.0%. In some instances, the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture. In some cases, the cementitious mixture includes LKD treated with PVA powder but not CKD treated with PVA powder. In some instances, the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture.

[0010] In some cases, the cementitious mixture includes both CKD treated with PVA powder and LKD treated with PVA powder.

[0011] In some cases, the perlite includes raw perlite ore. In some instances, the raw perlite ore has a D90 particle size distribution in the range of about 30-40 pm. In some such instances, the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm. In some instances, the raw perlite ore constitutes about 15-90 wt% of the cementitious mixture produced. In some instances, the raw perlite ore constitutes about 90-99 wt% of the cementitious mixture produced. In some instances, the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite. In some such instances, in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has been washed with water. In some further such instances, in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%. In some instances, the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

[0012] In some cases, producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, and the polycarboxylate material. In some instances, the intergrinding is performed until a D90 particle size distribution of about 25-45 pm is achieved for the cementitious mixture. In some such instances, the intergrinding is performed until a D90 particle size distribution of about 38 pm ± 3 pm is achieved for the cementitious mixture. In some further such instances, the intergrinding is performed until a D90 particle size distribution of about 28 pm ± 3 pm is achieved for the cementitious mixture.

[0013] In some cases, the cementitious mixture further includes expanded perlite waste. In some instances, producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, the polycarboxylate material, and the expanded perlite waste. In some instances, the expanded perlite waste has a D90 particle size distribution in the range of about 30-42 pm. In some such instances, the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm. In some instances, the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture. In some such instances, the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture. In some cases, a method is provided. The method includes producing a concrete including: (a) the aforementioned cementitious mixture; (b) ordinary Portland cement (OPC); (c) water; and (d) at least one of rock and sand. In some instances, a concrete product including the aforementioned concrete is provided.

[0014] Anothed example embodiment provides a cementitious mixture. The cementitious mixture includes: (a) at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; (b) perlite; and (c) a poly carboxylate material.

[0015] In some cases, the cementitious mixture includes CKD treated with PVA powder but not LKD treated with PVA powder. In some instances, the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm. In some such instances, the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm. In some instances, the CKD treated with PVA powder has a pH of about 11.5 ± 0.5. In some instances, the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5-6.0%. In some instances, the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture.

[0016] In some cases, the cementitious mixture includes LKD treated with PVA powder but not CKD treated with PVA powder. In some instances, the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture.

[0017] In some cases, the cementitious mixture includes both CKD treated with PVA powder and LKD treated with PVA powder.

[0018] In some cases, the perlite includes raw perlite ore. In some instances, the raw perlite ore has a D90 particle size distribution in the range of about 30-40 pm. In some such instances, the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm. In some instances, the raw perlite ore constitutes about 15-90 wt% of the cementitious mixture. In some instances, the raw perlite ore constitutes about 90-99 wt% of the cementitious mixture. In some instances, the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite. In some such instances, in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%. In some instances, the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

[0019] In some cases, the cementitious mixture has a D90 particle size distribution in the range of about 25-45 pm. In some instances, the cementitious mixture has a D90 particle size distribution of about 38 pm ± 3 pm. In some instances, the cementitious mixture has a D90 particle size distribution of about 28 pm ± 3 pm.

[0020] In some cases, the cementitious mixture further includes expanded perlite waste. In some instances, the expanded perlite waste has a D90 particle size distribution in the range of about 30-42 pm. In some such instances, the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm. In some instances, the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture. In some such instances, the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture.

[0021] In some cases, concrete is provided. The concrete includes: (a) the aforementioned cementitious mixture; (b) ordinary Portland cement (OPC); (c) water; and (d) at least one of rock and sand. In some instances, a concrete product including the aforementioned concrete is provided.

[0022] The features and advantages described herein are not all-inclusive and, in particular, many additional features and advantages will be apparent to one of ordinary skill in the art in view of the drawings, specification, and claims. Moreover, it should be noted that the language used in the specification has been selected principally for readability and instructional purposes and not to limit the scope of the inventive subject matter.

[0023] BRIEF DESCRIPTION OF THE DRAWINGS

[0024] FIG. 1 illustrates a method of making a cementitious material in accordance with an embodiment of the present disclosure.

[0025] FIG. 2 is a graph illustrating X-ray powder diffraction (XRD) results of a CKD sample suitable for use in the method of FIG. 1, in accordance with an embodiment of the present disclosure.

[0026] FIG. 3 is a graph illustrating XRD results of a raw perlite ore sample suitable for use in the method of FIG. 1, in accordance with an embodiment of the present disclosure.

[0027] FIG. 4 illustrates a method of making concrete in accordance with an embodiment of the present disclosure.

[0028] These and other features of the present embodiments will be understood better by reading the following detailed description, taken together with the figures herein described. The accompanying drawings are not intended to be drawn to scale. In the drawings, each identical or nearly identical component that is illustrated in various figures may be represented by a like numeral. For purposes of clarity, not every component may be labeled in every drawing. DETAILED DESCRIPTION

[0029] Cement kiln dust (CKD)-based and lime kiln dust (LKD)-based cementitious materials, concrete, and related techniques are disclosed. In accordance with some embodiments, a cementitious material may be produced by intergrinding (1) at least one of CKD which has been pre-treated with polyvinyl alcohol (PVA) powder and LKD which has been pre-treated with PVA powder, (2) raw perlite ore, and (3) a polycarboxylate material. In accordance with some embodiments, expanded perlite wastes also may be included in the cementitious material. In at least some cases, the cementitious material may be provided as an all-in-one powder blend. In accordance with some embodiments, concrete may be produced by mixing the cementitious material with ordinary Portland cement (OPC), water, and at least one of sand and rock. Numerous configurations and variations will be apparent in light of this disclosure.

[0030] General Overview

[0031] In accordance with some embodiments of the present disclosure, cement kiln dust (CKD)-based and lime kiln dust (LKD)-based cementitious materials, concrete, and related techniques are disclosed. In accordance with some embodiments, a cementitious material may be produced by intergrinding (1) at least one of CKD which has been pre-treated with polyvinyl alcohol (PVA) powder and LKD which has been pre-treated with PVA powder, (2) raw perlite ore, and (3) a polycarboxylate material. In accordance with some embodiments, expanded perlite wastes also may be included in the cementitious material. In at least some cases, the cementitious material may be provided as an all-in-one powder blend. In accordance with some embodiments, concrete may be produced by mixing the cementitious material with OPC, water, and at least one of sand and rock.

[0032] As will be appreciated in light of this disclosure, techniques disclosed herein may provide, at least in some instances, a more economical way to make concrete using familiar curing times and to make the concrete more durable with up to about a 50% OPC replacement factor while utilizing wastes generated from cement production in an environmentally conscientious (“green”) manner, in accordance with some embodiments. As will be further appreciated in light of this disclosure, techniques disclosed herein may be utilized, in accordance with some embodiments, in any of a wide range of contexts and applications, including, for example, horticulture, insulation, fills, ceiling tiles, and mortars, among others. Cementitious Material

[0033] FIG. 1 illustrates a method 1000 of making a cementitious material in accordance with an embodiment of the present disclosure. As can be seen, method 1000 may include, as in block 1002, adding cement kiln dust (CKD) which has been pre-treated with polyvinyl alcohol (PVA) powder. As will be appreciated in light of this disclosure, the PVA-treated CKD may be sourced as desired for a given target application or end-use. In accordance with some embodiments, the PVA-treated CKD may be (or otherwise may include) PVA-treated CKD available from Martin Marietta Materials, Inc. In accordance with some embodiments, the PVA-treated CKD may be (or otherwise may include) PVA-treated CKD available from Buzzi Unicem Prior Oklahoma CKD (“MUSTANG”). As will be further appreciated in light of this disclosure, the presence of PVA may help to slow water absorption on the CKD, thereby slowing the overall hydroscopic reaction in method 1000.

[0034] In accordance with some embodiments, the PVA-treated CKD may have been ground down to a given target particle size distribution (PSD) prior to being added at block 1002. For example, in some instances, the PVA-treated CKD may have been ground down to a D90 PSD in the range of about 30-60 pm (e.g., about 30-35 pm, about 35-40 pm, about 40- 45 pm, about 45-50 pm, about 50-55 pm, about 55-60 pm, or any other sub-range in the range of about 30-60 pm). In some cases, the PVA-treated CKD may have been ground down to a D90 PSD of about 45 pm (± 3 pm).

[0035] In at least some instances, it may be desirable to utilize PVA-treated CKD having a relatively high pH in the range of about 11.5 (± 0.5). In at least some instances, it may be desirable to utilize PVA-treated CKD having a relatively high aluminum / calcium mineral ratio, such as, for example, in the range of about 3.5-6.0% (e.g., about 3.5-4.0%, about 4.0- 4.5%, about 4.5-5.0%, about 5.0-5.5%, about 5.5-6.0%, or any other sub-range in the range of about 3.5-6.0%). For example, consider FIG. 2, which is a graph illustrating X-ray powder diffraction (XRD) results of a PVA-treated CKD sample suitable for use in method 1000, in accordance with an embodiment of the present disclosure.

[0036] The amount of PVA-treated CKD added may be customized, as desired for a given target application or end-use. For instance, in accordance with some embodiments, the PVA- treated CKD may constitute about 5-30 wt% (e.g., about 5-10 wt%, about 10-15 wt%, about 15-20 wt%, about 20-25 wt%, about 25-30 wt%, or any other sub-range in the range of about 5-30 wt%) of a given mixture produced according to method 1000). As will be appreciated in light of this disclosure, the amount of PVA-treated CKD present may depend, at least in part, on the particular chemistry of the CKD utilized. Other suitable types, characteristics, and quantities of PVA-treated CKD will be apparent in light of this disclosure.

[0037] It should be noted, however, that the present disclosure is not intended to be limited only to the use of PVA-treated CKD. For example, in accordance with some other embodiments, PVA-treated lime kiln dust (LKD) additionally (or alternatively) may be utilized. The PVA-treated LKD may be sourced as desired for a given target application or end-use.

[0038] The amount of PVA-treated LKD added may be customized, as desired for a given target application or end-use. For instance, in accordance with some embodiments, the PVA- treated LKD may constitute about 3-20 wt% (e.g., about 3-5 wt%, about 5-10 wt%, about 10-15 wt%, about 15-20 wt%, or any other sub-range in the range of about 3-20 wt%) of a given mixture produced according to method 1000. Other suitable types and quantities of PVA-treated LKD will be apparent in light of this disclosure.

[0039] Method 1000 may include, as in block 1004, adding raw perlite ore. As will be appreciated in light of this disclosure, the raw perlite ore may be sourced as desired for a given target application or end-use. In accordance with some embodiments, the raw perlite ore may be (or otherwise may include) perlite available from Imerys USA, Inc. In accordance with some embodiments, the raw perlite ore may be (or otherwise may include) DICAPERL® perlite available from Dicalite Management Group. In at least some instances, it may be desirable to utilize raw perlite ore having an amorphous glass content which has a silicates content of at least about 70% (e.g., about 75% or more, about 80% or more, about 85% or more, about 90% or more, or any other sub-range in the range of about 70% or more). For example, consider FIG. 3, which is a graph illustrating XRD results of a raw perlite ore sample suitable for use in method 1000, in accordance with an embodiment of the present disclosure.

[0040] As will be appreciated in light of this disclosure, clay contamination may interfere with strengthening of cement. For instance, a clay contamination in the range of about 6- 12% may interfere with cement strengthening, resulting in sub-grade 80 slag performance. As such, it may be desirable, at least in some instances, to have the perlite ore undergo one or more processes to remove clay and / or other contaminant(s) which might be present. For example, in accordance with some embodiments, the perlite ore may undergo one or more suitable cleaning processes (e.g., washing with water or other suitable cleaning agent) to remove most (or substantially all) of any montmorillonite clay and / or bentonite that might be present. In at least some instances, it may be desirable to treat the perlite ore in this manner before introduction thereof to method 1000. In some instances, the resultant treated raw perlite ore may have a clay contamination of less than about 6% (e.g., about 5% or less, about 4% or less, about 3% or less, about 2% or less, about 1% or less, about 0.5% or less, about 0.1% or less, about 0%, or any other sub-range in the range of about 6% or less). In some instances, the resultant treated raw perlite ore may have substantially no (or otherwise negligible) clay contamination.

[0041] In accordance with some embodiments, the raw perlite ore may have been ground down to a given target PSD prior to being added at block 1004. For example, in some instances, the raw perlite ore may have been ground down to a D90 PSD in the range of about 30-42 pm (e.g., about 30-32 pm, about 32-34 pm, about 34-36 pm, about 36-38 pm, about 38-40 pm, about 40-42 pm, or any other sub-range in the range of about 30-42 pm). In some cases, the raw perlite ore may have been ground down to a D90 PSD of about 38 pm (± 3 pm).

[0042] The amount of raw perlite ore added may be customized, as desired for a given target application or end-use. In accordance with some embodiments, the raw perlite ore may constitute about 15-90 wt% (e.g., about 15-30 wt%, about 30-45 wt%, about 45-60 wt%, about 60-75 wt%, about 75-90 wt%, or any other sub-range in the range of about 15- 90 wt%) of a given mixture produced according to method 1000. In some cases, the raw perlite ore may constitute about 90-99 wt% (e.g., about 90-95 wt%, about 95-99 wt%, or any other sub-range in the range of about 90-99 wt%) of a given mixture produced according to method 1000. Other suitable types, characteristics, and quantities of perlite will be apparent in light of this disclosure.

[0043] Method 1000 may include, as in block 1006, adding one or more poly carboxylate materials. In general, the polycarboxylate material may be any of a wide range of polycarboxylate heteropolymer or copolymer (i.e., made from two monomers) materials. In accordance with some embodiments, the polycarboxylate material may be a high-range water reducer. In some instances, a single polycarboxylate material may be utilized, whereas in other instances, a combination of two or more different polycarboxylate materials may be utilized. In at least some cases, it may be desirable for the polycarboxylate material(s) to be in powder form, though this is not required. The amount of polycarboxylate material(s) added may be customized, as desired for a given target application or end-use. In accordance with some embodiments, the polycarboxylate material(s) may constitute about 0.1-0.3 wt% (e.g., about 0.1-0.15 wt%, about 0.15-0.2 wt%, about 0.2-0.25 wt%, about 0.25-0.3 wt%, or any other sub-range in the range of about 0.1-0.3 wt%) of a given mixture produced according to method 1000. Other suitable quantities of poly carboxylate material(s) will be apparent in light of this disclosure.

[0044] In accordance with a specific example embodiment, the polycarboxylate material may be a polycarboxylate copolymer, such as Polycarboxylate-PCX CAS NO. 59233-52-2, available from WEGO Chemical and Mineral Corporation of Great Neck, New York, (hereinafter, WEGO Polycarboxylate-PCX), described as a high-range water reducer. WEGO Polycarboxylate-PCX has the following general chemical structure, where (1) M, Y, and X are leaving groups, (2) Ri-R4are aliphatic carbon chains, (3) ethylene oxide (EO) is a hydrophilic component, and (4) propylene oxide (PO) is a hydrophobic component:

[0045] The hydrophilic EO component of WEGO Polycarboxylate-PCX has the following chemical structure:

[0046] Also, the hydrophobic PO component of WEGO Polycarboxylate-PCX has the following chemical structure:

[0047] For WEGO Polycarboxylate-PCX, variables a, b, c, and n may be whole integers greater than or equal to 1, and carbon bonds omitted from the illustrated chemical structure of WEGO Polycarboxylate-PCX may be bonded with hydrogen (H). Furthermore, it should be noted that the M, Y, and X leaving groups are proprietary constituents not known outside of WEGO Chemical and Mineral Corp. Nevertheless, even without knowing the M, Y, and X leaving groups, a person having ordinary skill in the art can utilize techniques disclosed herein, including making use of WEGO’s commercially available Polycarboxylate-PCX, to produce products, as variously described herein, in accordance with some embodiments of the present disclosure. Also, it should be noted that one or more polycarboxylate materials of chemistry similar to that of WEGO polycarboxylate-PCX may be utilized additionally or alternatively, in accordance with some embodiments.

[0048] Method 1000 optionally may include, as in block 1008, adding expanded perlite waste (e.g., material produced while expanding raw perlite ore to make “popped” perlite). As will be appreciated in light of this disclosure, the expanded perlite waste may be sourced as desired for a given target application or end-use. In some instances, the expanded perlite waste may have a D90 PSD in the range of about 30-42 pm (e.g., about 30-32 pm, about 32- 34 pm, about 34-36 pm, about 36-38 pm, about 38-40 pm, about 40-42 pm, or any other sub-range in the range of about 30-42 pm). In some cases, the expanded perlite waste may have a D90 PSD of about 38 pm (± 3 pm).

[0049] The amount of expanded perlite waste added may be customized, as desired for a given target application or end-use. For instance, in accordance with some embodiments, the expanded perlite waste may constitute about 1-15 wt% (e.g., about 1-5 wt%, about 5- 10 wt%, about 10-15 wt%, or any other sub-range in the range of about 1-15 wt%) of a given mixture produced according to method 1000. In some cases, the expanded perlite waste may constitute about 5 wt% (± 3 wt%) of a given mixture produced according to method 1000. Other suitable types, characteristics, and quantities of the expanded perlite waste will be apparent in light of this disclosure.

[0050] Method 1000 may include, as in block 1010, intergrinding the (1) PVA-treated CKD and / or PVA-treated LKD, (2) raw perlite ore, (3) polycarboxylate material(s), and (optionally) (4) expanded perlite waste. The noted materials may be interground with one another (e.g., all at once or in one or more intermediate combinations) to provide a cementitious material, in accordance with some embodiments. In some instances, a given material may have been ground down prior to beginning method 1000, though in other instances, the grinding down of a given material may occur (at least in part) at one or more points during method 1000.

[0051] Intergrinding may be performed utilizing any suitable grinding means, as will be apparent in light of this disclosure. For example, in accordance with some embodiments, intergrinding may be performed, in part or in whole, utilizing a mill with a grinding aid and media. The specific type of mill may be customized, as desired for a given target application or end-use. In some cases, the mill may be, for instance, a rotary mill, such as a ball mill. In accordance with some embodiments, intergrinding may be performed (in part or in whole) utilizing a mill configured as disclosed in U.S. Patent No. 9,254,490 (“Process for Treating Fly Ash and a Rotary Mill Therefor”), the entire disclosure of which is herein incorporated by reference. In accordance with some embodiments, intergrinding may involve a grinding aid and media configured as disclosed in U.S. Patent No. 9,254,490.

[0052] The duration of the intergrinding of the materials related to method 1000 may be customized, as desired for a given target application or end-use. For example, in accordance with some embodiments, intergrinding may be performed for about 20-60 minutes (e.g., about 20-30 minutes, about 30-40 minutes, about 40-50 minutes, about 50-60 minutes, or any other sub-range in the range of about 20-60 minutes). In some cases, intergrinding may be performed for about 30 minutes (± 10 minutes). As will be appreciated in light of this disclosure, the intergrinding of materials may be performed, for example, until a given target PSD is achieved, at least in some instances. For example, in some instances, intergrinding may occur until a D90 PSD in the range of about 25-45 pm (e.g., about 25-30 pm, about 30- 35 pm, about 35-40 pm, about 40-45 pm, or any other sub-range in the range of about 25- 45 pm) is achieved. In some cases, intergrinding may occur until a D90 PSD of about 38 pm (± 3 pm) is achieved. In some cases, intergrinding may occur until a D90 PSD of about 28 pm (± 3 pm) is achieved. Other suitable durations and target particle size distributions for the materials associated with method 1000 will be apparent in light of this disclosure.

[0053] Concrete

[0054] FIG. 4 illustrates a method 2000 of making concrete in accordance with an embodiment of the present disclosure. As can be seen, method 2000 may include, as in block 2002, adding the cementitious material produced via method 1000 (see FIG. 1). The amount of such cementitious material added may be customized, as desired for a given target application or end-use. In accordance with some embodiments, the cementitious material may constitute about 50 wt% or less (e.g., about 1-10 wt%, about 10-20 wt%, about 20- 30 wt%, about 30-40 wt%, about 40-50 wt%, or any other sub-range in the range of about 50 wt% or less) of a given concrete produced according to method 2000. In some cases, the cementitious material may constitute about 4.5-10 wt% of a given concrete produced according to method 2000. In some cases, the cementitious material may constitute about 9 wt% (± 3 wt%) of a given concrete produced according to method 2000. Other suitable quantities of cementitious material will be apparent in light of this disclosure.

[0055] Method 2000 may include, as in block 2004, adding OPC. The amount of OPC added may be customized, as desired for a given target application or end-use. In accordance with some embodiments, the OPC may constitute about 50 wt% or less (e.g., about 1-10 wt%, about 10-20 wt%, about 20-30 wt%, about 30-40 wt%, about 40-50 wt%, or any other subrange in the range of about 50 wt% or less) of a given concrete produced according to method 2000. In some cases, the OPC may constitute about 4.5-10 wt% of a given concrete produced according to method 2000. In some cases, the OPC may constitute about 9 wt% (± 3 wt%) of a given concrete produced according to method 2000. In some cases, the OPC and the cementitious material may be provided in a 50:50 (one-to-one) powder blend ratio. In some other cases, the cementitious material may be about 30-60% with the OPC making up the balance. Other suitable quantities of OPC will be apparent in light of this disclosure.

[0056] Method 2000 may include, as in block 2006, adding water and at least one of sand and rock. In accordance with some embodiments, the sand may include, for example, screened sand meeting ASTM C989 standards. In accordance with some embodiments, the rock material may include, for example, %” limestone rock meeting ASTM C33 standards. The amounts of sand and / or rock added may be customized, as desired for a given target application or end-use. In accordance with some embodiments, the sand may constitute about 35-45 wt% (e.g., about 35-40 wt%, about 40-45 wt%, or any other sub-range in the range of about 35-45 wt%) of a given concrete produced according to method 2000. In some cases, the sand may constitute about 41 wt% (± 3 wt%) of a given concrete produced according to method 2000. In accordance with some embodiments, the rock may constitute about 38-48 wt% (e.g., about 38-43 wt%, about 43-48 wt%, or any other sub-range in the range of about 38-48 wt%) of a given concrete produced according to method 2000. In some cases, the rock may constitute about 42 wt% (± 3 wt%) of a given concrete produced according to method 2000. Other suitable types, characteristics, and quantities of sand and rock will be apparent in light of this disclosure.

[0057] The water-cement (w / c) ratio for concrete produced according to method 2000 also may be customized, as desired for a given target application or end-use. In some cases, the w / c ratio may be in the range of about 0.2-0.4 (e.g., about 0.2-0.25, about 0.25-0.3, about 0.3-0.35, about 0.35-0.4, or any other sub-range in the range of about 0.2-0.4). In some cases, the w / c ratio may be in the range of about 0.25-0.38 (e.g., about 0.25-0.31, about 0.31-0.38, or any other sub-range in the range of about 0.25-0.38). In some cases, the w / c ratio may be in the range of about 0.2-0.33 (e.g., about 0.2-0.26, about 0.26-0.33, or any other sub-range in the range of about 0.2-0.33). In some cases, the w / c ratio may be in the range of about 0.23-0.3 or 0.23-0.4. Other suitable w / c ratios for materials associated with method 2000 will be apparent in light of this disclosure.

[0058] Method 2000 may include, as in block 2008, mixing the (1) cementitious material, (2) OPC, (3) water, and (4) at least one of sand and rock. The noted materials may be mixed with one another (e.g., all at once or in one or more intermediate combinations) to provide a concrete including a (CKD-based and / or LKD-based) cementitious material, in accordance with some embodiments. Mixing may be performed as typically done with concrete products. Moreover, the duration of the mixing of the materials related to method 2000 may be customized, as desired for a given target application or end-use. As will be appreciated in light of this disclosure, it may be desirable to ensure that mixing is curtailed with sufficient time to provide for pouring, forming, etc., the concrete as desired.

[0059] Example Concrete Batch #1 (9,65% MM / Omni CKD)

[0060] In accordance with an example embodiment, a first concrete batch including the following constituent materials was made: (1) CKD-based cementitious material (e.g., Midlothian Bypass Texas Lehigh); (2) Type Eli OPC having typical fineness distribution;

[0061] (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 9.65 wt% replacement of OPC. The water-cement (w / c) ratio of this batch was 0.40.

[0062] The aforementioned CKD-based cementitious material was mixed as follows: (1) 9.65 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.); (2) 90.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Poly carb oxylate-PCX; and

[0063] (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD as follows in Table 1A. The constituent PVA-treated CKD had a D90 PSD as follows in Table IB, a chemical composition as follows in Table 1C, and an X-ray powder diffraction as follows in Table ID and shown in FIG. 2 (discussed above). The constituent raw perlite ore had an X-ray powder diffraction as shown in FIG. 3 (discussed above).

[0064] Table 1A Table IB

[0065] Table 1C

[0066] Table ID

[0067] Table IE below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.4 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0068] Table IE

[0069] Example Concrete Batch #2 (19,65% MM / Omni CKD)

[0070] In accordance with an example embodiment, a second concrete batch including the following constituent materials was made: (1) CKD-based cementitious material;

[0071] (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.40.

[0072] The aforementioned CKD-based cementitious material was mixed as follows: (1) 19.65 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.);

[0073] (2) 80.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate- PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD of about 45 pm. The data of Tables 1A-1D and plot of FIG. 2 apply equally here to the CKD-based cementitious material utilized in this example.

[0074] Table 2 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.4 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0075] Table 2

[0076] Example Concrete Batch #3 (29,65% MM / Omni CKD)

[0077] In accordance with an example embodiment, a third concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.45.

[0078] The aforementioned CKD-based cementitious material was mixed as follows:

[0079] (1) 29.65 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.);

[0080] (2) 70.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate- PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD of about 45 pm. The data of Tables 1A-1D and plot of FIG. 2 apply equally here to the CKD-based cementitious material utilized in this example.

[0081] Table 3 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.4 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0082] Table 3 Example Concrete Batch #4 (39,65% MM / Omni CKD)

[0083] In accordance with an example embodiment, a fourth concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.46.

[0084] The aforementioned CKD-based cementitious material was mixed as follows:

[0085] (1) 39.65 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.);

[0086] (2) 60.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate- PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD of about 45 pm. The data of Tables 1A-1D and plot of FIG. 2 apply equally here to the CKD-based cementitious material utilized in this example.

[0087] Table 4 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.0 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0088] Table 4

[0089] Example Concrete Batch #5 (5% MM / Omni CKD)

[0090] In accordance with an example embodiment, a fifth concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.39.

[0091] The aforementioned CKD-based cementitious material was mixed as follows: (1) 5.0 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.); (2) 89.75 wt% raw perlite ore (sourced from Oregon); (3) 5.0 wt% expanded perlite waste fines; (4) 0.2 wt% WEGO Polycarboxylate-PCX; and (5) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD of about 38 pm (± 1 pm). The raw perlite ore had a D90 PSD of about 36 pm (± 1 pm) and a mean PSD of about 16.5 pm (± 1 pm). The data of Tables 1A-1D and plot of FIG. 2 apply equally here to the CKD-based cementitious material utilized in this example.

[0092] Table 5 below tabulates measured compressive strengths for several cylinders of concrete cured at an ambient temperature in the range of about 78 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cylinders.

[0093] Table 5

[0094] Example Concrete Batch #6 (10% MM / Omni CKD)

[0095] In accordance with an example embodiment, a sixth concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.54.

[0096] The aforementioned CKD-based cementitious material was mixed as follows:

[0097] (1) 10.0 wt% PVA-treated CKD (sourced from Martin Marietta Materials, Inc.);

[0098] (2) 89.75 wt% raw perlite ore (sourced from Oregon); (3) 0.2 wt% WEGO Polycarboxylate- PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD-based cementitious material had a D90 PSD of about 47 pm (± 1 pm). The raw perlite ore had a D90 PSD of about 36 pm (± 1 pm) and a mean PSD of about 16.5 pm (± 1 pm). The data of Tables 1A- 1D and plot of FIG. 2 apply equally here to the CKD-based cementitious material utilized in this example.

[0099] Table 6 below tabulates measured compressive strengths for several cylinders of concrete cured at an ambient temperature in the range of about 75 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cylinders.

[0100] Table 6

[0101] Example Concrete Batch #7 (5,65% Mustang CKD)

[0102] In accordance with an example embodiment, a seventh concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.37.

[0103] The aforementioned CKD-based cementitious material was mixed as follows: (1) 5.65 wt% PVA-treated CKD (sourced from Buzzi Unicem Prior Oklahoma CKD (“MUSTANG”)); (2) 94.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate-PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD- based cementitious material had a D90 PSD of about 45 pm.

[0104] Table 7 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.0 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0105] Table 7

[0106] Example Concrete Batch #8 (10,65% Mustang CKD)

[0107] In accordance with an example embodiment, an eighth concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.38.

[0108] The aforementioned CKD-based cementitious material was mixed as follows: (1) 10.65 wt% PVA-treated CKD (sourced from Buzzi Unicem Prior Oklahoma CKD (“MUSTANG”)); (2) 89.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate-PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD- based cementitious material had a D90 PSD of about 45 gm.

[0109] Table 8 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.4 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0110] Table 8

[0111] Example Concrete Batch #9 (15,65% Mustang CKD)

[0112] In accordance with an example embodiment, a ninth concrete batch including the following constituent materials was made: (1) CKD-based cementitious material; (2) Type VII OPC having typical fineness distribution; (3) screened sand meeting ASTM C989 standards; and (4) water. The CKD-based cementitious material was used at about 50 wt% (± 5 wt%) replacement of OPC. The water-cement (w / c) ratio of this batch was 0.38.

[0113] The aforementioned CKD-based cementitious material was mixed as follows: (1) 15.65 wt% PVA-treated CKD (sourced from Buzzi Unicem Prior Oklahoma CKD (“MUSTANG”)); (2) 84.0 wt% raw perlite ore (sourced from Oregon); (3) 0.3 wt% WEGO Polycarboxylate-PCX; and (4) 0.05 wt% triethanolamine (TEA) grinding aid. The CKD- based cementitious material had a D90 PSD of about 45 pm.

[0114] Table 9 below tabulates measured compressive strengths for several cubes of concrete cured at an ambient temperature in the range of about 73.4 °F (± 3 °F) in conditions meeting ASTM C989 standards. The compressive strengths were obtained by breaking the cubes.

[0115] Table 9

[0116] Analysis & Conclusions

[0117] The data of Tables #l-#9 above, corresponding with Example Concrete Batches #1- #9, generally indicate that, utilizing techniques disclosed herein, strength gains equivalent to, for example, a grade 120 slag performance may be achieved from a natural pozzolan material in accordance with some embodiments. As will be appreciated in light of this disclosure, this is an unexpected result given the use of such natural pozzolanic material(s).

[0118] Further Examples

[0119] The following examples pertain to some further embodiments of the disclosure, from which numerous permutations and combinations will be apparent.

[0120] Example 1 is a method. The method includes producing a cementitious mixture including: (a) at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; (b) perlite; and (c) a poly carboxylate material.

[0121] Example 2 includes the subject matter of any of Examples 1, 3-7, and 11-31, wherein the cementitious mixture includes CKD treated with PVA powder but not LKD treated with PVA powder.

[0122] Example 3 includes the subject matter of any of Examples 1-2, 4-7, and 10-31, wherein the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm.

[0123] Example 4 includes the subject matter of any of Examples 1-3, 5-7, and 10-31, wherein the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm.

[0124] Example 5 includes the subject matter of any of Examples 1-4, 6-7, and 10-31, wherein the CKD treated with PVA powder has a pH of about 11.5 ± 0.5.

[0125] Example 6 includes the subject matter of any of Examples 1-5, 7, and 10-31, wherein the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5-6.0%.

[0126] Example 7 includes the subject matter of any of Examples 1-6 and 10-31, wherein the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture.

[0127] Example 8 includes the subject matter of any of Examples 1, 9, and 11-31, wherein the cementitious mixture includes LKD treated with PVA powder but not CKD treated with PVA powder.

[0128] Example 9 includes the subject matter of any of Examples 1, 8, and 11-31, wherein the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture. Example 10 includes the subject matter of any of Examples 1, 3-7, 9, and 11-31, wherein the cementitious mixture includes both CKD treated with PVA powder and LKD treated with PVA powder.

[0129] Example 11 includes the subject matter of any of Examples 1-10 and 12-31, wherein the perlite includes raw perlite ore.

[0130] Example 12 includes the subject matter of any of Examples 1-11 and 13-31, wherein the raw perlite ore has a D90 particle size distribution in the range of about 30-40 pm.

[0131] Example 13 includes the subject matter of any of Examples 1-12 and 14-31, wherein the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm.

[0132] Example 14 includes the subject matter of any of Examples 1-13 and 16-31, wherein the raw perlite ore constitutes about 15-90 wt% of the cementitious mixture produced.

[0133] Example 15 includes the subject matter of any of Examples 1-13 and 16-31, wherein the raw perlite ore constitutes about 90-99 wt% of the cementitious mixture produced.

[0134] Example 16 includes the subject matter of any of Examples 1-15 and 17-31, wherein the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite.

[0135] Example 17 includes the subject matter of any of Examples 1-16 and 18-31, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has been washed with water.

[0136] Example 18 includes the subject matter of any of Examples 1-17 and 19-31, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%.

[0137] Example 19 includes the subject matter of any of Examples 1-18 and 20-31, wherein the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

[0138] Example 20 includes the subject matter of any of Examples 1-19 and 21-31, wherein producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, and the polycarboxylate material.

[0139] Example 21 includes the subject matter of any of Examples 1-20 and 22-31, wherein the intergrinding is performed until a D90 particle size distribution of about 25-45 pm is achieved for the cementitious mixture. Example 22 includes the subject matter of any of Examples 1-21 and 24-31, wherein the intergrinding is performed until a D90 particle size distribution of about 38 pm ± 3 pm is achieved for the cementitious mixture.

[0140] Example 23 includes the subject matter of any of Examples 1-21 and 25-31, wherein the intergrinding is performed until a D90 particle size distribution of about 28 pm ± 3 pm is achieved for the cementitious mixture.

[0141] Example 24 includes the subject matter of any of Examples 1-23 and 25-31, wherein the cementitious mixture further includes expanded perlite waste.

[0142] Example 25 includes the subject matter of any of Examples 1-24 and 26-31, wherein producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, the polycarboxylate material, and the expanded perlite waste.

[0143] Example 26 includes the subject matter of any of Examples 1-25 and 27-31, wherein the expanded perlite waste has a D90 particle size distribution in the range of about 30- 42 pm.

[0144] Example 27 includes the subject matter of any of Examples 1-26 and 28-31, wherein the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm.

[0145] Example 28 includes the subject matter of any of Examples 1-27 and 29-31, wherein the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture.

[0146] Example 29 includes the subject matter of any of Examples 1-28 and 30-31, wherein the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture.

[0147] Example 30 is a method. The method includes producing a concrete including: (a) a cementitious mixture including the subject matter of any of Examples 1-29 and 31; (b) ordinary Portland cement (OPC); (c) water; and (d) at least one of rock and sand.

[0148] Example 31 is a concrete product including concrete including the subject matter of any of Examples 1-30.

[0149] Example 32 is a cementitious mixture. The cementitious mixture includes: (a) at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; (b) perlite; and (c) a poly carboxylate material.

[0150] Example 33 includes the subject matter of any of Examples 32, 34-38, and 42-59, wherein the cementitious mixture includes CKD treated with PVA powder but not LKD treated with PVA powder. Example 34 includes the subject matter of any of Examples 32-33, 35-38, and 42-59, wherein the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm.

[0151] Example 35 includes the subject matter of any of Examples 32-34, 36-38, and 42-59, wherein the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm.

[0152] Example 36 includes the subject matter of any of Examples 32-35, 37-38, and 42-59, wherein the CKD treated with PVA powder has a pH of about 11.5 ± 0.5.

[0153] Example 37 includes the subject matter of any of Examples 32-36, 38, and 42-59, wherein the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5 -6.0%.

[0154] Example 38 includes the subject matter of any of Examples 32-37 and 42-59, wherein the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture.

[0155] Example 39 includes the subject matter of any of Examples 32, 40, and 42-59, wherein the cementitious mixture includes LKD treated with PVA powder but not CKD treated with PVA powder.

[0156] Example 40 includes the subject matter of any of Examples 32, 39, and 42-59, wherein the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture.

[0157] Example 41 includes the subject matter of any of Examples 32, 34-38, 40, and 42-59, wherein the cementitious mixture includes both CKD treated with PVA powder and LKD treated with PVA powder.

[0158] Example 42 includes the subject matter of any of Examples 32-41 and 43-59, wherein the perlite includes raw perlite ore.

[0159] Example 43 includes the subject matter of any of Examples 32-42 and 44-59, wherein the raw perlite ore has a D90 particle size distribution in the range of about 30- 40 pm.

[0160] Example 44 includes the subject matter of any of Examples 32-43 and 45-59, wherein the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm.

[0161] Example 45 includes the subject matter of any of Examples 32-44 and 47-59, wherein the raw perlite ore constitutes about 15-90 wt% of the cementitious mixture.

[0162] Example 46 includes the subject matter of any of Examples 32-44 and 47-59, wherein the raw perlite ore constitutes about 90-99 wt% of the cementitious mixture. Example 47 includes the subject matter of any of Examples 32-46 and 48-59, wherein the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite.

[0163] Example 48 includes the subject matter of any of Examples 32-47 and 49-59, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%.

[0164] Example 49 includes the subject matter of any of Examples 32-48 and 50-59, wherein the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

[0165] Example 50 includes the subject matter of any of Examples 32-49 and 51-59, wherein the cementitious mixture has a D90 particle size distribution in the range of about 25-45 pm.

[0166] Example 51 includes the subject matter of any of Examples 32-50 and 53-59, wherein the cementitious mixture has a D90 particle size distribution of about 38 pm ± 3 pm.

[0167] Example 52 includes the subject matter of any of Examples 32-50 and 53-59, wherein the cementitious mixture has a D90 particle size distribution of about 28 pm ± 3 pm.

[0168] Example 53 includes the subject matter of any of Examples 32-52 and 54-59, further including expanded perlite waste.

[0169] Example 54 includes the subject matter of any of Examples 32-53 and 55-59, wherein the expanded perlite waste has a D90 particle size distribution in the range of about 30-42 pm.

[0170] Example 55 includes the subject matter of any of Examples 32-54 and 56-59, wherein the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm.

[0171] Example 56 includes the subject matter of any of Examples 32-55 and 57-59, wherein the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture.

[0172] Example 57 includes the subject matter of any of Examples 32-56 and 58-59, wherein the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture.

[0173] Example 58 is concrete. The concrete includes: (a) a cementitious mixture including the subject matter of any of Examples 32-57 and 59; (b) ordinary Portland cement (OPC); (c) water; and (d) at least one of rock and sand.

[0174] Example 59 is a concrete product including concrete including the subject matter of any of Examples 32-58. The foregoing description of example embodiments has been presented for the purposes of illustration and description. It is not intended to be exhaustive or to limit the present disclosure to the precise forms disclosed. Many modifications and variations are possible in light of this disclosure. It is intended that the scope of the present disclosure be limited not by this detailed description. Future-filed applications claiming priority to this application may claim the disclosed subject matter in a different manner and generally may include any set of one or more limitations as variously disclosed or otherwise demonstrated herein.

Claims

CLAIMSWhat is claimed is:

1. A method comprising: producing a cementitious mixture comprising: at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; perlite; and a polycarboxylate material.

2. The method of claim 1, wherein the cementitious mixture comprises CKD treated with PVA powder but not LKD treated with PVA powder.

3. The method of claim 2, wherein the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm.

4. The method of claim 3, wherein the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm.

5. The method of claim 2, wherein the CKD treated with PVA powder has a pH of about 11.5 ± 0.5.

6. The method of claim 2, wherein the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5-6.0%.

7. The method of claim 2, wherein the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture.

8. The method of claim 1, wherein the cementitious mixture comprises LKD treated with PVA powder but not CKD treated with PVA powder.

9. The method of claim 8, wherein the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture.

10. The method of claim 1, wherein the cementitious mixture comprises both CKD treated with PVA powder and LKD treated with PVA powder.

11. The method of claim 1, wherein the perlite comprises raw perlite ore.

12. The method of claim 11, wherein the raw perlite ore has a D90 particle size distribution in the range of about 30-40 pm.

13. The method of claim 12, wherein the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm.

14. The method of claim 11, wherein the raw perlite ore constitutes about 15- 90 wt% of the cementitious mixture produced.

15. The method of claim 11, wherein the raw perlite ore constitutes about 90- 99 wt% of the cementitious mixture produced.

16. The method of claim 11, wherein the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite.

17. The method of claim 16, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has been washed with water.

18. The method of claim 16, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%.

19. The method of claim 11, wherein the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

20. The method of claim 1, wherein producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, and the poly carboxylate material.

21. The method of claim 20, wherein the intergrinding is performed until a D90 particle size distribution of about 25-45 pm is achieved for the cementitious mixture.

22. The method of claim 21, wherein the intergrinding is performed until a D90 particle size distribution of about 38 pm ± 3 pm is achieved for the cementitious mixture.

23. The method of claim 21, wherein the intergrinding is performed until a D90 particle size distribution of about 28 pm ± 3 pm is achieved for the cementitious mixture.

24. The method of claim 1, wherein the cementitious mixture further comprises expanded perlite waste.

25. The method of claim 24, wherein producing the cementitious mixture involves intergrinding the at least one of CKD treated with PVA powder and LKD treated with PVA powder, the perlite, the polycarboxylate material, and the expanded perlite waste.

26. The method of claim 24, wherein the expanded perlite waste has a D90 particle size distribution in the range of about 30-42 pm.

27. The method of claim 26, wherein the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm.

28. The method of claim 24, wherein the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture.

29. The method of claim 28, wherein the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture.

30. A method comprising: producing a concrete comprising:the cementitious mixture produced according to any of claims 1-29; ordinary Portland cement (OPC); water; and at least one of rock and sand.

31. A concrete product comprising the concrete produced according to claim 30.

32. A cementitious mixture comprising: at least one of: cement kiln dust (CKD) treated with polyvinyl alcohol (PVA) powder; and lime kiln dust (LKD) treated with PVA powder; perlite; and a polycarboxylate material.

33. The cementitious mixture of claim 32, wherein the cementitious mixture comprises CKD treated with PVA powder but not LKD treated with PVA powder.

34. The cementitious mixture of claim 33, wherein the CKD treated with PVA powder has a D90 particle size distribution in the range of about 30-60 pm.

35. The cementitious mixture of claim 34, wherein the CKD treated with PVA powder has a D90 particle size distribution of about 45 pm ± 3 pm.

36. The cementitious mixture of claim 33, wherein the CKD treated with PVA powder has a pH of about 11.5 ± 0.5.

37. The cementitious mixture of claim 33, wherein the CKD treated with PVA powder has an aluminum / calcium mineral ratio in the range of about 3.5-6.0%.

38. The cementitious mixture of claim 33, wherein the CKD treated with PVA powder constitutes about 5-30 wt% of the cementitious mixture.

39. The cementitious mixture of claim 32, wherein the cementitious mixture comprises LKD treated with PVA powder but not CKD treated with PVA powder.

40. The cementitious mixture of claim 39, wherein the LKD treated with PVA powder constitutes about 3-20 wt% of the cementitious mixture.

41. The cementitious mixture of claim 32, wherein the cementitious mixture comprises both CKD treated with PVA powder and LKD treated with PVA powder.

42. The cementitious mixture of claim 32, wherein the perlite comprises raw perlite ore.

43. The cementitious mixture of claim 42, wherein the raw perlite ore has a D90 particle size distribution in the range of about 30-40 pm.

44. The cementitious mixture of claim 43, wherein the raw perlite ore has a D90 particle size distribution of about 38 pm ± 3 pm.

45. The cementitious mixture of claim 42, wherein the raw perlite ore constitutes about 15-90 wt% of the cementitious mixture.

46. The cementitious mixture of claim 42, wherein the raw perlite ore constitutes about 90-99 wt% of the cementitious mixture.

47. The cementitious mixture of claim 42, wherein the raw perlite ore has been treated to remove at least one of montmorillonite clay and bentonite.

48. The cementitious mixture of claim 47, wherein in having been treated to remove the at least one of montmorillonite clay and bentonite, the raw perlite ore has a clay contamination of less than about 6%.

49. The cementitious mixture of claim 42, wherein the raw perlite ore has an amorphous glass content having a silicates content of at least about 70%.

50. The cementitious mixture of claim 32, wherein the cementitious mixture has a D90 particle size distribution in the range of about 25-45 pm.

51. The cementitious mixture of claim 50, wherein the cementitious mixture has a D90 particle size distribution of about 38 pm ± 3 pm.

52. The cementitious mixture of claim 50, wherein the cementitious mixture has a D90 particle size distribution of about 28 pm ± 3 pm.

53. The cementitious mixture of claim 32, further comprising expanded perlite waste.

54. The cementitious mixture of claim 53, wherein the expanded perlite waste has a D90 particle size distribution in the range of about 30-42 pm.

55. The cementitious mixture of claim 54, wherein the expanded perlite waste has a D90 particle size distribution of about 38 pm ± 3 pm.

56. The cementitious mixture of claim 53, wherein the expanded perlite waste constitutes about 1-15 wt% of the cementitious mixture.

57. The cementitious mixture of claim 56, wherein the expanded perlite waste constitutes about 5 wt% ± 3 wt% of the cementitious mixture.

58. A concrete comprising: the cementitious mixture according to any of claims 32-57; ordinary Portland cement (OPC); water; and at least one of rock and sand.

59. A concrete product comprising the concrete according to claim 58.

Citation Information

Patent Citations

  • concrete producing to use cement kiln dust

    KR1020040078466A

  • Soil conditioning agglomerates containing cement kiln dust

    US5997599A

  • Settable compositions comprising unexpanded perlite and methods of cementing in subterranean formations

    WO2012085509A1

  • Chemically activated cement using industrial waste

    WO2017089899A1

  • Perlite-based cementitious materials, concrete, and related techniques

    WO2023282939A1