Rapid synthesis method for two-dimensional molecular sieve and two-dimensional molecular sieve

By using the seed induction method and argon purge technology in a tubular reactor, the problems of long time consumption and template agent decomposition in the preparation process of two-dimensional molecular sieves are solved, and the rapid synthesis of two-dimensional molecular sieves with ultra-large lateral dimensions is achieved, which improves the efficiency of the two-dimensional molecular sieves. Preparative efficiency and yield.

WO2024212213A1PCT designated stage expired Publication Date: 2024-10-17ZHEJIANG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/088368
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of two-dimensional molecular sieves is time-consuming, the morphology is difficult to accurately control, the template agent is easy to decompose under high temperature conditions, and the lateral size is limited, resulting in low preparation efficiency and low yield.

Method used

Using a tubular reactor combined with a seed induction method, the precursor sol is formed by hydrolysis under argon purge conditions, and mixed with MFI seeds for hydrothermal reaction, using high temperature to quickly synthesize two-dimensional molecular sieves, avoiding the need for a kettle reactor The heating hysteresis and Hofmann degradation of the template agent enable the synthesis of nanosheets with extremely large lateral dimensions.

Benefits of technology

The rapid synthesis of two-dimensional molecular sieves is achieved, the preparation time is shortened to half an hour, the stability of the template agent and crystallization under high temperature conditions are ensured, nanosheets with ultra-large lateral dimensions are obtained, and the yield and preparation efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023088368_17102024_PF_FP_ABST
    Figure CN2023088368_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a rapid synthesis method for a two-dimensional molecular sieve and the two-dimensional molecular sieve. The method comprises: (1) fully mixing a silicon source, potassium hydroxide, a template agent, and water in a molar ratio of (60-100):(2-5):(10-30):(7500-9500), and carrying out aging hydrolysis under the condition of argon purging to form a precursor sol; (2) mixing the precursor sol with a dispersion liquid with MFI seed crystals, and fully stirring the mixture, wherein the dispersion liquid with the MFI seed crystals is obtained by dispersing the MFI seed crystals into deionized water, the MFI seed crystals are obtained by carrying out a hydrothermal reaction after the silicon source, the template agent, and water are heated and aged, and the molar ratio of the dispersion liquid to the silicon source of the precursor sol is 1:(50-1000); and (3) transferring the mixture obtained in step (2) into a tubular reactor made of stainless steel, and carrying out a hydrothermal reaction, such that a large-size two-dimensional molecular sieve can be synthesized within a few hours.
Need to check novelty before this filing date? Find Prior Art

Description

A rapid synthesis method of two-dimensional molecular sieve and two-dimensional molecular sieve Technical Field

[0001] The present invention belongs to the technical field of preparation of two-dimensional molecular sieves, and in particular relates to a rapid synthesis method of a two-dimensional molecular sieve and the two-dimensional molecular sieve. Background Art

[0002] Zeolite molecular sieves with well-defined microporous structures are widely used as novel membrane separation and membrane catalysis materials in fields such as fine chemicals, petroleum refining, and environmental protection. However, diffusion of substances within the microporous structure of zeolites is often limited, significantly impacting their separation and catalytic performance. For these specific applications, thin, oriented sheets can be prepared by controlling crystal size and shape. Nanoparticle-thick sheets have been incorporated with struts and self-struts to modify mass transfer characteristics in certain adsorption and catalytic applications. Furthermore, (intergrown or multilayer) nanosheets have been used to form membrane layers, potentially improving the energy efficiency of separation processes. To date, a number of successful strategies have been developed to synthesize two-dimensional zeolites with controllable thickness. A range of layered zeolite nanosheets can be prepared by designing organic templates. When a template, additive, or zeolite seed crystal is added, the zeolite grows in a unique direction, resulting in the formation of a zeolite nanosheet morphology. Molecular sieve nanosheets can also form after the organic template decomposes and generates gas expansion during crystallization. Furthermore, nanosheets can be formed by exfoliating layered three-dimensional zeolites using organic surfactants. However, simultaneously controlling the framework structure and composition, crystal orientation, and large-scale nanosheets remains a major challenge.

[0003] To date, nanosheets have been prepared using a multi-step process based on the exfoliation of layered molecular sieves, followed by centrifugation to remove unexfoliated particles. This top-down approach is time-consuming, costly, and has low yields, with limited lateral dimensions (<1 μm). Conversely, bottom-up synthesis can produce high-aspect-ratio molecular sieve nanosheets with high yields and lower costs. This method is mostly carried out in a stainless steel hydrothermal reactor lined with polytetrafluoroethylene. While this method is simple to operate and has a certain degree of universality, it suffers from poor experimental reproducibility and difficulty in precisely controlling the microstructure and morphology of the molecular sieve. Furthermore, due to the heating hysteresis of this reactor, the synthesis of two-dimensional molecular sieves using this reactor typically requires days or even weeks to complete. Therefore, this method has the disadvantages of low efficiency and long processing time. The synthesis of layered molecular sieves typically requires the use of organic templates, which decompose at certain temperatures, thus limiting the temperature of synthesis using reactors.

[0004] Summary of the Invention

[0005] The purpose of the embodiments of the present application is to provide a rapid synthesis method of a two-dimensional molecular sieve and a two-dimensional molecular sieve to solve the problems existing in the related art, such as: the preparation of two-dimensional molecular sieves is slow and time-consuming, the morphology is difficult to accurately control, the template used for synthesis during the preparation process decomposes under high temperature conditions, and the lateral size of the two-dimensional molecular sieve is limited.

[0006] According to a first aspect of an embodiment of the present application, a method for rapidly synthesizing a two-dimensional molecular sieve is provided, comprising:

[0007] (1) fully mixing a silicon source, potassium hydroxide, a template, and water in a molar ratio of 60-100:2-5:10-30:7500-9500, and hydrolyzing the mixture under argon purge to form a precursor sol;

[0008] (2) mixing the precursor sol with a dispersion containing MFI crystal seeds and stirring them thoroughly, wherein the dispersion containing MFI crystal seeds is obtained by dispersing MFI crystal seeds in deionized water, wherein the MFI crystal seeds are obtained by hydrothermal reaction of a silicon source, a template agent, and water after heating and aging, and the molar ratio of silicon dioxide in the dispersion to the precursor sol is 1:50 to 1000;

[0009] (3) The mixture obtained in step (2) is transferred to a stainless steel tubular reactor for hydrothermal reaction to synthesize a two-dimensional molecular sieve.

[0010] Furthermore, in step (1), the argon purge rate is 50-200 mL / min, the aging and hydrolysis temperature is from room temperature to 90° C., the aging time is 8-24 h, and the hydrolysis time is 8-36 h.

[0011] Furthermore, in step (1), the template is bis-1,5 (tripropyl ammonium) pentamethylene diiodide (dC5), so that the molecular sieve grows in the form of 2D nanosheets.

[0012] Furthermore, the dC5 is obtained by heating 1,5-diaminopentane and 1-iodopropane under reflux reaction in the absence of water and oxygen, wherein the reflux temperature is 75-85° C. and the argon purge rate is 50-100 mL / min.

[0013] Furthermore, in step (1), the silicon source is colloidal silicon dioxide with a mass content of 25 to 30%.

[0014] Furthermore, in step (1), the water is deionized water.

[0015] Furthermore, in step (2), the mass ratio of the MFI seed crystals to the precursor sol is 2% to 10%.

[0016] Furthermore, the preparation process of the MFI seed crystal is as follows:

[0017] The silicon source, template and water are fully mixed in a molar ratio of 1:0.4 to 1:10 to 30, and aged under heating conditions to promote the full hydrolysis of the silicon source, wherein the aging time is 8 to 24 hours and the aging temperature is room temperature to 90°C;

[0018] The reaction solution after aging and hydrolysis is transferred to a stainless steel autoclave reactor for hydrothermal reaction to obtain seed crystals with a size of 80-90 nm, wherein the temperature of the hydrothermal reaction is 170-210° C.

[0019] Furthermore, in step (3), the hydrothermal reaction is carried out at 160-200° C. for 0.5 h to 3 d.

[0020] Furthermore, the length of the tubular reactor is 10 to 15 cm.

[0021] According to a second aspect of an embodiment of the present application, a two-dimensional molecular sieve is provided, which is prepared by the method described in the first aspect.

[0022] The technical solutions provided by the embodiments of the present application may have the following beneficial effects:

[0023] As can be seen from the above embodiments, the present application utilizes a seed-induced method to perform epitaxial growth of molecular sieves; utilizing a tubular reactor, rapid synthesis of two-dimensional molecular sieves is achieved, thereby avoiding the heating hysteresis problem existing in kettle reactors, and the preparation can be completed within half an hour, thereby avoiding degradation of the organic template during high-temperature synthesis; at the same time, under high-temperature conditions, the crystallization of layered molecular sieve nanosheets can be completed before Hofmann degradation of the template occurs, thereby realizing the synthesis of two-dimensional molecular sieves with ultra-large lateral dimensions.

[0024] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0026] FIG1 is a flow chart of a method for rapid synthesis of a two-dimensional molecular sieve provided in this application.

[0027] FIG2 is a schematic diagram of a tubular reactor.

[0028] FIG3 is a carbon 13 nuclear magnetic spectrum of the template agent dC5 product synthesized in Example 1.

[0029] FIG4 is a scanning electron microscope photograph of the MFI seed crystals synthesized in Example 1.

[0030] FIG5 is an X-ray powder diffraction spectrum of the MFI NS product synthesized in Example 1.

[0031] FIG6 is a scanning electron microscope photograph of the MFI NS product synthesized in Example 1.

[0032] FIG7 is an atomic force microscope photograph of the synthesized MFI NS in Example 1 and a schematic diagram of thickness measurement.

[0033] FIG8 is a scanning electron microscope photograph of the synthesized MFI NS in Example 2.

[0034] FIG9 is a scanning electron micrograph of the rapidly synthesized MFI NS in Example 3 (180° C., 0.5 h-4 h). DETAILED DESCRIPTION

[0035] Exemplary embodiments are described in detail herein, with examples illustrated in the accompanying drawings. When the following description refers to the drawings, identical numerals in different drawings represent identical or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments are not intended to represent all embodiments consistent with this application.

[0036] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. As used in this application and the appended claims, the singular forms "a," "an," "the," and "the" are intended to include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "and / or" as used herein refers to and encompasses any and all possible combinations of one or more of the associated listed items.

[0037] It should be understood that although the terms first, second, third, etc. may be used in this application to describe various information, such information should not be limited to these terms. These terms are only used to distinguish information of the same type from each other. For example, without departing from the scope of this application, first information may also be referred to as second information, and similarly, second information may also be referred to as first information. Depending on the context, the word "if" as used herein may be interpreted as "at the time of" or "when" or "in response to determining".

[0038] The present application provides a method for rapid synthesis of a two-dimensional molecular sieve, as shown in FIG1 , which may include:

[0039] (1) fully mixing a silicon source, potassium hydroxide, a template, and water in a molar ratio of 60-100:2-5:10-30:7500-9500, and aging and hydrolyzing the mixture under argon purge to form a precursor sol;

[0040] Specifically, the silicon source can be slowly hydrolyzed under low pH conditions, and will not aggregate due to excessive hydrolysis, ultimately forming very thick nanosheets. More specifically, the silicon source is actually various forms of silicon dioxide. In this step, colloidal silicon dioxide with a mass content of 25-30% is used. This form of silicon source is convenient for experimental operation and will not cause physical harm to the experimenter. Secondly, it is dispersed in an aqueous solution and can be better evenly dispersed during synthesis. The ethanol produced by the hydrolysis of the silicon source can be removed by argon purging. The presence of ethanol will slow down the synthesis rate;

[0041] In this step, the argon purge rate is 50-200 mL / min, the aging and hydrolysis temperature is from room temperature to 90°C, the aging time is 8-24 hours, and the hydrolysis time is 8-36 hours. Sufficient aging is required to completely hydrolyze the silicon source, eliminating the need for a hydrolysis step during the crystallization process. If the aging temperature is low and the time is short, the silicon source will hydrolyze during high-temperature crystallization, which will prolong the crystallization time of the nanosheets. If the argon flow rate is too high during the purge, it is easy to remove water from the reaction precursor solution, which is not conducive to subsequent synthesis.

[0042] In this step, the template is bis-1,5 (tripropyl ammonium) pentamethylene diiodide (dC5), which allows the molecular sieve to grow in the form of 2D nanosheets. Other templates that allow the molecular sieve to grow in the form of 2D nanosheets can also be used. The dC5 is obtained by heating 1,5-diaminopentane and 1-iodopropane under reflux reaction in the absence of water and oxygen, wherein the reflux temperature is between 75 and 85°C. The anhydrous and oxygen-free conditions can be achieved by purging with an inert gas, for example, when purging with argon, the purge rate is 50 to 100 mL / min. Under the condition of argon purging, the main purpose is to prevent oxidation of 1-iodopropane, so inert gas protection is required. The water used in this step is deionized water to avoid interference from other ions and affect the reaction.

[0043] (2) mixing the precursor sol with a dispersion containing MFI crystal seeds and stirring them thoroughly, wherein the dispersion containing MFI crystal seeds is obtained by dispersing MFI crystal seeds in deionized water, and the MFI crystal seeds are obtained by hydrothermal reaction of a silicon source, a template agent, and water after heating and aging, and the molar ratio of the silicon source in the dispersion to the precursor sol is 1:50 to 1000;

[0044] Specifically, the ratio of seed crystals can regulate the reaction rate: more seed crystals result in a faster reaction. Too few seed crystals can result in a very slow reaction, sometimes requiring four days or a week for complete crystallization. The mass ratio of MFI seed crystals to precursor sol is 2% to 10%. A higher seed crystal ratio increases the reaction rate, while a seed crystal ratio below 2% makes it difficult to achieve rapid synthesis in a short period of time.

[0045] Furthermore, the preparation process of the MFI seed crystal is as follows:

[0046] The silicon source, template, and water are thoroughly mixed at a molar ratio of 1:0.4 to 1:10-30. The mixture is then aged under heating conditions to promote complete hydrolysis of the silicon source. The aging time is 8 to 24 hours, and the aging temperature is between room temperature and 90°C. The aging temperature affects the speed of rapid synthesis. The aging temperature is adjustable. For a faster reaction rate, a higher aging temperature is sufficient. However, too high a temperature may cause some product to crystallize prematurely, resulting in uneven seed crystal size.

[0047] The aged, hydrolyzed reaction solution was transferred to a stainless steel autoclave reactor for a hydrothermal reaction at a temperature of 170-210°C to produce seed crystals with a size of 80-90 nm. The reaction temperature controls the size of the seed crystals. At low reaction temperatures, the seed crystals were approximately 70-80 nm in size, while at 210°C, the seed crystals were approximately 90-100 nm in size.

[0048] (3) The mixture obtained in step (2) is transferred to a stainless steel tubular reactor for a hydrothermal reaction, thereby synthesizing a large-sized two-dimensional molecular sieve within a few hours.

[0049] In this step, the hydrothermal reaction is carried out at 160-200°C for 0.5 hours to 3 days. Both temperature and time affect the size and thickness of the nanosheets. Lower temperatures and shorter times result in smaller and thinner nanosheets, while higher temperatures result in larger and thicker nanosheets. These parameters can be adjusted to tailor the nanosheet growth to the application.

[0050] The tubular reactor (shown in Figure 2) is 10-15 cm long, a perfect fit for laboratory oil baths. A longer length would be inconvenient to operate. The stainless steel tubular reactor can withstand high pressures in an oil bath. Furthermore, its thin 1-2 mm tube wall allows for rapid heating, shortening heating time by approximately 4 hours compared to traditional reactors. Tubular reactors are key to achieving rapid nanosheet synthesis.

[0051] The following describes the method in conjunction with embodiments.

[0052] Example 1

[0053] 1) First, the template agent dC5 was synthesized. dC5 was synthesized by the complete alkylation of 1,5-diaminopentane with 1-iodopropane. 4.75 g of 1,5-diaminopentane and 20.59 g of anhydrous potassium carbonate were added to a brown three-necked round-bottom flask containing 112.5 ml of 2-butanone. The brown flask was used to prevent iodide oxidation. With vigorous stirring, the reactor was slowly heated to 80°C under an argon atmosphere. 25 mL of 1-iodopropane was then added dropwise to the reactor. After reflux for 10 hours, the reaction mixture was cooled and filtered to remove the potassium salt. The solvent (2-butanone) in the filtrate was then removed by rotary evaporation.

[0054] The purification process involves two steps. First, the product was dissolved in 50 mL of acetone and stirred for 1 hour, followed by the addition of an equal amount of ethyl acetate. After stirring overnight, the solid powder was recovered by filtration. Further purification was performed using ethanol to remove KI. The recovered solid was dissolved in 100 mL of anhydrous ethanol and then filtered to remove KI. The product was recovered from the filtrate using rotary evaporation. This process was repeated 4 times. The purity of the product was determined by 13 The results were confirmed by C nuclear magnetic resonance (NMR) spectrum, as shown in Figure 3.

[0055] 2) Synthesis of seed crystals (80-90nm). The silicon source, organic template and water were fully mixed. The molar ratio of the precursor solution was SiO2:0.4TPAOH:16H2O. The precursor solution was aged at 90°C for 24h. The reaction solution was transferred to a stainless steel autoclave reactor and reacted at 170°C for 24h. Before the synthesis of nanosheets, the seed crystals were washed with deionized water. The MFI crystals were collected by centrifugation at 13,122RCF (relative centrifugal force) for 1h and then decanting the supernatant. The solid was redispersed in deionized water using water bath ultrasound. After repeated washing twice, the dispersed solid was dried in an oven at 80 degrees overnight and then weighed. The size and morphology of the obtained product were confirmed by scanning electron microscopy, as shown in Figure 4.

[0056] 3) Synthesis of MFI nanosheets based on seed-assisted epitaxial growth using dC5 as an organic template. A silicon source, potassium hydroxide, template, and water were thoroughly mixed at a molar ratio of 80TEOS:3.75dC5:20KOH:9500H2O and hydrolyzed at 50°C for 24 hours under an argon purge (50mL / min). The mixture was then mixed with a dispersion containing MFI seeds and stirred for 10 minutes. The mixture was then transferred to a stainless steel tubular reactor and subjected to a hydrothermal reaction in an oil bath at 180°C for half an hour. The reaction mixture was then removed from the reactor and cooled in cold water for 3 minutes.

[0057] 4) After the reaction, a purification step was performed by washing away any amorphous silica contained in the synthesis with deionized water. The synthesized nanosheet dispersion was diluted with 10 mL of water and centrifuged at 10,000 relative centrifugal force (RCF) for 30 seconds. The supernatant from the centrifuge tube was poured into a new centrifuge tube and centrifuged at 13,122 relative centrifugal force (RCF) for 5 minutes. The supernatant was discarded and the solid product was collected. The solid was redispersed in deionized water and evenly dispersed using a vortex mixer and waterbath sonication. The sample was then centrifuged at 13,122 relative centrifugal force (RCF) for 5 minutes, and the supernatant was discarded to collect the product. The deionized water rinsing process was repeated three times. The collected nanosheet slurry was then dispersed in 2 mL of deionized water for characterization. After centrifugation, the sample was dried overnight. The crystallinity and orientation of the powder sample were determined by X-ray powder diffraction (XRD), as shown in Figure 5. The morphology of the nanosheets (NS) was observed by scanning electron microscopy, as shown in Figure 6. To measure the thickness of the nanosheets, 0.2 mL of the dispersion was dispersed in 2 mL of anhydrous ethanol and then deposited onto a SiO2 substrate. The monolayer thickness was approximately 4–5 nm, as shown in Figure 7.

[0058] Example 2

[0059] 1) The template used is the product of step (1) in Example 1.

[0060] 2) Seed crystals: the seed crystals from step (2) in Example 1

[0061] 3) Thoroughly mix the silicon source, potassium hydroxide, template, and water at a molar ratio of 80TEOS:3.75dC5:20KOH:9500H2O. Hydrolyze at 50°C for 24 hours under an argon purge (50 mL / min). Then, mix with the dispersion containing MFI seeds and stir for 10 minutes. The mixture is then transferred to a Teflon autoclave reactor and subjected to a hydrothermal reaction in a 155°C oven. After three days, remove the mixture, cool for three hours, and purify.

[0062] 4) The purification step was the same as step (4) in Example 1. The morphology of the obtained sample was observed by scanning electron microscopy, as shown in Figure 8. Compared with the result of rapid synthesis (4), using a reaction kettle as a reactor not only takes a long time, but also contains many unreacted amorphous impurities.

[0063] Example 3

[0064] 1) The template used is the product of step (1) in Example 1.

[0065] 2) Seed crystals: the seed crystals from step (2) in Example 1

[0066] 3) Thoroughly mix the silicon source, potassium hydroxide, template, and water at a molar ratio of 80TEOS:3.75dC5:20KOH:9500H2O. Hydrolyze at 50°C for 24 hours under an argon purge (50 mL / min). Then, mix with the dispersion containing MFI seeds and stir for 10 minutes. The mixture is then transferred to a tubular reactor and reacted in an oil bath at 180°C for 0.5, 2, and 4 hours, respectively. Afterwards, remove the mixture and cool in cold water for 3 minutes.

[0067] 4) The purification step is the same as step (4) in Example 1. The morphology of the obtained sample was observed by scanning electron microscopy, as shown in Figure 9. As the reaction time increases, the lateral size of the layered molecular sieve increases from about 20 μm to about 132 μm.

[0068] Those skilled in the art will readily conceive of other embodiments of the present application after considering the specification and practicing the contents disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present application that follow the general principles of this application and include common knowledge or customary techniques in the art that are not disclosed in this application.

[0069] It will be understood that the present application is not limited to the exact results which have been described above and shown in the accompanying drawings, and that various modifications and changes may be made without departing from the scope thereof.

Claims

1. A method for rapid synthesis of a two-dimensional molecular sieve, characterized in that: include: (1) mixing a silicon source, potassium hydroxide, a template and water in a molar ratio of 60-100:2-5:10-30:7500-9500, aging and hydrolyzing under argon purge to form a precursor sol; (2) mixing the precursor sol with a dispersion containing MFI crystal seeds and stirring them thoroughly, wherein the dispersion containing MFI crystal seeds is obtained by dispersing MFI crystal seeds in deionized water, the MFI crystal seeds are obtained by hydrothermal reaction of a silicon source, a template agent and water after heating and aging, and the molar ratio of the silicon source in the dispersion to the precursor sol is 1:50 to 1000; (3) The mixture obtained in step (2) is transferred to a stainless steel tubular reactor for hydrothermal reaction to synthesize a two-dimensional molecular sieve.

2. The method according to claim 1, characterized in that In step (1), the argon purging rate is 50-200 mL / min, the aging and hydrolysis temperature is 25 to 90° C., the aging time is 8 to 24 h, and the hydrolysis time is 8 to 36 h.

3. The method according to claim 1, characterized in that In step (1), the template is dC5.

4. The method according to claim 3, characterized in that The dC5 is obtained by heating 1,5-diaminopentane and 1-iodopropane for reflux reaction under anhydrous and oxygen-free conditions, wherein the reflux temperature is 75-85° C. and the argon purge speed is 50-100 mL / min.

5. The method according to claim 1, characterized in that: In step (1), the silicon source is colloidal silicon dioxide with a mass content of 25 to 30%.

6. The method according to claim 1, characterized in that In step (1), the water is deionized water.

7. The method according to claim 1, characterized in that In step (2), the mass ratio of the MFI seed crystal to the precursor sol is 2% to 10%.

8. The method according to claim 1, characterized in that The preparation process of the MFI seed crystal is as follows: The silicon source, the template and water are fully mixed in a molar ratio of 1:0.4 to 1:10 to 30, and aged under heating conditions to promote the full hydrolysis of the silicon source, wherein the aging time is 8 to 24 hours and the aging temperature is room temperature to 90° C.; The reaction solution after aging and hydrolysis is transferred to a stainless steel autoclave reactor for hydrothermal reaction to obtain seed crystals with a size of 80-90 nm, wherein the temperature of the hydrothermal reaction is 170-210°C.

9. The method according to claim 1, characterized in that: In step (3), the hydrothermal reaction is carried out at 160-200° C. for 0.5 h to 3 d.

10. The method according to claim 1, characterized in that The length of the tubular reactor is 10 to 15 cm.

11. A two-dimensional molecular sieve, characterized in that: The invention is prepared by the method according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Preparation method of nanorod particle ordered-assembly ZSM-5 zeolite molecular sieve

    CN103708495A

  • Method and device for continuously producing molecular sieve in tubular reactor

    CN115215351A

  • Molecular crosslinking molecular sieve nanosheet hybrid membrane, preparation method and application in flow battery

    CN115411292A

  • Continuous process and apparatus for preparing inorganic materials employing microwave