Rigid polyurethane foam raw material composition, and rigid polyurethane foam and preparation method therefor
By using high-viscosity Mannich polyether polyol and silicone oil premix to introduce nano-silica into rigid polyurethane foam, combined with supercritical carbon dioxide dispersion technology, the problem of poor storage and dispersion of nano-SiO2 in rigid polyurethane foam has been solved, and the efficiency has been improved. Foam performance and storage stability, reducing losses and CO2 emissions.
Patent Information
- Application Number
- PCT/CN2023/092324
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-05-05
- Publication Date
- 2024-10-17
AI Technical Summary
In existing rigid polyurethane foams, due to the vaporization of low-boiling point foaming agents and the loss of CO2, large mass losses occur, low foam strength, high thermal conductivity, and poor storage and dispersion effects of nanoscale SiO2, affecting production.
Using a polyurethane rigid foam raw material composition containing a large proportion of nano-silica, nano-silica is introduced in the form of Mannich polyether polyol and silicone oil premix, combined with supercritical carbon dioxide dispersion technology to form a high-viscosity pre-mix to improve the nanometer The stable dispersion and storage time of SiO2 adjust the surface tension of the liquid and enhance the toughness of the bubble wall.
It significantly reduces the agglomeration of nano-SiO2, improves the closed cell ratio, pressure bubble compression strength and adhesive force of the foam, reduces the thermal conductivity and CO2 emissions, extends the storage time of raw materials, and avoids damage to the foaming machine equipment.
Smart Images

Figure PCTCN2023092324-FTAPPB-I100001 
Figure PCTCN2023092324-FTAPPB-I100002 
Figure PCTCN2023092324-FTAPPB-I100003
Abstract
Description
A polyurethane rigid foam raw material composition and polyurethane rigid foam and preparation method thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application number CN2023103751980 filed with the Patent Office of China on April 10, 2023, entitled “A polyurethane rigid foam raw material composition and polyurethane rigid foam and preparation method thereof,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present invention belongs to the technical field of polyurethane rigid foam, and particularly relates to a polyurethane rigid foam raw material composition and polyurethane rigid foam and a preparation method thereof. Background Art
[0004] Currently, in rigid polyurethane foam, zero ODP (ozone depletion potential) is a Globally Preferred Product (GWP) requirement for blowing agents. The currently used mixed blowing agents include low-boiling-point blowing agents. Due to their low boiling point, low-boiling-point blowing agents vaporize and escape during the rigid polyurethane foam reaction, failing to form bubbles. This is because when the gas concentration is low, the surface tension of the liquid is high, resulting in a thin bubble surface and easy bubble breakage. Furthermore, CO2 released during the reaction escapes before bubbles form, causing significant losses. (In current rigid foam reactions, CO2 from the chemical reaction and the volatilization of the blowing agent typically results in a total mass loss of 3-7%, of which CO2 accounts for approximately 80% and the blowing agent for 20%. This loss not only contributes to mass loss, but also contributes to the greenhouse effect caused by CO2 emissions and the VOC impact caused by the volatilization of the blowing agent.) Furthermore, the foam has numerous bubbles, poor fluidity, and high thermal conductivity. Existing polyurethane foams also suffer from low foam strength and are prone to shrinkage. The introduction of nano-SiO2 can offer some improvement.
[0005] However, the storage requirements of nano-SiO2 are very high. It easily absorbs water and produces agglomeration effect with the moisture in the foaming combination polyether (white material), and its dispersion effect is poor. Generally, the amount added cannot exceed 0.3wt%, but a small amount will not achieve the above effect. The storage time of the added nano-SiO2 combination polyether is short and turbidity is prone to occur. At the same time, due to the agglomeration effect, the metering pump head of the foaming machine will be damaged by solid friction, resulting in inaccurate metering and damage to the metering pump. At the same time, it will also damage the nozzle of the foaming machine gun head, resulting in inaccurate proportions and leakage. Therefore, in the application of SiO2 in polyurethane rigid foam, it is necessary to seek new ways or materials so that it can effectively apply a large proportion of nano-SiO2, and can be stably stored without affecting production, and further improve performance.
[0006] Summary of the Invention
[0007] The present disclosure provides a polyurethane rigid foam raw material composition containing a large proportion of nano-silica, comprising a white material and a black material containing isocyanate, wherein the white material comprises a polyether polyol, a polyester polyol, a catalyst, water, a blowing agent, and silicone oil, and further comprises a Mannich polyether polyol and nano-silica, wherein the viscosity of the Mannich polyether polyol at 25° C. is greater than 13,000 MPa·s, and based on the total mass of the white material, the content of the Mannich polyether polyol is 3.7 wt%-10.5 wt%, the content of the silicone oil is 1 wt%-3 wt%, and the content of the nano-silica is 0.3 wt%-3 wt%.
[0008] Optionally, the Mannich polyether polyol, silicone oil and at least part of the nano-silica are introduced or present in the form of a premix, and the remaining part of the nano-silica is directly introduced or present in the white material. The amount of nano-silica in the premix accounts for 0.3wt%-1.5wt% of the total amount of the white material, and the viscosity of the premix at 25°C is 5700-10000 MPa·s.
[0009] Optionally, the remaining nano-silicon dioxide accounts for 0.1wt%-1.5wt% of the total amount of the white material, and the mass ratio of the partial nano-silicon dioxide in the premix to the remaining nano-silicon dioxide is 15:1-1:1.
[0010] Optionally, the premixed liquid is obtained by dispersion with supercritical carbon dioxide, and the premixed liquid also includes carbon dioxide.
[0011] Optionally, the nano-silica is hydrophobic nano-silica.
[0012] Optionally, the hydroxyl value of the Mannich polyether polyol is 470-520 mgKOH / g, and the viscosity of the Mannich polyether polyol at 25° C. is 25,000-35,000 MPa·s.
[0013] Optionally, the polyether polyol has a hydroxyl value of 430-470 mgKOH / g and a viscosity of 3000-5000 MPa·s at 25° C.; the polyester polyol has a hydroxyl value of 290-350 mgKOH / g and a viscosity of 2000-3000 MPa·s at 25° C.
[0014] Optionally, the total viscosity of the white material is controlled within a range of 4400-11000 MPa·s.
[0015] Optionally, the foaming agent can be selected from at least one of pentane, methyl formate, R245fa, LBA foaming agent, R600 foaming agent, R600a foaming agent, R-152a foaming agent, R-1234yf, Chemours Opteon 1100, Chemours Opteon 1150, and HCFO-1224yd.
[0016] Optionally, the polyether polyol is a polyether using compounds such as sucrose as an initiator.
[0017] Optionally, the polyester polyol is a polyester polyol based on diethylene glycol-phthalic anhydride.
[0018] Optionally, the catalyst is cycloethylamine.
[0019] Optionally, based on the total mass of the white material, the content of the polyether polyol is 45wt%-55wt%, the content of the polyester polyol is 2.5wt%-37wt%, the content of the catalyst is 2wt%-3wt%, the content of water is 1wt%-3wt%, and the content of the foaming agent is 10wt%-20wt%.
[0020] The present disclosure also provides a method for preparing polyurethane rigid foam, which is prepared using the polyurethane rigid foam raw material composition described above; the preparation method comprises the following steps:
[0021] Preparing a premix: mixing a Mannich polyether polyol, silicone oil, and at least a portion of nano-silicon dioxide with supercritical carbon dioxide at 32°C-40°C and 7.9-9 MPa, followed by venting the carbon dioxide; wherein the supercritical carbon dioxide is introduced at a rate of 3-4.5 kg / h and the mixing time is 0.5-3 hours;
[0022] The premixed liquid is mixed with other components of the white material to form a white material, and the white material is reacted with the black material to prepare a polyurethane rigid foam.
[0023] Optionally, the co-mixing method includes: first stirring and mixing, and then performing ultrasonic circulation dispersion, and the ultrasonic circulation dispersion process includes: turning on the ultrasonic wave for 3-7 seconds, stopping the ultrasonic wave for 8-15 seconds, and then turning on and stopping the ultrasonic wave in this cycle; wherein the stirring and mixing time is 0.5-3 hours, and the ultrasonic circulation dispersion time is 10-60 minutes.
[0024] The present disclosure also provides a polyurethane rigid foam, which is prepared by the method described above.
[0025] Optionally, the polyurethane rigid foam has a loss of 1.6%-2.4% by mass within three months of storage, a closed cell rate of 93%-99%, a pressure bubble compression strength of 155-170 kPa, a thermal conductivity of 0.0173-0.0184 W / (m·K), and an adhesion of 149-167 kPa. DETAILED DESCRIPTION
[0026] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Among them, the terms "optional" and "optional" all mean that they may be included or not (or may be present or not).
[0027] One embodiment of the present disclosure provides a polyurethane rigid foam raw material composition containing a large proportion of nano-silica, comprising a white material and a black material containing isocyanate, wherein the white material comprises a polyether polyol, a polyester polyol, a catalyst, water, a blowing agent, and silicone oil, and further comprises a Mannich polyether polyol and nano-silica, wherein the viscosity of the Mannich polyether polyol at 25° C. is greater than 13,000 MPa·s, and based on the total mass of the white material, the content of the Mannich polyether polyol is 3.7 wt%-10.5 wt%, the content of the silicone oil is 1 wt%-3 wt%, and the content of the nano-silica is 0.3 wt%-3 wt%. Alternatively, the content of the Mannich polyether polyol can be 4.0wt%-10.0wt%, 4.5wt%-9.5wt% or 5.0wt%-9.0wt%, such as 3.7wt%, 3.9wt%, 4.1wt%, 4.5wt%, 5.0wt%, 5.5wt%, 6.0wt%, 6.5wt%, 7.0wt%, 7.5wt%, 8.0wt%, 8.5wt%, 9.0wt%, 9.5wt%, 10.0wt% or 10.5wt%, or an interval value between any two of the above endpoints, but not limited to the above numerical range. Optionally, the content of silicone oil can be 1.2wt%-2.8wt%, 1.5wt%-2.5wt% or 1.8wt%-2.2wt%, such as 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt% or 3.0wt%, or an interval value between any two of the above endpoint values, but not limited to the above numerical range. Optionally, the content of nano-silica can be 0.4wt%-2.8wt%, 0.6wt%-2.5wt% or 0.8wt%-2.2wt%, such as 0.4wt%, 0.6wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt% or 3.0wt%, or an interval value between any two of the above endpoint values, but not limited to the above numerical range.
[0028] The present disclosure particularly introduces a special polyether with a special cyclic structure: a Mannich polyether polyol with a viscosity (25°C) greater than 13000 MPa.s, which has good dispersibility, good compatibility, compatibility and tolerance. It is combined with a foam leveling agent with very good dispersibility: silicone oil, which can reduce the possibility of agglomeration of a large proportion of nano-scale dioxide and play a role in the hard foam reaction without affecting other properties and without damaging the metering pump and gun nozzle.
[0029] The inventors of the present disclosure have discovered that the addition of nano-SiO2 to the white material significantly increases viscosity, resulting in excessively high viscosity and poor fluidity before the added portion is evenly mixed, which in turn exacerbates the formation of agglomerates, greatly affecting the effect of adding a large proportion of nano-SiO2. In this regard, in some optional embodiments of the present disclosure, the Mannich polyether polyol, silicone oil, and at least a portion of the nano-silica are introduced or present in the form of a premix, and the remaining nano-silica is directly introduced or present in the white material, with the amount of nano-silica in the premix accounting for 0.3wt%-1.5wt% of the total amount of the white material. Under this optional scheme, nano-SiO2 is at least partially present or introduced in the form of a premix, and the remaining part is directly added or present in the white material. The amount of nano-SiO2 in the premix is within the range of a suitable large proportion of 0.3-1.5%. Silicone oil itself is a foaming agent with very good dispersibility. It is combined with Mannich polyether, which is a cyclic structure with good compatibility, compatibility and tolerance. A premix with a suitable high viscosity is formed by combining silicone oil and Mannich polyether. After nano-SiO2 is added, a suitable high viscosity premix is formed, which greatly improves the compatibility with other white material components such as polyether polyols and polyester polyols, and can make nano-SiO2 more stably dispersed, increase the amount of nano-SiO2 added, and improve the stability of nano-SiO2 under higher proportions. The nano-SiO2 reduces the occurrence of agglomeration and has a better effect; by obtaining a premix, the storage time of the raw materials can be greatly increased; at the same time, the premix has suitable viscosity, fluidity and clarity, and the components in the premix are highly dispersed and there is no solid precipitation, so that the large proportion of nano-silica can fully play its role in optimizing the performance of polyurethane rigid foam during application; and it reduces damage to the nozzle of the foaming machine gun head, the raw materials can be stored stably, and the surface tension of the liquid can be adjusted, thereby enhancing the stabilizing dispersion effect of SiO2, making the bubbles less likely to break, reducing losses, enhancing the toughness of the bubble wall, improving the closed-cell rate of the bubbles, increasing the closed-cell rate, making the bubbles more uniformly arranged, the strength of the foam high, improving the compression strength of the pressure bubble, reducing the thermal conductivity, improving the bonding force, and reducing CO2 emissions. Under the same conditions, if the amount of nano-silica in the premix is greater than 1.5%, the viscosity of the nano-SiO2 premix changes too much, the fluidity deteriorates, it is easy to become turbid, and solids precipitate; if the amount of nano-silica in the premix is too low, the amount of nano-SiO2 added is significantly reduced and the performance cannot be optimized. Optionally, the amount of nano-silicon dioxide in the premixed liquid can be 0.4wt%-1.4wt%, 0.6wt%-1.2wt% or 0.8wt%-1.0wt% of the total white material, such as 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, or an interval value between any two of the above endpoint values, but not limited to the above numerical range.
[0030] Alternatively, the viscosity of the premix at 25 ° C is for example 5700-10000MPa·s, 6000-9000MPa·s or 7000-8000MPa·s, such as 5700MPa·s, 6000MPa·s, 6500MPa·s, 7000MPa·s, 7500MPa·s, 800MPa·s, 8500MPa·s, 9000MPa·s, 9500MPa·s or 10000MPa·s, or the interval value between any two endpoint values, but is not limited to above-mentioned numerical range. Under this optional scheme, the viscosity of the premix of the present disclosure is controlled within the suitable range of 5700-10000MPa·s, which is more conducive to the compatibility, fluidity and clarity of the premix, and there is no solid precipitation, and large proportion of nano-SiO2 will not reunite. Under the same conditions, if the viscosity is too high, the compatibility and fluidity of the mixture will deteriorate, it will easily become turbid, and solids will precipitate; if the viscosity is too low, there is a risk of nano-SiO2 agglomeration.
[0031] Alternatively, the remaining nano-silicon dioxide accounts for 0.1wt%-1.5wt% of the total amount of the white material. The remaining nano-silicon dioxide of the present disclosure accounts for the total amount of the white material within the above range, which can ensure fluidity, so that under the same conditions, nano-SiO2 exists stably, avoids its agglomeration, and effectively prolongs the storage time. Alternatively, the remaining nano-silicon dioxide accounts for 0.1wt%-0.29wt% of the total amount of the white material. In the optional scheme of the present disclosure, the amount of nano-silicon dioxide added to the white material is larger, and the viscosity and fluidity of the white material are suitable, and a large proportion of nano-SiO2 can exist stably, is not easy to agglomerate, and has a long storage time.
[0032] Alternatively, the mass ratio of the part of nano silicon dioxide in the premix and the remainder of nano silicon dioxide is 15:1-1:1. Under this optional scheme, it is more conducive to ensuring that the viscosity of the premix is suitable, fluidity is suitable, and the storage time is long, and production needs can be met, and it is not easy for muddiness, and there is no solid to separate out, and large-scale nano-SiO2 will not reunite. Under the same conditions, if higher than this ratio, in premix, addition is too high, causing the premix to add a high ratio, and viscosity excessively increases, and fluidity deteriorates, and the storage time is short, and production needs cannot be met, and it is easy to muddiness, and there is solid to separate out, and it is too low, and in white material, adding a high ratio, there is the possibility of reunion, and after adding, the effect cannot be effectively improved. Optionally, the mass ratio of some nano-silica to the remaining nano-silica in the premix can be 14:1-1:1, 12:1-1:1 or 10:1-1:1, such as 15:1, 14:1, 13:1, 12:1, 11:1, 10:1, 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2:1 or 1:1, or an interval value between any two of the above endpoint values, but is not limited to the above numerical range.
[0033] Optionally, the premix is obtained by dispersion through supercritical carbon dioxide, and the premix also includes carbon dioxide. Under this optional scheme, a large proportion of nano-SiO2 is added to the high-viscosity Mannich polyether polyol and silicone oil through the supercritical state of CO2, so that it can exist stably and reduce the possibility of agglomeration, thereby forming a premix containing a large proportion of nano-SiO2. In addition, the retention of some CO2 in the premix can achieve the combined effect of water, CO2, and nano-silica in the foaming process to improve the foaming and uniform foaming effect, thereby further improving the performance of polyurethane rigid foam.
[0034] Optionally, the nano-silica is hydrophobic nano-silica. In this optional solution, hydrophobic nano-silica has hydrophobic and lipophilic properties, making SiO2 more soluble in various polyethers. At the same time, due to its polarity, during the bubble formation process, the polarity difference formed by the hydrophilic ordinary polyether group at one end and the non-hydrophilic group at the other end is more easily formed when the polarity is balanced. At the same time, it is easier to form bubbles, which is more likely to reduce the liquid surface tension, reduce the foam diameter, and increase the number of bubbles, thereby enhancing storage stability.
[0035] In some optional embodiments of the present disclosure, the hydroxyl value of the Mannich polyether polyol is 470-520 mgKOH / g. The hydroxyl value of the Mannich polyether polyol is within the above range, which can be beneficial to optimizing the stable dispersion effect of large-scale nano-silica. The hydroxyl value of the Mannich polyether polyol is optionally 480-520 mgKOH / g, such as 480 mgKOH / g, 485 mgKOH / g, 490 mgKOH / g, 500 mgKOH / g, 510 mgKOH / g or 520 mgKOH / g, or an interval value between any two of the above endpoint values. Optionally, the viscosity of the Mannich polyether polyol at 25°C is 25000-35000 MPa·s. Selecting a Mannich polyether polyol with a hydroxyl value similar to that of polyether polyol and polyester polyol is more conducive to improving the miscibility with polyether polyol and polyester polyol, and is more conducive to optimizing the stable dispersion effect of large-scale nano-silica.
[0036] In some optional embodiments of the present disclosure, the hydroxyl value of the polyether polyol is 430-470 mgKOH / g, such as 430 mgKOH / g, 440 mgKOH / g, 450 mgKOH / g, 460 mgKOH / g or 470 mgKOH / g, or an interval value between any two of the above endpoint values; the viscosity of the polyether polyol at 25°C is 3000-5000 MPa·s, such as 3000 MPa·s, 3400 MPa·s, 3600 MPa·s, 3800 MPa·s, 4200 MPa·s, 4500 MPa·s, 4800 MPa·s or 5000 MPa·s, or an interval value between any two of the above endpoint values. The hydroxyl value of the polyether polyol and the viscosity of the polyether polyol are within the above ranges, which can improve compatibility, help optimize the stable dispersion effect of large-proportion nano-silica, improve fluidity, improve mixing uniformity with the premixed liquid, improve stability after mixing, improve foaming performance, and improve the hardness of the polyurethane rigid foam product. Optionally, the hydroxyl value of the polyester polyol is 290-350 mgKOH / g, optionally 300-330 mgKOH / g, and the viscosity of the polyester polyol at 25°C is 2000-3000 MPa·s. In the optional scheme disclosed herein, polyether polyols and polyester polyols with low viscosity and similar viscosities are used, and the hydroxyl values are similar, which can improve compatibility, and are more conducive to optimizing the stable dispersion effect of large-proportion nano-silica, improving fluidity, improving mixing uniformity with the premixed liquid, being more stable after mixing, and having good foaming performance, so that the polyurethane rigid foam product has better hardness.
[0037] Optionally, based on the total mass of the white material, the content of the polyether polyol is 45wt%-55wt%, the content of the polyester polyol is 2.5wt%-37wt%, the content of the catalyst is 2wt%-3wt%, the content of water is 1wt%-3wt%, and the content of the foaming agent is 10wt%-20wt%.
[0038] In some optional embodiments of the present disclosure, the white material total viscosity is controlled at 4400-11000MPa·s. Optionally, the white material total viscosity is 4500-10500MPa·s, 5500-9500MPa·s or 6500-8500MPa·s, such as 4500MPa·s, 5000MPa·s, 5500MPa·s, 6000MPa·s, 6500MPa·s, 7000MPa·s, 7500MPa·s, 8000MPa·s, 9500MPa·s, 10000MPa·s or 11000MPa·s, or an interval value between any two endpoint values. Without being bound by theory, the white material of the present disclosure has good fluidity and suitable viscosity, is more conducive to improving nano-SiO2 stability, avoids agglomeration, and realizes long-term stable storage (more than three months).
[0039] In some optional embodiments of the present disclosure, the total viscosity of the white material is controlled within a range of 4400-7400 MPa·s.
[0040] In the present disclosure, the polyether polyol, polyester polyol, catalyst, foaming agent, and silicone oil can achieve the purpose of the present disclosure on the basis of satisfying the above conditions, and existing corresponding types can be used. For example, the polyether polyol can be a polyether using a compound such as sucrose as an initiator. For example, the polyester polyol can be a polyester polyol based on diethylene glycol-phthalic anhydride. For example, the catalyst can be cyclohexylamine. For example, the foaming agent can be selected from at least one of pentane, methyl formate, R245fa, LBA foaming agent, R600 foaming agent, R600a foaming agent, R-152a foaming agent, R-1234yf, Chemours Opteon 1100, Chemours Opteon 1150, and HCFO-1224yd.
[0041] The black material disclosed herein may be crude MDI (BASF M20S).
[0042] In the present disclosure, those skilled in the art can mix the white material and the black material according to the existing conventional ratio. For example, the mass ratio of the white material to the black material can be 1:1-3.
[0043] One embodiment of the present disclosure provides a method for preparing a polyurethane rigid foam, which is prepared using the polyurethane rigid foam raw material composition described in the first aspect; the preparation method comprises the following steps:
[0044] S1. Preparing a premix: subjecting a Mannich polyether polyol, silicone oil, and at least a portion of nano-silicon dioxide to a supercritical carbon dioxide mixture at 32°C-40°C and 7.9-9 MPa, followed by venting the carbon dioxide; wherein the supercritical carbon dioxide is introduced at a rate of 3-4.5 kg / h;
[0045] S2, the premixed liquid is mixed with other components of the white material to form a white material, and the white material is reacted with the black material to prepare a polyurethane rigid foam. It is understood that the other components of the white material here may include the remaining nano-silicon dioxide not added to the premixed liquid, or may not include separate nano-silicon dioxide.
[0046] The temperature, pressure, introduction speed and other conditions of the supercritical carbon dioxide mixing treatment in the preparation of the premixed liquid in S1 of the present disclosure provide a better dispersion effect. At the same time, part of the CO2 is retained through the high-viscosity premixed liquid containing nano-SiO2, thereby achieving the combined effect of water, CO2 and nano-silica in the foaming process to improve the foaming and uniform foaming effect, thereby further improving the performance of the polyurethane rigid foam.
[0047] Optionally, the conditions for the supercritical carbon dioxide mixing treatment also include: the mixing treatment time is 0.5-3 hours.
[0048] In some optional embodiments of the present disclosure, the co-mixing (which can be any of the two methods of adding the premixed liquid in S2) includes: first stirring and mixing, and then performing ultrasonic cyclic dispersion, and the process of ultrasonic cyclic dispersion includes: turning on the ultrasonic wave for 3-7 seconds, stopping the ultrasonic wave for 8-15 seconds, and then turning on the ultrasonic wave and stopping the ultrasonic wave in this cycle. Under this optional scheme, the use of the ultrasonic periodic application method can improve the dispersibility of nano-silicon dioxide and the fusion effect of different materials, especially for the addition of a large proportion of nano-SiO2 0.3%-1.5% to the white material. It is more suitable, further effectively reducing the possibility of agglomeration of a larger proportion of nano-SiO2 in the white material during the mixing process.
[0049] Optionally, the stirring and mixing time is 0.5-3 hours, and the ultrasonic circulation dispersion time is 10-60 minutes.
[0050] One embodiment of the present disclosure provides a polyurethane rigid foam, which is prepared by the preparation method described in the second aspect.
[0051] The polyurethane rigid foam disclosed in the present invention meets the following requirements: in the machine test under the national standard test conditions, the mass loss is 1.6%-2.4%, the closed cell rate is 93%-99%, the pressure bubble compression strength is 155-170kPa, the thermal conductivity is 0.0173-0.0184W / (m·K), and the adhesion is 149-167kPa. The polyurethane rigid foam here refers to the machine test performance within three months of storage. Among them, the closed cell rate is measured according to GB / T10799-2008, the pressure bubble compression strength is measured according to GB / T8813-2020 / ISO 844:2014, the thermal conductivity is measured according to GB / T10294 / ISO 8302:1991, and the adhesion is measured according to GB / T20219-2006 / ISO 8073:1987.
[0052] The present disclosure provides a polyurethane rigid foam raw material composition, a polyurethane rigid foam and a preparation method thereof. The polyurethane rigid foam raw material composition can increase the addition amount of nano-scale SiO2, reduce the agglomeration of nano-scale SiO2, and improve storage stability, thereby overcoming the defects of the prior art of nano-scale SiO2, such as high storage requirements, easy water absorption and agglomeration effect with moisture in the foaming combination polyether, and poor dispersion effect.
[0053] The polyurethane rigid foam raw material composition disclosed in the present invention specifically introduces a special polyether with a special cyclic structure: a Mannich polyether polyol with a viscosity (25°C) greater than 13000 MPa.s. The high-viscosity special Mannich polyether polyol is selected and combined with a high proportion of nano-SiO2 and silicone oil to stably disperse the nano-SiO2, improve the dispersion effect of the nano-SiO2, improve its storage stability, increase the amount of nano-SiO2 added, reduce the agglomeration of high-proportion nano-SiO2, reduce damage to the nozzle of the foaming machine gun during application, and ensure stable storage of the raw materials; it can also adjust the surface tension of the liquid, enhance the stable dispersion effect of SiO2, make bubbles less likely to break, reduce loss (such as a relatively good low loss rate of 2.8%), enhance the toughness of the bubble wall, improve the closed-cell rate of the bubble (such as the closed-cell rate can be increased to 93%, etc.), make the bubble arrangement more uniform, the foam strength is high, the pressure bubble compression strength is improved, the thermal conductivity coefficient is reduced, the adhesion is improved, and the CO2 emissions are reduced.
[0054] In the optional scheme disclosed herein, an appropriate amount of nano-silicon dioxide is present or introduced in the form of a premixed liquid, which is more conducive to improving the dispersion effect of nano-SiO2, improving its storage stability, increasing the amount of nano-SiO2 added, reducing the agglomeration of high-proportion nano-SiO2, reducing damage to the nozzle of the foaming machine gun head during application, increasing the closed-cell rate of bubbles, arranging bubbles more evenly, increasing the strength of the foam, improving the compression strength of the pressure bubble, reducing the thermal conductivity coefficient, and improving the adhesion and other properties.
[0055] In the preparation method disclosed herein, Mannich polyether polyol, silicone oil, and at least a portion of nano-silica are mixed with supercritical carbon dioxide to prepare a premix. The nano-silica enters the mixture in a supercritical state, and its dispersibility is increased by 100 times, thereby enhancing the dispersibility of a large proportion of nano-silica and the storage stability after dispersion.
[0056] Example
[0057] The embodiments of the present disclosure are described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present disclosure and are not to be construed as limiting the present disclosure. The raw materials in all examples (including the following comparative examples and examples) are as follows:
[0058] Polyether polyol 4110, with a hydroxyl value of 450 ± 20 mgKOH / g and a viscosity of 4000 ± 1000 MPa·s at 25°C, was purchased from Hebei Yadong Chemical Group Co., Ltd.
[0059] Polyether polyol 3152, with a hydroxyl value of 300-330 mgKOH / g and a viscosity of 2000-3000 MPa·s at 25°C, was purchased from Jiahua Chemical (Fushun) New Materials Co., Ltd.
[0060] The catalyst is cycloethylamine;
[0061] Silicone oil was L-6813, purchased from Momentive (formerly Toshiba GE) Advanced Materials Company;
[0062] The blowing agent is pentane;
[0063] Nano-sized SiO2 (particle size 20 nm) was purchased from Hubei Huifu Nanomaterials Co., Ltd.;
[0064] Mannich polyether polyol was RF-3778, with a hydroxyl value of 480-520 mgKOH / g and a viscosity of 25,000-35,000 MPa·s at 25°C, purchased from Jiahua Chemical (Fushun) New Materials Co., Ltd.
[0065] Black material B is crude MDI (BASF M20S).
[0066] Among them, the national standards for each test index are as follows: closed cell rate is measured according to GB / T10799-2008, pressure bubble compression strength is measured according to GB / T8813-2020 / ISO 844:2014, thermal conductivity is measured according to GB / T10294 / ISO 8302:1991, and adhesion is measured according to GB / T20219-2006 / ISO 8073:1987. Loss is obtained based on actual measurement comparison and is calculated as loss / total amount. Comparative Example 1
[0067] The components of the white material and their mass contents, as well as the liquid conditions of the white material components after being mixed and stored for a certain period of time, are shown in Table 1.
[0068] Table 1 (All components are measured by mass)
[0069] As can be seen from Table 1 above, when the addition of nano-silica exceeds 3%, solids precipitate and the product becomes turbid. At the same time, when the addition amount increases from 0.2% to 1.8%, its storage stability gradually decreases. When 0.2% is added, the product becomes turbid after 3 months of storage; when 0.3% is added, the product becomes turbid after 1 month of storage; and when 1.8% is added, solids precipitate after 1 month of storage.
[0070] The polyurethane rigid foam was obtained by mixing the white material and the black material B for reaction. The mixing quality ratio of the white material and the black material B is shown in Table 2, and the test indicators of the polyurethane rigid foam are shown in Table 2.
[0071] Table 2
[0072] From the tests in Table 1-2, we can see that:
[0073] 1) Adding less than 0.3% nano-SiO2 has little effect on foam performance.
[0074] 2) When the addition of nano-SiO2 exceeds 0.3%, various properties are significantly improved.
[0075] 3) When the addition of nano-SiO2 exceeds 0.3%, the white material becomes turbid during storage, solids precipitate, and performance deteriorates. At the same time, the foaming machine pump head and gun nozzle wear and tear occur.
[0076] 4) When the amount of nano-SiO2 was increased from 0.3% to 1.8%, the performance changed more significantly. After long storage time, the performance decreased and the degree of wear increased.
[0077] 5) When the addition of nano-SiO2 exceeds 3%, the ingredients become turbid and solids precipitate.
[0078] From the above, we can see that 1) Nano-SiO2 can improve various properties within the range of 0.3%-3%; 2) The storage period of nano-SiO2 added is less than one month, which cannot meet production requirements.
[0079] Example 1
[0080] A polyurethane rigid foam, the preparation method of which is as follows:
[0081] S1. Preparation of premix: Under the conditions of 35° C. and 8 MPa, the components of the premix shown in Table 3 in the pressure tank were subjected to supercritical carbon dioxide mixing treatment, and then the carbon dioxide was vented; wherein the supercritical carbon dioxide was introduced at a rate of 4 kg / h and the mixing time was 1 h; the viscosity of the premix and the liquid stored for a certain period of time after mixing were respectively as shown in Table 3, and the amount of each component in Table 3 was measured based on the content in the white material.
[0082] S2. The premixed liquid is co-mixed with other components of the white material to form a white material. The viscosity of the white material and the liquid state after storage for a certain period of time after mixing are shown in Table 4. The co-mixing method includes: first stirring and mixing for 1 hour, and then performing ultrasonic cyclic dispersion. The ultrasonic cyclic dispersion process includes: turning on the ultrasonic wave for 5 seconds, stopping for 10 seconds, then turning on the ultrasonic wave for 5 seconds, stopping for 10 seconds, and cyclic dispersion for 20 minutes.
[0083] S3. White material D was then mixed with black material B for a reaction test. The mass ratio of D:B was 1:1.2. The test indicators of the polyurethane rigid foam are shown in Table 5.
[0084] Table 3
[0085] Table 4
[0086] Tables 3-4 above demonstrate that the white stock prepared with a premix that meets the three-month storage requirement achieves the same results as the premix. When the premix contains nanosilica at a concentration of 0.175wt% to 1.5wt% of the total white stock, the three-month production requirement of no turbidity can be met. However, when the premix contains nanosilica at a concentration above 1.5wt%, the product can only be stored stably for less than one month, failing to achieve the three-month storage requirement of no turbidity.
[0087] Table 5
[0088] From the data in Table 5 above, we can see that:
[0089] 1) In the experiment of Group A without adding SiO2 (its composition is the same as Group A in Comparative Example 1), there are many bubbles, coarse cells, and corrosion of the inner tank occurs.
[0090] 2) When the amount of SiO2 added is less than 0.175%, the effect does not change much.
[0091] 3) The experimental groups with SiO2 additions exceeding 0.25% and below 3% showed significant improvements in loss, closed cell ratio, pressure bubble strength, thermal conductivity, adhesion, and bubble reduction. The magnitude of these improvements increased with increasing SiO2 addition. Storage stability was minimally impacted. Neither the foaming machine metering pump nor the nozzle wear was observed. This significantly improved performance while meeting production needs.
[0092] Example 2
[0093] The same method as in Example 1 was used for the preparation of D4 and its experimental group, except that the components in C4 were not pre-mixed into a premixed solution, but were directly mixed with other components of the white material to obtain white material D7. The viscosity of the white material was 10,000-11,000 MPa·s, and the other properties were the same.
[0094] The storage conditions of white material D7 were the same as those of the D4 experimental group in Example 1. The test results of D7 are shown in Table 5.
[0095] It can be seen that the optional solution of forming a premixed liquid in advance according to the present disclosure is more conducive to improving the performance of polyurethane rigid foam while ensuring long-term storage, among which the loss, closed cell rate, pressure bubble strength, thermal conductivity, adhesion, and bubble reduction are all significantly improved.
[0096] The above describes in detail the optional embodiments of the present disclosure, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure can be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as the contents disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability
[0097] The present disclosure provides a polyurethane rigid foam raw material composition and a polyurethane rigid foam and a preparation method thereof, which can stably disperse a large proportion of nano-scale SiO2, improve its storage stability, reduce the agglomeration of a high proportion of nano-scale SiO2, and reduce damage to the nozzle of the foaming machine gun head during application, thereby having excellent practical properties.
Claims
1. A polyurethane rigid foam raw material composition containing a large proportion of nano-silicon dioxide, comprising a white material and a black material containing isocyanate, wherein the white material comprises polyether polyol, polyester polyol, a catalyst, water, a blowing agent and silicone oil, characterized in that: The white material further comprises Mannich polyether polyol and nano-silicon dioxide. The viscosity of the Mannich polyether polyol at 25° C. is greater than 13000 MPa·s. Based on the total mass of the white material, the content of the Mannich polyether polyol is 3.7wt%-10.5wt%, the content of the silicone oil is 1wt%-3wt%, and the content of the nano-silicon dioxide is 0.3wt%-3wt%.
2. The polyurethane rigid foam raw material composition according to claim 1, characterized in that: The Mannich polyether polyol, silicone oil and at least part of the nano-silicon dioxide are introduced or present in the form of a premixed liquid, and the remaining part of the nano-silicon dioxide is directly introduced or present in the white material. The amount of the nano-silicon dioxide in the premixed liquid accounts for 0.3wt%-1.5wt% of the total amount of the white material, and the viscosity of the premixed liquid at 25° C. is 5700-10000 MPa·s.
3. The polyurethane rigid foam raw material composition according to claim 1 or 2, characterized in that: The remaining nano silicon dioxide accounts for 0.1wt%-1.5wt% of the total amount of the white material, and the mass ratio of the part of nano silicon dioxide in the premixed liquid to the remaining nano silicon dioxide is 15:1-1:
1.
4. The polyurethane rigid foam raw material composition according to claim 1 or 2, characterized in that: The premixed liquid is obtained by dispersion through supercritical carbon dioxide, and the premixed liquid also includes carbon dioxide; and / or the nano-silicon dioxide is hydrophobic nano-silicon dioxide.
5. The polyurethane rigid foam raw material composition according to claim 1, characterized in that: The hydroxyl value of the Mannich polyether polyol is 470-520 mgKOH / g, and the viscosity of the Mannich polyether polyol at 25° C. is 25000-35000 MPa·s; And / or, the hydroxyl value of the polyether polyol is 430-470 mgKOH / g, and the viscosity of the polyether polyol at 25°C is 3000-5000 MPa·s; the hydroxyl value of the polyester polyol is 290-350 mgKOH / g, and the viscosity of the polyester polyol at 25°C is 2000-3000 MPa·s.
6. The polyurethane rigid foam raw material composition according to claim 5, characterized in that: Based on the total mass of the white material, the content of the polyether polyol is 45wt%-55wt%, the content of the polyester polyol is 2.5wt%-37wt%, the content of the catalyst is 2wt%-3wt%, the content of water is 1wt%-3wt%, and the content of the foaming agent is 10wt%-20wt%.
7. The polyurethane rigid foam raw material composition according to any one of claims 1 to 6, characterized in that: The total viscosity of the white material is controlled within the range of 4400-11000 MPa·s.
8. The polyurethane rigid foam raw material composition according to any one of claims 1 to 6, characterized in that: The blowing agent may be selected from at least one of pentane, methyl formate, R245fa, LBA blowing agent, R600 blowing agent, R600a blowing agent, R-152a blowing agent, R-1234yf, Chemours Opteon 1100, Chemours Opteon 1150, and HCFO-1224yd; and / or The polyether polyol is a polyether using compounds such as sucrose as an initiator; and / or The polyester polyol is a polyester polyol based on diethylene glycol-phthalic anhydride; and / or The catalyst is cycloethylamine.
9. A method for preparing polyurethane rigid foam, characterized in that: It is prepared using the polyurethane rigid foam raw material composition according to any one of claims 1 to 8; the preparation method comprises the following steps: Preparing a premixed liquid: subjecting Mannich polyether polyol, silicone oil and at least a portion of nano-silicon dioxide to a supercritical carbon dioxide mixing treatment at 32-40° C. and 7.9-9 MPa, and then venting the carbon dioxide; wherein the supercritical carbon dioxide is introduced at a rate of 3-4.5 kg / h and the mixing treatment time is 0.5-3 h; The premixed liquid is mixed with other components of the white material to form a white material, and the white material is reacted with the black material to prepare a polyurethane rigid foam.
10. The method according to claim 9, characterized in that The co-mixing method includes: first stirring and mixing, and then ultrasonic cyclic dispersion, the process of ultrasonic cyclic dispersion includes: turning on the ultrasonic wave for 3-7 seconds, stopping the ultrasonic wave for 8-15 seconds, and then turning on and stopping the ultrasonic wave in this cycle; wherein the stirring and mixing time is 0.5-3 hours, and the ultrasonic cyclic dispersion time is 10-60 minutes.
11. A polyurethane rigid foam, characterized in that: It is prepared by the method according to claim 9 or 10.
12. A polyurethane rigid foam according to claim 11, characterized in that: The polyurethane rigid foam has a loss of 1.6%-2.4% by mass within three months of storage, a closed cell rate of 93%-99%, a pressure bubble compression strength of 155-170 kPa, a thermal conductivity of 0.0173-0.0184 W / (m·K), and an adhesive force of 149-167 kPa.
Citation Information
Patent Citations
Rigid foam polyurethane thermal insulation material
CN105601868A
Modified silica sol, preparation method thereof, and application of same in all-water-based foaming polyurethane spraying foam
CN111171374A
Premixed polyether, polyurethane material for door plate filling and preparation method and application of polyurethane material
CN114149553A
Rigid polyurethane foam
JP2005307143A
Rigid polyurethane foam
US20200299453A1