Method for preparing perovskite complex for x-ray detection, and product of method and use thereof
By introducing polar solvents into perovskite powder to synthesize perovskite-solvent complexes, the challenges of perovskite single crystal growth and thick film preparation have been solved, achieving densification and improved stability of high-efficiency X-ray detectors to meet market demands.
Patent Information
- Application Number
- PCT/CN2023/093009
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2023-05-09
- Publication Date
- 2024-10-17
AI Technical Summary
In existing technologies, the growth of perovskite single crystals is time-consuming and difficult to prepare on a large scale. The limited solubility of the precursor makes it difficult to prepare perovskite thick films that meet the requirements. Furthermore, voids and grain boundaries in polycrystalline perovskite wafers affect the efficiency and stability of the detector.
By introducing a polar solvent into perovskite powder to synthesize a perovskite-solvent complex, the affinity of the solvent is used to promote wafer densification and recrystallization during the pressing process. Combined with a conductive substrate, a high-efficiency X-ray detector is fabricated.
Obtaining dense and uniform perovskite wafers improves the photoresponse sensitivity and stability of X-ray detectors, enabling integration with substrates and meeting market demands.
Smart Images

Figure CN2023093009_17102024_PF_FP_ABST
Abstract
Description
A preparation method of perovskite complex for X-ray detection and its products and applications Technical Field
[0001] The present application belongs to the field of perovskite X-ray detection, and relates to a preparation method of a perovskite complex for X-ray detection, and its products and applications. Background Art
[0002] X-ray detection has been widely used in medical imaging, industrial inspection, security inspection and other fields, and is closely related to people's lives. In order to reduce the radiation damage caused by high-dose X-rays, X-ray detectors are currently required to have higher sensitivity and lower detection limits. Generally, X-ray detectors have two different detection modes: direct and indirect. Indirect detection relies on scintillators for secondary photoelectric conversion, which inevitably suffers from difficult-to-overcome problems such as low efficiency and visible light dispersion, resulting in low detection sensitivity, high radiation dose and poor spatial resolution. In contrast, direct X-ray detectors based on semiconductor materials can directly convert X-rays into electrical signals through a single photoelectric conversion, thus having higher detection efficiency and lower detection limits. The development of new and efficient photosensitive semiconductor materials is the key to the application of direct X-ray imaging detectors.
[0003] Perovskite has great application potential in the field of direct X-ray detection due to its advantages such as large X-ray stopping energy, high carrier mobility and long carrier lifetime. In order to fully absorb high-energy X-rays, the thickness of the perovskite active layer should reach hundreds of microns. At present, the application of perovskite in X-ray is mainly based on single crystals and thin films, but the growth of perovskite single crystals is time-consuming and difficult to prepare on a large scale. Due to the limited solubility of the precursor, it is also difficult to prepare a perovskite thick film that meets the requirements through the solution method. Compacting perovskite powder to form a polycrystalline perovskite wafer can construct a perovskite X-ray detection photosensitive layer with adjustable size and thickness, but the polycrystalline inorganic perovskite wafer prepared in this way usually contains many voids and grain boundaries, which seriously affect the efficiency and working stability of the X-ray detector, and it is difficult to further integrate it with the substrate circuit.
[0004] In summary, in order to further promote the application of perovskite materials in the field of X-ray detectors, it is necessary to improve the quality of perovskite crystals and perovskite thick films to prepare high-performance X-ray detectors.
[0005] Summary of the Invention
[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0007] The present application provides a preparation method of a perovskite complex for X-ray detection, and its products and applications.
[0008] In a first aspect, the present application provides a method for preparing a perovskite complex for X-ray detection, the preparation method comprising: mixing perovskite with a solvent to obtain a mixture, and drying the mixture to obtain the perovskite complex;
[0009] The solvent includes a polar solvent A and a solvent B; the polar solvent A includes any one or a combination of at least two of DMF (dimethyl sulfoxide), DMSO (N,N-dimethylformamide), GBL (γ-butyrolactone) or NMP (N-methyl-2-pyrrolidone);
[0010] The perovskite comprises a chemical formula of X n Pb n Y 3n The lead halide perovskite, wherein n is an integer of 1 or greater than 1 (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.), the X is independently selected from any one of MA (methylamine), FA (formamidine) or Cs (cesium), and the Y is independently selected from I or Br.
[0011] Preferably, the X n Pb n Y 3n For example, MAPbI3, MAPbBr3, FAPbI3, FAPbBr3, CsPbI3, CsPbBr3, MAPbI2Br, MAPbIBr2, FAPbI2Br, FAPbIBr2, CsPbI2Br, CsPbIBr2, MAFAPb2I6, MAFAPb2Br6, MAFAPb2I2Br4, MAFAPb2I4Br2, MA2Pb2I6, MA2Pb2Br6, FA2Pb2I6, FA2Pb2Br6, Cs2Pb2I6, Cs2Pb2Br6, MA3Pb3I9, MA3Pb3Br9, FA3Pb3I9, FA3Pb3Br9, Cs3Pb3I9, Cs3Pb3Br9, etc.
[0012] Preferably, the solvent B comprises any one of chloroform, toluene, isopropyl alcohol, acetone, chlorobenzene or diethyl ether, or a combination of at least two thereof.
[0013] Preferably, the mass ratio of perovskite to solvent in the mixture is 1:(5-20);
[0014] Specific numerical values in the above (5-20) include 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, etc.
[0015] Preferably, the volume ratio of the polar solvent A to the solvent B is (1-10):(100-200);
[0016] The specific values in the above (1-10) are, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.;
[0017] The specific numerical values in the above (100-200) include, for example, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc.
[0018] Preferably, the mixing temperature is 15-40°C, for example, 15°C, 17°C, 20°C, 22°C, 25°C, 27°C, 30°C, 32°C, 35°C, 37°C, 40°C, etc., and the mixing time is 30-120min, for example, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, etc.
[0019] Preferably, the mixing is performed under stirring, and the stirring speed is 200-1000 rpm, for example, 200 rpm, 400 rpm, 500 rpm, 600 rpm, 800 rpm, 1000 rpm, etc.
[0020] Preferably, the drying temperature is 20-60°C, such as 20°C, 30°C, 40°C, 50°C, 60°C, etc.
[0021] Preferably, the process further comprises centrifuging the mixture and discarding the supernatant (discarding the solvent) before drying.
[0022] Preferably, the centrifugal rotation speed is 2000-6000 rpm, for example, 2000 rpm, 3000 rpm, 4000 rpm, 5000 rpm, 6000 rpm, etc.
[0023] Preferably, the perovskite is prepared by a preparation method comprising the following steps:
[0024] Lead halide, a halogen-containing compound and an organic solvent are mixed to obtain a precursor solution, which is then mixed with an anti-solvent to precipitate a reaction product, which is then dried to obtain the perovskite.
[0025] The lead halide includes PbI2 and / or PbBr2; the halogen-containing compound includes any one or a combination of at least two of MAI (methylamine iodide), FAI (formamidine iodide), CsI, MABr (methylamine bromide), FABr (formamidine bromide) or CsBr.
[0026] Preferably, the molar ratio of the lead halide to the halogen-containing compound is (1-2):(1-2);
[0027] The specific numerical values in (1-2) above are, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, etc.;
[0028] The preferred molar ratio is 1:1.
[0029] Preferably, the organic solvent includes any one of DMF, DMSO, NMP or GBL, or a combination of at least two thereof.
[0030] Preferably, the anti-solvent comprises any one of chloroform, toluene, isopropanol, acetone, chlorobenzene or diethyl ether, or a combination of at least two thereof.
[0031] Preferably, the volume ratio of the organic solvent to the anti-solvent is (1-10):(10-200);
[0032] The specific values in the above (1-10) are, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.;
[0033] Specific numerical values in the above (10-200) include 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc.
[0034] In a second aspect, the present application provides a perovskite complex prepared by the preparation method described in the first aspect.
[0035] In a third aspect, the present application provides a method for preparing a perovskite wafer, the method comprising: preparing a perovskite complex by the preparation method as described in the first aspect, and pressing the perovskite complex into a sheet; or
[0036] The prepared perovskite complex is mixed with perovskite, and then tabletted to obtain the product.
[0037] In the present application, the perovskite wafer can be obtained by pressing the perovskite complex alone, or the perovskite complex and perovskite can be mixed and pressed to obtain the perovskite wafer.
[0038] Preferably, in the mixing, the mass ratio of the perovskite complex to the perovskite is (1-10):(1-10);
[0039] Specific numerical values in the above (1-10) include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.
[0040] Preferably, the tableting is carried out under the conditions of 3-20 MPa and 80-150°C;
[0041] Specific values in the above 3-20 MPa include 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa, 16 MPa, 17 MPa, 18 MPa, 19 MPa, 20 MPa, etc.;
[0042] Specific values in the above 80-150°C include 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc.
[0043] Preferably, when the pressing pressure is 5 MPa and the temperature is 100° C., the obtained wafer has a good surface morphology.
[0044] Preferably, the tableting time is 10-40 min, for example, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, etc.
[0045] In the technical solution of the present application, by selecting molds of different sizes and changing the mass of the powder (perovskite complex powder and optional perovskite powder), wafers with controllable size and thickness can be obtained; taking a mold size of 10mm×10mm as an example, 180-300mg of the above powder is weighed, and wafers with a thickness of 500μm-1mm can be obtained by tableting.
[0046] Preferably, the tableting is followed by annealing to ensure that all residual solvents have evaporated.
[0047] Preferably, the annealing temperature is 80-200°C, for example, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, etc., and the annealing time is 30-120min, for example, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, etc.
[0048] In a fourth aspect, the present application provides a perovskite wafer prepared by the preparation method described in the third aspect.
[0049] In a fifth aspect, the present application provides the use of the perovskite complex prepared by the preparation method described in the first aspect or the perovskite wafer prepared by the preparation method described in the third aspect in the preparation of an X-ray detector.
[0050] In a sixth aspect, the present application provides an X-ray detector, the components of which include an active layer, an electrode and an optional transmission layer, and the material of the active layer includes a perovskite wafer prepared by the preparation method described in the third aspect.
[0051] The X-ray detector: ① can be a PIN or NIP photodiode device including an active layer, a transmission layer and an electrode, wherein the perovskite wafer is used as the active layer material; ② can only include an active layer and an electrode, wherein the perovskite wafer is used as the active layer material.
[0052] Preferably, the transmission layer can be made of a commonly used transmission layer material in the art, such as C 60 , BCP, PCBM, poly-TPD, PEDOT:PSS, NiO x , PTAA, TAPC, P3HT, TiO x 、MoO x , MoO3, V2O5, WO3 and other materials or a multilayer structure composed thereof, the thickness can be 1-300nm.
[0053] Preferably, the electrode can be made of conventional electrode materials in the art, such as metal electrodes such as Cu, Ag, Au, Al, Cr, or carbon electrodes, and the thickness can be 30-200 nm.
[0054] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to limited space and for the sake of simplicity, this application no longer exhaustively lists the specific point values included in the range.
[0055] Compared with the prior art, this application has the following beneficial effects:
[0056] The following problems exist in the current state of the art when using perovskite materials to prepare X-ray detectors: (1) The growth of perovskite single crystals takes a long time and is difficult to prepare on a large scale; (2) Due to the limited solubility of the precursor, it is difficult to prepare a perovskite thick film that meets the requirements through a solution method; and (3) The prepared perovskite powder is difficult to compact into wafers. Even if compacted, the polycrystalline inorganic perovskite wafers contain many voids and grain boundaries, which seriously affect the efficiency and working stability of the X-ray detector and are difficult to further integrate with the substrate circuit.
[0057] The purpose of this application is to overcome the above problems and prepare a high-efficiency (high-sensitivity) X-ray detector using perovskite materials.
[0058] The preparation method provided in the present application utilizes the affinity between lead halide perovskite and polar organic solvents, and synthesizes a perovskite-solvent complex by introducing an appropriate amount of polar solvent into the perovskite powder. The obtained solvent complex is soft in texture, has better processing flexibility, and can obtain dense and uniform perovskite wafers under less pressure. Not only that, the pressure applied during the tableting process can cause the solvent in the complex to be squeezed out. On the one hand, the solvent can act as an adhesive to promote further bonding of the wafer to the substrate; on the other hand, the solvent can effectively promote recrystallization during volatilization, further promote grain boundary fusion on the wafer surface, improve charge transfer performance, and reduce dark current. In addition, during the wafer growth process, it can be integrated with a conductive substrate (ITO glass, TFT or CMOS pixel chip), so that it can be used to prepare high-efficiency X-ray detectors (the light response sensitivity of the X-ray detector made from the perovskite-solvent complex provided in the present application can reach 6737μC Gy air -1 cm -2 The method is simple to operate, novel and unique, and can obtain a perovskite X-ray detector that meets market demand, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 is a physical picture of the MAPbI3 perovskite powder obtained in step 1 and the MAPbI3-DMSO complex powder obtained in step 3 in Example 1; A is a physical picture of the MAPbI3 perovskite powder, and B is a physical picture of the MAPbI3-DMSO complex powder;
[0060] FIG2 is an X-ray diffraction (XRD) pattern of MAPbI3 obtained in step 1 and MAPbI3-DMF complex powder obtained in step 3 in Example 2;
[0061] FIG3 is a scanning electron microscope (SEM) image of FAPbI3-NMP obtained in step 3 of Example 3;
[0062] FIG4 is a physical picture of the perovskite wafer obtained in step 4 of Example 4;
[0063] FIG5 is a surface SEM image of the perovskite wafer obtained in Example 5;
[0064] FIG6 is a surface SEM image of the perovskite wafer obtained after annealing in step 5 of Example 5;
[0065] FIG7 is an IV diagram of light-dark current comparison of the X-ray detector prepared in Example 6;
[0066] FIG8 is a light response diagram of the X-ray detector prepared in Example 6 under a bias voltage of 5V;
[0067] FIG9 is a graph showing the responses of the X-ray detector prepared in Example 6 to different doses of X-rays at a bias voltage of 10 V. DETAILED DESCRIPTION
[0068] The technical solution of the present application is described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0069] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.
[0070] Example 1
[0071] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0072] Step 1: Weigh 0.461 g of PbI2 and 0.159 g of MAI (iodine methylamine), dissolve them in DMF (2 mL) to prepare a perovskite precursor solution, then quickly add the above precursor dropwise to chloroform (30 mL) at room temperature (25 ° C) under stirring conditions of 800 rpm to precipitate, and obtain perovskite powder after low-temperature vacuum drying (40 ° C);
[0073] Step 2: Mix 50 μL of polar solvent DMSO (dimethyl sulfoxide) with 2 mL of chlorobenzene, add 200 mg of the perovskite powder obtained in step 1, and stir at room temperature (500 rpm) until the mixture changes color and viscosity (time 60 min) before proceeding to the next step;
[0074] Step 3: Centrifuge the mixture obtained in step 2 (6000 rpm), discard the solvent (supernatant), and then vacuum dry (40°C) to obtain MAPbI3-DMSO complex powder. As shown in Figure 1, the color of the complex powder changes from black perovskite to yellow-green;
[0075] Step 4: Weigh 200 mg of the powder obtained in step 3, select a mold with a size of 1 cm × 1 cm, and use a hydraulic press to press it at 80°C and 5 MPa for 10 minutes to form a wafer;
[0076] Step 5: annealing the wafer obtained in step 4 at 100° C. for 2 hours; and
[0077] Step 6: Use Ag and Cu as the two end electrodes (150 nm) to evaporate the wafer without adding a transmission layer to complete the preparation of the X-ray detector.
[0078] Example 2
[0079] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0080] Step 1: Weigh 0.461 g of PbI2 and 0.159 g of MAI, dissolve them in DMSO (1.5 mL) to prepare a perovskite precursor solution, then quickly add the above precursor dropwise to chloroform (30 mL) under stirring at room temperature and 600 rpm to precipitate, and dry in a low-temperature vacuum (40°C) to obtain a perovskite powder;
[0081] Step 2: Mix 60 μL of polar solvent DMF and 2 mL of toluene, add 250 mg of the perovskite powder obtained in step 1, and stir at room temperature (300 rpm) until mixed (time 45 min);
[0082] Step 3: The mixture obtained in step 2 was centrifuged (4000 rpm), the solvent was discarded, and then dried (35°C) to obtain MAPbI3-DMF complex powder. The XRD signals of the perovskite and its complex are shown in Figure 2. The diffraction peak appearing before 2θ = 10° indicates that the solvent is intercalated in the perovskite lattice;
[0083] Step 4: Weigh 150 mg of the powder from step 3 and 100 mg of the powder from step 1, select a mold with a size of 1 cm × 1 cm, and use a hydraulic press to press it at 100°C and 10 MPa for 10 minutes to press the wafer;
[0084] Step 5: annealing the wafer obtained in step 4 at 100° C. for 1 hour; and
[0085] Step 6: Use Au as the two end electrodes (150 nm) to evaporate the wafer without adding a transmission layer to complete the preparation of the X-ray detector.
[0086] Example 3
[0087] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0088] Step 1: Weigh 0.461 g of PbI2 and 0.172 g of FAI (iodine formamidine), dissolve them in DMSO (1.5 mL) to prepare a perovskite precursor solution, then quickly add the above precursor dropwise to toluene (20 mL) under stirring at 600 rpm to precipitate, and dry under low-temperature vacuum (50°C) to obtain a perovskite powder;
[0089] Step 2: Mix 40 μL of polar solvent NMP and 2 mL of chloroform, add 150 mg of the perovskite powder obtained in step 1, and stir at room temperature (400 rpm) for 60 min.
[0090] Step 3: The mixture obtained in step 2 was centrifuged (4000 rpm), the solvent was discarded, and then dried (45° C.) to obtain a FAPbI3-NMP complex powder, the SEM image of which is shown in FIG3 , showing a needle-like morphology;
[0091] Step 4: Weigh 50 mg of the powder from step 3 and 150 mg of the powder from step 1, select a mold with a size of 1 cm × 1 cm, and use a hydraulic press to press it at 100°C and 15 MPa for 15 minutes to press the wafer;
[0092] Step 5: annealing the wafer obtained in step 4 at 120° C. for 1 hour; and
[0093] Step 6: Prepare an X-ray detector with the structure of Cu (150nm)-FAPbI3 chip-PCBM (30nm)-C 60 (60nm)—BCP (10nm)—Ag (150nm).
[0094] Example 4
[0095] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0096] Step 1: Weigh 0.367 g of PbBr2 and 0.159 g of MAI, dissolve them in a mixed solution of DMF (1.8 mL) and DMSO (0.2 mL) to prepare a perovskite precursor solution. Then, under stirring at 600 rpm, the above precursor is quickly added dropwise to toluene (20 mL) to precipitate. After low-temperature vacuum drying (40°C), perovskite powder is obtained;
[0097] Step 2: Mix 30 μL of polar solvent DMSO and 1 mL of chloroform, add 150 mg of the perovskite powder obtained in step 1, and stir at room temperature (400 rpm) to mix evenly (time 30 min);
[0098] Step 3: Centrifuge the mixture obtained in step 2 (4000 rpm), discard the solvent, and then dry (25° C.) to obtain MAPbIBr2-DMSO complex powder;
[0099] Step 4: Weigh 200 mg of the powder from step 3 and 100 mg of the powder from step 1, select a mold with dimensions of 1.5 cm × 1.5 cm, and press it using a hydraulic press at 100°C and 10 MPa for 30 minutes to form a wafer, as shown in Figure 4.
[0100] Step 5: annealing the wafer obtained in step 4 at 100° C. for 1 hour; and
[0101] Step 6: Prepare an X-ray detector with the structure of Cu (150nm)-MAPbIBr2 chip-PCBM (30nm)-C 60 (60nm)—BCP (10nm)—Ag (150nm).
[0102] Example 5
[0103] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0104] Step 1: Weigh 0.461 g of PbI2 and 0.212 g of CsBr raw materials, dissolve them in DMF (2 mL) to prepare a perovskite precursor solution, then quickly add the above precursor dropwise into chloroform (20 mL) under stirring at 600 rpm to precipitate, and dry in a vacuum at low temperature (40°C) to obtain a perovskite powder;
[0105] Step 2: Mix 30 μL of polar solvent GBL with 2 mL of toluene, add 250 mg of the perovskite powder obtained in step 1, and stir (400 rpm) to mix evenly (time 60 min);
[0106] Step 3: Centrifuge the mixture obtained in step 2 (6000 rpm), discard the solvent, and then dry (40° C.) to obtain CsPbI2Br-DBL complex powder;
[0107] Step 4: Weigh 150 mg of the powder obtained in step 3, select a mold with a size of 1 cm × 1 cm, and use a hydraulic press to press it at 150°C and 10 MPa for 30 minutes to form a wafer;
[0108] Step 5: Anneal the wafer obtained in step 4 at 150°C for 1 hour. Its morphology is shown in Figure 5. The surface and interface are very dense, and obvious grain fusion can be observed. The cross-sectional SEM is shown in Figure 6, and the thickness is about 500μm; and
[0109] Step 6: Use Au as the two end electrodes (150 nm) to evaporate the wafer without adding a transmission layer to complete the preparation of the X-ray detector.
[0110] Example 6
[0111] This embodiment provides a method for preparing a perovskite complex, and a method for using the same to prepare a polycrystalline pressed wafer X-ray detector. The specific steps are as follows:
[0112] Step 1: Weigh 0.922 g of PbI2, 0.159 g of MAI, and 0.172 g of FAI raw materials, dissolve them in DMF (3 mL) to prepare a perovskite precursor solution, then quickly add the above precursor dropwise to toluene (50 mL) under stirring at 600 rpm to precipitate, and dry in a vacuum at low temperature (40°C) to obtain a perovskite powder;
[0113] Step 2: Mix 40 μL of polar DMSO and 2 mL of toluene, add 200 mg of the perovskite powder obtained in step 1, and stir (600 rpm) to mix evenly (time 30 min);
[0114] Step 3: Centrifuge the mixture obtained in step 2 (3000 rpm), discard the solvent, and then dry (30° C.) to obtain MAFAPb2I6-DMSO complex powder;
[0115] Step 4: Weigh 500 mg of the powder obtained in step 3, select a mold with a size of 2 cm × 2 cm, and press it with a hydraulic press at 100°C and 3 MPa for 20 minutes to form a wafer;
[0116] Step 5: annealing the wafer obtained in step 4 at 100° C. for 2 hours; and
[0117] Step 6: Use Au as the two end electrodes (150 nm) to evaporate the wafer without adding a transmission layer to complete the preparation of the X-ray detector.
[0118] X-ray response testing
[0119] The detectors prepared in each embodiment respond well to X-rays and have high photoresponse sensitivity (the results are listed in Table 1). Taking Example 6 as an example, its IV diagram of light-dark current comparison is shown in Figure 7, which has a large switching ratio; the response under 5V bias is shown in Figure 8, with a fast response speed and a stable baseline. The prepared detector responds well to X-rays, and its photoresponse to different doses of X-rays under a bias of 10V is shown in Figure 9. By calculation (the slope of the photocurrent density and X-ray dose rate curve, the sensitivity calculation method is well known in the art and will not be repeated here), it can be obtained that the sensitivity is 18080μC Gy air -1 cm -2 .
[0120] Table 1
[0121] In the present application, if the perovskite powder obtained by step 1 of each embodiment alone cannot be pressed into a tablet under the corresponding tableting conditions, even if it is further pressed into a tablet, the wafer contains many voids and grain boundaries and cannot be used for the preparation of an X-ray detector. However, by introducing an appropriate amount of polar solvent into the perovskite powder to synthesize a perovskite-solvent complex, the obtained solvent complex has a soft texture and better processing flexibility. A dense and uniform perovskite wafer can be obtained under a smaller pressure, and the X-ray detector further prepared has high sensitivity. In addition, the perovskite-solvent complex can be mixed with uncomplexed perovskite powder and then pressed into a tablet, which can also prepare an X-ray detector with higher sensitivity.
[0122] The applicant declares that this application uses the above-mentioned embodiments to illustrate the preparation method of a perovskite complex for X-ray detection, its products, and applications, but this application is not limited to the above-mentioned embodiments, that is, it does not mean that this application must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent replacement of various raw materials in the products of this application, addition of auxiliary components, and selection of specific methods, etc., are all within the scope of protection and disclosure of this application.
[0123] The preferred embodiments of the present application are described in detail above. However, the present application is not limited to the specific details of the above embodiments. Within the technical concept of the present application, various simple modifications can be made to the technical solution of the present application, and these simple modifications all fall within the scope of protection of the present application.
[0124] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any appropriate manner unless there is any contradiction. In order to avoid unnecessary repetition, this application will not further describe various possible combinations.
Claims
1. A method for preparing a perovskite complex for X-ray detection, comprising: mixing the perovskite with a solvent to obtain a mixture, and drying the mixture to obtain a perovskite complex; Wherein, the solvent includes polar solvent A and solvent B; the polar solvent A includes any one or a combination of at least two of DMF, DMSO, NMP or GBL; The perovskite comprises a chemical formula of X n Pb n Y 3n The lead halide perovskite, wherein n is an integer of 1 or greater than 1, the X is each independently selected from any one of MA, FA or Cs, and the Y is each independently selected from I or Br.
2. The preparation method according to claim 1, wherein The solvent B includes any one of chloroform, toluene, isopropanol, acetone, chlorobenzene or ether, or a combination of at least two thereof.
3. The preparation method according to claim 1 or 2, wherein: The mass ratio of perovskite to solvent in the mixture is 1:(5-20); Preferably, the volume ratio of the polar solvent A to the solvent B is (1-10):(100-200); Preferably, the mixing temperature is 15-40°C, and the mixing time is 30-120min; Preferably, the mixing is carried out under stirring, and the stirring speed is 200-1000rpm; Preferably, the drying temperature is 20-60°C; Preferably, before drying, the mixture is centrifuged and the supernatant is discarded; Preferably, the centrifugal rotation speed is 2000-6000 rpm.
4. The preparation method according to any one of claims 1 to 3, wherein The perovskite is prepared by a preparation method comprising the following steps: Lead halide, halogen-containing compounds and an organic solvent are mixed to obtain a precursor solution, which is then mixed with an anti-solvent to precipitate a reaction product, and dried to obtain the perovskite.
5. The preparation method according to any one of claims 1 to 4, wherein The lead halide includes PbI2 and / or PbBr2; the halogen-containing compound includes any one of MAI, FAI, CsI, MABr, FABr or CsBr, or a combination of at least two thereof; Preferably, the molar ratio of the lead halide to the halogen-containing compound is (1-2):(1-2); Preferably, the organic solvent comprises any one or a combination of at least two of DMF, DMSO, NMP or GBL; Preferably, the anti-solvent comprises any one or a combination of at least two of chloroform, toluene, isopropanol, acetone, chlorobenzene or ether; Preferably, the volume ratio of the organic solvent to the anti-solvent is (1-10):(10-200).
6. A perovskite complex prepared by the preparation method according to any one of claims 1 to 5.
7. A method for preparing a perovskite wafer, comprising: The perovskite complex is prepared by the preparation method according to any one of claims 1 to 5, and tabletted to obtain; or The prepared perovskite complex is mixed with perovskite, and then tablets are pressed to obtain the product.
8. The preparation method according to claim 7, wherein The tabletting is carried out under the conditions of 3-20MPa and 80-150°C; Preferably, the tableting time is 10-40 min; Preferably, the tableting further includes annealing; Preferably, the annealing temperature is 80-200° C. and the annealing time is 30-120 min.
9. A perovskite wafer prepared by the preparation method according to any one of claims 7 to 8.
10. Use of the perovskite complex prepared by the preparation method according to any one of claims 1 to 5 or the perovskite wafer prepared by the preparation method according to any one of claims 7 to 8 in the preparation of an X-ray detector.
11. An X-ray detector, wherein: The components of the X-ray detector include an active layer, an electrode and an optional transmission layer, and the material of the active layer includes a perovskite wafer prepared by the preparation method according to any one of claims 7 to 8.
Citation Information
Patent Citations
Method for using recrystallization method to prepare lead-halide perovskite nanowire
CN106629834A
Method for preparing perovskite thin film by using anti-solvent one-step method
CN113410399A
One-step in situ solution growth for lead halide perovskite
US20190003074A1
Cited By
Perovskite single crystal, preparation method and planar photoelectric detector
CN120401016A