Method for preparing baking-free bricks from laterite-nickel ore high-pressure acid leaching smelting tailings, and baking-free brick
By dehydrating and crushing the high-pressure acid leaching smelting tailings of laterite nickel ore, and then mixing it with aggregate and cement to press it into burn-free bricks, the problem of tailings treatment is solved, resource utilization and production efficiency are improved, costs are reduced, and The bricks have high strength and are suitable for mass production.
Patent Information
- Application Number
- PCT/CN2023/117025
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2023-09-05
- Publication Date
- 2024-10-17
AI Technical Summary
Existing technology cannot effectively handle the high-pressure acid leaching smelting tailings of laterite nickel ore, leading to problems such as marine pollution, high tailings inventory costs, and large land occupation. It is necessary to improve resource utilization and reduce production and operation costs.
After the high-pressure acid leaching smelting tailings of laterite nickel ore are dehydrated and crushed, they are mixed with aggregate and cement in a certain proportion, pressed and molded, and cured to be made into unfired bricks to achieve resource utilization.
It improves the utilization rate of laterite nickel ore resources, reduces tailings storage costs and risks, and reduces land occupation and production costs. At the same time, the unfired bricks produced have high strength and are suitable for mass production.
Smart Images

Figure CN2023117025_17102024_PF_FP_ABST
Abstract
Description
Method for producing unburned bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore and unburned bricks Technical Field
[0001] The present invention relates to the technical field of solid waste resource treatment, and in particular to a method for producing unburned bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore, and the unburned bricks. Background Art
[0002] Laterite nickel ore is formed by the weathering, leaching, alteration, and enrichment of nickel-bearing rocks. It is primarily a loose, clay-like ore composed of hydrous oxides of iron, aluminum, and silicon. Low-grade laterite nickel ore is currently the primary source of nickel production worldwide. Nickel production from laterite nickel ore can be achieved through two processes: pyrometallurgical and hydrometallurgical. The primary hydrometallurgical process for processing laterite nickel ore is high-pressure acid leaching. High-pressure acid leaching is suitable for processing low-magnesium limonite laterite nickel ore, offering high metal recovery and high processing capacity, but it also produces significant amounts of tailings.
[0003] Currently, the common practices for tailings disposal include deep-sea landfill, wet stacking in tailings ponds, or dry stacking in tailings ponds. Deep-sea landfill carries the risk of marine pollution, while tailings pond storage has disadvantages such as high cost and large land occupation. Therefore, it is necessary to find an effective method for treating tailings from high-pressure acid leaching of laterite nickel ore to improve resource utilization and reduce project construction investment and production and operating costs.
[0004] Summary of the Invention
[0005] The present invention aims to provide a method for producing unburned bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore. By preparing tailings from high-pressure acid leaching of laterite nickel ore, aggregate and cement in a certain proportion and then pressing them into bricks, the resource utilization of tailings from high-pressure acid leaching of laterite nickel ore can be achieved.
[0006] The present invention provides a method for producing unburned bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore, comprising the following steps:
[0007] S10: Dehydration and crushing of tailings from high-pressure acid leaching of laterite nickel ore;
[0008] S20: mixing the crushed laterite nickel ore high-pressure acid leaching smelting tailings with a certain amount of aggregate, cement and water, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into bricks;
[0009] S30: The pressed bricks are cured for a period of time and then made into unfired bricks.
[0010] In one feasible manner, in the above-mentioned step S10, the specific step of dehydrating the laterite nickel ore high-pressure acid leaching smelting tailings includes: first performing a filter press treatment on the laterite nickel ore high-pressure acid leaching smelting tailings, and then performing a drying treatment on the laterite nickel ore high-pressure acid leaching smelting tailings.
[0011] In one achievable manner, in the above step S10, the moisture content of the tailings from the high-pressure acid leaching of laterite nickel ore after pressure filtration is 25%-40%.
[0012] In one achievable manner, in the above step S10, the moisture content of the dried laterite nickel ore high-pressure acid leaching smelting tailings is less than 10%.
[0013] In one achievable manner, in the above step S10, the particle size of the crushed laterite nickel ore high-pressure acid leaching smelting tailings is less than 5 mm.
[0014] In one achievable manner, in the above step S20, the aggregate includes one or more of water-quenched nickel-iron slag, water-quenched blast furnace slag and sand.
[0015] In one feasible manner, in the above-mentioned step S20, the weight percentages of aggregate, cement and laterite nickel ore high-pressure acid leaching smelting tailings in the mixed slurry are: 10%-80% aggregate, 10%-50% cement, and the rest is laterite nickel ore high-pressure acid leaching smelting tailings, and the sum of the weight percentages of aggregate, cement and laterite nickel ore high-pressure acid leaching smelting tailings in the mixed slurry is 100%.
[0016] In one achievable manner, in the above step S20, the water content of the mixed slurry is 10%-30%.
[0017] In one achievable manner, in the above step S30, the curing time of the bricks is 7-28 days.
[0018] The present invention also provides an unburned brick, which is produced by the above-mentioned method of producing unburned bricks by utilizing the tailings of high-pressure acid leaching of laterite nickel ore.
[0019] The present invention provides a method for preparing unburned bricks from high-pressure acid leaching smelting tailings of laterite nickel ore. The method comprises the following steps: dehydrating and crushing the smelting tailings of laterite nickel ore, uniformly mixing the smelting tailings with a certain amount of aggregate, cement and water, and then pressing and forming the unburned bricks. The unburned bricks are then prepared after curing, thereby realizing resource utilization of the smelting tailings of laterite nickel ore, improving the resource utilization rate of laterite nickel ore, reducing the cost and risk of tailings storage, reducing the amount of land resources occupied, and reducing project construction investment and production and operation costs. At the same time, the method is not only simple in manufacturing process, but also does not require high-temperature sintering. The raw materials are cheap and readily available, which can save a lot of energy consumption and production costs. The unburned bricks prepared are high in strength and suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 is a schematic diagram of a process for producing unburned bricks by utilizing tailings from high-pressure acid leaching of laterite nickel ore in an embodiment of the present invention. DETAILED DESCRIPTION
[0021] The following embodiments of the present invention are described in further detail with reference to the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0022] The terms "first," "second," "third," "fourth," and the like (if any) in the description and claims of the present invention are used to distinguish similar objects and are not necessarily used to describe a particular sequential order or sequence.
[0023] The directional terms "up," "down," "left," "right," "front," "back," "top," and "bottom" (if any) used in the specification and claims of the present invention are defined by the positions of the structures in the drawings and the positions of the structures relative to each other, and are intended only for clarity and convenience in expressing the technical solution. It should be understood that the use of directional terms should not limit the scope of protection claimed in the present invention.
[0024] FIG1 is a schematic diagram of a process for producing unburned bricks using tailings from high-pressure acid leaching of laterite nickel ore according to an embodiment of the present invention. As shown in FIG1 , the method for producing unburned bricks using tailings from high-pressure acid leaching of laterite nickel ore provided by an embodiment of the present invention comprises the following steps:
[0025] S10: dehydrating and crushing the tailings from high-pressure acid leaching of laterite nickel ore; wherein the tailings from high-pressure acid leaching of laterite nickel ore are tailings obtained after nickel is produced from laterite nickel ore by a high-pressure acid leaching process;
[0026] S20: mixing the crushed laterite nickel ore high-pressure acid leaching smelting tailings with a certain amount of aggregate, cement and water, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into bricks;
[0027] S30: The pressed bricks are cured for a period of time and then made into unfired bricks.
[0028] Specifically, the present embodiment provides a method for making unburned bricks from high-pressure acid leaching smelting tailings of laterite nickel ore. After dehydration and crushing, the high-pressure acid leaching smelting tailings of laterite nickel ore are mixed evenly with a certain amount of aggregate, cement and water, and then pressed into shape. After curing, unburned bricks are made, thereby realizing the resource utilization of high-pressure acid leaching smelting tailings of laterite nickel ore, improving the resource utilization rate of laterite nickel ore, reducing the cost and risk of tailings storage, reducing the amount of land resources occupied, and reducing project construction investment and production and operation costs. At the same time, the method is not only simple in manufacturing process, but also does not require high-temperature sintering. At the same time, raw materials are cheap and easily available, which can save a lot of energy consumption and production costs, and the unburned bricks obtained are high in strength and suitable for mass production.
[0029] As an embodiment, in the above-mentioned step S10, the specific step of dehydrating the laterite nickel ore high-pressure acid leaching smelting tailings includes: first performing a filter press treatment on the laterite nickel ore high-pressure acid leaching smelting tailings, and then performing a drying treatment on the laterite nickel ore high-pressure acid leaching smelting tailings.
[0030] As an embodiment, in the above step S10, the moisture content of the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration is 25%-40%.
[0031] As an embodiment, in the above step S10, the moisture content of the dried laterite nickel ore high-pressure acid leaching smelting tailings is less than 10%.
[0032] Specifically, since the high-pressure acid leaching smelting tailings of laterite nickel ore are tailings obtained after nickel is produced from laterite nickel ore by a high-pressure acid leaching method, the water content of the high-pressure acid leaching smelting tailings of laterite nickel ore is relatively high (the water content generally reaches 50%-60%), and dehydration treatment is required during brick making. By successively subjecting the high-pressure acid leaching smelting tailings of laterite nickel ore to a filter press treatment and a drying treatment, that is, gradually dehydrating the tailings, the water content of the tailings is reduced to below 10%, which not only facilitates the subsequent crushing of the tailings, but also avoids affecting the mass ratio of the tailings to aggregate and cement due to excessive water content in the tailings; at the same time, since the water content in the bricks during the pressing process to form the green bricks (as described below, 10%-30%) is less than the initial water content of the tailings, the tailings need to be dehydrated first to avoid affecting the pressing and forming of the green bricks and the quality of the finally produced unfired bricks.
[0033] As an embodiment, in the above step S10, the particle size of the crushed laterite nickel ore high-pressure acid leaching smelting tailings is less than 5 mm.
[0034] Specifically, by crushing the tailings, the particle size of the tailings is reduced to below 5 mm, which not only makes the subsequent mixing with aggregate and cement more uniform, but also facilitates the pressing and molding of bricks. At the same time, it avoids the tailings particles being too large and protruding from the brick surface, which affects the flatness of the unfired bricks, thereby improving the quality of the unfired bricks.
[0035] As an embodiment, in the above-mentioned step S20, the aggregate includes one or more of water-quenched nickel-iron slag, water-quenched blast furnace slag, and sand. This aggregate is not only cheap and readily available, but also can achieve a high structural strength after being mixed with tailings and cement, thereby making the unburned bricks have a higher strength. Among them, water-quenched nickel-iron slag and water-quenched blast furnace slag are both solid wastes. Using water-quenched nickel-iron slag and water-quenched blast furnace slag as aggregates can further achieve solid waste recycling, reduce production costs, and alleviate the pressure of solid waste treatment. Of course, in other embodiments, other materials can also be used as aggregates.
[0036] Specifically, cement, as a cementitious material, can bind tailings and aggregates together, thereby improving the strength of unfired bricks. Using water-quenched ferronickel slag and water-quenched blast furnace slag as aggregates not only provides a skeletal support (tailings are finer in particle size and cannot provide this support on their own), but also generates reinforcing hydration products or promotes hydration reactions, thereby increasing the chemical reactivity of the tailings and the strength of unfired bricks.
[0037] As an embodiment, in the above-mentioned step S20, the weight percentages of aggregate, cement, and laterite nickel ore high pressure acid leaching smelting tailings in the mixed slurry are (excluding the weight of water): 10%-80% aggregate, 10%-50% cement, and the remainder is laterite nickel ore high pressure acid leaching smelting tailings (excluding the weight of water in the laterite nickel ore high pressure acid leaching smelting tailings, that is, the laterite nickel ore high pressure acid leaching smelting tailings is the dry weight). The sum of the weight percentages of aggregate, cement, and laterite nickel ore high pressure acid leaching smelting tailings in the mixed slurry is 100%. For example, if the weight percentage of aggregate is 40% and the weight percentage of cement is 20%, then the weight percentage (dry weight) of laterite nickel ore high pressure acid leaching smelting tailings is 40%.
[0038] As an embodiment, in step S20, the water content of the mixed slurry is 10%-30%. Maintaining the water content of the mixed slurry within this range allows for better cross-linking between the tailings, aggregate, and cement, thereby allowing the mixed slurry to gradually harden during the pressing and subsequent curing of bricks, ultimately achieving a high structural strength while preventing the impact of excessive water content on the pressing and forming of the bricks.
[0039] As an embodiment, in the above step S20, the crushed laterite nickel ore high-pressure acid leaching smelting tailings are mixed with a certain amount of aggregate, cement and water, and stirred evenly to obtain a mixed slurry, which specifically comprises the following steps:
[0040] A certain amount of aggregate and cement are added to the crushed laterite nickel ore high-pressure acid leaching smelting tailings, and the mixture is evenly mixed to obtain a mixture; then a certain amount of water is added to the mixture, and the mixture is evenly stirred to obtain a mixed slurry.
[0041] As an embodiment, in the above step S20, the specific steps of pressing the mixed slurry into a brick blank include: filling the mixed slurry into a mold, then punching the mixed slurry in the mold to obtain a brick blank of a certain shape, and then separating the brick blank from the mold.
[0042] As an embodiment, in the above step S30, the bricks are cured for 7-28 days, and the bricks can be naturally cured at room temperature and normal pressure, so that the bricks are hardened to a higher structural strength during the curing process.
[0043] An embodiment of the present invention further provides an unburned brick, which is produced by the above-described method of producing unburned bricks using tailings from high-pressure acid leaching of laterite nickel ore.
[0044] The method for making unburned bricks from high-pressure acid leaching smelting tailings of laterite nickel ore provided in an embodiment of the present invention comprises the following steps: drying and crushing the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration, adding a certain amount of aggregate and cement to mix evenly, then adding a certain amount of water to stir evenly and pressing to form, and making unburned bricks after curing, thereby realizing resource utilization of high-pressure acid leaching smelting tailings of laterite nickel ore, improving resource utilization of laterite nickel ore, reducing tailings storage cost and risk, reducing land resource occupation, reducing project construction investment and production and operation costs. At the same time, the method not only has a simple manufacturing process, but also does not require high-temperature sintering, and the raw materials are cheap and easily available, which can save a lot of energy consumption and production costs, and the unburned bricks obtained have high strength and are suitable for mass production.
[0045] Example 1
[0046] The water content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are dried and crushed to a moisture content of less than 10% and a particle size of less than 5mm. The crushed tailings are then mixed with cement and water-quenched ferronickel slag in a weight ratio of 40:35:25. Water is added to a water content of 20%, and the mixture is then pressed into unfired bricks measuring 240mm x 115mm x 53mm. After 28 days of natural curing, the unfired bricks were tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks exceeded 10 MPa, and the strength after immersion in water exceeded 6.5 MPa.
[0047] Example 2
[0048] The moisture content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are then dried and crushed to a moisture content of less than 10% and a particle size of less than 5mm. The crushed tailings are then mixed with cement and water-quenched ferronickel slag in a weight ratio of 45:35:20. Water is added to a moisture content of 20%, and the mixture is then pressed into unfired bricks measuring 240mm x 115mm x 53mm. After 28 days of natural curing, the bricks were tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks exceeded 10 MPa, and after immersion in water, the strength exceeded 6.5 MPa.
[0049] Example 3
[0050] The moisture content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are then dried and crushed to a moisture content of less than 10% and a particle size of less than 5mm. The crushed tailings are then mixed with cement and water-quenched blast furnace slag in a weight ratio of 45:35:20. Water is added to a moisture content of 20%, and the mixture is then pressed into unfired bricks measuring 240mm x 115mm x 53mm. After 28 days of natural curing, the bricks were tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks exceeded 10 MPa, and after immersion in water, the strength exceeded 6.5 MPa.
[0051] Example 4
[0052] The moisture content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are then dried and crushed to a moisture content of less than 10% and a particle size of less than 5mm. The crushed tailings are then mixed with cement and sand in a weight ratio of 45:35:20. Water is added to a moisture content of 20%, and the mixture is then pressed into unfired bricks measuring 240mm x 115mm x 53mm. After 28 days of natural curing, the bricks are tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks exceeds 10 MPa, and the strength after immersion in water exceeds 6.5 MPa.
[0053] Example 5
[0054] The water content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are dried and crushed to a moisture content of less than 10% and a particle size of less than 5 mm. The crushed tailings are then mixed with cement and water-quenched ferronickel slag in a weight ratio of 62:35:3. Water is added to a moisture content of 20%, and the mixture is then pressed into unfired bricks measuring 240 mm x 115 mm x 53 mm. After 28 days of natural curing, the bricks are tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks is less than 10 MPa, and the strength after immersion in water is less than 6.5 MPa.
[0055] Example 6
[0056] The water content of the high-pressure acid leaching tailings from laterite nickel ore after filtration is 30%. The tailings are dried and crushed to a moisture content of less than 10% and a particle size of less than 5 mm. The crushed tailings are then mixed with cement and water-quenched ferronickel slag in a weight ratio of 75:5:20. Water is added to a moisture content of 20%, and the mixture is then pressed into unfired bricks measuring 240 mm x 115 mm x 53 mm. After 28 days of natural curing, the unfired bricks were tested according to the national standard GB / T 2542-2012, "Test Methods for Wall Bricks." The strength of the unfired bricks was less than 10 MPa, and the strength after immersion in water was less than 6.5 MPa.
[0057] The above are merely specific embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.
Claims
1. A method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore, characterized in that: The following steps are involved: S10: Dehydration and crushing of tailings from high pressure acid leaching of laterite nickel ore; S20: mixing the crushed laterite nickel ore high pressure acid leaching smelting tailings with a certain amount of aggregate, cement and water, stirring evenly to obtain a mixed slurry, and then pressing the mixed slurry into a brick; S30: The pressed bricks are cured for a period of time to form unfired bricks.
2. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, the specific steps of dehydrating the laterite-nickel ore high-pressure acid leaching smelting tailings include: firstly performing filter pressing treatment on the laterite-nickel ore high-pressure acid leaching smelting tailings, and then performing drying treatment on the laterite-nickel ore high-pressure acid leaching smelting tailings.
3. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 2, characterized in that: In the above step S10, the moisture content of the high-pressure acid leaching smelting tailings of laterite nickel ore after pressure filtration is 25%-40%.
4. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 2, characterized in that: In the above step S10, the moisture content of the dried laterite nickel ore high pressure acid leaching smelting tailings is less than 10%.
5. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S10, the particle size of the crushed laterite nickel ore high pressure acid leaching smelting tailings is less than 5 mm.
6. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S20, the aggregate includes one or more of water-quenched nickel-iron slag, water-quenched blast furnace slag and sand.
7. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above-mentioned step S20, the weight percentages of aggregate, cement and laterite nickel ore high pressure acid leaching smelting tailings in the mixed slurry are: 10%-80% aggregate, 10%-50% cement, and the rest is laterite nickel ore high pressure acid leaching smelting tailings. The sum of the weight percentages of aggregate, cement and laterite nickel ore high pressure acid leaching smelting tailings in the mixed slurry is 100%.
8. The method for preparing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S20, the water content of the mixed slurry is 10%-30%.
9. The method for producing unburned bricks by utilizing high pressure acid leaching smelting tailings of laterite nickel ore as claimed in claim 1, characterized in that: In the above step S30, the bricks are naturally cured at room temperature and normal pressure for 7-28 days.
10. A non-fired brick, characterized in that: The brick is made by the method for making unburned bricks using high-pressure acid leaching smelting tailings of laterite nickel ore as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Laterite slag baking-free brick and preparation method thereof
CN102424550A
Method for preparing autoclaved brick from electrolytic manganese dioxide waste residues
CN102775116A
Method for making bricks by using hydrometallurgical tailings of laterite nickel ore
CN103496902A
Method for manufacturing brick for building and brick manufactured by the same
KR1020120018996A
Manufacture and composition of high strength concrete using fine aggregate from fe-ni slag
KR1020120066769A
Cited By
Pressure-free baking-free brick for synergistically recovering solid waste molten water-quenched slag and sludge incineration ash and preparation method of pressure-free baking-free brick
CN119285288A