Heat-resistant conductive polymer composite material, preparation method therefor, and use thereof

By copolymerizing tetrathiafulvalene and cobalt salt to form a conductive polymer, combined with thermoplastic polyurethane and polyimide, the durability problem of traditional grounding materials in highly corrosive environments is solved, achieving high conductivity and corrosion resistance, and It reduces the maintenance cost of the grounding grid and is suitable for highly corrosive soils and coastal areas.

WO2024212574A1PCT designated stage expired Publication Date: 2024-10-17INST OF CORROSION SCI & TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/139663
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2023-12-18
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Traditional grounding materials are prone to corrosion in acidic, alkaline, high-salt and corrosive soils with high water content, leading to grounding grid failure. Moreover, flexible graphite materials have poor high-frequency tolerance, and traditional polymer conductive materials have insufficient temperature resistance. , threatening grounding safety.

Method used

A conductive polymer formed by the copolymerization of tetrathiafulvalene and cobalt salt is used, combined with thermoplastic polyurethane and polyimide, to form a temperature-resistant conductive polymer composite material, which enhances conductivity and corrosion resistance, and reduces the use of conductive fillers to improve Elongation at break.

Benefits of technology

It achieves the combination of high conductivity, corrosion resistance and high temperature resistance, extends the service life of the grounding grid, reduces maintenance costs, is suitable for highly corrosive environments and ensures the full life cycle service of the grounding device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023139663-FTAPPB-I100001
    Figure PCTCN2023139663-FTAPPB-I100001
  • Figure PCTCN2023139663-FTAPPB-I100002
    Figure PCTCN2023139663-FTAPPB-I100002
  • Figure PCTCN2023139663-FTAPPB-I100003
    Figure PCTCN2023139663-FTAPPB-I100003
Patent Text Reader

Abstract

The present application belongs to the field of grounding of electric power, petrochemistry, transportation and communication, and discloses a heat-resistant conductive polymer composite material, a preparation method therefor, and a use thereof. A heat-resistant conductive polymer composite material, the conductive polymer composite material comprising the following components: 20-40 parts of a thermoplastic polyurethane; 15-25 parts of a thermoplastic polyimide; 20-35 parts of a polytetrathiafulvalene conductive polymer; 1-5 parts of a lubricant; 1-3 parts of a coupling agent; 0.5-2 parts of an antioxidant; 2-5 parts of a flame retardant; and 1-5 parts of an anti-aging agent; said parts are calculated by mass. The described heat-resistant conductive polymer composite material has good conductivity and good flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

A heat-resistant conductive polymer composite material and its preparation method and application Technical Field

[0001] The present application relates to a temperature-resistant conductive polymer composite grounding material and a preparation method and application thereof, and belongs to the grounding field of electric power, petrochemicals, transportation, and communications. Background Art

[0002] Critical infrastructure such as power, petrochemicals, transportation, and communications has increasingly stringent grounding requirements. The stability, efficiency, and longevity of power grid grounding systems are particularly crucial for power safety. Failures in the grounding grids of transmission and distribution stations can cause serious accidents in the power grid and the power supply area, endangering the safety of nearby personnel. Corrosion and failure of grounding materials, leading to increased grounding resistance or fracture, are the primary causes of grounding grid failures. Traditional grounding materials, primarily carbon steel, galvanized steel, copper-clad steel, or copper, are subject to corrosion, especially in acidic, alkaline, high-salt, and water-rich soils. These materials typically require modification or even replacement every 5-10 years, significantly increasing lifecycle costs.

[0003] In response to the long-standing corrosion problem of metal grounding materials, relevant scientific researchers have developed some non-metallic grounding materials, such as flexible graphite grounding materials and organic grounding materials. However, these materials also have their own shortcomings when actually used on site. For example, flexible graphite grounding materials have poor power frequency tolerance, poor longitudinal distal drainage capacity, and are not suitable for areas with debris flows or long-term water erosion; traditional polymer conductive materials have poor heat resistance. When excessive current causes local high temperature, the drainage effect is reduced, threatening grounding safety. Therefore, the development of new grounding materials with high conductivity, high corrosion resistance and high temperature resistance is of great significance to extending the service life of the grounding network, ensuring the safety of the power grid, and reducing the construction and maintenance costs of the grounding network. The prior art CN115536958A discloses the use of tetrathiafulvalene copolymerized with styrene and butadiene to obtain a thermoplastic elastomer, so that the thermoplastic elastomer has the advantages of an elastomer while improving conductivity; and a large amount of conductive filler is added to the composite material. Due to the addition of a large amount of conductive filler (15-35 parts), the flexibility of the composite material is reduced.

[0004] Summary of the Invention

[0005] According to a first aspect of the present application, a temperature-resistant conductive polymer composite material is provided. By incorporating a conductive polymer copolymerized from tetrathiafulvalene and a cobalt salt, the conductive polymer composite material significantly improves electrical conductivity while also eliminating the need for conductive fillers required in the prior art, thereby increasing the composite material's elongation at break.

[0006] A heat-resistant conductive polymer composite material, comprising the following components:

[0007] The above parts are calculated by mass.

[0008] Optionally, the particle size of the conductive polymer composite material is 30 μm to 2 mm.

[0009] Optionally, during extrusion production, the particle size of the conductive polymer composite material is 1 mm to 2 mm;

[0010] When electrostatic spraying is used, the particle size of the conductive polymer composite material is 30 μm to 35 μm.

[0011] Optionally, the polytetrathiafulvalene conductive polymer is obtained by forming a coordination polymer between tetrathiafulvalene and cobalt atoms.

[0012] A mixture containing tetrathiafulvalene and cobalt salt is copolymerized to obtain polytetrathiafulvalene conductive polymer.

[0013] Optionally, the thermoplastic polyurethane is selected from at least one of Huntsman IROGRAN A 85D 6003, BASF 685A, and Lubrizol ESTANE 2355-75A.

[0014] Optionally, the weight average molecular weight of the thermoplastic polyimide is 20,000 to 40,000.

[0015] Optionally, the weight average molecular weight of the thermoplastic polyimide is independently selected from any value among 20000, 21000, 22000, 23000, 24000, 25000, 26000, 27000, 28000, 29000, 30000, 31000, 32000, 33000, 34000, 35000, 36000, 37000, 38000, 39000, 40000 or any range therebetween.

[0016] Optionally, the glass transition temperature of the thermoplastic polyimide is 180°C to 220°C.

[0017] The glass transition temperature of the thermoplastic polyimide is 201°C.

[0018] Optionally, the lubricant is selected from at least one of graphite, molybdenum disulfide, niobium diselenide, and paraffin.

[0019] Optionally, the coupling agent is selected from at least one of a silane coupling agent and an aluminate coupling agent.

[0020] Optionally, the antioxidant is selected from at least one of flavonoid antioxidants, β-naphthoflavone, zedoaria flavonoids, and glycyrrhizin flavonoids A.

[0021] Optionally, the flame retardant is selected from at least one of phosphorus-nitrogen halogen-free flame retardants, melamine, ammonium polyphosphate, and DOPO derivatives.

[0022] Optionally, the antioxidant is selected from at least one of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and N-phenyl-α-aniline.

[0023] According to a second aspect of the present application, a method for preparing a conductive polymer composite material is provided.

[0024] The method for preparing the conductive polymer composite material comprises the following steps:

[0025] S1. Obtaining thermoplastic polyimide powder;

[0026] S2, copolymerizing a mixture containing tetrathiafulvalene and a cobalt salt to obtain a polytetrathiafulvalene conductive polymer;

[0027] S3. Extruding and granulating the material containing thermoplastic polyurethane, the thermoplastic polyimide powder, the polytetrathiafulvalene conductive polymer, the lubricant, the coupling agent, the antioxidant, the flame retardant, and the antioxidant to obtain the conductive polymer composite material.

[0028] Optionally, in step S2, the tetrathiafulvalene is selected from at least one of bis(carbonyldithio)tetrathiafulvalene, formyltetrathiafulvalene and tetra(methylthio)tetrathiafulvalene.

[0029] Optionally, in step S2, the cobalt salt is selected from at least one of cobalt acetate, cobalt chloride and cobalt nitrate.

[0030] Optionally, in step S2, the mass ratio of the tetrathiafulvalene to the cobalt salt is 1:1 to 8:1.

[0031] The tetrathiafulvalene is calculated by mass, and the cobalt salt is calculated by mass.

[0032] Optionally, the mass ratio of the tetrathiafulvalene and the cobalt salt is independently selected from any value of 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, or any range between the two.

[0033] Optionally, in step S2, the copolymerization conditions are as follows:

[0034] Time is 8h~24h;

[0035] The temperature is 100℃~150℃.

[0036] Optionally, the time is independently selected from any value of 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, or a range between any two of them.

[0037] Optionally, the temperature is independently selected from any value of 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or any range therebetween.

[0038] Optionally, in step S3, the extrusion granulation includes twin-screw extrusion and single-screw extrusion.

[0039] Optionally, in step S3, during twin-screw extrusion, the temperatures of the conveying section, melting section, mixing section, exhaust section, homogenizing section and die head of the twin-screw extruder are 130℃~150℃, 180℃~200℃, 195℃~205℃, 185℃~195℃, 175℃~195℃ and 195℃~205℃ respectively.

[0040] Optionally, in step S3, during single-screw extrusion, the processing temperatures of the single-screw extruder are: 170°C to 185°C in the first zone, 195°C to 205°C in the second zone, 195°C to 205°C in the third zone and 185°C to 195°C in the die.

[0041] Optionally, the following steps are included:

[0042] A1. First, a polyamic acid precursor solution is obtained, and polyimide is prepared by chemical imidization dehydration in the presence of a dehydrating agent and a catalyst, and then polyimide powder is obtained after drying;

[0043] A2. copolymerizing a mixture containing tetrathiafulvalene and a cobalt salt to obtain a polytetrathiafulvalene conductive polymer;

[0044] A3. Extruding and granulating the material containing thermoplastic polyurethane, the thermoplastic polyimide powder, the polytetrathiafulvalene conductive polymer, the lubricant, the coupling agent, the antioxidant, the flame retardant, and the antioxidant to obtain the conductive polymer composite material.

[0045] Optionally, in step A1, the polyamic acid precursor solution is prepared by stirring in an inert atmosphere at room temperature.

[0046] Optionally, in step A1, the dehydrating agent is selected from at least one of acetic anhydride and phthalic anhydride.

[0047] Optionally, in step A1, the catalyst is selected from at least one of isoquinoline and pyridine.

[0048] Optionally, in step A1, the mixing conditions are as follows:

[0049] The reaction time of polyamic acid is 20h to 30h.

[0050] According to a third aspect of the present application, an application of a conductive polymer composite material is provided.

[0051] Application of the conductive polymer composite material described above and / or the conductive polymer composite material obtained by the preparation method described above in grounding materials.

[0052] Optionally, the following steps are included:

[0053] Placing the conductive polymer composite material and the metal rod core on a production line, extruding and heating them to obtain a temperature-resistant conductive polymer composite grounding material;

[0054] or,

[0055] The conductive polymer composite material is ground using an air classifying mill (ACM), passed through a 180-mesh standard sieve to obtain a heat-resistant conductive polymer composite powder coating, and then electrostatically sprayed on the surface of a metal rod, and baked at 200° C. for 20 minutes to obtain a heat-resistant conductive polymer composite grounding material.

[0056] Optionally, during the extrusion process, the processing temperatures of the single-screw extruder are: 170°C to 195°C in the first zone, 195°C to 210°C in the second zone, 195°C to 205°C in the third zone and 190°C to 200°C in the die.

[0057] Optionally, during the heating process, the thermal extension is controlled within a range of 15% to 25%.

[0058] The beneficial effects of this application include:

[0059] 1) The present application provides a heat-resistant conductive polymer composite material. The thermoplastic polyurethane used in the conductive polymer composite material has the characteristics of an elastomer and can provide good mechanical properties. Thermoplastic polyimide is a heat-resistant, acid-resistant, and corrosion-resistant polymer that can improve the heat and corrosion resistance of the composite material. At the same time, the glass transition temperature of thermoplastic polyimide is lower than that of thermosetting polyimide, and it can be processed and formed at a lower temperature. Polytetrathiafulvalene conductive polymer is a conductive polymer copolymerized by tetrathiafulvalene and cobalt salt, has good conductivity, and improves the conductive properties of the polymer composite material.

[0060] 2) The heat-resistant conductive polymer composite material provided in this application can be wrapped or electrostatically sprayed onto the exterior of a metal fiber core to create a grounding material. This material exhibits excellent grounding and current drainage performance. In the event of a fault current or lightning strike, the current can be rapidly transmitted laterally through the metal core to the distal end and dispersed longitudinally into the soil through the heat-resistant conductive polymer composite coating, achieving rapid drainage. Its resistivity is no greater than 1 / 10 of the buried soil resistivity. This corrosion-resistant conductive polymer composite grounding material also exhibits excellent resistance to acid, alkali, and seawater corrosion, with an annual corrosion rate of less than 0.03% and a water absorption rate of less than 0.05%.

[0061] 3) The present application provides a temperature-resistant conductive polymer composite material, which can be widely used in highly corrosive soils, coastal areas and highly polluted areas. It has excellent environmental universality and is environmentally friendly. It solves the failure of grounding devices caused by corrosion and realizes the full life cycle service of grounding devices. DETAILED DESCRIPTION

[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0063] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased from commercial sources. The parts in the following examples are calculated by mass.

[0064] Example 1

[0065] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0066] First, add 10.0 parts (g) of 1,3-bis(4-aminophenoxy)benzene and 0.7 parts of 4,4'-diaminodiphenyl ether to a 500mL beaker equipped with a magnetic stirrer. Add 200.0 parts (g) of N,N-dimethylacetamide solution and stir to fully dissolve the diamine. Then, slowly add 10.5 parts of 3,3',4,4'-biphenyltetracarboxylic dianhydride (solids content of the mixed solution is 10%). After the addition of 3,3',4,4'-biphenyltetracarboxylic dianhydride, react at room temperature under nitrogen for 24 hours to obtain a light yellow polyamic acid solution. 25.0 parts of acetic anhydride and 12.5 parts of isoquinoline were added to the above polyamic acid solution at room temperature, stirred for 2 hours, heated to 85°C and stirred for 5 hours. After cooling to room temperature, the reaction mixture was poured into ethanol to obtain a fibrous polyimide. The polyimide material was filtered and washed thoroughly with hot ethanol, and then dried in a vacuum drying oven at 60°C overnight to obtain a thermoplastic polyimide powder.

[0067] A mixture of 50.0 parts of tetrakis(methylthio)tetrathiafulvalene and 12.5 parts of cobalt acetate was copolymerized at 133° C. for 12 hours to obtain a polytetrathiafulvalene conductive polymer.

[0068] (2) Preparation of temperature-resistant conductive polymer composite materials

[0069] 40.0 parts of thermoplastic polyurethane, 20.0 parts of thermoplastic polyimide, 30.0 parts of polytetrathiafulvalene conductive polymer, 1.0 part of lubricant molybdenum disulfide, 1.5 parts of lubricant niobium diselenide, 2.0 parts of coupling agent aluminate, 1.0 part of antioxidant β-naphthoflavone, 0.3 part of antioxidant zedoaria flavonoid, 3.0 parts of flame retardant DOPO, 0.5 part of anti-aging agent 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, and 0.5 part of anti-aging agent N-phenyl-α-aniline are mixed for 9 minutes; then the uniformly mixed materials are added to a twin-screw extruder for extrusion and granulation, and the granules are then dried in a hot air dryer to obtain a conductive polymer composite material. The temperatures of the conveying section, melting section, mixing section, exhaust section, homogenizing section and die head of the twin-screw extruder are 130℃~150℃, 180℃~200℃, 195℃~205℃, 185℃~195℃, 175℃~195℃ and 195℃~205℃ respectively.

[0070] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0071] (a) The conductive polymer composite material and the metal rod core are placed on a production line, extruded, and heated to obtain a temperature-resistant conductive polymer composite grounding material. During the extrusion process, the processing temperatures of the single-screw extruder are: 170°C to 195°C in the first zone, 195°C to 210°C in the second zone, 195°C to 205°C in the third zone, and 190°C to 200°C in the die. During the heating process, the thermal extension is controlled to be 15% to 25%.

[0072] (b) The conductive polymer composite material is ground using an air classifying mill (ACM) and passed through a 180-mesh standard sieve to obtain a heat-resistant conductive polymer composite powder coating. The powder is then electrostatically sprayed onto the surface of a metal rod and baked at 200°C for 20 minutes to obtain a heat-resistant conductive polymer composite grounding material. Alternatively, the conductive polymer powder coating can be electrostatically sprayed onto the surface of a lithium-ion battery positive electrode to produce a long-life composite positive electrode.

[0073] Performance is shown in Table 1.

[0074] Example 2

[0075] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0076] The same as Example 1, no further details will be given.

[0077] (2) Preparation of temperature-resistant conductive polymer composite materials

[0078] 35.0 parts of thermoplastic polyurethane, 25.0 parts of thermoplastic polyimide, and 30.0 parts of polytetrathiafulvalene conductive polymer. Other parts are the same as in Example 1 and will not be repeated here.

[0079] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0080] The same as in Example 1, no further description is given. The performance is shown in Table 1.

[0081] Example 3

[0082] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0083] The same as Example 1, no further details will be given.

[0084] (2) Preparation of temperature-resistant conductive polymer composite materials

[0085] 30.0 parts of thermoplastic polyurethane, 25.0 parts of thermoplastic polyimide, and 35.0 parts of polytetrathiafulvalene conductive polymer. Other parts are the same as in Example 1 and will not be repeated here.

[0086] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0087] The same as in Example 1, no further description is given. The performance is shown in Table 1.

[0088] Example 4

[0089] (1) Preparation of Thermoplastic Polyimide and Polytetrathiafulvalene Conductive Polymers

[0090] The same as Example 1, no further details will be given.

[0091] (2) Preparation of temperature-resistant conductive polymer composite materials

[0092] 40.0 parts of thermoplastic polyurethane, 25.0 parts of thermoplastic polyimide, and 20.0 parts of polytetrathiafulvalene conductive polymer. Other parts are the same as in Example 1 and will not be repeated here.

[0093] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0094] The same as in Example 1, no further description is given. The performance is shown in Table 1.

[0095] Example 5

[0096] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0097] The same as Example 1, no further details will be given.

[0098] (2) Preparation of temperature-resistant conductive polymer composite materials

[0099] 40.0 parts of thermoplastic polyurethane, 15.0 parts of thermoplastic polyimide, and 35.0 parts of polytetrathiafulvalene conductive polymer. Other parts are the same as in Example 1 and will not be repeated here.

[0100] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0101] The same as in Example 1, no further description is given. The performance is shown in Table 1.

[0102] The properties of the corrosion-resistant conductive polymer composite grounding materials prepared in Examples 1 to 5 were tested, and the results are shown in Tables 1 and 2.

[0103] Table 1 Performance test of conductive polymer composite materials in Examples 1 to 5

[0104] Note: The UV aging test in Table 1 refers to GB / T2951.11-2008, the air oven aging test refers to GB / T2951.12-2008, the water absorption test refers to Section 9.2 (weight method) of GB / T2951.13-2008, the resistivity test refers to GB / T3048.3-2007, and the power frequency high current refers to the provisions of DL / T1342-2014.

[0105] Table 2 Performance test of corrosion-resistant conductive polymer-based metal composite grounding electrodes in Examples 1 to 5

[0106] Note: All tests in Table 2 refer to the relevant provisions of "Technical Requirements for Composite Grounding Electrodes" GB / T21698-2008.

[0107] It can be seen from Table 1 that the conductive materials prepared in Examples 1 to 5 have excellent weather resistance and water absorption resistance, with a resistivity of about 0.95-1.48Ω·cm, good electrical conductivity, and do not soften or melt under high power frequency current. It can also be seen from Table 2 that the grounding materials prepared in Examples 1 to 5 have excellent corrosion resistance, excellent thermal stability, resistance to high power frequency current, and resistance to freeze-thaw cycles, regardless of whether they are in a neutral high-salt or acidic alkaline environment. The grounding material prepared by the present invention can solve the failure of the grounding device caused by corrosion, and can be used for grounding drainage and high current remote drainage such as fault current and lightning current in the power grid system, to achieve full life cycle service of the power grid grounding device, and can be used in materials for power, transportation, and communication systems. It has excellent electrical conductivity, low resistivity, thermal stability, corrosion resistance, resistance to high power frequency current, and resistance to freeze-thaw cycles, and also has excellent universality of grounding environments, excellent grounding performance, and environmental friendliness.

[0108] In the prior art CN115536958A, the resistivity is about 1.5-2.5Ω·cm, and the elongation at break is 39-61%.

[0109] Comparative Example 1

[0110] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0111] The same as Example 1, no further details will be given.

[0112] (2) Preparation of temperature-resistant conductive polymer composite materials

[0113] The polytetrathiafulvalene conductive polymer was replaced with polypyrrole in an amount of 30.0 parts. The other parts were the same as those in Example 1 and will not be described in detail.

[0114] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0115] The same as Example 1, no further details will be given.

[0116] Resistivity tests were conducted on the conductive materials in Example 1 and Comparative Example 1 using a four-probe tester. The volume resistivity of the conductive material in Example 1 was 1.12 Ω·cm, and the surface resistivity was 1.97 Ω. The volume resistivity of the conductive material in Comparative Example 1 was 9.39 Ω·cm, and the surface resistivity was 15.78 Ω. This indicates that polytetrathiafulvalene conductive polymer can significantly reduce the resistivity of the composite grounding material compared to polypyrrole.

[0117] Comparative Example 2

[0118] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0119] The same as Example 1, no further details will be given.

[0120] (2) Preparation of temperature-resistant conductive polymer composite materials

[0121] The polytetrathiafulvalene conductive polymer was replaced with polyaniline in an amount of 30.0 parts. The other parts were the same as those in Example 1 and will not be described in detail.

[0122] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0123] The same as Example 1, no further details will be given.

[0124] Resistivity tests were conducted on the conductive materials in Example 1 and Comparative Example 2 using a four-probe tester. The volume resistivity of the conductive material in Example 1 was 1.12 Ω·cm, and the surface resistivity was 1.97 Ω. The volume resistivity of the conductive material in Comparative Example 2 was 10.47 Ω·cm, and the surface resistivity was 17.03 Ω. This indicates that polytetrathiafulvalene conductive polymer can significantly reduce the resistivity of the composite grounding material compared to polyaniline.

[0125] Comparative Example 3

[0126] (1) Preparation of thermoplastic polyimide and polytetrathiafulvalene conductive polymers

[0127] The same as Example 1, no further details will be given.

[0128] (2) Preparation of temperature-resistant conductive polymer composite materials

[0129] Thermoplastic polyimide was replaced with low-density polyethylene in an amount of 40.0 parts. Other parts were the same as those in Example 1 and will not be described in detail.

[0130] (3) Preparation of temperature-resistant conductive polymer composite grounding materials

[0131] The same as Example 1, no further details will be given.

[0132] The glass transition temperatures of Example 1 and Comparative Example 3 were measured using a thermal analyzer. The glass transition temperatures of Example 1 and Comparative Example 3 were 201° C. and 103° C., respectively. It can be seen that without the thermoplastic polyimide, the temperature resistance of the composite material is greatly reduced.

[0133] The above descriptions are merely a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application discloses the preferred embodiments as above, they are not intended to limit the present application. Any technical personnel familiar with the present profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A temperature-resistant conductive polymer composite material, characterized in that: The conductive polymer composite material comprises the following components: The above parts are calculated by mass.

2. The conductive polymer composite material according to claim 1, characterized in that: The particle size of the conductive polymer composite material is 30 μm to 2 mm.

3. The conductive polymer composite material according to claim 1 or 2, characterized in that: The polytetrathiafulvalene conductive polymer is obtained by forming a coordination polymer of tetrathiafulvalene and cobalt atoms.

4. The conductive polymer composite material according to any one of claims 1 to 3, characterized in that: The thermoplastic polyurethane is selected from at least one of Huntsman IROGRAN A 85D 6003, BASF 685A, and Lubrizol ESTANE 2355-75A.

5. The conductive polymer composite material according to any one of claims 1 to 4, characterized in that: The weight average molecular weight of the thermoplastic polyimide is 20,000 to 40,000.

6. The conductive polymer composite material according to any one of claims 1 to 5, characterized in that: The glass transition temperature of the thermoplastic polyimide is 180°C to 220°C.

7. The conductive polymer composite material according to any one of claims 1 to 6, characterized in that: The lubricant is selected from at least one of graphite, molybdenum disulfide, niobium diselenide and paraffin.

8. The conductive polymer composite material according to any one of claims 1 to 7, characterized in that: The coupling agent is selected from at least one of a silane coupling agent and an aluminate coupling agent.

9. The conductive polymer composite material according to any one of claims 1 to 8, characterized in that: The antioxidant is selected from at least one of flavonoid antioxidants, β-naphthoflavone, zedoaria flavonoids, and glycyrrhizin flavonoids A.

10. The conductive polymer composite material according to any one of claims 1 to 9, characterized in that: The flame retardant is selected from at least one of phosphorus-nitrogen halogen-free flame retardants, melamine, ammonium polyphosphate, and DOPO derivatives.

11. The conductive polymer composite material according to any one of claims 1 to 10, characterized in that: The antioxidant is selected from at least one of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and N-phenyl-α-aniline.

12. The method for preparing the conductive polymer composite material according to any one of claims 1 to 11, characterized in that: The following steps are involved: S1, obtaining thermoplastic polyimide powder; S2, copolymerizing a mixture containing tetrathiafulvalene and a cobalt salt to obtain a polytetrathiafulvalene conductive polymer; S3, extruding and granulating the material containing thermoplastic polyurethane, the thermoplastic polyimide powder, the polytetrathiafulvalene conductive polymer, the lubricant, the coupling agent, the antioxidant, the flame retardant, and the antioxidant to obtain the conductive polymer composite material.

13. The preparation method according to claim 12, characterized in that: In step S2, the tetrathiafulvalene is selected from at least one of bis(carbonyldithio)tetrathiafulvalene, formyltetrathiafulvalene and tetra(methylthio)tetrathiafulvalene.

14. The preparation method according to claim 12 or 13, characterized in that: In step S2, the cobalt salt is selected from at least one of cobalt acetate, cobalt chloride and cobalt nitrate.

15. The preparation method according to any one of claims 12 to 14, characterized in that: In step S2, the mass ratio of the tetrathiafulvalene to the cobalt salt is 1:1 to 8:

1.

16. The preparation method according to any one of claims 12 to 15, characterized in that: In step S2, the copolymerization conditions are as follows: time is 8h to 24h; temperature is 100°C to 150°C.

17. The preparation method according to any one of claims 12 to 16, characterized in that: In step S3, the extrusion granulation includes twin-screw extrusion and single-screw extrusion.

18. The preparation method according to any one of claims 12 to 17, characterized in that: In step S3, during twin-screw extrusion, the temperatures of the conveying section, melting section, mixing section, exhaust section, homogenizing section and die head of the twin-screw extruder are 130°C to 150°C, 180°C to 200°C, 195°C to 205°C, 185°C to 195°C, 175°C to 195°C and 195°C to 205°C, respectively.

19. The preparation method according to any one of claims 12 to 18, characterized in that: In step S3, during single screw extrusion, the processing temperatures of the single screw extruder are: 170°C to 185°C in the first zone, 195°C to 205°C in the second zone, 195°C to 205°C in the third zone and 185°C to 195°C in the die.

20. The preparation method according to any one of claims 12 to 19, characterized in that: The following steps are involved: A1, first obtain a polyamic acid precursor solution, prepare polyimide by chemical imidization dehydration under the action of a dehydrating agent and a catalyst, and obtain polyimide powder after drying; A2, copolymerizing a mixture containing tetrathiafulvalene and a cobalt salt to obtain a polytetrathiafulvalene conductive polymer; A3. Extruding and granulating the material containing thermoplastic polyurethane, the thermoplastic polyimide powder, the polytetrathiafulvalene conductive polymer, the lubricant, the coupling agent, the antioxidant, the flame retardant and the antioxidant to obtain the conductive polymer composite material.

21. The preparation method according to claim 20, characterized in that: In step A1, the polyamic acid precursor solution is prepared by stirring in an inert atmosphere at room temperature.

22. The preparation method according to claim 20 or 21, characterized in that: In step A1, the dehydrating agent is selected from at least one of acetic anhydride and phthalic anhydride.

23. The preparation method according to any one of claims 20 to 22, characterized in that: In step A1, the catalyst is selected from at least one of isoquinoline and pyridine.

24. The preparation method according to any one of claims 20 to 23, characterized in that: In step A1, the mixing conditions are as follows: the polyamic acid reaction time is 20 h to 30 h.

25. Use of the conductive polymer composite material obtained by the preparation method according to any one of claims 12 to 24 in grounding materials.

26. The use according to claim 25, characterized in that The following steps are involved: Placing the conductive polymer composite material and the metal rod core on a production line, extruding and heating, and obtaining a temperature-resistant conductive polymer composite grounding material; or, The conductive polymer composite material is ground by an air classifying mill ACM, and passed through a 180-mesh standard sieve to obtain a heat-resistant conductive polymer composite powder coating, and then the powder is electrostatically sprayed on the surface of a metal rod and baked at 200° C. for 20 minutes to obtain a heat-resistant conductive polymer composite grounding material.

27. The preparation method according to claim 26, characterized in that: During the extrusion process, the processing temperatures of the single-screw extruder are: 170°C to 195°C in the first zone, 195°C to 210°C in the second zone, 195°C to 205°C in the third zone and 190°C to 200°C in the die.

28. The preparation method according to claim 26 or 27, characterized in that: During the heating process, the thermal extension is controlled within 15% to 25%.

Citation Information

Patent Citations

  • Method for preparing tetrathiafulvalene molecule-based micrometer and / or nanometer functional materials

    CN101913555A

  • Conductive polyimide composite material and preparation method thereof

    CN112795185A

  • Corrosion-resistant conductive polymer composite material as well as preparation method and application thereof

    CN115536958A

  • Composite copper current collector and preparation method thereof, electrode and secondary battery

    CN115799525A

  • Temperature-resistant conductive polymer composite material as well as preparation method and application thereof

    CN116144163A