Process for the synthesis of a glycerol polyester
The controlled esterification and polycondensation of glycerol and dicarboxylic acid in a water medium addresses the challenges of unoptimized glycerol polyester synthesis, achieving high molar masses and low polydispersity, resulting in improved mechanical strength and processing capacity.
Patent Information
- Application Number
- PCT/EP2023/085400
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-17
AI Technical Summary
The synthesis of glycerol polyesters, particularly poly(glycerol sebacate), faces challenges in controlling macro and microstructure, leading to unoptimized physicochemical properties and processing difficulties due to poor solubility of monomers and uncontrolled esterification reactions, resulting in polymers with high molar masses but high polydispersity and excessive branching.
A process involving the controlled esterification and polycondensation of glycerol and dicarboxylic acid in a water medium, with specific molar ratios and temperature conditions, to achieve a number average molar mass of at least 1500 g/mol and a polydispersity index less than 6, while limiting the molar rate of (1,2,3-triacylglyceride) units to less than 15%, thereby improving the polymer's mechanical strength and processing capacity.
This process enables the production of glycerol polyesters with controlled macro and microstructure, achieving high molar masses and low polydispersity, enhancing mechanical strength and processing capabilities, while maintaining industrial compatibility.
Smart Images

Figure EP2023085400_17102024_PF_FP_ABST
Abstract
Description
[0001] Process for the synthesis of a polyester from glycerol
[0002] Technical field
[0003] The field of the present invention is that of the synthesis of polyesters, in particular biocompatible polyester, obtained by esterification of hydroxyl groups of a polyol and carboxyl groups of a diacid by a polycondensation reaction.
[0004] State of the art
[0005] A conventional method for synthesizing a polymer of glycerol and a diacid is carried out in a molten medium at high temperature with long reaction times and consists of an esterification step followed by a polycondensation. Such a method is for example described in EP1448656A1. The monomers constituting such a polymer have different affinities. Thus, glycerol is typically poorly soluble with dicarboxylic acids (or their corresponding diesters). This poor affinity between monomers has the consequence of making the reaction difficult to control and reproduce, due to difficult homogenization of the reaction medium. It also leads to the production of polymers with uncontrolled macrostructural and microstructural properties, which result in limited physicochemical properties that do not meet application needs.
[0006] In order to overcome these drawbacks, a process for synthesizing a biocompatible and biodegradable polymer has been developed, in particular by the polycondensation of a diacid and a polyol, in the presence of water, which allows the control and modification of the polymerization reaction that occurs. Such a process is described in document WO2015184313A1. This process consists of preparing a polymer material comprising, firstly, dissolving a polyol monomer, which may be glycerol, in an aqueous liquid in a reactor. Secondly, the process involves adding a diacid monomer to the aqueous solution, then refluxing the reaction mixture comprising the polyol monomer, the aqueous liquid and the acid monomer. The process includes removing water from the reactor, for example by distillation, if necessary. The resulting polyester is then recovered.This process is particularly suitable for the synthesis of poly(glycerol sebacate) from glycerol and sebacic acid.
[0007] Furthermore, the glycerol monomer involved in the preparation of glycerol polyesters is trifunctional. In other words, during polymerization, the esterification reaction can take place on the three alcohol functions of glycerol. This leads to the creation of crosslinking points or branching points in the polymer by the creation of units (1,2,3-triacylglyceride) and therefore leads to branched polyester structures. When the branching points are not controlled and undergone, a gelled product can quickly be obtained and therefore a product that flows with difficulty and whose shaping is complicated.
[0008] It is a constant concern of polyester manufacturers to offer products with optimized characteristics. In terms of macro- and microstructural characteristics, with existing methods, high molar masses could be achieved but often at the expense of the polydispersity index with an esterification time, not always compatible with the industrial application of the process.
[0009] Technical problem
[0010] The technical problem that the present invention aims to solve is to better control the macro and microstructure of the polymer during the synthesis of a glycerol polyester, in an industrially compatible time and in particular during the synthesis of poly(glycerol sebacate) or PGS, in order to give it better processing capacity. In particular, the aim of the present invention is to propose a process for the synthesis of a glycerol polyester, more particularly poly(glycerol sebacate) or PGS, having a high molar mass greater than or equal to 1500 g / mol, while controlling the dispersity of the polyester and its molar content of unit (1,2,3-triacylglyceride).
[0011] Statement of the invention
[0012] Continuing its research efforts in this direction, the Applicant has developed a process which makes it possible, in a controlled and reproducible manner, to obtain in an industrially compatible time a polyester, in particular a glycerol polyester, in particular a poly(glycerol sebacate) or PGS, with improved characteristics, namely a number-average molar mass (Mn) greater than or equal to 1500 g / mol which ensures good mechanical strength of the material at room temperature, while maintaining a polydispersity index D (Mw / Mn) less than 6 and a molar rate of unit (1,2,3-triacylglyceride) less than 15 mol% relative to all the units of the polyester. This improvement through the control of an optimal macro- and microstructure of the polyester predicts a better processing capacity of the polymer.
[0013] Thus, a first object of the invention is a process for synthesizing a polyester from glycerol and a dicarboxylic acid comprising the steps:
[0014] (a) bringing into contact in water the glycerol monomers and the dicarboxylic acid with a glycerol / diacid molar ratio ranging from 1 / 1 to 1.5 / 1, preferably ranging from 1.1 / 1 to 1.4 / 1;
[0015] (b) esterification under an inert atmosphere at a temperature ranging from 100°C to 180°C for a period ranging from 4 to 55 h,
[0016] (c) polycondensation at a temperature varying from 100°C to 180°C under vacuum and for a duration varying from 0 to 10 hours, in which process, the esterification duration TE expressed in hours satisfies the following inequality:
[0017] TP being the polycondensation time R being the glycerol / diacid molar ratio TempE being the reaction temperature It is understood that the term "reaction" refers to the reaction that is always carried out, i.e. the esterification reaction. TempE is the temperature of the esterification reaction.
[0018] A second subject of the invention is a polyester obtained from glycerol and a dicarboxylic acid having the following characteristics: a number-average molar mass (Mn) greater than or equal to 1500 g / mol, a polydispersity index D (Mw / Mn) less than 6, a molar rate of unit (1,2,3-triacylglyceride) less than 15 mol% relative to all the units of the polyester.
[0019] Summary of the invention
[0020] The invention, described in more detail below, relates to at least one of the embodiments listed in the following points:
[0021] 1. Process for the preparation of a polyester of a glycerol and a dicarboxylic acid comprising the steps
[0022] (a) contacting in water glycerol monomers and the dicarboxylic acid with a glycerol / diacid molar ratio ranging from 1 / 1 to 1.5 / 1, preferably ranging from 1 / 1 to 1.4 / 1, preferably ranging from 1.1 / 1 to 1.4 / 1;
[0023] (b) esterification under an inert atmosphere at a temperature ranging from 100°C to 180°C, for a period ranging from 4 to 55 h,
[0024] (c) polycondensation at a temperature varying from 100°C to 180°C, under vacuum and for a duration varying from 0 to 100, in which process, the esterification duration TE expressed in hours satisfying the following inequality:
[0025] 15 - 0.3* (TempE- 140) - 3.5*TP + 80*(Rl) <TE <42 - 0,3* (TempE- 140) - 3,5*TP + 100*(R-l)
[0026] TP being the polycondensation duration in hours
[0027] R being the polyol / diacid molar ratio, i.e. the glycerol / diacid molar ratio
[0028] TempE being the reaction temperature in °C
[0029] 2. Method according to the embodiment in which the dicarboxylic acid is an aliphatic dicarboxylic acid comprising 3 to 36 carbon atoms.
[0030] 3. Process according to any one of the preceding embodiments in which the dicarboxylic acid is an aliphatic dicarboxylic acid corresponding to the formula [HOOC- (CEEjn-COOH], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
[0031] 4. Process according to any one of the preceding embodiments in which the dicarboxylic acid is chosen from malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid or a mixture of two or more of these dicarboxylic acids.
[0032] 5. A method according to any one of the preceding embodiments wherein the dicarboxylic acid comprises sebacic acid. A method according to any one of the preceding embodiments wherein the dicarboxylic acid is sebacic acid. A method according to any one of the preceding embodiments wherein the monomers are brought into contact by introducing the dicarboxylic acid monomer into a mixture comprising the glycerol monomer and water. A method according to any one of the preceding embodiments wherein the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in liquid form. A method according to any one of the preceding embodiments wherein the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form. A method according to any one of the preceding embodiments wherein the mixture does not comprise a catalyst.Process according to any one of the preceding embodiments in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form and the contacting of the monomers of step (a) is followed by a step of melting the diacid monomer in the aqueous medium. Process according to any one of the preceding embodiments in which at the end of the contacting of the monomers of step (a), the reaction medium is brought to reflux. Process according to any one of the preceding embodiments in which the process comprises at the end of step (a) a step of removing the water introduced for the contacting of the monomers, preferably by distillation.A process according to any one of the preceding embodiments wherein the process comprises a step of removing water, preferably by distillation, which follows or is concomitant with the esterification step (b), polycondensation step (c) or esterification (b) and polycondensation step (c). A process according to any one of the preceding embodiments wherein the esterification temperature of step (b) is in a range from 130°C to 150°C. A process according to any one of the preceding embodiments wherein the polycondensation temperature of step (c) is in a range from 130°C to 150°C. A process according to any one of the preceding embodiments wherein the esterification temperature and the polycondensation temperature are identical. 18.Process according to any one of the preceding embodiments in which the esterification time varies from more than 4h to 55h, advantageously from 5h to 55h, more advantageously from 15h to 55h, even more advantageously from 20h to 55h.
[0033] 19. Method according to any one of the preceding embodiments not comprising a catalyst addition step.
[0034] 20. Poly(glycerol sebacate) obtainable by the process defined in any one of the preceding embodiments.
[0035] 21. Poly(glycerol sebacate) having the following characteristics: a. A number-average molar mass (Mn) greater than or equal to 1500 g / mol; b. A dispersity D (Mw / Mn) less than 6; c. A rate of (1,2,3,-triacylglyceride) units less than 15mol% relative to all the units of the poly(glycerol sebacate).
[0036] 22. Poly(glycerol sebacate) according to the preceding embodiment having a cumulative rate of (1,2-diacylglyceride) and (1,3-diacylglyceride) units greater than or equal to 40 mol% relative to all the units of the poly(glycerol sebacate).
[0037] 23. Poly(glycerol sebacate) according to any one of embodiments 21 to 22 having a molar ratio of the (1,3-diacylglyceride) unit to the (1,2-diacylglyceride) unit greater than 1.
[0038] Definitions
[0039] In this document, unless expressly stated otherwise, all percentages (%) indicated are percentages (%) in moles.
[0040] The letter E is used to denote esterification and the letter P is used to denote polycondensation.
[0041] On the other hand, any interval of values designated by the expression "between a and b" represents the range of values from more than a to less than b (i.e., excluding the limits a and b), while any interval of values designated by the expression "from a to b" means the range of values from a to b (i.e., including the strict limits a and b). In this document, when an interval of values is designated by the expression "from a to b", the interval represented by the expression "between a and b" is also and preferably designated.
[0042] When a "majority" compound is referred to, within the meaning of the present invention, this compound is the majority among the compounds of the same type in the composition, i.e. it is the one that represents the largest quantity by mass among the compounds of the same type. On the contrary, a "minority" compound is a compound that does not represent the largest mass fraction among the compounds of the same type. Preferably, by majority, we mean a mass proportion of more than 50%; when the compound represents 100% by mass, it is also referred to as "majority".
[0043] The compounds mentioned in the description may be of fossil or bio-sourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already in use, that is to say, they may be, partially or totally, derived from a recycling process, or obtained from raw materials themselves derived from a recycling process. This particularly concerns monomers.
[0044] Detailed description of the invention
[0045] The process according to the invention for preparing a polyester of a glycerol and a dicarboxylic acid comprises the steps: o (a) of bringing the glycerol and dicarboxylic acid monomers into contact in water with a glycerol / diacid molar ratio ranging from 1 / 1 to 1.5 / 1, preferably ranging from 1.1 / 1 to 1.4 / 1; o (b) of esterification under an inert atmosphere at a temperature varying from 100°C to 180°C for a duration varying from 4 to 50 h, o (c) of polycondensation at a temperature varying from 100°C to 180°C under vacuum and for a duration varying from 0 to 10 h, the esterification duration TE expressed in hours satisfying the following inequality:
[0046] 15 - 0.3*(TempE-140) - 3.5*TP + 80*(Rl) <TE <42 - 0,3*(TempE-140) - 3,5*TP + 100*(R-l)
[0047] TP being the polycondensation duration
[0048] R being the polyol / diacid molar ratio, i.e. the glycerol / diacid molar ratio
[0049] TempE being the esterification reaction temperature
[0050] According to step (a) of the process of the invention, the glycerol and dicarboxylic acid monomers are brought into contact in water.
[0051] The dicarboxylic acid monomer according to the invention may be aliphatic, aromatic or aliphatic / aromatic. In the latter case, the diacid comprises an aliphatic part and an aromatic part. It preferably comprises from 4 to 36 carbon atoms. Aliphatic means linear, cyclic or branched aliphatic, whether saturated or unsaturated.
[0052] According to preferred variants of the invention, the dicarboxylic acid monomer is aliphatic.
[0053] According to these variants, the dicarboxylic acid monomer may have the formula [HOOC- (CEEjn-COOH], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
[0054] Preferably, according to these variants of the invention, the dicarboxylic acid monomer may be chosen from malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid or a mixture of two or more of these dicarboxylic acids.
[0055] According to variants of the invention, the dicarboxylic acid monomer may be a mixture of at least two dicarboxylic acids. Preferably then, the dicarboxylic acid monomer comprises sebacic acid.
[0056] According to preferred variants of the invention, the dicarboxylic acid monomer is sebacic acid. The polyester according to the invention may be derived from glycerol, dicarboxylic acid and at least one other monomer.
[0057] Preferably then the dicarboxylic acid comprises sebacic acid. More preferably then, the dicarboxylic acid is sebacic acid.
[0058] As another monomer, we can cite for example diol monomers, >
[0059] According to preferred variants of the invention, the dicarboxylic acid monomer and glycerol are the only monomers. Very preferably then, the sebacic acid monomer and glycerol are the only monomers.
[0060] The invention makes it possible to dispense with the presence of a catalyst. Thus, advantageously, the mixture does not comprise a catalyst. This concerns the mixture of step a) and also the mixture of each of the following steps. Thus, advantageously, the process does not comprise a step of adding a catalyst.
[0061] According to any of the variants of the invention, the contacting of the monomers is carried out in a reactor. The following reactions can take place in the same reactor. Given the heating and pressure conditions, a person skilled in the art will be able to adapt the type of container or reactor necessary for the process.
[0062] According to variants of the invention, the contacting of the monomers of step (a) is carried out by adding water to the mixture of glycerol and dicarboxylic acid. The addition of water to the mixture of monomers allows homogenization of the mixture and thus reduces its overall viscosity. In order to promote this homogenization, stirring is carried out in a known manner.
[0063] According to these variants, the water is added to the monomers in a quantity by mass of between 0%m and 100%m of the mass of the monomers involved, preferably ranging from 5%m to 50%m of the mass of the monomers involved, more preferably ranging from 10%m to 40%m of the mass of the monomers involved.
[0064] According to other particularly preferred variants of the invention, the contacting of the monomers is carried out by introducing the dicarboxylic acid monomer into a mixture comprising glycerol and water, improving the homogenization of the reaction mixture after the addition of the dicarboxylic acid. In order to promote this homogenization, stirring is carried out in a known manner.
[0065] According to these preferred variants, prior to step (a), the glycerol and the water are mixed with a molar ratio of glycerol to water advantageously varying from 1 / 10 to 10 / 1.
[0066] The step of mixing the glycerol and the aqueous solution may take place at room temperature (approximately 23°C at atmospheric pressure) in a container, which may be the same as that of step (a). This preliminary mixing may optionally include heating the glycerol and water to a temperature ranging from approximately 50 to 100°C. The medium is then heated for a time sufficient to dissolve or disperse the glycerol homogeneously in the water. In order to promote homogenization of the medium, stirring is carried out in a known manner, whether or not there is heating.
[0067] According to any of these variants, the dicarboxylic acid monomer can be introduced into the mixture comprising glycerol and water, in liquid form or in solid form. According to preferred variants of the invention, the dicarboxylic acid monomer is introduced into a mixture comprising glycerol and water, in solid form and the contacting of the monomers is followed by a step of melting the diacid monomer in the aqueous medium.
[0068] According to an advantageous implementation of the invention, after bringing the monomers of step (a) into contact, the reaction medium can be brought to reflux by heating it. The reflux of the medium allows, for example, the melting of the dicarboxylic acid monomer when it is introduced in solid form. For example, sebacic acid is slightly soluble in water at room temperature, and this solubility is increased when the temperature increases. The reflux of the reaction medium can be carried out by heating the medium to a temperature varying from approximately 50 to 150°C for a sufficient time to obtain the melting and intimate mixing of the monomers.
[0069] According to other variants, when the dicarboxylic acid is introduced as a liquid at room temperature, the reflux step is optional.
[0070] Those skilled in the art will understand that in certain embodiments, the reaction medium may be pressurized to reach temperatures up to 200°C, or higher in order to shorten the reflux time and / or for the case where the diacid monomer only melts at elevated temperatures.
[0071] According to step (a) of the process of the invention, the glycerol and dicarboxylic acid monomers are brought into contact in an aqueous medium with a glycerol / diacid molar ratio ranging from 1 / 1 to 1.5 / 1, preferably ranging from 1 / 1 to 1.4 / 1, preferably ranging from 1.1 / 1 to 1.4 / 1.
[0072] At the end of step (a), the water added for carrying out this step can be removed, for example by distillation or any other known water removal process. The monomers are then in liquid form and homogeneously mixed, thus allowing the subsequent esterification and polycondensation reactions to take place in a controlled manner.
[0073] The esterification step produces water as a by-product of the reaction. Thus, some of the water removed is the water added to carry out step (a), while the other part of the water is the by-product of the monomers reacting with each other. By measuring the amount of water removed, it can be determined when the water from step (a) has been completely removed. This makes it possible to determine when step (b) has started.
[0074] The water removal step may comprise heating the reaction medium to a temperature of about 50 to 200°C or, in particular, about 80 to 150°C, although water removal under vacuum at lower temperatures is also possible.
[0075] Where water removal is by distillation, this may occur in conjunction with agitation and / or purging of the vessel contents by reaction under an inert gas, such as after an initial distillation step after reflux to remove water added as a processing aid.
[0076] After the removal of the added water, the glycerol and dicarboxylic acid monomers react with each other according to step (b) of the process of the invention, under an inert atmosphere at a temperature in the range from 100°C to 180°C, preferably from 130°C to 150°C, for a period varying from 4 to 55 h, advantageously for a period varying from more than 4 h to 55 h. Thus TempE varies from 100°C to 180°C, preferably from 130°C to 150°C. Advantageously, step (b) lasts from 5 h to 55 h, more advantageously from 15 h to 55 h, even more advantageously from 20 h to 55 h.
[0077] A reaction under an inert atmosphere is known to mean a reaction in an inert gas such as nitrogen, carbon dioxide, a rare gas or a mixture thereof.
[0078] According to advantageous variants of the invention, concomitantly with step (b), the water produced by the esterification reaction is removed, for example by distillation or any other method known for removing water. According to these variants, the removal of water, for example by distillation, can be carried out directly following the step of removing the water initially added.
[0079] The process of the invention continues with a step (c) of polycondensation at a temperature, TempP, varying from 100°C to 180°C, advantageously from 130°C to 150°C, under vacuum and for a duration varying from 0 to 10 h. The esterification and polycondensation steps are advantageously isothermal. Thus, the polycondensation temperature is advantageously identical to the esterification temperature. Thus, advantageously, the polycondensation is carried out at TempE, which means that TempP=TempE.
[0080] According to a variant of the invention, at the end of step (b), prior to placing under vacuum, the pressure is preferably reduced to an intermediate pressure between atmospheric pressure and vacuum, possibly in stages. Any method known to those skilled in the art can be used to lower the pressure, in particular using a peristaltic pump, a membrane pump, a rotary pump, etc. Such an intermediate pressure is less than 1 bar and varies, for example, from 800 mbar to 50 mbar.
[0081] The reaction medium is then placed under vacuum. Here, "vacuum" means that the pressure is reduced until it reaches a value around Imbar.
[0082] Polycondensation can then take place instantly or for a period of up to 10 hours.
[0083] According to advantageous variants of the invention, concomitantly with step (c), the water produced by the polycondensation reaction is removed, for example, by distillation or any other method known for removing water. According to these variants, the removal of water, for example, by distillation, can be carried out following the step of removing the initially added water by reflux.
[0084] According to advantageous variants of the invention, concomitantly with step (b) and step (c), the water produced by the esterification and polycondensation reactions is removed, for example, by distillation or any other method known for removing water. According to these variants, the removal of water, for example by distillation, can be carried out following the step of removing the initially added water by reflux.
[0085] An essential element of the process according to the invention is that the esterification time TE expressed in hours satisfies the following inequality:
[0086] TP being the polycondensation time R being the glycerol / diacid molar ratio TempE being the reaction temperature The implementation of the process of the invention in all its variants and aspects, preferred or not, makes it possible to obtain in an industrially compatible time, a polyester of glycerol and a dicarboxylic acid, in particular a poly(glycerol sebacate) or PGS, which very advantageously has the following physicochemical characteristics: a number-average molar mass (Mn) greater than or equal to 1500 g / mol a polydispersity index D (Mw / Mn) less than 6, a molar rate of unit (1,2,3-triacylglyceride) less than 15 mol% relative to all the units of the polyester.
[0087] Such a polyester is also the subject of the invention.
[0088] Advantageously, such a polyester mainly has 1,2-diacylglyceride and 1,3-diacylglyceride units to have linear chains, preferably the cumulative molar rate of the 1,2-diacylglyceride and 1,3-diacylglyceride units is greater than or equal to 40 mol% relative to all the units of the polyester.
[0089] According to these variants, preferably the molar ratio of 1,3-diacylglyceride to 1,2-diacylglyceride is greater than 1 / 1, or greater than or equal to 1.5 / 1.
[0090] The physicochemical characteristics of the polyester obtained with the process of the invention suggest interesting homogeneous and reproducible properties, due to a controlled polydispersity index of less than 6, and in particular improved processing properties due to the low rate of unit (1,2,3-triacylglyceride) and therefore of branching leading to early gelling during the process not allowing number-average molar masses greater than 1500 g / mol to be reached.
[0091] The above-mentioned characteristics of the present invention, as well as others, will be better understood upon reading the following description of several exemplary embodiments of the invention, given for illustrative and non-limiting purposes.
[0092] EXAMPLES OF CARRYING OUT THE INVENTION
[0093] 1- Synthesis of poly(glycerol sebacate):
[0094] Table 1 shows the molar ratios between monomers and the reaction conditions of the different stages of the PGS synthesis process.
[0095] The polymerization tests are carried out according to the procedure described below with the following variable parameters described in Table 1:
[0096] TE: esterification time
[0097] TP: polycondensation time
[0098] R: glycerol / sebacic acid molar ratio TempE: reaction temperature
[0099] Test procedure
[0100] In a 500 mL double jacketed reactor topped with a distillation column configured in total reflux and a condenser connected to a distillate recovery pot, glycerol (112 g, 1.3 molar equiv.) is mixed with water (25 g) at room temperature under nitrogen flow (0.1 L / min). Gentle stirring is implemented (50 rpm) for 5 min. After dissolving the glycerol, sebacic acid (mass of sebacic acid = mass of glycerol / 92.09 * 202.25 / R, i.e. 189 g for R = 1 molar equiv.) is added to the aqueous mixture in the reactor. Finally, the remaining water is added to the medium (25 g). The reactor vessel is then heated to a jacket temperature allowing TempE to be reached. Stirring is gradually increased to 100 rpm and then 150 rpm with increasing melting and solubilization of the acid.When the medium in the tank has become clear (around 95°C), the stirring is increased to a final value of 200 rpm and the medium is left at reflux. When the vapor temperature at the top of the distillation column reaches 98°C, and after an equilibration time of 15 min, the column configuration is switched to total withdrawal. Esterification of the medium is carried out over a period of TE hours. The water distilled during the test is recovered in a dedicated heat-insulated recovery pot.
[0101] Next, a vacuum system is connected to the distillation condenser and a pressure below atmospheric pressure is applied to the reactor contents. The pressure is reduced slowly and stepwise (approximately 10 to 15% per step) over approximately 30 minutes to a target value of less than 10 mbar.
[0102] Once the pressure in the reaction vessel stabilizes at 5 mbar, the medium is left to react at TempE (thus TempP=TempE) for an additional TP hours. During this polycondensation step, the stirring speed is reduced to 115 rpm to account for the increased viscosity of the mixture.
[0103] The produced PGS is transferred from the reactor vessel to a container after the facility has been depressurized and allowed to cool to room temperature. The product is then transferred to a freezer for storage, where it is frozen for at least approximately 24 hours before analysis.
[0104] 2- Measurement methods used:
[0105] 2-1 Determination of the microstructure of PGS polymers:
[0106] The microstructure of polymers is determined by NMR analysis 1 H, supplemented by NMR analysis 13 C when the resolution of the NMR spectra of the XH does not allow the attribution and quantification of all species. Measurements are carried out using a BRUKER 500MHz NMR spectrometer at frequencies of 500.43 MHz for proton observation and 125.83 MHz for carbon observation.
[0107] 2-2 Determination of the macrostructure of PGS polymers:
[0108] The SEC (Size Exclusion Chromatography) technique separates macromolecules in solution according to their size through columns filled with a porous gel. The macromolecules are separated according to their hydrodynamic volume, with the largest being eluted first.
[0109] Although not an absolute method, SEC allows us to understand the molar mass distribution of a polymer. From commercial standard products, the different number-average (Mn) and weight-average (Mw) molar masses can be determined and the polydispersity index (£> = Mw / Mn), also called "dispersity", calculated. Size exclusion chromatography analyses were carried out with a Viscotek apparatus (Malvern Instruments) equipped with 3 columns (SDVB, 5 pm, 300 x 7.5 mm from Polymer Standard Service), a guard column and 3 detectors (differential refractometer and viscometer, and light scattering). 1 mL of a solution of the sample with a concentration of 5 mg mL-1 in THF was filtered through a 0.45 pm PTFE membrane. 100 pL of this solution was eluted in THF using a flow rate of 0.8 mL min-1 at a temperature of 35 °C. OmniSEC software was used for data acquisition and analysis.The number (Ain) and mass (A- / w) molar masses of the polymers as well as their dispersity (£>) were calculated using a calibration curve from standard polystyrenes (A7p: 1,306 to 2,520,000 g mol-1) from Polymer Standard Service (Mainz).
[0110] 3- Results:
[0111] Tables 1a and 1b below give the operating conditions of the synthesis process, as well as the results of the measurements carried out on the PGS obtained at the end of these syntheses according to the parameters TE, TP, R and TempE. [Table 1a]:
[0112] [Table lb]:
[0113] Examples 1, 2, 5, 6, 7, 11, 12, 14 and 16 were carried out with esterification times (TE) adjusted as a function of the glycerol / sebacic acid molar ratio (R), the temperature (TempE) and the polycondensation time (TP), the polymers obtained have molar masses Mn greater than 1500 g / mol and limited branching rates (measured by molar % of 1,2,3-triacylglyceride unit less than 15% mol). They are in accordance with the invention.
[0114] On the contrary, examples 3, 4, 8, 9, 10, 13 and 15 are not in accordance with the invention. The polymers obtained do not exhibit all of the expected characteristics.
Claims
CLAIMS 1. Process for the preparation of a polyester of a glycerol and a dicarboxylic acid comprising the steps o (a) of bringing into contact in water the glycerol monomers and the dicarboxylic acid with a glycerol / diacid molar ratio ranging from 1 / 1 to 1.5 / 1, preferably ranging from 1.1 / 1 to 1.4 / 1; o (b) esterification under an inert atmosphere at a temperature varying from 100°C to 180°C, preferably from 130°C to 150°C, for a duration varying from 4 to 55 h, advantageously from more than 4 h to 55 h (c) polycondensation at a temperature varying from 100°C to 180°C, preferably from 130°C to 150°C under vacuum and for a duration varying from 0 to 10 h, in which process, the esterification duration TE, expressed in hours, satisfies the following inequality: TP being the polycondensation duration in hours R being the glycerol / diacid molar ratio TempE being the reaction temperature in °C.
2. Process according to the preceding claim in which the dicarboxylic acid is an aliphatic dicarboxylic acid corresponding to the formula [H00C-(CH2)n-C00H], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
3. A method according to any one of the preceding claims wherein the dicarboxylic acid is sebacic acid.
4. Process according to any one of the preceding claims in which the contacting of the monomers is carried out by the introduction of the dicarboxylic acid monomer into a mixture comprising the glycerol monomer and water.
5. Process according to any one of the preceding claims in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form.
6. Process according to any one of the preceding claims in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form and the contacting of the monomers of step (a) is followed by a step of melting the diacid monomer in the aqueous medium.
7. Process according to any one of the preceding claims in which, at the end of the contacting of the monomers from step (a), the reaction medium is brought to reflux.
8. Process according to any one of the preceding claims in which the process comprises at the end of step (a) a step of removing the water introduced for bringing the monomers into contact, preferably by distillation.
9. Process according to any one of the preceding claims in which the process comprises a step of removing water, preferably by distillation, which follows or is concomitant with the step of esterification (b), polycondensation (c) or esterification (b) and polycondensation (c).
10. A method according to any one of the preceding claims wherein the method does not comprise a catalyst addition step.
11. Poly(glycerol sebacate) obtainable by the process defined in any one of the preceding claims.
12. Poly(glycerol sebacate) having the following characteristics: a. A number-average molar mass (Mn) greater than or equal to 1500 g / mol; b. A dispersity D (Mw / Mn) less than 6; c. A rate of (1,2,3,-triacylglyceride) units less than 15mol% relative to all the units of the poly(glycerol sebacate).
13. Poly(glycerol sebacate) according to the preceding claim having a cumulative level of (1,2-diacylglyceride) and (1,3-diacylglyceride) units greater than or equal to 40 mol% relative to all the units of the poly(glycerol sebacate).
14. Poly(glycerol sebacate) according to any one of claims 12 and 13 having a molar ratio of the (1,3-diacylglyceride) unit to the (1,2-diacylglyceride) unit greater than 1.
Citation Information
Patent Citations
Water-mediated preparations of polymeric materials
WO2015184313A1
Biodegradable polymer
EP1448656A2
Water-mediated preparations of polymeric materials
US20150344618A1
Cited By
Silicone substitute and topical compositions containing it
FR3164379A1
Silicone substitute and topical compositions comprising same
WO2026013103A1