Process for the synthesis of a glycerol polyester
The synthesis of glycerol polyesters using a controlled esterification and polycondensation process with a food-grade tin catalyst addresses the challenges of monomer solubility and toxicity, achieving high molar masses and controlled properties, improving the polymer's industrial compatibility and properties.
Patent Information
- Application Number
- PCT/EP2024/059915
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional methods for synthesizing glycerol polyesters face challenges such as poor solubility of monomers, leading to uncontrolled macrostructural and microstructural properties, long reaction times, and toxicity issues with metal catalysts, which result in polymers with limited physicochemical properties and industrial incompatibility.
A process involving the esterification of glycerol and dicarboxylic acid in the presence of water at controlled temperatures, followed by polycondensation under vacuum with a food-grade tin-based catalyst, such as monobutyltin oxide, to achieve high molar masses, controlled dispersity, and low residual monomer levels, while minimizing reaction time and toxicity.
The process effectively synthesizes glycerol polyesters with high number average molar masses greater than 2500 g/mol, low dispersity, and controlled branching, reducing residual monomers and gel formation, thus enhancing the polymer's thermomechanical properties and industrial compatibility.
Smart Images

Figure IMGF000015_0001 
Figure IMGF000016_0001 
Figure IMGF000016_0002
Abstract
Description
[0001] Process for the synthesis of a polyester from glycerol
[0002] Technical field
[0003] The field of the present invention is that of the synthesis of polyesters obtained by esterification of hydroxyl groups of a polyol and carboxyl groups of a diacid by a polycondensation reaction.
[0004] State of the art
[0005] A conventional method for synthesizing a polymer of glycerol and a diacid is carried out in a molten medium at high temperature with long reaction times and consists of an esterification step followed by a polycondensation carried out at very low pressure. Such a method is for example described in EP1448656A1. The constituent monomers of such a polymer have different affinities. Thus, glycerol is typically poorly soluble with dicarboxylic acids. This poor affinity between monomers has the consequence of making the reaction difficult to control and reproduce due to difficult homogenization of the reaction medium. This leads to the production of polymers with uncontrolled macrostructural and microstructural properties, which result in limited physicochemical properties that do not meet application needs.
[0006] Document EP3149067A1 describes a process for synthesizing a polymer of glycerol and a dicarboxylic acid which is improved from the point of view of implementation by using a synthesis process in water at the beginning of the esterification step, facilitating the obtaining of a homogeneous medium and a polymer with better controlled physicochemical properties making it possible to envisage certain applications, such as those requiring strict control of the distribution of the molar mass, in particular the controlled release of substances.
[0007] Other processes for the synthesis of glycerol polyesters have been described. For example, the use of metal catalysts for the production of polyesters from the condensation of glycerol and dicarboxylic acids, in particular PGS, has been considered. Such metal catalysts have a toxicological profile that is not always compatible with the use of these polyesters to prepare biomaterials, which requires syntheses in a highly controlled toxicity environment. The article in Polymer 55 (2014) 5065-5072 describes the synthesis of a polymer of glycerol and a dicarboxylic acid, adipic acid, in bulk medium (without solvent) in the presence of dibutyltin oxide, which has a level of acute toxicity. The resulting polymers are hyperbranched with relatively low molar masses, even after 111130 of reaction.
[0008] As this article shows, the glycerol monomer involved in the preparation of glycerol polyesters is trifunctional. In other words, during polymerization, the esterification reaction can take place on the three alcohol functions of glycerol. This leads to the creation of crosslinking points or branching points in the polymer by the creation of units (1,2,3-triacylglyceride) and therefore leads to branched polyester structures. When the branching points are not controlled and undergone, a gelled product can quickly be obtained and therefore a product that flows with difficulty, causing risks of clogging and material breakage, and whose shaping is complicated.
[0009] There is a continuing need to develop efficient synthesis processes for a biocompatible glycerol-dicarboxylic acid polymer, particularly PGS, with reduced reaction times for better industrial compatibility. In this regard, one should not lose sight of the need to control the structure of the resulting polymer, in particular by ensuring a high molar mass greater than 2500g / mol, maintaining an acceptable dispersity and a controlled branching rate.
[0010] Furthermore, shortening reaction times for better process efficiency can result in generating a certain amount of residual monomers that can complicate the control of the thermomechanical properties of the resulting polymer. This is why the development of efficient synthesis processes for a biocompatible glycerol and dicarboxylic acid polymer, particularly PGS, must be done by controlling the amount of residual monomers.
[0011] In addition, some applications of such a polyester require syntheses in a very controlled toxicity environment which must also be taken into account.
[0012] Technical problem
[0013] The objective of the invention is to provide a process for the efficient synthesis of a polymer of glycerol and a dicarboxylic acid, in particular PGS, which meets all the constraints defined above and which overcomes the problems encountered with prior processes. In particular, the objective of the invention is to provide a process for the efficient synthesis of a polymer of glycerol and a dicarboxylic acid, in particular PGS, with reduced reaction times, compatible with industrial application, while controlling the structure of the polymer obtained, in particular by ensuring a high molar mass greater than 2500g / mol, maintaining an acceptable dispersity and a controlled level of (1,2,3-triacylglyceride) units, while minimizing the amount of residual monomers to a low level.
[0014] Statement of the invention
[0015] Continuing its efforts, the Applicant has developed a process for synthesizing a polymer of glycerol and a dicarboxylic acid with accelerated kinetics that overcomes the synthesis difficulties described above and provides an acceptable toxicological environment. In particular, the Applicant has developed a synthesis process that makes it possible to obtain a polymer of glycerol and a dicarboxylic acid having high number-average molar masses greater than 2500g / mol, a contained dispersity less than or equal to 10 and a content of (1,2,3-triacylglyceride) units less than 15 mol% relative to all the units of the polymer without gel formation, as well as a low residual monomer content, less than 5% by mass relative to the polymer.
[0016] Thus, a first object of the invention is a process for preparing a polymer of glycerol and a dicarboxylic acid which comprises
[0017] (a) bringing into contact the monomers comprising at least glycerol and a dicarboxylic acid in the presence of water, at a temperature below 100°C, according to a glycerol / dicarboxylic acid molar ratio varying from 0.5 / 1 to 10 / 1;
[0018] (b) esterification under an inert atmosphere at a temperature above 100°C;
[0019] (c) placing the reaction medium under vacuum at a pressure of less than 100 mbara, at a temperature of more than 110°C;
[0020] (d) maintaining a vacuum and a temperature above 110°C to carry out a polycondensation; which process comprises introducing a polycondensation catalyst at the end of the esterification of step (b), before the vacuuming of step (c) or after the vacuuming of step (c), in an amount less than or equal to 5000 ppm relative to the total mass of the monomers, said catalyst being a food grade tin-based catalyst chosen from organotin compounds comprising a carboxyl function (-C(O)OH), organotin compounds comprising a (-Sn(O)OH) function and tin bis(2(ethylhexanoate).
[0021] More specifically, said catalyst is food grade monobutyltin oxide, also known as butyl stannic acid, which catalyst is marketed under the name FASCAT 9100 by the company PMC Organometallix.
[0022] Another subject of the invention is a polymer of glycerol and a dicarboxylic acid having a level of residual glycerol and dicarboxylic acid monomers of less than 5% by weight of the weight of the polymer obtained, measured by SEC / RI and 13C NMR; a high number-average molar mass Mn greater than 2500 g / mol; a dispersity of less than or equal to 10; a level of (1,2,3-triacylglyceride) units of less than 15 mol% relative to all the units of the polymer.
[0023] Summary of the invention
[0024] The invention, described in more detail below, relates to at least one of the embodiments listed in the following points:
[0025] 1. A process for preparing a polyester of glycerol and a dicarboxylic acid which comprises
[0026] (a) bringing into contact the monomers comprising at least glycerol and a corresponding dicarboxylic acid in the presence of water, at a temperature below 100°C, according to a glycerol / dicarboxylic acid molar ratio varying from 0.5 / 1 to 10 / 1,
[0027] (b) esterification under an inert atmosphere at a temperature above 110°C, preferably ranging from 130°C to 180°C
[0028] (c) placing the reaction medium under vacuum at a pressure below 100 mbar at a temperature above 110°C, preferably ranging from 130°C to 180°C,
[0029] (d) maintaining a vacuum and a temperature above 110°C, preferably ranging from 130°C to 180°C, to carry out a polycondensation, which process comprises introducing a polycondensation catalyst at the end of the esterification of step (b), before the vacuuming of step (c) or after the vacuuming of step (c), in an amount less than or equal to 5000 ppm relative to the total mass of monomers, said catalyst being a food grade tin-based catalyst chosen from organotin compounds comprising a carboxyl function (-C(O)OH), organotin compounds comprising a (-Sn(O)OH) function and monobutyltin tris(2(ethylhexanoate).
[0030] 2. Method according to embodiment 1 in which the dicarboxylic acid is aliphatic and comprises 3 to 36 carbon atoms.
[0031] 3. Process according to any one of the preceding embodiments in which the dicarboxylic acid has the formula [HOOC-(CH2)n-COOH], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
[0032] 4. Process according to any one of the preceding embodiments in which the dicarboxylic acid is chosen from malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid or a mixture of two or more of these dicarboxylic acids.
[0033] 5. A method according to any one of the preceding embodiments wherein the dicarboxylic acid comprises sebacic acid.
[0034] 6. Method according to any one of the preceding embodiments in which the dicarboxylic acid is sebacic acid.
[0035] 7. Process according to any one of the preceding embodiments in which the glycerol / dicarboxylic acid molar ratio varies from 0.9 / 1 to 2 / 1, preferably from 1 / 1 to 1.5 / 1.
[0036] 8. Method according to any one of the preceding embodiments in which the contacting of the monomers is carried out by the introduction of the dicarboxylic acid monomer into a mixture comprising the glycerol monomer and water.
[0037] 9. Method according to any one of the preceding embodiments in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in liquid form.
[0038] 10. Method according to any one of the preceding embodiments in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form.
[0039] 11. Method according to any one of the preceding embodiments in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form and the contacting of the monomers of step (a) is followed by a step of melting the diacid monomer in the aqueous medium.
[0040] 12. Process according to any one of the preceding embodiments in which, at the end of the contacting of the monomers of step (a), the reaction medium is brought to reflux.
[0041] 13. Method according to any one of the preceding embodiments in which the method comprises at the end of step (a) a step of removing the water introduced for bringing the monomers into contact, preferably by distillation.
[0042] 14. Process according to any one of the preceding embodiments in which the process comprises a step of removing water, preferably by distillation, which follows or is concomitant with the esterification step (b), the polycondensation step (c) or the esterification step (b) and the polycondensation step (c).
[0043] 15. Process according to any one of the preceding embodiments in which the evacuation of the reaction medium of step (c) is carried out at a pressure of less than 50 mbara, preferably less than 10 mbara.
[0044] 16. Process according to any one of the preceding embodiments in which the food grade tin-based catalyst is chosen from food grade alkyltins comprising a carboxyl function (-C(O)OH) or a function (-Sn(O)OH), the alkyl group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms. 17. Process according to any one of embodiments 1 to 15 in which the food grade tin-based catalyst is chosen from food grade monobutyltin oxide (or stannoic acid) and food grade monobutyltin tris(2-ethylhexanoate).
[0045] 18. A method according to any one of the preceding embodiments wherein the food grade tin-based catalyst is food grade monobutyltin oxide (or stannoic acid).
[0046] 19. Method according to any one of the preceding embodiments in which the catalyst is introduced in an amount less than or equal to 3000 ppm.
[0047] 20. Method according to any one of the preceding embodiments in which the catalyst is introduced in an amount greater than or equal to 1000 ppm.
[0048] 21. Polyester of glycerol and a dicarboxylic acid, capable of being obtained by the process defined in any one of the preceding embodiments.
[0049] 22. Polyester of glycerol and a dicarboxylic acid having a residual monomer content of less than 5% by weight of the polymer weight; a number-average molar mass Mn greater than 2500 g / mol; a dispersity D (Mw / Mn) less than or equal to 10; a content of (1,2,3-triacylglyceride) units of less than 15 mol% relative to all the units of the polymer.
[0050] 23. Polyester of glycerol and a dicarboxylic acid according to embodiment 21 having a number-average molar mass Mn greater than or equal to 2700 g / mol.
[0051] 24. Polyester of glycerol and a dicarboxylic acid according to any one of embodiments 21 and 23 having a number-average molar mass Mn of less than 3500 g / mol, preferably less than 3000 g / mol.
[0052] 25. Polyester of glycerol and a dicarboxylic acid according to any one of embodiments 21 to 24 having a dispersity D (Mw / Mn) less than or equal to 5.
[0053] Definitions
[0054] In this document, unless expressly stated otherwise, all percentages (%) indicated are percentages (%) in moles.
[0055] In this document, unless otherwise indicated, pressure is expressed in absolute pressure indicated by the unit "bara" which corresponds to "absolute bar".
[0056] On the other hand, any interval of values designated by the expression "between a and b" represents the range of values from more than a to less than b (i.e., excluding the limits a and b), while any interval of values designated by the expression "from a to b" means the range of values from a to b (i.e., including the strict limits a and b). In this document, when an interval of values is designated by the expression "from a to b", the interval represented by the expression "between a and b" is also and preferably designated.
[0057] When a "majority" compound is referred to, within the meaning of the present invention, this compound is the majority among the compounds of the same type in the composition, i.e. it is the one that represents the largest quantity by mass among the compounds of the same type. On the contrary, a "minority" compound is a compound that does not represent the largest mass fraction among the compounds of the same type. Preferably, by majority, we mean a mass proportion of more than 50%; when the compound represents 100% by mass, it is also referred to as "majority".
[0058] When a "food grade" catalyst is referred to, it is understood herein that the catalyst is safe for human consumption. It complies with FDA (Food and Drug Administration) standards 21 CFR 175.300, 21 CFR 177.2420 and 21 CFR 175.105.
[0059] The compounds mentioned in the description may be of fossil or bio-sourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. Similarly, the compounds mentioned may also come from the recycling of materials already in use, that is to say, they may be, partially or totally, derived from a recycling process, or obtained from raw materials themselves derived from a recycling process. This particularly concerns monomers.
[0060] Detailed description of the invention
[0061] The process according to the invention for preparing a polyester of glycerol and a dicarboxylic acid comprises steps (a), (b), (c) and (d) as presented above in embodiment 1.
[0062] According to step (a) of the process of the invention, the glycerol and dicarboxylic acid monomers are brought into contact in water.
[0063] The dicarboxylic acid monomer according to the invention may be aliphatic, aromatic or aliphatic / aromatic. In the latter case, the diacid comprises an aliphatic part and an aromatic part. It preferably comprises from 4 to 36 carbon atoms. Aliphatic means linear, cyclic or branched aliphatic, whether saturated or unsaturated.
[0064] According to preferred variants of the invention, the dicarboxylic acid monomer is aliphatic comprising 3 to 36 carbon atoms.
[0065] According to these variants, the dicarboxylic acid monomer may preferably correspond to the formula [HOOC-(CH2)n-COOH], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
[0066] Preferably, according to these variants of the invention, the dicarboxylic acid monomer may be chosen from malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid or a mixture of two or more of these dicarboxylic acids.
[0067] According to variants of the invention, the dicarboxylic acid monomer may be a mixture of at least two dicarboxylic acids. Preferably then, the dicarboxylic acid monomer comprises sebacic acid. According to preferred variants of the invention, the dicarboxylic acid monomer is sebacic acid.
[0068] According to preferred variants of the invention, the dicarboxylic acid monomer and glycerol are the only monomers. Very preferably then, the sebacic acid monomer and glycerol are the only monomers.
[0069] According to any of the variants of the invention, the contacting of the monomers is carried out in a container or reactor. The following reactions can take place in the same reactor. Given the heating and pressure conditions, a person skilled in the art will be able to adapt the type of container or reactor necessary for the process.
[0070] According to variants of the invention, the contacting of the monomers of step (a) is carried out by adding water to the mixture of glycerol and dicarboxylic acid. The addition of water to the mixture of monomers allows homogenization of the mixture and thus reduces its overall viscosity. In order to promote this homogenization, stirring is carried out in a known manner.
[0071] According to these variants, the water is added to the monomers in a quantity by mass of between 0%m and 100%m of the mass of the monomers involved, preferably ranging from 5%m to 50%m of the mass of the monomers involved, more preferably ranging from 10%m to 40%m of the mass of the monomers involved.
[0072] According to other particularly preferred variants of the invention, the contacting of the monomers is carried out by introducing the dicarboxylic acid monomer into a mixture comprising glycerol and water, improving the homogenization of the reaction mixture after the addition of the dicarboxylic acid. In order to promote this homogenization, stirring is carried out in a known manner.
[0073] According to these preferred variants, prior to step (a), the glycerol and the water are mixed with a molar ratio of glycerol to water advantageously varying from 1 / 10 to 10 / 1.
[0074] The step of mixing the glycerol and the aqueous solution may take place at room temperature (from 20°C to 30°C, generally about 23°C, at atmospheric pressure) in a container, which may be the same as that of step (a). This preliminary mixing may optionally include heating the glycerol and water to a temperature ranging from about 50 to 100°C. The medium is then heated for a time sufficient to dissolve or disperse the glycerol homogeneously in the water. In order to promote homogenization of the medium, stirring is carried out in a known manner, whether or not there is heating.
[0075] According to any of these variants, the dicarboxylic acid monomer can be introduced into the mixture comprising glycerol and water, in liquid form or in solid form, preferably in solid form.
[0076] According to the invention, the contacting of the monomers is carried out at a temperature below 100°C. Advantageously, in particular when the dicarboxylic acid monomer is introduced in solid form, the contacting of the monomers is followed by a step of melting the diacid monomer in the aqueous medium.
[0077] According to an advantageous implementation of the invention, after bringing the monomers of step (a) into contact, the reaction medium is heated, optionally brought to reflux. Heating the medium allows, for example, the melting of the dicarboxylic acid monomer when it is introduced in solid form. For example, sebacic acid is slightly soluble in water at room temperature, and this solubility is increased when the temperature increases. The reaction medium is heated to a temperature varying from approximately 50 to 150°C for a sufficient time to obtain the melting and intimate mixing of the monomers. During this temperature increase step which makes it possible to obtain a homogeneous medium, care is taken to condense the vapors well in the reactor, for example by configuring the column in total reflux, according to methods well known to those skilled in the art.
[0078] In other variants, for example when the dicarboxylic acid is introduced as a liquid at room temperature, the reflux step is optional.
[0079] Those skilled in the art will understand that in certain embodiments, the reaction medium may be pressurized to reach temperatures up to 200°C, or higher in order to shorten the reflux time and / or for the case where the diacid monomer only melts at elevated temperatures.
[0080] According to step (a) of the process of the invention, the glycerol and dicarboxylic acid monomers are brought into contact in an aqueous medium with a glycerol / diacid molar ratio of between 0.5 / 1 and 10 / 1, preferably ranging from 0.9 / 1 to 2 / 1, more preferably from 1 / 1 to 1.5 / 1.
[0081] At the end of step (a), the water added for carrying out this step can be removed, for example by distillation or any other known water removal process. The monomers are then in liquid form and homogeneously mixed, thus allowing the subsequent esterification and polycondensation reactions to take place in a controlled manner.
[0082] The water removal step may comprise heating the reaction medium to a temperature of about 50 to 200°C, in particular, about 80 to 180°C, under atmospheric pressure, although water removal under lower pressure at lower temperatures is also conceivable.
[0083] When water removal is by distillation, this may occur in conjunction with agitation and / or purging of the container contents by reaction under an inert gas.
[0084] After the removal of the added water, the glycerol and dicarboxylic acid monomers react with each other according to step (b) of the process of the invention, under an inert atmosphere at a temperature above 110°C, preferably ranging from 110°C to 200°C, more preferably from 120°C to 180°C, more preferably from 130°C to 180°C, for a period advantageously ranging from 4 to 48 h.
[0085] A reaction under an inert atmosphere is known to mean a reaction in an inert gas such as nitrogen, carbon dioxide, a rare gas or a mixture thereof.
[0086] This esterification step (b) is preferably carried out at atmospheric pressure. Those skilled in the art will understand that an alternative is to carry out this step at lower pressures in order to lower the temperatures and / or pressures, for example pressures between Ibara and 100 mbara.
[0087] According to advantageous variants of the invention, concomitantly with step (b), the water produced as a by-product of the esterification reaction is removed, for example by distillation or any other method known for removing water. According to these variants, the removal of water, for example by distillation, can be carried out directly following the step of removing the water initially added. Thus, at this stage of the process, part of the water removed is the water added to carry out step (a), while the other part of the water is the by-product of the reaction of the monomers with each other. By measuring the quantity of water removed, it is possible to determine when the water from step (a) has been completely removed. It is thus possible to determine the start of step (b).
[0088] The process of the invention continues with a step (c) by which the reaction medium is then placed under vacuum. Here, the term "vacuum" means the fact of lowering the pressure until it reaches a value less than or equal to 100 mbara, preferably less than 50 mbara, more preferably less than 10 mbara. According to one embodiment, the pressure is within a range from 5 mbara to 10 mbara.
[0089] An essential element of the invention consists of the introduction into the reaction medium, at the end of step (b), of a catalyst in an amount less than or equal to 5000 ppm relative to the total mass of the monomers, preferably an amount greater than or equal to 2500 ppm, said catalyst being a food grade catalyst based on tin chosen from organotin compounds comprising a carboxyl function (-C(O)OH) or a function (-Sn(O)OH).
[0090] By "food grade catalyst" is meant a catalyst suitable for food contact (for animals and humans) which meets requirements ensuring that there is no risk of toxicity induced by this catalyst for the polyester manufactured.
[0091] The introduction of the catalyst at the end of step (b) can be done before the evacuation of step (c) or after the evacuation of step (c), preferably before the evacuation of step (c) for reasons of ease of handling.
[0092] According to variants of the invention, at the end of step (b), prior to the vacuuming of step (c), the pressure can be reduced, possibly in stages, to an intermediate pressure between atmospheric pressure and vacuum. Any method known to those skilled in the art can be used to lower the pressure, in particular using a peristaltic pump, a membrane pump, a rotary pump, etc. Such an intermediate pressure is less than 1 bara and varies, for example, from 800 mbara to 50 mbara.
[0093] According to these variants of the invention, the introduction of the catalyst can then be done directly at the end of step (b) before reducing the pressure to an intermediate pressure, or during the reduction, for example upon reaching a plateau, or just before the evacuation of step (c), or even after the evacuation of step (c).
[0094] The catalyst may be introduced directly in solid form, in dissolved form or in suspension in a liquid (e.g. water) or in liquid form. The catalyst may be mixed with the reaction medium in a known manner, for example with stirring.
[0095] The catalyst according to the invention is introduced in an amount less than or equal to 5000 ppm relative to the mass of the monomers introduced, preferably in an amount less than or equal to 3000 ppm.
[0096] Generally, the catalyst is introduced in an amount of at least 200 ppm relative to the mass of the monomers introduced. This minimum catalyst value allows for optimized catalytic activity. Thus, preferably the catalyst according to the invention is introduced in an amount within a range from 200 ppm to 5000 ppm, more preferably from 200 ppm to 3000 ppm. According to variants of the invention, the catalyst according to the invention is preferably introduced in an amount greater than or equal to 1000 ppm relative to the mass of the monomers introduced. Thus, according to these variants, the catalyst according to the invention is introduced in an amount within a range from 1000 ppm to 5000 ppm, more preferably from 1000 ppm to 3000 ppm.
[0097] The catalyst according to the invention is of food grade based on tin chosen from organotin compounds comprising a carboxyl function (-C(O)OH), organotin compounds comprising a function (-Sn(O)OH) and monobutyltin tris(2(ethylhexanoate).
[0098] According to particular variants of the invention, the catalyst is chosen from alkyltins comprising a carboxyl function (-C(O)OH) or a function (-Sn(O)OH), the alkyl group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and monobutyltin tris(2(ethylhexanoate). Among these particular compounds, mention may be made of food grade monobutyltin oxide (or stannoic acid) and food grade monobutyltin tris(2-ethylhexanoate).
[0099] According to preferred variants of the invention, the catalyst is food grade monobutyltin oxide (or stannoic acid).
[0100] Examples of catalysts useful for the purposes of the invention include monobutyltin oxide marketed under the name FASCAT 9100 and monobutyltin tris(2-ethylhexanoate) marketed under the name FASCAT 9102 by the company PMC Organometallix. Particularly preferred is the catalyst monobutyltin oxide marketed under the name FASCAT 9100 by the company PMC Organometallix.
[0101] At the end of step (c) and the introduction of the catalyst into the reaction medium, the process of the invention continues with a step (d) of polycondensation at a temperature above 110°C, preferably varying from 110°C to 250°C, more preferably from 120°C to 200°C, more preferably from 130°C to 180°C, under vacuum and for a duration varying from 0 to 10 h.
[0102] Polycondensation can then take place instantly (i.e. in the time required to install the vacuum) or for a period of up to 10 hours.
[0103] According to advantageous variants of the invention, concomitantly with step (d), the water produced by the polycondensation reaction is removed, for example, by distillation or any other known method for removing water. According to advantageous variants of the invention, concomitantly with step (b) and step (d), the water produced by the esterification and polycondensation reactions is removed, for example, by distillation or any other known method for removing water. According to these variants, the removal of water, for example, by distillation, may be continuous from the step of removing the initially added water. When the removal of water is done by distillation, this may occur in conjunction with stirring and / or purging of the contents of the container by reaction under an inert gas.
[0104] At the end of these steps of the process according to the invention, the polyester produced can be recovered in a known manner, stored if necessary, and possibly treated for subsequent use.
[0105] The polyester of glycerol and a dicarboxylic acid, capable of being obtained by the process according to the invention defined above according to any one of its variants, is also the subject of the invention.
[0106] The implementation of the process of the invention in all its variants and aspects, preferred or not, makes it possible to obtain a polyester of glycerol and a dicarboxylic acid, in particular a poly(glycerol sebacate) or PGS, which very advantageously has the following physicochemical characteristics: a level of residual monomers less than 5% by weight of the weight of the polymer, preferably less than 2% by weight, a high number-average molar mass Mn greater than 2500 g / mol, preferably greater than or equal to 2700 g / mol, a dispersity less than or equal to 10, preferably less than or equal to 5, a level of (1,2,3-triacylglyceride) units less than 15 mol% relative to all the units of the polymer.
[0107] Such a polyester is also the subject of the invention.
[0108] Advantageously, according to preferred variants of the invention, such a polyester has a weight-average molar mass less than or equal to 3500 g / mol, preferably less than or equal to 3000 g / mol.
[0109] The physicochemical characteristics of the polyester obtained with the process of the invention suggest interesting homogeneous and reproducible properties, due to a controlled dispersity of 10 or less, and in particular improved processing properties due to the low unit rate (1,2,3-triacylglyceride), less than 15% by mole relative to all the acylglyceride functions present in the polymer determined by NMR. 13 C, and therefore the low branching rate. In fact, the branching rate is expressed as the molar ratio of the unit rate (1,2,3-triacylglyceride) to the sum of the rates of all the acylglyceride functions of the polymer
[0110] The residual monomer content is determined according to the method described in the examples.
[0111] The macrostructure (Mn, Mw and D (Mw / Mn)) of the polyester of glycerol and a dicarboxylic acid is determined by SEC according to the method described in the examples.
[0112] The microstructure of the polyester of glycerol and a dicarboxylic acid is determined by C NMR 13 according to the method described in the examples.
[0113] The above-mentioned characteristics of the present invention, as well as others, will be better understood upon reading the following description of several exemplary embodiments of the invention, given for illustrative and non-limiting purposes.
[0114] EXAMPLES OF CARRYING OUT THE INVENTION
[0115] 1- Synthesis of polyglycerol sebacate):
[0116] Table 1 shows the molar ratios between monomers and the reaction conditions of the different stages of the PGS synthesis process.
[0117] The general procedure used for all tests is as follows:
[0118] In a 500 mL double jacketed reactor topped with a distillation column configured in total reflux and a condenser connected to a distillate recovery pot, a defined amount of glycerol is mixed with a defined amount of water at room temperature under nitrogen flow (0.1 L / min). Low agitation is implemented (50 rpm) for 5 min. After dissolution of the glycerol, a defined amount of sebacic acid is added to the aqueous mixture in the reactor. Finally, the remaining water is added to the medium to reach the target monomer concentration in the medium. The reactor vessel is then heated to a jacket temperature described in Table 1. Agitation is gradually increased to 100 rpm and then to 150 rpm with the melting and increasing solubilization of the acid. When the medium in the tank has become clear (around 95°C), the stirring is increased to a final value of 200 rpm and the medium left to reflux.When the temperature of the vapors at the top of the distillation column reaches 98°C, and after an equilibration time of 15 min, the column configuration is switched to total withdrawal.
[0119] Where appropriate, a catalyst is introduced into the reaction medium in a concentration defined at the stage of the process specified in Table 1 and expressed relative to the total mass of monomers used.
[0120] The esterification of the medium is carried out over a defined period of time indicated in Table 1. The water distilled during the test is collected in a dedicated insulated recovery pot.
[0121] Next, a vacuum system is connected to the distillation condenser and a pressure below atmospheric pressure is applied to the reactor contents. The pressure is reduced slowly and stepwise (approximately 10 to 15% per step) over approximately 30 minutes to a target value of less than 10 mbar.
[0122] Once the pressure in the reaction vessel stabilizes at 5 mbar, the medium is left to react at a jacket temperature defined in Table 1 for an additional 3 h. During this polycondensation step, the stirring speed is reduced to 115 rpm to account for the increased viscosity of the mixture.
[0123] The produced PGS is transferred from the reactor vessel to a container after the facility has been depressurized and allowed to cool to room temperature. The product is then transferred to a freezer for storage, where it is frozen for at least approximately 24 hours before analysis.
[0124] 2- Measurement methods used:
[0125] 2-1 Determination of the microstructure of PGS polymers:
[0126] The microstructure of the polymers is determined by 1H NMR analysis, supplemented by 13C NMR analysis when the resolution of 1H NMR spectra does not allow the attribution and quantification of all species. The measurements are carried out using a BRUKER 500MHz NMR spectrometer at frequencies of 500.43 MHz for proton observation and 125.83 MHz for carbon observation.
[0127] 2-2 Determination of the macrostructure of PGS polymers and the level of residual monomers:
[0128] The SEC (Size Exclusion Chromatography) technique separates macromolecules in solution according to their size through columns filled with a porous gel. The macromolecules are separated according to their hydrodynamic volume, with the largest being eluted first.
[0129] Although not an absolute method, SEC allows us to understand the distribution of molar masses of a polymer. From commercial standard products, the different number-average (Mn) and weight-average (Mw) molar masses can be determined and the dispersity (£> = Mw / Mn) calculated.
[0130] Size exclusion chromatography analyses were performed using a Viscotek instrument (Malvem Instruments) equipped with 3 columns (SDVB, 5 μm, 300 x 7.5 mm of Polymer Standard Service), a guard column, and 3 detectors (differential refractometer and viscometer, and light scattering). 1 mL of a solution of the sample with a concentration of 5 mg mL-1 in THF was filtered through a 0.45 μm PTFE membrane. 100 pL of this solution was eluted in THF using a flow rate of 0.8 mL min-1 at a temperature of 35 °C. OmniSEC software was used for data acquisition and analysis. The number (Mn) and mass (ALw) molar masses of the polymers as well as their dispersity (£>) were calculated using a calibration curve from standard polystyrenes (Mp 1,306 to 2,520,000 g mol-1) from Polymer Standard Service (Mainz).
[0131] The technique used is size exclusion chromatography (SEC) with a set of columns optimized for the separation of low mass species.
[0132] The samples were dissolved at a concentration of 1 g / L in unstabilized THF, then stirred for 2 h before being injected.
[0133] The analytical conditions used in the study are described in the following table:
[0134] The calibration used for Moore's calculation is a PS calibration, covering a range from 2,520,000 to 162 g.mol 4
[0135] The calibration used is a mixed low-weight and medium-weight PS calibration from PSS Standards. The mass range is from 162 to 66,000 g.mol 4 . Calibration allows the determination of Mn values (g.mol 4 ) Mw (g.mol 4 ) D (Mw / Mn) in PS equivalent:
[0136] The macrostructure calculation takes into account zones 1 and 2, with residual monomers not being considered as part of the polymer.
[0137] The determination of the sebacic acid level is carried out by external calibration.
[0138] A standard range using samples of sebacic acid and glycerol at different concentrations was carried out.
[0139] 3- Tests and Results:
[0140] The tables below give the operating conditions of the synthesis process (table Xa), as well as the results of the measurements carried out on the PGS obtained at the end of these syntheses (table Xb). a- Syntheses of PGS carried out without catalyst in the presence of water (not in accordance with the invention): table la table 1b
[0141] According to the process carried out in the presence of water and without catalyst, a reaction time of more than 3 1h is necessary to reduce the residual monomer content below 5% and to reach an Mn of the order of the preferred minimum value of 2700 g / mol. It is noted that by thus extending the reaction time, the dispersity of the molar masses and the rate of units (1,2,3-triacylglyceride) are increased at the same time. b- Synthesis of PGS in the presence of water and in the presence of the catalyst TBT (titanium tetrabutanoate) (not in accordance with the invention): In this example the catalyst Ti(OBu)4 is added at a rate of 2500 ppm, i.e. 0.25% w / w after the esterification time, just before the polycondensation step. table 2a table 2b
[0142] It is found that when a catalyst not in accordance with the invention but having an acceptable toxicological profile is introduced, at the end of the esterification step (b) before placing under vacuum (c), the PGS obtained has a degraded macrostructure, its Mn is lower than the polymer obtained without using a catalyst with a similar reaction time (test 1). c- Syntheses of PGS carried out in the absence or presence of water and in the presence of the catalyst monobutyltin oxide (or stannoic acid) of food grade (FASCAT 9100) added at different stages of the process (in accordance and not in accordance with the invention). In these examples the Fascat 9100 catalyst is added according to the conditions described in the table below. table 3a table 3b
[0143] Tests 5, 9 and 10 are in accordance with the invention.
[0144] Tests 6, 7 and 8 are not in accordance with the invention.
[0145] The use of the FASCAT9100 catalyst in accordance with the process of the invention at the end of the esterification step makes it possible to obtain, in a time of the order of that of test 1 without catalyst, a poly(glycerol sebacate) having a high number-average molar mass greater than or equal to 2700 g / mol, a controlled dispersity of less than 5 and a low residual monomer mass content of less than 2% of the mass of the polymer, by limiting the content of (1,2,3-triacylglyceride) units below 15%.
[0146] It is also noted by comparing the data from tests 5 and 6 that when the FASCAT9100 catalyst is not introduced into the process in accordance with the invention at the end of the esterification step, the evolution of the macrostructural characteristics of the polyester is unfavorable. The characteristics are degraded in terms of Mn, dispersity and unit content (1,2,3-triacylglyceride), with gel formation. This leads to a polymer with degraded physicochemical properties.
[0147] It is also noted from tests 7 and 8 that when the FASCAT9100 catalyst is not used in a process in accordance with the invention comprising bringing the monomers into contact in the presence of water, a polyester with degraded characteristics in terms of dispersity and unit content (1,2,3-triacylglyceride) is obtained, with gel formation.
[0148] It is also noted by comparing the data from tests 2 and 10 that when the catalyst FASCAT9100 is introduced into the process in accordance with the invention at the end of the esterification step and the esterification time is reduced to 4 hours (test 10), a poly(glycerol sebacate) is obtained having a high number-average molar mass greater than 2500 g / mol at the end of a total reaction time of less than 10 hours. Whereas without catalyst (example 2), such a Mn is not reached after 14 hours. The catalyst makes it possible to accelerate the kinetics of the reaction while improving the macrostructural characteristics of the polymer. d. Syntheses of PGS carried out in the presence of water and in the presence of the catalyst tris(2(ethylhexanoate) of food-grade monobutyltin (FASCAT 9102) added at different stages of the process (in accordance with and not in accordance with the invention).
[0149] In these examples, the catalyst F ascat 9102 is added according to the conditions described in the table below. table 4a table 4b Test 11 is not in accordance with the invention.
[0150] Test 12 is in accordance with the invention.
[0151] It is found that when the catalyst is not introduced into the process in accordance with the invention at the end of the esterification step, the evolution of the macrostructural characteristics of the polyester is unfavorable, with a lower Mn and a higher residual monomer content (example 11). When the catalyst is introduced into the process in accordance with the end of the esterification step, the macrostructural characteristics of the polymer are favorable, with a higher Mn and a residual monomer content of less than 5% w / w (example 12).
Claims
CLAIMS 1. A process for preparing a polyester of glycerol and a dicarboxylic acid which comprises (a) bringing into contact the monomers comprising at least glycerol and a corresponding dicarboxylic acid in the presence of water, at a temperature below 100°C, according to a glycerol / dicarboxylic acid molar ratio varying from 0.5 / 1 to 10 / 1, (b) esterification under an inert atmosphere at a temperature above 110°C, preferably ranging from 130°C to 180°C (c) placing the reaction medium under vacuum at a pressure of less than 100 mbara, preferably less than 50 mbara, preferably less than 10 mbara, at a temperature of more than 110°C, preferably ranging from 130°C to 180°C, (d) maintaining a vacuum and a temperature above 110°C, preferably ranging from 130°C to 180°C, to carry out a polycondensation, which process comprises introducing a polycondensation catalyst at the end of the esterification of step (b), before the vacuuming of step (c) or after the vacuuming of step (c), in an amount less than or equal to 5000 ppm relative to the total mass of monomers, said catalyst being a food grade tin-based catalyst chosen from organotin compounds comprising a carboxyl function (-C(O)OH), organotin compounds comprising a (-Sn(O)OH) function and monobutyltin tris(2(ethylhexanoate).
2. Process according to the preceding claim in which the dicarboxylic acid has the formula [HOOC-(CÜ2)n-COOH], in which n is a number ranging from 1 to 30, preferably a number ranging from 1 to 10.
3. A method according to any one of the preceding claims wherein the dicarboxylic acid is sebacic acid.
4. Process according to any one of the preceding claims in which the glycerol / dicarboxylic acid molar ratio varies from 0.9 / 1 to 2 / 1, preferably from 1 / 1 to 1.5 / 1.
5. Process according to any one of the preceding claims in which the contacting of the monomers is carried out by introducing the dicarboxylic acid monomer into a mixture comprising the glycerol monomer and water.
6. Process according to any one of the preceding claims in which the diacid monomer is introduced into a mixture comprising the glycerol monomer and water, in solid form and the contacting of the monomers of step (a) is followed by a step of melting the diacid monomer in the aqueous medium.
7. Process according to any one of the preceding claims in which, at the end of the contacting of the monomers from step (a), the reaction medium is brought to reflux.
8. Process according to any one of the preceding claims in which the process comprises at the end of step (a) a step of removing the water introduced for bringing the monomers into contact, preferably by distillation.
9. A process according to any one of the preceding claims wherein the process comprises a step of removing water, preferably by distillation, which follows or is concomitant with the esterification step (b), the polycondensation step (c) or the esterification step (b) and the polycondensation step (c).
10. Process according to any one of the preceding claims in which the food grade tin-based catalyst is chosen from food grade alkyltins comprising a carboxyl function (-C(O)OH) or a function (- Sn(O)OH), the alkyl group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms.
11. A method according to any one of claims 1 to 9 wherein the food grade tin-based catalyst is chosen from food grade monobutyltin oxide (or stannoic acid) and food grade monobutyltin tris(2-ethylhexanoate).
12. A method according to any one of the preceding claims wherein the food grade tin-based catalyst is food grade monobutyltin oxide (or stannoic acid).
13. Method according to any one of the preceding claims in which the catalyst is introduced in an amount less than or equal to 3000 ppm.
14. Polyester of glycerol and a dicarboxylic acid having a residual monomer content of less than 5% by weight of the weight of the polymer; a number-average molar mass Mn greater than 2500 g / mol, preferably greater than or equal to 2700 g / mol, a dispersity D (Mw / Mn) less than or equal to 10, preferably less than or equal to 5; a content of (1,2,3-triacylglyceride) units less than 15 mol% relative to all the units of the polymer.
15. Polyester of glycerol and a dicarboxylic acid according to the preceding claim having a number-average molar mass Mn of less than 3500 g / mol, preferably less than 3000 g / mol.
Citation Information
Patent Citations
Water-mediated preparations of polymeric materials
EP3149067A1
Polyester, process for the production of the same, resin or rubb er compositions containing the same, and moldings of the compositions
EP0894815A1
Biodegradable polymer
EP1448656A2