Conductive paste and method for producing same
The conductive paste with surface-treated copper and glass powders of specific surface free energy and particle size ensures stable dispersion and prevents aggregate formation, addressing the challenge of achieving a uniform sintered film for chip-type ceramic electronic components.
Patent Information
- Application Number
- PCT/JP2024/006405
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-17
AI Technical Summary
The challenge is to develop a conductive paste for forming external electrodes in chip-type ceramic electronic components that minimizes the formation of aggregates, which can lead to defects such as cracks and voids in the sintered film, due to the strong cohesiveness of small-diameter powder particles, making it difficult to achieve a uniform and stable dispersion.
The conductive paste is formulated with copper powder and glass powder that have a surface free energy of 30 mJ/m² or more and 55 mJ/m², treated to improve crushability and dispersion stability, with a 50% volume cumulative particle size of 1.0 μm or less, and dispersed in an organic vehicle containing a resin and solvent, ensuring a stable interface and preventing agglomeration.
This approach enhances the crushability and dispersion stability of the powder materials, preventing the formation of aggregates and ensuring a uniform, defect-free sintered film, thereby improving the reliability and functionality of the external electrodes.
Smart Images

Figure JP2024006405_17102024_PF_FP_ABST
Abstract
Description
Conductive paste and method for producing the same
[0001] The present invention relates to a conductive paste for forming external electrodes in chip-type ceramic electronic components and a method for producing the same, and more particularly to improvements in the physical properties of the copper powder and glass powder contained in the conductive paste.
[0002] As a technology of interest to this invention, for example, Japanese Patent Application Laid-Open No. 2004-171804 (Patent Document 1) describes a conductive paste for forming external electrodes, which contains a conductive powder, glass frit, and an organic vehicle. In this conductive paste, the glass frit has a terminally functionalized polymeric substance attached to its surface. The terminally functionalized polymeric substance is contained in a ratio of 0.01 to 3 parts by mass per 100 parts by mass of glass. Furthermore, the terminally functionalized polymeric substance has a terminal group that is a carboxyl group or an amino group.
[0003] Patent Document 1 describes that such a conductive paste makes it possible to form highly reliable external electrodes and also makes it possible to form a uniform plating film on the surface of the formed external electrodes.
[0004] Japanese Patent Application Laid-Open No. 2004-171804
[0005] For example, in the development of conductive pastes containing copper as a conductive component for forming external electrodes in small, high-capacity multilayer ceramic capacitors, it is required to obtain thin, dense sintered films, and one practical means for achieving this requirement is to reduce the diameter of the powder material contained in the conductive paste.
[0006] However, as the diameter of powder materials decreases, the tendency for particles to aggregate increases, making them difficult to disperse when forming a paste. To effectively utilize small-diameter powders, advanced crushing technology is required. Generally, crushing is performed by mechanically applying shear stress to a slurry containing copper powder, glass powder, resin, and organic solvent.
[0007] As a result of the crushing process, it is desirable that all powders in the system are uniformly monodispersed. However, as shown schematically in Figure 3, for example, aggregates 11 may remain in some regions of the conductive paste. In Figure 3, the shaded circles represent copper powder 12, and the white circles represent glass powder 13. The copper powder 12 and glass powder 13 are dispersed in an organic vehicle 14 consisting of a resin and an organic solvent. In Figures 4 and 5, which will be described later, as well as Figure 2, the copper powder 12, the glass powder 13, and the organic vehicle 14 are illustrated in the same manner as in Figure 3.
[0008] Furthermore, unless the affinity between the components in the conductive paste, i.e., copper powder 12, glass powder 13, resin, and organic solvent, is appropriately controlled, aggregates 11 may be further generated over time, as shown in Figure 4. To prevent this situation from occurring, it is necessary to stabilize the dispersion state of the powder components in the conductive paste, i.e., copper powder 12 and glass powder 13.
[0009] To ensure the stability of the dispersion, a process may be performed in which a dispersant (organic compound) 15 is adsorbed onto the surfaces of the copper powder 12 and the glass powder 13, as shown in Fig. 5. However, the dispersant 15 is adsorbed not only onto the surfaces of the monodispersed copper powder 12 and the glass powder 13, but also onto the surfaces of the aggregates 11. This may make it more difficult to obtain a monodispersed state of the copper powder 12 and the glass powder 13.
[0010] In order to form an external electrode in a chip-type ceramic electronic component, when a conductive paste containing agglomerates 11 is applied to the component body and baked, abnormal grain growth of copper powder 12 and glass powder 13 containing agglomerates 11 can cause film defects such as cracks and lumps in the external electrode, preventing the external electrode from functioning properly as an electrode.
[0011] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a conductive paste for forming external electrodes in chip-type ceramic electronic components that is less likely to produce agglomerates, and a method for producing the same.
[0012] The present invention is first directed to a conductive paste for forming external electrodes in chip-type ceramic electronic components.
[0013] The conductive paste according to the present invention contains copper powder, glass powder, resin, and organic solvent, and in order to solve the above-mentioned technical problems, the copper powder and the glass powder have a surface free energy γsD50 of 30 mJ / m 2 or more and 55 mJ / m 2 The copper powder and glass powder are surface-treated to have a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction / scattering particle size distribution measurement method.
[0014] The present invention is also directed to a method for producing a conductive paste for forming external electrodes in chip-type ceramic electronic components.
[0015] The method for producing a conductive paste according to the present invention includes the steps of: preparing copper powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering particle size distribution measurement method; preparing glass powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering particle size distribution measurement method; preparing a resin; preparing an organic solvent; and mixing the copper powder with an organic solvent having a surface free energy γsD50 of 30 mJ / m 2 or more and 55 mJ / m 2 a step of surface-treating the glass powder so that the surface free energy γsD50 is 30 mJ / m or less; 2 or more and 55 mJ / m 2 The method is characterized by comprising the steps of: a step of performing a surface treatment as follows; and a step of dispersing the surface-treated copper powder and glass powder in an organic vehicle containing a resin and an organic solvent.
[0016] According to this invention, the surface free energy of the copper powder and glass powder, which are powder components, is set to 30 mJ / m 2 or more and 55 mJ / m 2 Since the particle size of the powder material is set to 1.0 μm or less, even if the particle size of the powder material is set to a small diameter of 1.0 μm or less, the crushability and dispersion stability of the powder material can be improved, and as a result, it is possible to make it less likely for agglomerates to occur.
[0017] Furthermore, when the interfacial tension between the powder and the organic material is high, agglomeration is likely to occur over time. This is because a more stable interface between the powder particles is created to resolve this energetically unstable state. In contrast, according to the present invention, by selecting the surface free energy as described above, the powder surface can be made more easily wetted by the organic solvent. This reduces the interfacial tension between the powder and the organic solvent, achieving an energetically stable state, and as a result, agglomeration over time is less likely to occur.
[0018] 1 is a cross-sectional view schematically showing a chip-type multilayer ceramic capacitor 1 as an example of a chip-type ceramic electronic component having external electrodes to which the conductive paste according to the present invention is applied. It is a diagram schematically showing the dispersion state of copper powder 12 and glass powder 13 contained in the conductive paste according to the present invention in an organic vehicle 14. It is a diagram schematically showing a conductive paste containing agglomerates 11 remaining after a crushing treatment, for explaining the problem to be solved by the present invention. It is a diagram schematically showing a conductive paste in which agglomerates 11 have further formed over time from the state shown in FIG. 3, for explaining the problem to be solved by the present invention. It is a diagram schematically showing a conductive paste in which a dispersant 15 is adsorbed to the surfaces of copper powder 12 and glass powder 13 to ensure the stability of the dispersion state, for explaining the problem to be solved by the present invention.
[0019] Referring to FIG. 1, the structure of a chip-type multilayer ceramic capacitor 1 will be described as an example of a chip-type ceramic electronic component to which the conductive paste according to the present invention can be applied.
[0020] The multilayer ceramic capacitor 1 includes a ceramic body 2 serving as a component body. The ceramic body 2 includes a plurality of stacked ceramic layers 3 and a plurality of internal electrodes 4 and 5 arranged along the interfaces between the plurality of ceramic layers 3. The internal electrodes 4 and 5 are classified into a plurality of first internal electrodes 4 and a plurality of second internal electrodes 5 arranged alternately in the stacking direction of the ceramic body 2. A first external electrode 6 and a second external electrode 7 are provided on the surface of the ceramic body 2, more specifically, on each of the opposing end faces. The first external electrode 6 is electrically connected to the first internal electrode 4, and the second external electrode 7 is electrically connected to the second internal electrode 5.
[0021] The ceramic layer 3 is made of, for example, ABO 3 (A is at least one of Ba, Ca and Sr, and B is at least one of Ti and Zr) as a main component. 3 The alloy may contain at least one of Mn, Mg, Si, Y, Dy and Gd as a secondary component.
[0022] The internal electrodes 4 and 5 contain, as a conductive component, a conductive metal or an alloy containing the same, for example, one selected from nickel, copper, silver, and a silver / palladium alloy, and preferably contain nickel in particular.
[0023] The external electrodes 6 and 7 are formed by applying the conductive paste according to the present invention to the end faces of the ceramic body 2 so as to contact the respective ends of the internal electrodes 4 and 5, and then baking the paste.
[0024] The conductive paste contains copper powder, glass powder, resin, and organic solvent. Fig. 2 shows a schematic diagram of copper powder 12 and glass powder 13 contained in the conductive paste. Copper powder 12 and glass powder 13 are dispersed in an organic vehicle 14 consisting of resin and organic solvent.
[0025] The copper powder 12 and the glass powder 13 have a 50% volume cumulative particle size D50 of 1.0 μm or less, as measured by a laser diffraction scattering particle size distribution measurement method, and a surface free energy γsD50 of 30 mJ / m2 or more and 55 mJ / m 2 The surface free energy is measured by, for example, IGC-SEA. In preparing the conductive paste, the powder surfaces of the copper powder 12 and the glass powder 13 are brought into contact with the surface treatment agent 16 in advance so as to have the above-mentioned surface free energy, and then the copper powder 12 and the glass powder 13 are dispersed in an organic vehicle consisting of a resin and an organic solvent.
[0026] In order to produce the conductive paste, the copper powder 12 and the glass powder 13 are pre-treated to have the surface free energy described above, and then dispersed in an organic vehicle. However, it has been confirmed that the copper powder 12 and the glass powder 13 extracted from the obtained conductive paste also maintain the same surface free energy.
[0027] In a preferred embodiment, the conductive paste is prepared as follows.
[0028] [Preparation of Copper Powder and Glass Powder] Copper powder and glass powder, each having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction / scattering particle size distribution measurement method, are prepared. As the glass powder, for example, a B—Si—Ba based glass powder is used.
[0029] Next, each of the copper powder and the glass powder is dispersed in, for example, isopropyl alcohol to prepare a dispersion.
[0030] Next, 0.005 g or more of a surface treatment agent is added per 1 g of copper powder or per 1 g of glass powder to each of the isopropyl alcohol dispersion of copper powder and the isopropyl alcohol dispersion of glass powder, and the mixture is subjected to ultrasonic treatment to bring the copper powder or glass powder in the dispersion into sufficient contact with the surface treatment agent. After that, the copper powder or glass powder is recovered as a residue from the dispersion, and a drying step is carried out to volatilize the remaining solvent.
[0031] The above-mentioned ultrasonic treatment is carried out, for example, at an output of 50 to 600 W per 100 mL and a frequency of 20 kHz to 100 kHz for 30 minutes.
[0032] As the surface treatment agent, for example, at least one selected from the saturated fatty acids enanthic acid, caprylic acid, pelargonic acid, capric acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachic acid, and behenic acid can be used.
[0033] [Preparation of Resin] The resin used was a resin having a surface free energy of 25 mJ / m as measured by the contact angle method. 2 or more and 55 mJ / m 2 The following can be advantageously used, for example, an acrylic resin, more specifically, a homopolymer of any of isobutyl methacrylate, methyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, n-butyl methacrylate, and 2-ethylhexyl methacrylate, or a copolymer composed of two or more of these homopolymers.
[0034] [Preparation of Organic Solvent] As the organic solvent, an organic solvent having a surface tension measured by the ring method of 25 mN / m or more and 55 mN / m or less can be advantageously used, such as an alcohol-based solvent such as terpineol. More specifically, examples of the organic solvent include terpineol, dihydroterpineol, dihydroterpinyl acetate, propylene glycol phenyl ether, benzyl alcohol, Texanol, and butyl carbitol acetate.
[0035] [Preparation of Conductive Paste] The copper powder and glass powder that have been surface-treated as described above are pre-mixed with a resin and an organic solvent using, for example, a planetary mixer, and then dispersed using a three-roll mill to prepare a conductive paste. Here, the resin is prepared by dissolving it in an organic solvent, for example, a terpineol solution of polymethyl methacrylate.
[0036] By setting the surface free energy within the above-mentioned range, it is possible to improve the crushability and dispersion stability of the powder components, copper powder 12 and glass powder 13. More specifically, the surfaces of the powders, such as copper powder 12 and glass powder 13, can be made more easily wettable by the organic solvent by the surface treatment agent 6. This reduces the interfacial tension between the powder and the organic solvent, achieving an energetically stable state, and as a result, it is possible to make it less likely for aggregation to occur over time.
[0037] In particular, the resin has a surface free energy of 25 mJ / m as measured by the contact angle method. 2 or more and 55 mJ / m 2 The following materials are used, and by advantageously using an organic solvent having a surface tension of 25 mN / m or more and 55 mN / m or less as measured by the ring method, the compatibility between the components of the conductive paste is improved, and the above-mentioned effects are more reliably achieved.
[0038] As shown in FIG. 2, the conductive paste preferably does not contain agglomerates of copper powder 12 and glass powder 13, particularly agglomerates of 10 μm or larger.
[0039] Furthermore, the smaller the diameter of the copper powder 12 and the glass powder 13, the more significant the surface free energy as described above becomes. Therefore, in the present invention, the particle diameter of the copper powder 12 and the glass powder 13 is set to 1.0 μm or less in terms of the 50% volume cumulative particle diameter D50 measured by a laser diffraction / scattering particle size distribution measurement method.
[0040] The copper powder 12 is preferably a spherical powder having a crystallinity of 80 nm or more by XRD. The organic solvent is preferably contained in the conductive paste in an amount of 40% by volume or more.
[0041] Below, an explanation will be given of an experiment carried out to determine the surface free energy of copper powder and glass powder, which are characteristic of the present invention.
[0042] Copper powder and B—Si—Ba-based glass powder were prepared. The copper powders had 50% volume cumulative particle diameters D50 of 0.30 μm, 0.45 μm, and 1.00 μm, as measured by a laser diffraction / scattering particle size distribution measurement method. The glass powders had 50% volume cumulative particle diameters D50 of 0.60 μm, 0.63 μm, 0.64 μm, and 0.92 μm, as measured by a laser diffraction / scattering particle size distribution measurement method.
[0043] Next, an isopropyl alcohol dispersion (1% by mass) of copper powder and an isopropyl alcohol dispersion (1% by mass) of glass powder were prepared.
[0044] Next, 0.005 g of lauric acid was added as a surface treatment agent per 1 g of copper powder or per 1 g of glass powder to each of the isopropyl alcohol dispersions of copper powder and the isopropyl alcohol dispersions of glass powder. The mixture was subjected to ultrasonic treatment for 30 minutes at an output of 50 to 600 W per 100 mL and a frequency of 10 kHz to 1 MHz. After the copper powder and glass powder in the dispersion were sufficiently contacted with the surface treatment agent, the copper powder and glass powder were recovered as residues from the dispersion, and a drying step was carried out at 100°C for 30 minutes to volatilize the remaining solvent.
[0045] In the above-mentioned process, variations occur even when the same type of powder, the same type of surface treatment agent, and the same processing conditions are used. Taking advantage of this variation, copper powders and glass powders with various different surface free energies γsD50 were used as samples, as shown in Table 1.
[0046] On the other hand, polyisobutyl methacrylate as a resin was dissolved in terpineol as an organic solvent to prepare an organic binder.
[0047] Next, the copper powder and glass powder described above were pre-mixed together with an organic binder using a planetary mixer, and then dispersed using a three-roll mill to prepare conductive pastes for each sample shown in Table 1.
[0048] Next, the conductive paste for each sample was applied to a glass plate to a thickness of 25 μm and dried at 100° C. for 15 minutes to obtain a conductive paste dry film for evaluation. The thickness of the conductive paste dry film is preferably 10 μm or less.
[0049] Next, the conductive paste dry film for evaluation was observed with a digital microscope to check for the presence or absence of aggregates of 10 μm or more. 2 A product was judged to be non-defective when no aggregates of 10 μm or larger were present, and this was indicated by "○" in the "Aggregate Presence Evaluation Result" in Table 1. A product was judged to be defective when aggregates of 10 μm or larger were present, and this was indicated by "×" in the "Aggregate Presence Evaluation Result" in Table 1. The digital microscope used for observation was a VHX-600 model with a contact lens, a 100x magnification, and a ring-type one-sided illumination.
[0050]
[0051] The surface free energy γsD50 of copper powder and glass powder is 30 mJ / m 2 or more and 55 mJ / m 2 According to Examples 1 and 2, which satisfied the conditions that the 50% volume cumulative particle diameter D50 of the copper powder and the glass powder measured by the laser diffraction scattering particle size distribution measurement method was 1.0 μm or less, the "assessment result for the presence or absence of agglomerates" was "○", and it was confirmed that the powder material had high crushability and dispersion stability.
[0052] In contrast, in Comparative Example 1, the surface free energy γsD50 of both the copper powder and the glass powder was 55 mJ / m 2 In Comparative Example 2, the surface free energy γsD50 of the glass powder was 55 mJ / m 2 In Comparative Example 3, the surface free energy γsD50 of the copper powder was 30 mJ / m 2 Therefore, in Comparative Examples 1 to 3, the "assessment result for the presence or absence of agglomerates" was "x," and it was confirmed that the crushability and dispersion stability of the powder material were insufficient.
[0053] The embodiments of the present invention include the following:
[0054] <1> A conductive paste for forming external electrodes in a chip-type ceramic electronic component, comprising copper powder, glass powder, resin, and an organic solvent, wherein the copper powder and the glass powder have a surface free energy γsD50 of 30 mJ / m 2 or more and 55 mJ / m 2 the copper powder and the glass powder have a 50% volume cumulative particle size D50 of 1.0 μm or less, as measured by a laser diffraction / scattering particle size distribution measurement method.
[0055] <2> The resin has a surface free energy γsD50 measured by a contact angle method of 25 mJ / m 2 or more and 55 mJ / m 2 The conductive paste according to <1>, wherein the organic solvent has a surface tension measured by a ring method of 25 mN / m or more and 55 mN / m or less.
[0056] <3> The conductive paste according to <1> or <2>, which does not contain aggregates of the copper powder and the glass powder having a size of 10 μm or more.
[0057] <4> The conductive paste according to any one of <1> to <3>, wherein the copper powder is a spherical powder.
[0058] <5> The conductive paste according to any one of <1> to <4>, wherein the glass powder is a B—Si—Ba based glass powder.
[0059] <6> A method for producing a conductive paste for forming external electrodes in a chip-type ceramic electronic component, comprising the steps of: preparing copper powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering particle size distribution measurement method; preparing glass powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering particle size distribution measurement method; preparing a resin; preparing an organic solvent; and mixing the copper powder with a glass powder having a surface free energy γsD50 of 30 mJ / m 2 or more and 55 mJ / m 2 a step of surface-treating the glass powder so that the surface free energy γsD50 is 30 mJ / m or less;2 or more and 55 mJ / m 2 A method for manufacturing a conductive paste, comprising: a step of performing a surface treatment so that the copper powder and the glass powder are surface-treated; and a step of dispersing the surface-treated copper powder and the glass powder in an organic vehicle containing the resin and the organic solvent.
[0060] <7> In the step of preparing the resin, a surface free energy γsD50 measured by a contact angle method is 25 mJ / m 2 or more and 55 mJ / m 2 The method for producing a conductive paste according to <6>, comprising: preparing a resin as follows: wherein the step of preparing an organic solvent includes a step of preparing an organic solvent having a surface tension measured by a ring method of 25 mN / m or more and 55 mN / m or less.
[0061] REFERENCE SIGNS LIST 1 Multilayer ceramic capacitor 2 Ceramic element 3 Ceramic layer 4, 5 Internal electrode 6, 7 External electrode 11 Aggregate 12 Copper powder 13 Glass powder 14 Organic vehicle 16 Surface treatment agent
Claims
1. A conductive paste for forming external electrodes in chip-type ceramic electronic components, comprising copper powder, glass powder, resin, and an organic solvent, wherein the copper powder and the glass powder have a surface free energy γsD50 of 30 mJ / m 2 More than 55 mJ / m 2 the copper powder and the glass powder have a 50% volume cumulative particle size D50 of 1.0 μm or less, as measured by a laser diffraction / scattering particle size distribution measurement method.
2. The resin has a surface free energy γsD50 of 25 mJ / m as measured by the contact angle method. 2 55 mJ / m or more 2 The conductive paste according to claim 1 , wherein the organic solvent has a surface tension of 25 mN / m or more and 55 mN / m or less as measured by a ring method.
3. The conductive paste according to claim 1 or 2, which does not contain agglomerates of said copper powder and said glass powder having a size of 10 μm or more.
4. The conductive paste according to any one of claims 1 to 3, wherein the copper powder is a spherical powder.
5. The conductive paste according to any one of claims 1 to 4, wherein the glass powder is a B-Si-Ba based glass powder.
6. A method for producing a conductive paste for forming external electrodes in chip-type ceramic electronic components, comprising the steps of: preparing copper powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering type particle size distribution measurement method; preparing glass powder having a 50% volume cumulative particle size D50 of 1.0 μm or less as measured by a laser diffraction scattering type particle size distribution measurement method; preparing a resin; preparing an organic solvent; and mixing the copper powder with an organic solvent having a surface free energy γsD50 of 30 mJ / m. 2 More than 55 mJ / m 2 and subjecting the glass powder to a surface treatment so that the surface free energy γsD50 is 30 mJ / m or less. 2 More than 55 mJ / m 2 A method for producing a conductive paste, comprising: a step of performing a surface treatment so as to obtain the following: and a step of dispersing the surface-treated copper powder and glass powder in an organic vehicle containing the resin and the organic solvent.
7. The step of preparing the resin is carried out by using a resin having a surface free energy γsD50 of 25 mJ / m as measured by a contact angle method. 2 More than 55 mJ / m 2 7. The method for producing a conductive paste according to claim 6, further comprising the step of preparing a resin having a surface tension of 25 mN / m or more and 55 mN / m or less, as measured by a ring method, in which the step of preparing an organic solvent comprises the step of preparing an organic solvent having a surface tension measured by a ring method of 25 mN / m or more and 55 mN / m or less.
Citation Information
Patent Citations
Conductive paste and ceramic electronic part
JP2005085703A
Paste for external electrode
JP2021077750A