Method for producing granulated material for chemical recycling, and granulated material for chemical recycling
The method of forming granules through crushing, melt extrusion, and air cooling of polyester waste addresses the inefficiencies in existing recycling methods by enhancing reactivity and handling in chemical recycling, achieving effective and environmentally friendly polyester waste processing.
Patent Information
- Application Number
- PCT/JP2024/007370
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-17
AI Technical Summary
Current recycling methods for polyester waste, such as material recycling and thermal recycling, degrade the quality of polyester and are not environmentally friendly, while chemical recycling faces inefficiencies due to the shape and physical properties of polyester waste granules in depolymerization reactions.
A method involving crushing, melt extrusion, air cooling, and pulverization of polyester waste to form granules with specific density and cavity properties, optimized using a plast compactor, to enhance reactivity and handling efficiency in chemical recycling.
The resulting granules exhibit high reactivity in depolymerization reactions, improved handling properties, and efficient filling into reaction equipment, allowing for effective chemical recycling without quality degradation and environmental impact.
Smart Images

Figure JP2024007370_17102024_PF_FP_ABST
Abstract
Description
Manufacturing method of granulated material for chemical recycling and granulated material for chemical recycling
[0001] The present disclosure relates to a method for producing granulated material for chemical recycling and a granulated material for chemical recycling.
[0002] Polyesters such as polyethylene terephthalate (PET) have excellent chemical stability and are therefore produced and used in large quantities as daily living materials such as fibers, films, and containers, as well as in the food industry, such as bottles for drinking water or carbonated drinks. Various attempts have been made to recycle waste generated in the production and use of polyester.
[0003] Recycling of polyester waste can be broadly classified into three categories: material recycling, thermal recycling, and chemical recycling.
[0004] Material recycling involves converting polyester waste into lower quality products through melt molding, but repeated recycling further reduces the quality, making it difficult to avoid final disposal.
[0005] Thermal recycling involves reusing the heat generated during the incineration of polyester waste. However, thermal recycling does not allow for the recycling of polyester or its raw materials, and carbon dioxide is generated during incineration, so it is not always desirable from the perspectives of resource conservation and environmental protection.
[0006] Chemical recycling involves depolymerizing polyester contained in polyester waste to convert it into monomers, which are the building blocks of polyester, and then reusing the resulting monomers in polyester synthesis. One example of a chemical recycling method for polyester waste is the glycolysis-transesterification reaction method, which involves depolymerizing (alcoholyzing) polyester waste in the presence of ethylene glycol (EG) to produce bis-2-hydroxyethyl terephthalate (BHET), which is then converted into dimethyl terephthalate (DMT) and ethylene glycol by a transesterification reaction with methanol. Chemical recycling allows polyester to be resynthesized without degrading its quality, making it possible to reuse resources in the true sense of the word.
[0007] Patent Document 1 (JP 2003-128626 A) describes a "method for recovering terephthalic acid from polyester waste, which is substantially composed of polyalkylene terephthalate fibers and natural fibers and / or chemical fibers other than polyalkylene terephthalate fibers, characterized by combining a pretreatment step of analyzing the polyester fiber waste with a discrimination device, pulverizing and granulating those determined to be polyester to form crude polyester, and transporting the crude polyester to a reaction step, with a reaction step including the following steps (a) to (j)," in which the steps (a) to (j) are described as (a) a depolymerization step, (b) a foreign matter removal step, (c) a filtration and separation step, (d) a concentration step, (e) a transesterification reaction step, (f) a purification step, (g) a hydrolysis reaction step, (h) a separation step, (i) a substitution step, and (j) a slurry preparation step.
[0008] Patent Document 2 (JP 2021-533211 A) describes a "method for recovering waste polyester material, comprising: a material pretreatment step of removing water and oxygen from waste polyester material to obtain a waste polyester raw material; a melt supply step of melting the waste polyester raw material to obtain molten waste polyester, which is continuously fed into an alcoholysis vessel and, during the melting process of the waste polyester raw material, adding ethylene glycol as an alcoholysis agent to perform pre-alcohololysis; an alcoholysis step of depolymerizing the molten waste polyester, the alcoholysis agent, and the alcoholysis catalyst in the alcoholysis vessel to obtain an alcoholysis product; and a transesterification step of transesterifying a transesterification agent, a transesterification catalyst, and the alcoholysis product in the transesterification vessel."
[0009] Japanese Patent Application Laid-Open No. 2003-128626 Special Publication No. 2021-533211
[0010] From the viewpoints of ease of handling and efficiency of filling a reactor, it is desirable to pulverize and granulate polyester waste before the depolymerization step. On the other hand, since the depolymerization reaction is a solid-liquid heterogeneous phase reaction between solid polyester and liquid ethylene glycol, the shape and physical properties of the granulated polyester waste have a significant effect on the reaction efficiency of the depolymerization reaction.
[0011] The present disclosure provides a method for chemically recycling polyester waste by forming the polyester waste into a granule suitable for a depolymerization process, and such a granule for chemical recycling.
[0012] The present inventors have found that granules having high reactivity in a depolymerization reaction and excellent handleability and packing efficiency into a reaction apparatus can be obtained by melt-extruding pulverized polyester waste and then solidifying the granules by air-cooling, and have thus completed the present invention.
[0013] The present disclosure includes the following aspects. [Aspect 1] A method for producing granules for chemical recycling, comprising: pulverizing polyester waste; melt-extruding the pulverized polyester waste; solidifying the melt-extruded polyester waste by air-cooling; and pulverizing the solidified polyester waste to form granules. [Aspect 2] The method according to Aspect 1, wherein the melt-extrusion and solidification are carried out using a plast compactor. [Aspect 3] The method according to Aspect 1 or 2, further comprising classifying the granules. [Aspect 4] The method according to Aspect 3, further comprising reusing a residue generated by the classification in the melt-extrusion. [Aspect 5] The method according to any one of Aspects 1 to 4, wherein the ratio of apparent density to bulk density (apparent density / bulk density) of the granules is 1.80 to 2.40. [Aspect 6] The apparent density of the granules is 1.23 g / cm 3 ~1.33 g / cm 3 and the bulk density is 0.60 g / cm 3 ~0.67 g / cm 3 [Aspect 7] The method according to any one of Aspects 1 to 6, wherein the granules have closed cavities inside. [Aspect 8] A granule for chemical recycling comprising a compressed and solidified polyester waste, wherein the ratio of apparent density to bulk density of the granules (apparent density / bulk density) is 1.80 to 2.40. [Aspect 9] The apparent density of the granules is 1.23 g / cm 3 ~1.33 g / cm 3 and the bulk density is 0.60 g / cm 3 ~0.67g / cm 3 Aspect 10: The granules for chemical recycling according to Aspect 8 or 9, having a particle size of 10 mm or less and a content of granules having a particle size of 900 μm or less of 0.2 mass% or less. Aspect 11: The granules for chemical recycling according to any one of Aspects 8 to 10, wherein the granules have a closed cavity therein.
[0014] According to the present invention, there is provided a granulated product for chemical recycling of polyester waste, which has high reactivity in a depolymerization reaction, and is easy to handle and can be efficiently packed into a reactor.
[0015] It should be noted that the above description should not be considered as disclosing all the embodiments of the present invention and all the advantages associated with the present invention.
[0016] 1 is a graph showing the depolymerization reactivity of samples of Example 1, Comparative Example 1, and Comparative Example 2. FIG. 2 is a photograph of the granulated product of Example 1. FIG. 3 is a photograph of the granulated product of Comparative Example 1.
[0017] Representative embodiments of the present invention will be described in more detail below for the purpose of illustrating them, but the present invention is not limited to these embodiments.
[0018] In the present disclosure, true density, apparent density, and bulk density are defined by the following formulas in accordance with the definitions in JIS R 1634:1998. The external volume is the total volume including the solid portion of the sample as well as closed and open pores. The apparent volume is the volume obtained by excluding open pores from the external volume of the sample. If there are closed cavities (closed pores) inside the particles, the apparent density will be smaller than the true density. If there are no closed cavities (closed pores) inside the particles, the apparent density will be approximately equal to the true density, regardless of the presence or absence of cavities (open pores) on the particle surface that are connected to the outside. True density (g / cm 3 ) = mass of sample (g) / volume occupied by sample alone (cm 3 ) apparent density (g / cm 3 ) = mass of sample (g) / apparent volume of sample (cm 3 ) Bulk density (g / cm 3 ) = mass of sample (g) / external volume of sample (cm 3 )
[0019] [Method for producing granules for chemical recycling] In one embodiment, a method for producing granules for chemical recycling includes: pulverizing polyester waste; melt-extruding the pulverized polyester waste; solidifying the melt-extruded polyester waste by air-cooling; and pulverizing the solidified polyester waste to form granules.
[0020] <Crushing Process> The form of polyester waste is not particularly limited, but examples thereof include carpets, carpet fibers, yarns, woven fabrics, knitted fabrics, strings, ropes, twine, fillers, filtration media, bottles, and films, which are discharged as industrial waste or post-consumer materials or products. Polyester waste may also include scraps, surplus products, etc., generated during the production of products.
[0021] Examples of polyesters contained in polyester waste include polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT). The polyester contained in polyester waste is preferably PET.
[0022] Polyester waste may contain other materials besides polyester, such as nylon, polyethylene, polypropylene, and cotton, but these materials are not involved in chemical recycling. The polyester content of polyester waste is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 97% by mass or more. Polyester waste with a low polyester content may be rejected at the raw material receiving stage. For example, the composition of polyester waste may be analyzed from the absorption pattern obtained using a near-infrared spectrometer, and polyester waste that does not have the desired composition may be rejected without being transported to the next process.
[0023] Polyester waste is pulverized to a size that can be fed into an extruder in the melt extrusion process. The size of the pulverized material can be appropriately set depending on the type of extruder, and is usually 2 mm to 15 mm. Pulverization can be performed, for example, using a single-shaft pulverizer. The pulverizer may be configured as a two-stage pulverizer to increase the efficiency of the pulverization process. When a two-stage pulverizer is used, for example, the polyester waste is coarsely pulverized to a size of 30 mm to 150 mm in a primary pulverizer, and then pulverized to a size of 2 mm to 15 mm in a secondary pulverizer. In the present disclosure, the size of the pulverized material is defined as the smallest mesh opening within the range that the pulverized material can pass through when allowed to fall freely onto a metal mesh. For example, the size of pulverized material that passes through a 15 mm square metal mesh is 15 mm or less, while the size of pulverized material that does not pass through a 2 mm square metal mesh is greater than 2 mm.
[0024] <Melt Extrusion Process> Next, the pulverized polyester waste is melt-extruded. The polyester waste is compressed by melt extrusion to a state suitable for forming granules. Melt extrusion can be carried out using a general single-screw or twin-screw extruder. In melt extrusion, as the polyester waste moves through the barrel of the extruder under pressure, frictional heat generated on the surface of the polyester waste melts at least the surface, and the molten polyester acts as a binder to compress the polyester waste. The inner diameter, screw shape, motor output, die shape, etc. of the extruder barrel are appropriately designed so that at least the surface of the polyester waste can be melted.
[0025] The diameter of the molten extrudate is preferably 2 mm to 20 mm, more preferably 3 mm to 15 mm, and even more preferably 4 mm to 10 mm. The diameter of the molten extrudate is determined by the shape and size of the opening of the die.
[0026] <Air-cooling solidification process> Melt-extruded polyester waste is solidified by air-cooling. Without being bound by any theory, solidification of the surface of melt-extruded polyester waste by air-cooling proceeds more slowly than solidification by water-cooling. Since the polyester waste, which was under pressure during the melt-extrusion process, is released to atmospheric pressure after melt-extrusion, volatilization of moisture and other substances present inside the melt-extruded product and surface solidification of the melt-extruded product proceed in competition with each other. Therefore, it is believed that cavities due to moisture remaining inside the melt-extruded product are formed inside the compressed solidified product formed by air-cooling solidification. Furthermore, air may enter the polyester waste during the melt-extrusion process, and the melt-extruded product may be solidified by air-cooling while still containing air, forming cavities inside the compressed solidified product. Such internal cavities are advantageous in increasing the contact efficiency between the granules and ethylene glycol during the depolymerization reaction. Furthermore, because the solidification of the surface proceeds slowly, although minute irregularities or inlets may exist on the surface of the compacted product, the surface of the compacted product is relatively smooth macroscopically. As a result, the bulk density of the granulated product can be increased despite the presence of internal cavities, i.e., the relatively low apparent density, thereby improving the handleability of the granulated product and the efficiency of packing it into a reactor. Furthermore, air-cooling solidification can reduce the amount of moisture remaining inside the granulated product or adhering to the surface of the granulated product, thereby simplifying or eliminating the subsequent drying process.
[0027] The air cooling may be carried out by leaving the molten extrudate as it is, or may be carried out by forcing a gas such as air onto the molten extrudate.
[0028] <<Plastcompactor>> The melt extrusion and air-cooling solidification are preferably carried out using a plastcompactor. By using a plastcompactor, the physical properties of the granules, such as apparent density, bulk density, particle size and particle size distribution, and moisture content, can be stabilized regardless of the type of polyester waste material fed.
[0029] The plastocompactor includes a rotating compression disc and a fixed compression disc, defining a compression zone between them. The fixed compression disc is connected to a replaceable kneading rail via a threaded joint. Crushed polyester waste is fed from a supply silo to the kneading rail and continuously fed through the center of the fixed compression disc into the compression zone of the plastocompactor. The polyester waste is rapidly heated in the compression zone due to friction with the compression discs and friction within the polyester waste. The heated polyester waste melts at least on its surface and stretches toward the periphery of the compression disc, forming elongated, worm-like structures. Heating in the compression zone further reduces the moisture content of the polyester waste. The elongated molten extrudates that emerge from the periphery of the plastocompactor's compression discs fall while being air-cooled and collected in a collection device. Plastcompactors are commercially available, for example, from Herbold Meckesheim GmbH (Meckesheim, Baden-Württemberg, Germany) as the Plastcompactor HV series.
[0030] In melt extrusion and air-cooling solidification using a plastocompactor, the diameter of the elongated molten extrudate is largely determined by the width of the grooves on the surface of the fixed compression disc. Furthermore, because the heated polyester waste material extends toward the outer periphery of the compression disc while in contact with the grooves, the surface of the molten extrudate becomes relatively smooth. Therefore, by using a plastocompactor, granules with a uniform particle size and a relatively smooth surface can be obtained. Such granules have a small angle of repose, making them easy to handle.
[0031] <Granule Formation Step> The solidified polyester waste (compressed solid) is transferred to a pulverizer using compressed air or the like, and pulverized to form granules of a desired size. The pulverization can be carried out using, for example, a uniaxial pulverizer. The pulverization is preferably carried out so that the particle size of the granules becomes 10 mm or less.
[0032] <Classification Step> The obtained granules may be classified to obtain granules having a narrower particle size distribution. Granules having a narrow particle size distribution are excellent in terms of handling properties and packing efficiency into a reaction apparatus.
[0033] Classification can be performed by sieving. By sieving, granules exceeding the desired size can be separated and removed, and granules below the desired size can be sent to the next step. Granules exceeding the desired size can be collected as residue and returned to the grinding step.
[0034] After classification by sieving, granules smaller than the desired size can be separated and removed using an air classifier such as a zigzag classifier, and granules larger than the desired size can be sent to the next step. Granules smaller than the desired size can be recovered as residue and reused in the melt extrusion step.
[0035] [Granulated material for chemical recycling] In one embodiment, the granulated material for chemical recycling comprises a compressed and solidified polyester waste. The ratio of apparent density to bulk density of the granulated material (apparent density / bulk density) is preferably 1.80 to 2.40, more preferably 1.84 to 2.22, and particularly preferably 1.92 to 2.10. By adjusting the ratio to 1.84 to 2.22, the granulated material can exhibit the excellent handleability and reactor packing efficiency described above, and can also exhibit good depolymerization reactivity, as described below. If either the apparent density or the bulk density is too large or too small, causing the ratio to deviate significantly from the above range, the granulated material will not be able to exhibit all of the above effects at a high level.
[0036] Without being bound by any theory, the granules of this embodiment have a lower apparent density than polyester pellets and are therefore believed to have closed cavities within the granules. The closed cavities within the granules are exposed as the depolymerization reaction progresses from the surface of the granules, thereby increasing the efficiency of contact of the granules with ethylene glycol. On the other hand, the granules are heavier than ethylene glycol (the specific gravity of ethylene glycol is 1.116 at 20°C), and therefore settle in the reaction solution in the depolymerization step. This also contributes to increasing the efficiency of contact of the granules with ethylene glycol.
[0037] Furthermore, since the granules of this embodiment have a relatively high bulk density, a larger amount of the granules can be transported and stored in a smaller space, and they are less likely to form bridges in storage devices such as hoppers, resulting in excellent handleability and efficient filling of the reactor. Granules with a relatively high bulk density have a smooth surface with few irregularities and are considered to be less susceptible to the surface tension of the reaction liquid. Therefore, the granules of this embodiment quickly blend into the reaction liquid in the depolymerization step and are easily dispersed in the reaction liquid. Furthermore, the solid-liquid volume ratio (solid volume / liquid volume) in the reaction liquid can be reduced, thereby reducing the load on the stirring power in the depolymerization step.
[0038] In the present disclosure, the apparent density of the granules is determined by a pycnometer method using helium gas. C (m 3 The sample chamber is then filled with helium gas, and the open pores of the granules are purged and replaced with helium gas. After the replacement is complete, the sample chamber is filled with helium gas to a pressure P 1 (Pa) and seal the sample chamber. Once the pressure inside the sample chamber has stabilized, open the solenoid valve downstream of the sample chamber to increase the volume V A (m 3 ) and the pressure P 2 The apparent volume V of the granulated material is calculated from the following equation using the equation of state of an ideal gas: P (m 3The apparent density of the granules is calculated from the apparent volume and the mass of the granules. 1 (V C -V P ) = n 1 RTP 2 (V C +V A -V P ) = n 1 RT ⇔ P 1 (V C -V P ) = P 2 (V C +V A -V P ) ⇔V P =V C -V A / [(P 1 / P 2 ) −1]
[0039] The apparent density of the granules is preferably 1.23 g / cm 3 ~1.33 g / cm 3 , more preferably 1.25 g / cm 3 ~1.30 g / cm 3 is.
[0040] In the present disclosure, the bulk density of a granulated material is determined from the mass of the granulated material that can fit into a container of a given volume. Specifically, the bulk density is calculated by filling a 1 L measuring cylinder with the granulated material at room temperature and atmospheric pressure, and determining the mass of the filled granulated material from the change in mass before and after filling.
[0041] The bulk density of the granules is preferably 0.60 g / cm 3 ~0.67g / cm 3 , more preferably 0.62 g / cm 3 ~0.65g / cm 3 is.
[0042] In one embodiment, the granules have internally closed cavities. The presence of internally closed cavities can be confirmed by image analysis of X-ray CT images.
[0043] The ratio of the apparent density of the granules to the true density of the polyester contained in the granules (apparent density of granules / true density of polyester) is preferably 0.90 to 0.99, more preferably 0.91 to 0.96. By setting this ratio to 0.90 or more, the granules tend to sink in the reaction solution in the depolymerization step. As a result, the contact area between the reaction solution and the granules can be increased immediately after the granules are added to the reaction solution, thereby accelerating the depolymerization reaction. By setting this ratio to 0.99 or less, the depolymerization reactivity can be improved compared to PET resin pellets.
[0044] The particle size of the granulated material is preferably 10 mm or less. In the present disclosure, the particle size of the granulated material is the sieve diameter measured using a metal mesh sieve specified in JIS Z 8801-1:2019. By setting the particle size of the granulated material to 10 mm or less, it is possible to improve handleability and the efficiency of packing into a reaction apparatus.
[0045] The content of granules having a particle size of 900 μm or less is preferably 0.2% by mass or less, which can prevent the granules from scattering during handling and can also suppress the granules from floating to the surface of the reaction solution during the depolymerization step.
[0046] In one embodiment, the granules are substantially free of binders. Here, "substantially free" means that the binder content is less than 1% by mass, preferably less than 0.5% by mass, and more preferably less than 0.1% by mass. Examples of binders include thermoplastic resins such as polyethylene, polypropylene, and acrylonitrile-butadiene-styrene copolymer (ABS), and wood flour. Granules that are substantially free of binders can provide monomers with fewer impurities after the depolymerization reaction.
[0047] [Method of Using Granules for Chemical Recycling] The granules for chemical recycling can be suitably used for recycling polyester waste by a glycolysis-transesterification reaction method using ethylene glycol (EG).
[0048] The method for producing granulated material for chemical recycling and the granulated material of the present disclosure are not limited to chemical recycling applications, and can be applied and used for other applications as well.
[0049] The following examples illustrate specific embodiments of the present disclosure, but the present invention is not limited thereto. All parts and percentages, including those in tables, are by weight unless otherwise specified. Numerical values inherently contain errors resulting from measurement principles and measuring devices. Numerical values, including those in tables, are presented to significant digits using ordinary rounding techniques.
[0050] Example 1 The granulated material for chemical recycling in Example 1 was prepared according to the following procedure. Raw fabrics of 100% polyester and 100% cotton were mixed uniformly to prepare a raw material with an average of 95% polyester and 5% cotton by mass. The raw material was crushed to 15 mm or less and compressed in a plast compactor to melt the raw material by frictional heat. The molten raw material was extruded between two disks with grooves spaced 5.2 mm apart and rotating at 425 rpm. The molten extrudate that passed through the grooves was cut to an appropriate length by centrifugal force and rapidly cooled in air to solidify. The resulting compressed and solidified material was crushed in a crusher to obtain granulated material with a particle size of 10 mm or less. The apparent density of the granulated material in Example 1 was 1.291 g / cm. 3 , bulk density is 0.632 g / cm 3 The particle size was 10 mm or less, and the content of granulated material with a particle size of 900 μm or less was 0.2 mass % or less.
[0051] [Comparative Example 1] In Comparative Example 1, a granule (a foaming agent, manufactured by Zhangjiagang Fiber Minghong Machinery Factory) prepared by melt-extruding polyester waste and then rapidly cooling it in water was used. The apparent density of the granule in Comparative Example 1 was 1.335 g / cm 3 , bulk density is 0.450 g / cm 3 The granules of Comparative Example 1 had large irregularities on the surface formed when the granules were rapidly cooled in water, and the particle size distribution was also larger than that of the granules of Example 1.
[0052] [Comparative Example 2] In Comparative Example 2, PET resin pellets (Semidal, manufactured by Zhejiang Jiaren New Materials Co., Ltd.) were used. The apparent density of the PET resin pellets in Comparative Example 2 was 1.345 g / cm 3 , bulk density is 0.80 g / cm 3 The particle size was 7 mm or less.
[0053] The depolymerization reactivity of the granules of Example 1, Comparative Example 1, and the PET resin pellets of Comparative Example 2 was evaluated using the following procedure. A 1-L flask was charged with a sample and ethylene glycol at a mass ratio ranging from 1:2 to 1:3. Under the same conditions, the mixture was stirred using a single-stage propeller blade as the stirring device, with the rotation speed gradually increased to 200 rpm or 300 rpm, and the temperature was raised to 190°C. Stirring was continued for a period of time while maintaining the mixture temperature at 190°C, and then a depolymerization catalyst was added to the flask. The catalyst addition time was designated as 0 minutes, and stirring was continued at 190°C for 4 hours. Samples of the reaction solution were taken at regular intervals, and the amount of bis(hydroxyethyl) terephthalate (BHET) in the flask was quantified by gas chromatography.
[0054] FIG. 1 is a graph showing the depolymerization reactivity of the samples of Example 1, Comparative Example 1, and Comparative Example 2. The horizontal axis represents reaction time (minutes), with 0 minutes representing the time when the catalyst was added. The vertical axis represents the amount of BHET (mol) in the flask. When the catalyst was added to the flask, depolymerization of the polyester gradually progressed, and BHET again rapidly increased (0 to 50 minutes). Example 1 and Comparative Example 1 had similar depolymerization reaction rates (slope) at the initial stage of the reaction, whereas Comparative Example 2 showed slower progress in the initial stage of the reaction. These results demonstrate that the granules for chemical recycling of Example 1 have the same depolymerization reactivity as the granules of Comparative Example 1.
[0055] Furthermore, the granulated material for chemical recycling in Example 1 had a high bulk density despite a lower apparent density compared to the granulated material in Comparative Example 1, and therefore had excellent flow characteristics as a granular material, and was easy to handle and had excellent filling efficiency into a reaction apparatus.
[0056] Photographs of the granules of Example 1 and Comparative Example 1 are shown in Figures 2 and 3, respectively. As shown in Figure 2, the granules for chemical recycling of Example 1 had a uniform particle size and a relatively smooth surface. They were also found to be hard enough that they did not deform under a certain pressure. On the other hand, as shown in Figure 3, the granules of Comparative Example 1 had surface irregularities formed by rapid water cooling, and were more likely to deform or break apart under external pressure than the granules for chemical recycling of Example 1.
[0057] It will be apparent to those skilled in the art that the above-described embodiments and examples can be modified in various ways without departing from the basic principles of the present invention, and that various improvements and modifications of the present invention can be made without departing from the spirit and scope of the present invention.
[0058] The method and granules of the present disclosure can be suitably used for chemical recycling of polyester waste.
Claims
1. A method for producing a granulated material for chemical recycling, comprising: pulverizing polyester waste; melt-extruding the pulverized polyester waste; solidifying the melt-extruded polyester waste by air-cooling; and pulverizing the solidified polyester waste to form a granulated material.
2. The method of claim 1, wherein said melt extruding and said solidifying are carried out using a plastcompactor.
3. The method according to claim 1 or 2, further comprising classifying the granulated material.
4. The method of claim 3, further comprising recycling a residue resulting from said classification into said melt extrusion.
5. The method according to claim 1 or 2, wherein the ratio of apparent density to bulk density of the granulated product (apparent density / bulk density) is 1.80 to 2.
40.
6. The apparent density of the granules is 1.23 g / cm 3 ~1.33g / cm 3 and the bulk density is 0.60 g / cm 3 ~0.67g / cm 3 The method according to claim 1 or 2, 7. The method according to claim 1 or 2, wherein the granules have closed cavities therein.
8. A granulated material for chemical recycling comprising compressed and solidified polyester waste, the granulated material having an apparent density to bulk density ratio (apparent density / bulk density) of 1.80 to 2.
40.
9. The apparent density of the granules is 1.23 g / cm 3 ~1.33g / cm 3 and the bulk density is 0.60 g / cm 3 ~0.67g / cm 3 The granules for chemical recycling according to claim 8, 10. A granulated material for chemical recycling according to claim 8 or 9, having a particle size of 10 mm or less and a content of granulated material having a particle size of 900 μm or less of 0.2 mass % or less.
11. The granulated material for chemical recycling according to claim 8 or 9, wherein the granulated material has a closed cavity inside.
Citation Information
Patent Citations
Method for separating recycled polyester from waste polyester raw material
CN110734578A
Method for recovering valuable component from waste polyester
JP2004300115A
Method and system for recycling used scrap film
JP2016522099A
Manufacturing method and equipment for plastic molded body
JP2023007040A
Method to increase intrinsic viscosity of recycling polyester waste
US20210179803A1
Cited By
Adsorption device and method for manufacturing an adsorption device
JP2026170601A