Polytrimethylene terephthalate fiber, method for producing same, air-mixed filament yarn containing said polytrimethylene terephthalate fiber, and fabric composed thereof

By controlling the elastic modulus and processing conditions of polytrimethylene terephthalate fibers, along with air-blended yarns and core-sheath structures, the challenges of high shrinkage and stiffness in polytrimethylene terephthalate fibers are overcome, resulting in low-shrinkage, soft-textured fabrics with improved stability and drapability.

WO2024214591A1PCT designated stage expired Publication Date: 2024-10-17TEIJIN FRONTIER CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013587
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2024-04-02
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing polytrimethylene terephthalate fibers exhibit high shrinkage rates and lack softness when used in fabrics, due to their high elastic modulus and poor spinning conditions, leading to unstable yarn production and poor textile properties.

Method used

Producing polytrimethylene terephthalate fibers with a boiling water shrinkage rate of 5% or less, an elastic modulus of 5 cN/dtex or less at 20% elongation, and specific processing conditions such as stretching and heating to achieve a soft texture and low shrinkage, combined with air-blended yarns and core-sheath structures for improved textile properties.

Benefits of technology

The resulting fibers and yarns exhibit low shrinkage rates and soft textures, enhancing fabric drapability and stability, while maintaining heat resistance and strength, thus addressing the limitations of previous methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000026_0000
    Figure 00000026_0000
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a low-shrinkage fiber substantially composed of polytrimethylene terephthalate, and capable of producing a raw yarn for fabric that has a soft texture and a low heat shrinkage rate; a method for producing the low-shrinkage fiber; an air-mixed filament yarn that contains said polytrimethylene terephthalate fiber; and a fabric composed thereof. The present invention is a polytrimethylene terephthalate fiber composed of at least 90 mol% of trimethylene terephthalate repeating units, wherein the boiling water shrinkage rate of said polytrimethylene terephthalate fiber is at most 5%, and the elastic modulus at 20% elongation of said polytrimethylene terephthalate fiber is at most 5 cN / dtex.
Need to check novelty before this filing date? Find Prior Art

Description

Polytrimethylene terephthalate fiber, its manufacturing method, air-mixed yarn containing the polytrimethylene terephthalate fiber, and fabric made of the same

[0001] The present invention relates to a fiber substantially consisting of polytrimethylene terephthalate, which can be used to produce raw yarn for fabrics having a small shrinkage rate on heating and a soft texture, a method for producing the same, an air-mixed yarn containing the polytrimethylene terephthalate fiber, and a fabric made from the same.

[0002] Polytrimethylene terephthalate (hereinafter sometimes referred to as PPT) has properties similar to polyamide, such as excellent elastic recovery and dyeability, as well as properties similar to polyethylene terephthalate, such as light resistance, heat setting, dimensional stability, and low water absorption, and so utilizing these characteristics, its use in many fields, such as BCF carpets and brushes, has been proposed (for example, JP-A Nos. 9-3724, 8-173244, and 5-262862). Furthermore, polytrimethylene terephthalate fiber has a low Young's modulus, and is therefore said to enable the production of products with a soft feel.

[0003] Furthermore, a method for producing polytrimethylene terephthalate fibers has been proposed in which an undrawn yarn melt-spun at 300 to 4,000 m / min is hot-drawn in one or multiple stages at a temperature equal to or higher than the glass transition temperature of the undrawn yarn, either after being temporarily wound up or continuously without being wound up. As spinning and drawing conditions, for example, Japanese Patent Laid-Open Publication No. 2001-207329 (Patent Document 1) discloses a method in which a polytrimethylene terephthalate polymer having an intrinsic viscosity [η] of 0.7 or more is taken up at a spinning speed of 3,000 m / min, and is subsequently drawn at 70°C without being temporarily wound up, followed by a relaxation heat treatment at a relaxation rate of 6 to 20%.

[0004] However, although the polytrimethylene terephthalate fibers proposed so far certainly have a lower Young's modulus than polyethylene terephthalate fibers, when they are made into fabrics, these properties are not fully exhibited, and fabrics that are fully satisfactory in terms of softness have not yet been obtained.

[0005] On the other hand, Japanese Patent Laid-Open Publication No. 2001-348729 (Patent Document 2) discloses that polytrimethylene terephthalate fiber with a soft texture can be obtained by winding at a spinning speed of 4,500 m / min or more. While this method certainly produces a soft fabric, problems arise, such as tight winding due to elastic deformation of the yarn during winding, resulting in poor winding shape and crushing of the wound paper tube. Furthermore, the high spinning speed makes the yarn prone to breakage, making it difficult to produce a stable yarn.

[0006] Japanese Patent Application Laid-Open No. 2001-207329 Japanese Patent Application Laid-Open No. 2001-348729

[0007] The present invention has been made in view of the above background, and its object is to provide a low-shrinkage fiber consisting essentially of polytrimethylene terephthalate, which can be used to produce raw yarn for fabrics having a small heat shrinkage rate and a soft texture, a method for producing the same, an air-mixed yarn containing the polytrimethylene terephthalate fiber, and a fabric made from the same.

[0008] As a result of intensive research to solve the above-mentioned problems, the present inventors have found that a desired polytrimethylene terephthalate fiber can be obtained when the boiling water shrinkage of a fiber substantially consisting of polytrimethylene terephthalate (hereinafter, may be referred to as "boiling water shrinkage") and the elastic modulus at 20% elongation of the polytrimethylene terephthalate fiber are controlled within ranges different from those of so-called straight drawn yarns and high-speed spun yarns described in the above-mentioned prior art documents, and have arrived at the present invention.

[0009] Thus, according to the present invention, there are provided: 1. A polytrimethylene terephthalate fiber composed of 90 mol % or more of trimethylene terephthalate repeating units, characterized in that the polytrimethylene terephthalate fiber has a boiling water shrinkage of 5% or less and a modulus of elasticity at an elongation of 20% of 5 cN / dtex or less; 2. A polytrimethylene terephthalate fiber as set forth in 1 above, which has a birefringence Δn of 0.040 or more and a specific gravity of 1.350 or less; 3. A polytrimethylene terephthalate fiber as set forth in 1 or 2 above, which has a thermal stress peak at 50 to 100°C and a thermal stress peak value of 0.2 cN / dtex or less; 4. 5. A polytrimethylene terephthalate fiber according to 1 or 2 above, wherein the polytrimethylene terephthalate fiber has a breaking strength of 1.5 to 3.5 cN / dtex and a breaking elongation of 30 to 100%, 5. A method for producing a polytrimethylene terephthalate fiber, comprising melting and solidifying polytrimethylene terephthalate comprising 90 mol % or more of trimethylene terephthalate repeating units, winding the melted polytrimethylene terephthalate at a winding speed of 1,000 m / min or more, stretching the stretched polytrimethylene terephthalate at a temperature not higher than the glass transition point of the polytrimethylene terephthalate, and then shrinking the stretched polytrimethylene terephthalate at a stretching ratio of 0.5 to 0.9 while heating, 6. An air-mixed yarn comprising the polytrimethylene terephthalate fiber according to any one of 1 to 4 above and a polyester-based fiber, 7. An air-mixed yarn according to 6 above, wherein the polyester-based fiber has a boiling water shrinkage rate of 7 to 50%, 8. 9. An air-mixed yarn according to 6 or 7 above, which contains modified cross-section fibers; 10. An air-mixed yarn comprising a core yarn and a sheath yarn and having a total fineness of 30 to 400 dtex, obtained by heat-treating the air-mixed yarn according to 6 above, wherein the core yarn is made of a polyester fiber and the sheath yarn is made of a polytrimethylene terephthalate fiber having a single fiber fineness of 0.3 to 10 dtex, and the yarn length difference between the core yarn and the sheath yarn as defined by the following method is 5% or more (Method for measuring yarn length difference)10. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 11. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 12. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 13. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 14. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 15. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 16. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 17. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 18. A sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath fiber to the total weight of the sheath-core air-mixed yarn is 50-90%. 19. A shea The present invention provides a sheath-core air-mixed yarn as described in items 9 or 10 above, which comprises a modified cross-section fiber, 12. a fabric comprising the air-mixed yarn as described in any one of items 6 to 8 above, and 13. a fabric comprising the sheath-core air-mixed yarn as described in any one of items 9 to 11 above.

[0010] According to the present invention, it is possible to provide a low-shrinkage fiber substantially made of polytrimethylene terephthalate, which can be used to produce raw yarn for fabrics having a small heat shrinkage rate and a soft texture, a method for producing the same, an air-mixed yarn containing the polytrimethylene terephthalate fiber, and a fabric made from the same.

[0011] 1 is a schematic diagram showing an example of the degree of irregularity in the modified cross-section fiber used in the present invention, and FIG. 2 is a schematic diagram showing an example of the degree of flatness in the flat cross-section fiber used in the present invention.

[0012] The present invention will be described in detail below. (1) Polymer Raw Material The polymer used in the present invention is polytrimethylene terephthalate (hereinafter sometimes referred to as PTT), which is composed of 90 mol % or more of trimethylene terephthalate repeating units. PTT is a polyester containing terephthalic acid as the acid component and trimethylene glycol (also known as 1,3-propanediol) as the diol component. The PTT may contain up to 10 mol % of other copolymerization components.

[0013] Examples of such copolymerization components include ester-forming monomers such as 5-sodium sulfoisophthalic acid, 5-potassium sulfoisophthalic acid, 3,5-dicarboxylic acid benzenesulfonic acid tetrabutylphosphonium salt, 3,5-dicarboxylic acid benzenesulfonic acid tributylmethylphosphonium salt, 1,4-butanediol, neopentyl glycol, 1,6-hexamethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, adipic acid, dodecanedioic acid, and 1,4-cyclohexanedicarboxylic acid.

[0014] If necessary, various additives such as a matting agent, a heat stabilizer, an antifoaming agent, a tinting agent, a flame retardant, an antioxidant, an ultraviolet absorber, an infrared absorber, a crystal nucleating agent, and a fluorescent whitening agent may be copolymerized with or mixed into the PTT.

[0015] The polytrimethylene terephthalate polymer used in the present invention preferably has an intrinsic viscosity [η] of 0.5 to 1.6, more preferably 0.6 to 1.5, and even more preferably 0.7 to 1.4.

[0016] If the intrinsic viscosity is less than 0.5, the molecular weight of the polymer is too low, making it difficult to achieve sufficient strength. On the other hand, if the intrinsic viscosity exceeds 1.6, the flowability is low, which impairs the spinnability of the low-viscosity polytrimethylene terephthalate, and this may cause yarn breakage during spinning, which is undesirable.

[0017] (2) Polytrimethylene terephthalate fiber The polytrimethylene terephthalate fiber of the present invention is small in deformation by hot water treatment, and therefore when made into a fabric, the yarn shrinks little and has a soft texture. In addition, one of the characteristics of this polytrimethylene terephthalate fiber is its low elastic modulus after the primary yield point in a tensile strength / elongation measurement, and when a fabric is made using this fiber, the resulting fabric has a softer drape than that of ordinary polytrimethylene terephthalate fibers.

[0018] As for the yarn properties of such polytrimethylene terephthalate fibers, the boiling water shrinkage rate of the polytrimethylene terephthalate fibers in the present application (hereinafter sometimes referred to as "boiling water shrinkage rate") must be 5% or less, preferably 4% or less, and more preferably 3% or less. If the boiling water shrinkage rate is greater than 5%, the fabric will become stiff due to shrinkage of the yarn caused by heat shrinkage.

[0019] Furthermore, the polytrimethylene terephthalate fiber of the present invention must have a modulus of elasticity at 20% elongation of 5 cN / dtex or less, preferably 4 cN / dtex or less, and more preferably 3 cN / dtex or less. If the modulus of elasticity at 20% elongation is greater than 5 cN / dtex, the fabric will become stiff during subsequent dyeing and other processes.

[0020] Furthermore, the birefringence index Δn of the polytrimethylene terephthalate fiber of the present invention is preferably 0.040 or more and 0.08 or less. The birefringence index Δn is more preferably 0.045 or more and 0.075 or less, and even more preferably 0.050 or more and 0.070 or less. If the birefringence index Δn is less than 0.040, the yarn strength decreases, and the fabric stretches due to external force, making it difficult to maintain its shape, which is undesirable.

[0021] Furthermore, the specific gravity of the polytrimethylene terephthalate fiber of the present invention, which is an alternative index of the crystallinity, is preferably 1.350 or less, and more preferably 1.319 to 1.350. If the specific gravity is less than 1.319, the yarn becomes embrittled during draw-twisting, causing frequent yarn breakage and making draw-twisting difficult. On the other hand, if the specific gravity is greater than 1.350, frequent fluffing occurs, which is undesirable.

[0022] It is also preferable that the thermal stress peak of the polytrimethylene terephthalate fiber of the present invention exists at 50°C to 100°C. If the peak exists at a temperature lower than 50°C, the heat resistance will be reduced, which is not preferable. If the peak exists at a temperature higher than 100°C, the crystallinity will be too high, which will result in a loss of soft drapeability, which is also not preferable.

[0023] Furthermore, the peak value of the thermal stress of the polytrimethylene terephthalate fiber of the present invention is preferably 0.2 cN / dtex or less. If the peak value of the thermal stress is greater than 0.2 cN / dtex, deformation due to hot water treatment such as dyeing becomes large, and when made into a fabric, the yarn shrinks and the texture becomes stiff, which is undesirable.

[0024] The breaking strength of the polytrimethylene terephthalate fiber of the present invention is 1.5 cN / dtex or more to 3.5 cN / dtex, preferably 1.7 cN / dtex to 3.3 cN / dtex, and more preferably 2.0 cN / dtex to 3.0 cN / dtex.

[0025] If the breaking strength of the polytrimethylene terephthalate fiber is less than 1.5 cN / dtex, the durability of the product will decrease, which is undesirable, whereas if the breaking strength of the polytrimethylene terephthalate fiber is more than 3.5 cN / dtex, the degree of crystallinity will be too high, which will result in a loss of soft drapeability, which is undesirable.

[0026] The breaking elongation of the polytrimethylene terephthalate fiber is preferably 30% to 100%. If the breaking elongation of the polytrimethylene terephthalate fiber is less than 30%, the degree of crystallinity becomes too high, resulting in a loss of flexible drapeability, which is undesirable. On the other hand, if the breaking elongation of the polytrimethylene terephthalate fiber is more than 100%, the fiber will stretch when a load is applied to it, resulting in poor dimensional stability, which is undesirable.

[0027] (3) Method for Producing Polytrimethylene Terephthalate Fibers The polytrimethylene terephthalate fibers described above can be produced, for example, by the following method: First, polytrimethylene terephthalate, which is composed of 90 mol % or more of trimethylene terephthalate repeating units, is melt-solidified, and then wound up at a take-up speed of 1,000 m / min or more. Subsequently, the polytrimethylene terephthalate is heated with a heating roller at a temperature of ±20°C of the glass transition point of the polytrimethylene terephthalate, and then stretched 1.0 to 2.0 times. Further, the polytrimethylene terephthalate is wound around a heating roller at a temperature of 50 to 150°C, and then temporarily wound into a cheese-shaped package at a speed of 2,000 to 4,800 m / min.

[0028] The polytrimethylene terephthalate fiber having a breaking elongation of 50 to 200% wound into a cheese-shaped package in this manner is stretched by 1.1 times or more at a temperature equal to or lower than the glass transition point of the polytrimethylene terephthalate, and then the fiber is shrunk by 0.5 to 0.9 times while being heated, thereby obtaining polytrimethylene terephthalate fiber that can be made into a fabric with little thermal shrinkage and a soft texture.

[0029] In this case, the total draw ratio, which is the product of the draw ratio at a temperature below the glass transition point and the shrinkage ratio while heating, is preferably 0.9 to 1.25 times, and more preferably 0.95 to 1.20 times. A total draw ratio of less than 0.90 times is not preferred because the yarn becomes loose and the yarn running becomes unstable during drawing, which may cause yarn breakage. Also, a total draw ratio of more than 1.25 times is not preferred because the shrinkage rate of the yarn becomes too high and the fabric made from it may not have a soft feel.

[0030] Incidentally, polytrimethylene terephthalate fibers having a breaking elongation of 50 to 200% and solidified after melting can also be produced by, for example, taking up the fiber at a spinning speed of 1000 m / min or more and subsequently drawing the fiber at a low drawing ratio of 1.0 to 2.0 times at a temperature within ±20°C of the glass transition point of polytrimethylene terephthalate.

[0031] It is also possible to wind the fiber onto a heated roller at a spinning speed of 4000 m / min or more and then wind it up with a winder. Among these methods, there is no problem with heating the fiber with a heated roller at 50 to 150°C before winding in order to prevent winding tension when the polytrimethylene terephthalate fiber is directly wound up with a winder.

[0032] The high elongation polytrimethylene terephthalate fiber thus obtained preferably has a breaking elongation of 50 to 200% or more, more preferably 60 to 190%, and even more preferably 70 to 180%.

[0033] If the breaking elongation of the high-elongation polytrimethylene terephthalate fiber is less than 50%, the crystallization of the fiber will be high, making it impossible to produce a fabric with a soft feel, which is undesirable.On the other hand, if the breaking elongation is greater than 200%, the crystallization will not progress when stretched at a temperature below the glass transition point, resulting in a significantly low strength and low durability when produced into a fabric, which is undesirable.

[0034] Subsequently, the polytrimethylene terephthalate fiber that has been melted and solidified is stretched at a temperature equal to or lower than the glass transition point of polytrimethylene terephthalate, more preferably at a temperature equal to or lower than the glass transition point −5° C., and even more preferably at a temperature equal to or lower than the glass transition point −10° C., by 1.1 times or more, more preferably 1.2 times or more, and even more preferably 1.3 times or more.

[0035] In this case, stretching at a temperature higher than the glass transition point is not preferred because the crystallinity becomes high and the fabric cannot have a soft feel, and stretching at a stretching ratio lower than 1.1 times is also not preferred because the fabric has low durability.

[0036] Furthermore, since the drawn fibers are not highly crystallized and the polymers are highly oriented, their dimensional stability due to heat is low. Therefore, the dimensional stability and durability can be improved by shrinking the fibers at a rate of 0.5 to 0.9 times while heating.

[0037] In this case, if the shrinkage of the fiber is less than 0.5 times, the degree of orientation crystallinity of the obtained polytrimethylene terephthalate fiber becomes too low, which is undesirable because the durability of the fabric when made into a fabric becomes low, whereas if the shrinkage of the fiber is more than 0.9 times, the degree of crystallinity becomes too high, which is undesirable because the fabric cannot have a soft feel.

[0038] (4) Polyester Fiber (for Core Yarn) In the present invention, the polytrimethylene terephthalate fiber and polyester fiber are mixed by air processing to obtain an air-mixed yarn.

[0039] Preferred examples of polyester fibers used in this case include fibers spun and drawn by conventional methods, such as polytrimethylene terephthalate (PTT) fibers, polyethylene terephthalate (PET) fibers, side-by-side or eccentric sheath-core composite fibers of polytrimethylene terephthalate and polyethylene terephthalate, side-by-side or eccentric sheath-core composite fibers of polytrimethylene terephthalate and polytrimethylene terephthalate, and side-by-side or eccentric sheath-core composite fibers of polyethylene terephthalate and polyethylene terephthalate. Additives such as antistatic agents, flame retardants, heat-resistant agents, weather-resistant agents, and titanium oxide may be added. For such polyester fibers, a boiling water shrinkage of 7 to 50% is preferred in order to increase the length difference between the core yarn and the sheath yarn by subjecting the air-mixed yarn to heat treatment or the like.

[0040] (5) Method for producing air-mixed yarn Next, the polytrimethylene terephthalate fiber as the sheath yarn and the polyester fiber as the core yarn are aligned, and entangled (preferably 30 to 150 pcs / m) by air processing (interlace or Taslan (registered trademark)), and then taken up with a roller to obtain an air-mixed yarn. The overfeed rate during air-mixing processing is preferably 0.5 to 2%.

[0041] Furthermore, the air-blended yarn of the present invention may contain fibers with irregular cross sections other than a circular cross section. For example, it may be composed of fibers with irregular cross sections such as cross-shaped, triangular, or star-shaped cross sections, which can produce a unique texture. The irregularity of the irregular cross section fiber is calculated by measuring the maximum inscribed circle diameter r and the minimum circumscribed circle diameter R of the fiber cross section, as shown in Figure 1, and then calculating the irregularity ratio R / r. The value of R / r is preferably 1.15 to 10.0, more preferably 1.2 to 10.0. If the irregularity ratio is less than 1.15, the difference from a circular cross section may become small. Furthermore, if the irregularity ratio exceeds 10.0, the orientation difference between the outer and inner cross sections of the yarn during spinning becomes large, and the resulting yarn may have a lot of fluff and slack, making it unsuitable for processing.

[0042] Another example of a modified cross-section fiber is a flat cross-section fiber. The use of a flat cross-section fiber is preferred because it can provide a unique texture. Here, the flatness of a flat cross-section fiber is a value calculated by drawing a rectangle circumscribing the fiber cross-section, measuring its long side L and short side H, and then calculating the flatness = L / H, as shown in FIG. 2 . In the present invention, the value of the flatness = L / H is preferably 2.0 to 10.0. If the flatness is less than 2.0, the difference from a round cross-section may become small. Furthermore, if the flatness exceeds 10.0, fluffing may occur easily during spinning, resulting in poor stability.

[0043] The air-mixed yarn thus obtained can be a sheath-core type air-mixed yarn with a large difference in the length between the core and sheath, using a low-shrinkage fiber made of polytrimethylene terephthalate having a soft texture as the sheath yarn.

[0044] (6) Manufacturing method of core-sheath type air-mixed yarn In the present invention, by subjecting the air-mixed yarn to a heat treatment such as dyeing processing, the polytrimethylene terephthalate fiber becomes a sheath yarn and the polyester fiber becomes a core yarn, thereby forming a core-sheath type air-mixed yarn containing a core yarn and a sheath yarn.

[0045] In such air-mixed yarns, the single fiber fineness of the sheath yarn must be 0.3 to 10 dtex, more preferably 0.5 to 8 dtex, and even more preferably 0.6 to 5 dtex. If the single fiber fineness is greater than 10 dtex, the thick single fiber may cause the fabric to lose its softness. If the single fiber fineness is less than 0.3 dtex, yarn breakage may occur frequently, making it impossible to produce fibers. The number of single fibers (number of filaments) in the sheath yarn is preferably 20 to 150. On the other hand, the single fiber fineness of the core yarn is preferably 1.0 to 5.0 dtex. The number of single fibers (number of filaments) in the core yarn is preferably 12 to 100.

[0046] Furthermore, the total fineness of the core-sheath type air-mixed yarn of the present invention must be 30 to 400 dtex, more preferably 50 to 200 dtex. If the total fineness is less than 30 dtex, the total fineness is too thin and air-mixing processing may be difficult. On the other hand, if the total fineness is more than 400 dtex, the fabric may lose its softness. The number of single fibers (filaments) is preferably 40 to 400 (more preferably 40 to 200).

[0047] In the above-mentioned core-sheath type air-mixed yarn, it is essential that the yarn length difference between the core yarn and the sheath yarn, as defined below, is 5% or more (more preferably 6 to 40%). If the yarn length difference is less than 5%, a sufficient fluffy feeling cannot be obtained.

[0048] The above-mentioned yarn foot difference is calculated by treating the air-mixed yarn in boiling water, applying a load of 0.1 cN (0.098 g) × the total fineness (dtex) of the air-mixed yarn, and cutting it to a length of 5 cm. From the cut air-mixed yarn, polyester fiber A (single fiber) and polytrimethylene terephthalate fiber B (single fiber) are removed, and their lengths are measured under a load of 0.1 cN (0.098 g) × the single fiber fineness (dtex). The yarn foot difference (%) is calculated using the following formula: Yarn foot difference (%) = (LB - LA) / LA × 100 where LA is the length (cm) of the polyester fiber core yarn, and LB is the length (cm) of the polytrimethylene terephthalate fiber sheath yarn.

[0049] In the sheath-core air-mixed yarn of the present invention, the polytrimethylene terephthalate fiber in the sheath yarn preferably accounts for 50 to 90% (more preferably 60 to 80%) of the weight of the mixed yarn. If the weight ratio of the polytrimethylene terephthalate fiber in the sheath yarn is 50% or less, not only will a soft feel not be obtained, but the difference in dye absorption between the core yarn and the sheath yarn may become more visible.

[0050] (7) Manufacturing method of fabric made of sheath-core air-mixed yarn In the present invention, fabric (grey fabric) is obtained by knitting or weaving the above-mentioned air-mixed yarn, and then dyeing and sweat-absorbing treatment are carried out as appropriate to obtain the fabric as a product. In this case, the heat treatment in the dyeing process causes the yarn length difference between the sheath yarn and the core yarn of the mixed yarn to appear, resulting in a fabric made of sheath-core air-mixed yarn.

[0051] The fabric may be made of only the sheath-core air-mixed yarn, or may be made of the sheath-core air-mixed yarn and other yarns. In this case, the other yarns are not particularly limited and may be non-crimped yarns, false-twisted crimped yarns, latent crimped yarns, spun yarns, etc.

[0052] The fabric structure is not particularly limited, and may be either a knitted fabric or a woven fabric. Examples include knitted fabrics having knitting structures such as plain weave, twill weave, satin weave, etc., but are not limited to these. The number of layers may be a single layer or two or more layers.

[0053] The fabric may then be used to make textile products such as sportswear, outerwear, innerwear, men's clothing, women's clothing, nursing clothing, workwear, car seat covering materials, bedding, etc. Since such fabrics and textile products use the air-mixed yarn, they have excellent soft texture and fluffiness.

[0054] Examples and comparative examples of the present invention will be described in detail below, but the present invention is not limited to these. The measurement items in the examples were measured by the following methods.

[0055] (1) Intrinsic viscosity [η] The intrinsic viscosity [η] was determined using an Ostwald viscometer by extrapolating the ratio ηsp / C of the specific viscosity ηsp in o-chlorophenol at 35°C to the concentration C (g / 100 ml) to a concentration of zero, according to the following formula (1): [η]=lim(ηsp / C) (1) C→0

[0056] (2) Glass Transition Point The glass transition point was measured from a temperature rise curve obtained by sealing a specified amount of polymer chips in an aluminum sample pan and heating the chips from room temperature to 300°C at a rate of 10°C / min in a nitrogen atmosphere using a DSC.

[0057] (3) Fineness (Fineness of Multifilament Yarn) The fineness of the multifilament yarn was measured in accordance with JIS-L-1013. The measured value was divided by the number of single yarns in the multifilament yarn to determine the fineness of the single yarn.

[0058] (4) Boiling Water Shrinkage (BWS) Based on JIS-L-1013, a fiber was rewound using a measuring machine with a frame circumference of 1.125 m, with an initial load of 1 / 30 g of decitex applied, to form a skein of 20 turns, and a load of 1.11 g of decitex was applied to measure the skein length. Next, the load was removed, and the skein was immersed in hot water at 100°C for 30 minutes, then removed and air-dried. A load was applied again, and the skein length was measured, and the boiling water shrinkage was calculated using the following formula: Boiling Water Shrinkage (%) = {(L0 - L1) / L0} x 100, where L0 is the skein length before immersion (mm), and L1 is the skein length after immersion (mm).

[0059] (5) Breaking Strength and Breaking Elongation Based on JIS-L-1013, measurements were made using a constant speed extension type tensile tester, Tensilon manufactured by Orientec Co., Ltd., at a gripping distance of 20 cm and a pulling speed of 20 cm / min.

[0060] (6) Elastic modulus at 20% elongation: Measurement was performed using a constant-speed extension tensile tester, Tensilon, manufactured by Orientec Co., Ltd., at a grip distance of 20 cm and a pulling speed of 20 cm / min in accordance with JIS-L-1013. The slope of the tangent to the SS curve at 20% elongation was determined as the elastic modulus at 20% elongation.

[0061] (7) Specific Gravity The specific gravity of the sample was measured based on the sink-float method of JIS-L-1013 8.17.1.

[0062] (8) Birefringence Δn: This was determined from the retardation of polarized light observed on the surface of the fiber using an optical microscope and a compensator, in accordance with Fiber Handbook - Raw Materials, p. 969 (5th edition, published by Maruzen Co., Ltd. in 1978).

[0063] (9) Temperature at which maximum thermal stress exists and maximum thermal stress value KE-2 manufactured by Kanebo Engineering Co., Ltd. was used. Measurements were performed with an initial load of 0.044 cN / dtex and a heating rate of 100°C / min. The obtained data was plotted with temperature on the horizontal axis and thermal stress on the vertical axis to draw a temperature-thermal stress curve. The temperature and thermal stress at the point where the differential coefficient of the temperature-thermal stress curve changed from positive to negative were determined, and the stress was divided by the fineness to determine the maximum stress.

[0064] (10) Number of entanglements A length of 1 m was taken from the air-textured yarn under a load of 8.82 mNx (0.1 g / dtex), and after the weight was reduced and the yarn was left to relax at room temperature for 24 hours, the number of knots was read and expressed in units per m.

[0065] (11) Yarn length difference After skein treatment in the same manner as in the boiling water shrinkage test, the yarn was cut to a length of 5 cm under a load of 0.1 cN (0.098 g) × the total fineness (dtex) of the air-mixed yarn, and polyester fiber A (single fiber) and polytrimethylene terephthalate fiber B (single fiber) were taken out from the cut air-mixed yarn and their lengths were measured under a load of 0.1 cN (0.098 g) × the single fiber fineness (dtex), and the yarn length difference (%) was calculated using the following formula: Yarn length difference (%) = (LB - LA) / LA × 100 where LA is the length (cm) of the polyester fiber core yarn, and LB is the length (cm) of the polytrimethylene terephthalate fiber sheath yarn.

[0066] (12) Feeling The tester touched the air-blended yarn with his / her hands and rated it on a three-point scale: ◯ (fluffy and soft), △ (normal), × (poor fluffiness or hard).

[0067] Example 1 Dimethyl terephthalate and 1,3-propanediol were charged in a molar ratio of 1:2, and titanium tetrabutoxide equivalent to 0.1% by weight of the dimethyl terephthalate was added, followed by completion of the transesterification reaction under normal pressure at a heater temperature of 240° C. Next, titanium tetrabutoxide was further added in an amount of 0.1% by weight of the theoretical polymer amount, and titanium dioxide was added in an amount of 0.5% by weight of the theoretical polymer amount, and the reaction was carried out at 270° C. for 3 hours.

[0068] The resulting polymer was composed of 100 mol% trimethylene terephthalate repeating units and had an intrinsic viscosity of 1.0 dl / g. The glass transition point of the resulting polymer was 51°C. The resulting polymer was dried by a conventional method to reduce the water content to 50 ppm, then melted at 265°C and extruded through a single-layer spinneret with 36 holes and a diameter of 0.27 mm.

[0069] The extruded molten multifilaments were rapidly cooled by blowing air at a speed of 4.0 m / min to convert them into solid multifilaments, and then a guide nozzle was used to apply an oil solution containing 60% by weight of octyl stearate, 15% by weight of polyoxyethylene alkyl ether, and 3% by weight of potassium phosphate as a 10% by weight water emulsion finishing agent so that the amount of oil solution applied to the fibers was 0.6% by weight.

[0070] Next, the solid multifilament was wound around a roll heated to 50°C with a peripheral speed of 2100 m / min, and then wound around a roll heated to 80°C so as to be stretched 1.3 times, and then wound at a winding speed of 2600 m / min using a winder that drives both the spindle and the touch roll, to obtain a cheese-shaped package wound with 72 dtex / 36 filament fibers.

[0071] The fiber wound on the package was then stretched to 1.5 times its original size at 30°C, heated with a contact-type hot plate heater at 190°C, shrunk to 0.7 times its original size, and wound at a speed of 600 m / min to obtain a low-shrinkage polytrimethylene terephthalate fiber (sheath yarn). Meanwhile, a polyester (polyethylene terephthalate) drawn yarn (total fineness 56 dtex / 36 strands, boiling water shrinkage 10%) was prepared as the core yarn.

[0072] The sheath yarn and the core yarn were then aligned and interlaced at an overfeed rate of 1.5% to obtain an air-mixed yarn with an entanglement number of 69 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2.

[0073] [Example 2] A polymer was produced in the same manner as in Example 1, and then the resulting polymer was dried in a conventional manner to reduce the water content to 50 ppm. The polymer was then melted at 265°C and extruded through a double-arranged spinneret having 72 holes with a diameter of 0.23 mm.

[0074] An oil agent was applied to the extruded molten multifilament in the same manner as in Example 1, and then the solid multifilament was wound around a roll heated to 50°C and having a peripheral speed of 2100 m / min, and then wound around a roll heated to 80°C so as to be stretched 1.3 times.Then, using a winder that drives both the spindle and the touch roll, the winding was performed at a winding speed of 2600 m / min to obtain a cheese-shaped package wound with 72 dtex / 72 filament fibers.

[0075] The fiber wound on the package was then drawn 1.4 times at 30°C, heated with a contact-type hot plate heater at 190°C, shrunk by 0.75 times, and wound at a speed of 600 m / min to obtain a low-shrinkage polytrimethylene terephthalate fiber (sheath yarn). Meanwhile, a polyester (polyethylene terephthalate) drawn yarn (total fineness 56 dtex / 36 strands, boiling water shrinkage 13%) was prepared as the core yarn.

[0076] Next, the sheath yarn and the core yarn were aligned and interlaced at an overfeed rate of 1.5% in the same manner as in Example 1 to obtain an air-mixed yarn with an entanglement number of 71 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2.

[0077] [Example 3] A polymer was produced in the same manner as in Example 1, and then the resulting polymer was dried in a conventional manner to reduce the water content to 50 ppm. The polymer was then melted at 265°C and extruded through a single-layer spinneret having 36 holes with a diameter of 0.27 mm.

[0078] An oil agent was applied to the extruded molten multifilament in the same manner as in Example 1, and then the solid multifilament was wound around a roll heated to 50°C and having a peripheral speed of 2350 m / min, and then wound around a roll heated to 80°C so as to be stretched 1.1 times.Then, using a winder that drives both the spindle and the touch roll, the winding was performed at a winding speed of 2600 m / min to obtain a cheese-shaped package wound with 72 dtex / 36 filament fibers.

[0079] The fiber wound on the package was then stretched to 1.6 times its original length at 30°C, heated with a contact-type hot plate heater at 190°C, shrunk to 0.65 times its original length, and wound at a speed of 600 m / min to obtain a low-shrinkage polytrimethylene terephthalate fiber (sheath yarn). Meanwhile, a conjugate drawn yarn (total fineness 56 dtex / 24 strands, boiling water shrinkage 17%) made by bonding two polyester components (polyethylene terephthalate / polyethylene terephthalate) was prepared as the core yarn.

[0080] Next, the sheath yarn and the core yarn were aligned and interlaced at an overfeed rate of 1.5% in the same manner as in Example 1 to obtain an air-mixed yarn with an entanglement number of 65 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2.

[0081] [Example 4] A polymer was produced in the same manner as in Example 1, and then the resulting polymer was dried in a conventional manner to reduce the water content to 50 ppm. Thereafter, the polymer was melted at 265°C and extruded through a single-layer spinneret having 36 holes with a diameter of 0.27 mm.

[0082] An oil agent was applied to the extruded molten multifilament in the same manner as in Example 1, and then the solid multifilament was wound around a roll heated to 50°C and having a peripheral speed of 3000 m / min, and then wound around a roll heated to 80°C so as to be stretched 1.2 times.Then, using a winder that drives both the spindle and the touch roll, the winding was performed at a winding speed of 3600 m / min, and a cheese-shaped package wound with 56 dtex / 36 filament fibers was obtained.

[0083] The fiber wound on the package was then stretched to 1.3 times at 30°C, heated with a contact-type hot plate heater at 190°C, shrunk to 0.85 times, and wound at a speed of 600 m / min to obtain a low-shrinkage polytrimethylene terephthalate fiber (sheath yarn). Meanwhile, a conjugate drawn yarn (total fineness 33 dtex / 24 strands, boiling water shrinkage 21%) made by bonding polyethylene terephthalate and polytrimethylene terephthalate was prepared as the core yarn.

[0084] Next, the sheath yarn and the core yarn were aligned and interlaced at an overfeed rate of 1.5% in the same manner as in Example 1 to obtain an air-mixed yarn with an entanglement number of 71 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2.

[0085] [Examples 5 and 6] The same procedures as in Example 1 were carried out except that the cross-sectional shape of the sheath yarn and the number of single fibers were changed as shown in Table 1. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2.

[0086] Comparative Example 1 A polymer was produced in the same manner as in Example 1, and then the resulting polymer was dried in a conventional manner to reduce the water content to 50 ppm. The polymer was then melted at 265°C and extruded through a single-layer spinneret having 36 holes with a diameter of 0.27 mm.

[0087] An oil was applied to the extruded molten multifilament in the same manner as in Example 1, and the solid multifilament was then wound around a roll heated to 55°C and having a peripheral speed of 1500 m / min, and then wound around a roll heated to 130°C so as to be drawn 2.1 times, and then wound at a winding speed of 3000 m / min using a winder that drives both the spindle and the touch roll, to obtain a cheese-shaped package wound with a 72 dtex / 36 filament fiber (polytrimethylene terephthalate fiber yarn for sheath yarn). Meanwhile, a polyester (polyethylene terephthalate) drawn yarn (total fineness 56 dtex / 36 filaments, boiling water shrinkage 12%) was prepared as a core yarn.

[0088] Next, the sheath yarn and core yarn were aligned and interlaced at an overfeed rate of 1.5% in the same manner as in Example 1 to obtain an air-mixed yarn with an entanglement number of 65 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2. The obtained air-mixed yarn had a small difference in the core-sheath length and was poor in fluffiness.

[0089] Comparative Example 2 A polymer was produced in the same manner as in Example 1, and then the resulting polymer was dried in a conventional manner to reduce the water content to 50 ppm. The polymer was then melted at 265°C and extruded through a single-layer spinneret having 36 holes, each 0.27 mm in diameter.

[0090] An oil agent was applied to the extruded molten multifilament in the same manner as in Example 1, and then the solid multifilament was wound around a roll heated to 55°C and having a peripheral speed of 1500 m / min, and then wound around a roll heated to 130°C so as to be stretched 2.1 times, and then wound at a winding speed of 3000 m / min using a winder that drives both the spindle and the touch roll, to obtain a cheese-shaped package wound with 56 dtex / 36 filament fibers.

[0091] The fiber wound on the package was then stretched 1.05 times at 30°C, heated with a contact-type hot plate heater at 190°C, shrunk by 0.92 times, and wound at a speed of 600 m / min to obtain a tritrimethylene terephthalate fiber (sheath yarn). Meanwhile, a polyester (polyethylene terephthalate) drawn yarn (total fineness 56 dtex / 36 strands, boiling water shrinkage 10%) was prepared as the core yarn.

[0092] Next, the sheath yarn and core yarn were aligned and interlaced at an overfeed rate of 1.5% in the same manner as in Example 1 to obtain an air-mixed yarn with an entanglement number of 63 / m. The physical properties of the obtained polytrimethylene terephthalate fiber are shown in Table 1, and the physical properties of the mixed yarn are shown in Table 2. The obtained air-mixed yarn had a stiff sheath yarn and was poor in texture.

[0093]

[0094]

[0095] According to the present invention, it is possible to provide a low-shrinkage fiber consisting essentially of polytrimethylene terephthalate, which can be used to produce raw yarn for fabrics having a small heat shrinkage rate and a soft texture, a method for producing the same, an air-mixed yarn containing the polytrimethylene terephthalate fiber, and a fabric made from the same, and therefore the industrial value of the present invention is extremely great.

Claims

1. A polytrimethylene terephthalate fiber, which is composed of 90 mol% or more of trimethylene terephthalate repeating units, characterized in that the boiling water shrinkage rate of the polytrimethylene terephthalate fiber is 5% or less, and the elastic modulus of the polytrimethylene terephthalate fiber at an elongation of 20% is 5 cN / dtex or less.

2. The polytrimethylene terephthalate fiber according to claim 1, which has a birefringence Δn of 0.040 or more and a specific gravity of 1.350 or less.

3. The polytrimethylene terephthalate fiber according to claim 1 or 2, wherein the peak of thermal stress of the polytrimethylene terephthalate fiber exists at 50 to 100° C. and the peak value of the thermal stress is 0.2 cN / dtex or less.

4. The polytrimethylene terephthalate fiber according to claim 1 or 2, which has a breaking strength of 1.5 to 3.5 cN / dtex and a breaking elongation of 30 to 100%.

5. A method for producing polytrimethylene terephthalate fibers, comprising melting and solidifying polytrimethylene terephthalate, which is composed of 90 mol % or more of trimethylene terephthalate repeating units, winding it up at a winding speed of 1,000 m / min or more, stretching it by 1.1 times or more at a temperature below the glass transition point of the polytrimethylene terephthalate, and then shrinking the fiber by 0.5 to 0.9 times while heating it.

6. An air-mixed yarn comprising the polytrimethylene terephthalate fiber according to any one of claims 1 to 4 and a polyester fiber.

7. The air-mixed yarn according to claim 6, wherein the boiling water shrinkage rate of the polyester fiber is 7 to 50%.

8. The air-mixed yarn of claim 6 or 7, which contains modified cross-section fibers.

9. A core-sheath type air-mixed yarn obtained by heat-treating the air-mixed yarn according to claim 6, which is composed of a core yarn and a sheath yarn and has a total fineness of 30 to 400 dtex, the core yarn being made of a polyester fiber, the sheath yarn being made of a polytrimethylene terephthalate fiber having a single fiber fineness of 0.3 to 10 dtex, and the yarn length difference between the core yarn and the sheath yarn, as defined by the method described below, being 5% or more. (Method of measuring yarn length difference) After treating the mixed yarn in boiling water, it was cut to a length of 5 cm under a load of 0.1 cN (0.098 g) × the total fineness (dtex) of the air-mixed yarn, and polyester fiber A (single fiber) and polytrimethylene terephthalate fiber B (single fiber) were taken out from the cut air-mixed yarn and their lengths were measured under a load of 0.1 cN (0.098 g) × the single fiber fineness (dtex), and the yarn length difference (%) was calculated using the following formula: Yarn length difference (%) = (LB - LA) / LA × 100, where LA is the yarn length (cm) of the polyester fiber core yarn, and LB is the yarn length (cm) of the polytrimethylene terephthalate fiber sheath yarn.

10. The sheath-core air-mixed yarn according to claim 9, wherein the weight ratio of the sheath yarn is 50 to 90% of the total weight of the sheath-core air-mixed yarn.

11. The sheath-core air-mixed yarn according to claim 9 or 10, comprising modified cross-section fibers.

12. A fabric comprising the air-mixed yarn of any one of claims 6 to 8.

13. A fabric comprising the sheath-core air-mixed yarn according to any one of claims 9 to 11.

Citation Information

Patent Citations

  • Poly(1,3-propylene terephthalate)

    JP1993262862A

  • High performance brush

    JP1996173244A

  • Production of poly(Trimethylene terephthalate) yarn

    JP1997003724A

  • Polyester fiber and method for producing the same

    JP2001348729A

  • Production of composite processed yarn

    JP1999107081A